Photovoltaic cell with metal net
By using cross-consolidated metal mesh as thin grid lines and main grid lines on photovoltaic cells, the problems of reduced light receiving area and grid breakage in the existing technology are solved, improving power generation efficiency and assembly stability, and reducing costs. .
Patent Information
- Application Number
- CN202420256975.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2034-02-02
AI Technical Summary
The manufacturing process of thin grid lines and main grid lines of existing photovoltaic cells results in a reduction in the light-receiving area of the cells, lower power generation efficiency, and easy disconnection, which increases manufacturing costs.
A metal mesh with cross-consolidation is used, including a first grid line with a width less than 35um and a second grid line with a width greater than 35um. Combined with the interspersed setting of the third grid line, a high-strength and stable metal mesh is formed, which serves as a fine structure for photovoltaic cells. Grid lines and main grid lines to prevent grid breakage and reduce the shading area.
It improves the power generation efficiency of photovoltaic cells, prevents grid breakage, reduces manufacturing costs, and enhances the stability and ease of assembly.
Smart Images

Figure CN221928097U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the field of photovoltaic cells, in particular to a photovoltaic cell with a metal mesh. Background Art
[0002] Photovoltaic cells are products that absorb sunlight and convert solar radiation energy directly or indirectly into electrical energy through photoelectric effect or photochemical effect. At present, in the process of photovoltaic cell power generation, it is necessary to set main grid lines and fine grid lines on the photovoltaic cell. The function of the fine grid lines is to realize the convergence of the current generated by the photovoltaic cell, and the function of the main grid lines is to realize the output of the current. The manufacturing process of the main grid lines and fine grid lines is usually achieved by printing silver paste on the photovoltaic cell by screen printing. However, the width of the fine grid lines manufactured by this process is usually 20~28μm, or even 25-35um. Therefore, the main grid lines and fine grid lines set by this process will reduce the light receiving area of the photovoltaic cell, thereby affecting the power generation efficiency of the photovoltaic cell. In addition, the grid lines formed by the screen printing process are easy to disconnect (i.e., broken grid), which greatly affects the derivation of current. At the same time, the main component of silver paste is silver powder. Due to the precious metal properties and processing particle size requirements, as well as specific requirements for fluid storage and transportation of silver powder, the price of silver powder remains high, which restricts the manufacturing cost of photovoltaic cells and makes it difficult to reduce the manufacturing cost of photovoltaic cells.
[0003] In view of the existence of the above problems, it is necessary to study a photovoltaic cell with a metal mesh, which has a small shading area for the cell body and can effectively prevent the problem of broken grid. Utility Model Content
[0004] The utility model aims to provide a photovoltaic cell sheet with a metal mesh, which has a small light-shielding area for the cell sheet body and can effectively prevent the problem of grid breakage.
[0005] In order to achieve the above purpose, the solution of the utility model is:
[0006] A photovoltaic cell with a metal mesh comprises a cell body and a metal mesh fixedly fitted on the cell body; the metal mesh comprises a first grid line and a second grid line that are cross-fixed and fixed together, the number density of the first grid lines is 5 to 15 grid lines / cm, and the number density of the second grid lines is 0.2 to 4 grid lines / cm; the shading rate of the metal mesh to the cell body is less than or equal to 6%.
[0007] The metal mesh is a copper mesh, a silver mesh, an aluminum mesh, a nickel mesh or an alloy metal mesh.
[0008] The surface of the metal mesh is plated with a coating.
[0009] The coating is a silver coating, a tin coating or a nickel coating; the metal mesh is a copper mesh, a silver mesh, an aluminum mesh, a nickel mesh or an alloy metal mesh.
[0010] The width of the first grid line of the metal mesh is less than or equal to 35 um.
[0011] The width of the first grid line of the metal mesh is less than or equal to 20 um.
[0012] The width of the second grid line of the metal mesh is greater than 35 um.
[0013] The shading rate of the metal mesh to the battery cell body is ≤4%.
[0014] The metal mesh also includes at least one third grid line with a width greater than that of the first grid lines, and the third grid lines are interspersed between the first grid lines; and when the number of the third grid lines of the metal mesh is greater than or equal to two, at least one first grid line is spaced between adjacent third grid lines.
[0015] When the number of the third grid lines of the metal mesh is greater than or equal to two, the widths of the third grid lines of the metal mesh are the same, completely different, or not exactly the same.
[0016] The metal mesh further includes a metal frame with a width greater than or equal to 200 um, and the metal frame is fixedly connected to each first grid line and each second grid line.
[0017] After adopting the above scheme, the utility model cooperates with a metal mesh on the battery cell body, and the metal mesh includes a first grid line and a second grid line that are cross-connected and solidified together; wherein, the first grid line of the metal mesh can be used as a fine grid line of the photovoltaic battery cell, and the fine grid line mainly plays the role of collecting photogenerated carriers, which can enhance the light absorption capacity of the battery cell surface, improve the utilization rate of sunlight, and thus improve the efficiency of the battery; and the second grid line of the metal mesh can be used as a main grid line of the photovoltaic battery cell, and the main grid line mainly plays the role of collecting current, and can concentrate the current to the output end of the photovoltaic battery cell, and is a bridge connecting the photovoltaic battery cell and the output wire.
[0018] In the utility model, the first grid line and the second grid line of the metal mesh are cross-connected and fixed together, so that the first grid line and the second grid line of the metal mesh have high strength and good stability, which can effectively prevent the problem of broken grids in the photovoltaic cell with a metal mesh of the utility model during installation and use; and the metal mesh has a certain strength, which makes assembly easier. In addition, compared with the solution of using only metal wire as a thin grid line, the metal mesh of the utility model can meet the assembly requirements while the width of the first grid line of the metal mesh can be smaller, so that the metal mesh can block a small area of the cell body, which helps to improve the power generation efficiency of the photovoltaic cell with a metal mesh of the utility model. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The manufacturing method of the photovoltaic cell of the first embodiment of the utility model is shown in FIG. Figure 1 ;
[0020] Figure 2 The manufacturing method of the photovoltaic cell of the first embodiment of the utility model is shown in FIG. Figure 2 ;
[0021] Figure 3 The structure of the photovoltaic cell of the first embodiment of the utility model is shown in FIG. Figure 1 ;
[0022] Figure 4 The structure of the photovoltaic cell of the first embodiment of the utility model is shown in FIG. Figure 2 ;
[0023] Figure 5 This is a schematic diagram of manufacturing a photovoltaic cell sheet according to the second embodiment of the present utility model;
[0024] Figure 6 Schematic diagram of the combination of the metal mesh and the mixture of silver powder and glass powder in the second embodiment of the present utility model Figure 1 ;
[0025] Figure 7 Schematic diagram of the combination of the metal mesh and the mixture of silver powder and glass powder in the second embodiment of the present utility model Figure 2 ;
[0026] Figure 8 This is a schematic diagram of the structure of a photovoltaic cell sheet according to the second embodiment of the present utility model;
[0027] Fig. 9 This is a schematic diagram of manufacturing a photovoltaic cell sheet according to the third embodiment of the present utility model;
[0028] Fig.10 This is a schematic diagram of manufacturing a photovoltaic cell sheet according to the fourth embodiment of the present utility model;
[0029] Fig.11 This is a schematic structural diagram of a photovoltaic cell sheet according to a fourth embodiment of the present utility model;
[0030] Fig.12 This is a schematic diagram of manufacturing a photovoltaic cell sheet according to the fifth embodiment of the present utility model;
[0031] Fig.13 This is a schematic diagram of the structure of a photovoltaic cell sheet according to Embodiment 5 of the present utility model;
[0032] Fig.14 This is a schematic structural diagram of a photovoltaic cell sheet according to a sixth embodiment of the present utility model;
[0033] Fig.15 It is a cross-sectional view of a photovoltaic cell sheet according to the sixth embodiment of the utility model;
[0034] Fig.16 This is a schematic diagram of manufacturing a photovoltaic cell sheet according to the sixth embodiment of the utility model;
[0035] Fig.17 This is a schematic diagram of the structure of a photovoltaic cell sheet according to Embodiment 7 of the present utility model;
[0036] Fig.18 This is a schematic structural diagram of a photovoltaic cell sheet according to an eighth embodiment of the present utility model;
[0037] Fig.19 This is a schematic diagram of manufacturing a photovoltaic cell sheet according to Embodiment 9 of the present utility model;
[0038] Fig. 20 This is a schematic diagram of manufacturing a photovoltaic cell sheet according to the tenth embodiment of the utility model;
[0039] Fig.21 This is a schematic diagram of manufacturing a photovoltaic cell according to the eleventh embodiment of the utility model.
[0040] Specific implementation number description:
[0041] A photovoltaic cell sheet a having a metal mesh,
[0042] Battery cell body 1,
[0043] Metal mesh 2, first grid line 21, second grid line 22, third grid line 23, metal frame 24,
[0044] Silver powder and glass powder mixture 3, silver powder and glass powder sintered product 3',
[0045] Glass powder 4,
[0046] Thermoplastic resin 5, transparent photovoltaic film 5',
[0047] Conductive glue 6,
[0048] Pressing roller A. DETAILED DESCRIPTION
[0049] like Figures 1 to 21As shown, the utility model discloses a photovoltaic cell a with a metal mesh, which includes a cell body 1 and a metal mesh 2 fixedly matched on the cell body 1; the metal mesh 2 includes a first grid line 21 and a second grid line 22 that are mutually crossed and fixed together; the width of the first grid line 21 of the metal mesh 2 is less than or equal to 35um, and the number density of the first grid line 21 is 5 to 15 lines / cm; the width of the second grid line 22 of the metal mesh 2 is greater than 35um, and the number density of the second grid line 22 is 0.2 to 4 lines / cm; the light shielding rate of the metal mesh 2 to the cell body 1 is less than or equal to 6%. Among them, the number density is the number of first grid lines 21 or second grid lines 22 per centimeter on the cell body 1.
[0050] In the present invention, the metal mesh 2 is used as the fine grid line and the main grid line of the photovoltaic cell (wherein the first grid line 21 is used as the fine grid line and the second grid line 22 is used as the main grid line), which can collect photogenerated carriers and collect current. The first grid line 21 and the second grid line 22 in the metal mesh 2 are cross-connected and solidified together, and the first grid line 21 and the second grid line 22 of the metal mesh 2 have high strength and good stability, which can effectively prevent the problem of grid breakage in the photovoltaic cell a with a metal mesh of the present invention during installation and use; and the metal mesh 2 has a certain strength, and it is easier to assemble; in addition, compared with the solution of using only metal wire as a fine grid line, the metal mesh 2 of the present invention can meet the assembly requirements while the width of the first grid line 21 of the metal mesh 2 can be smaller, so that the metal mesh 2 can block a small area of the cell body 1, which helps to improve the power generation efficiency of the metal mesh a of the present invention.
[0051] In the utility model, the metal mesh 2 can be a copper mesh, a silver mesh, an aluminum mesh, a nickel mesh or an alloy metal mesh, and the surface of the metal mesh 2 can be plated with a coating as required, and the coating can be a silver coating, a tin coating or a nickel coating. The cross-section of the first grid lines 21 and the second grid lines 22 in the metal mesh 2 can be circular, elliptical, triangular or polygonal, and the shape is not limited. The multiple first grid lines 21 or the multiple second grid lines 22 can be distributed in parallel with each other, or can be distributed crosswise with each other.
[0052] The method for measuring the width of the grid line (the first grid line 21 or the first grid line 22 or the third grid line 23 described below) of the metal mesh 2 is: use an ultra-depth of field 3D digital microscope (the model can be Keyence VHX-6000) to photograph the metal mesh 2, and then use the measurement software of the ultra-depth of field 3D digital microscope to measure the image of the metal mesh 2, measure the maximum width of a single grid line in the metal mesh 2 as the width of the grid line, measure 5 groups, and average the measured widths of the grid lines to obtain the width W of the grid lines.
[0053] The method for measuring the shading rate of the metal mesh 2 to the battery cell body 1 is: use an ultra-depth of field 3D digital microscope (the model may be KEYENCE VHX-6000) to measure the area S1 of the portion of the metal mesh 2 covering the battery cell body 1 and the area S2 of the battery cell body 1, and then calculate the shading rate f of the metal mesh 2 to the battery cell body 1 according to the formula f=S1 / S2·100%.
[0054] In order to further explain the technical solution of the present utility model, the present utility model is described in detail below through specific embodiments.
[0055] Embodiment 1:
[0056] Cooperate Figure 1 , Figure 2 , Figure 3 and Figure 4 As shown, in the first embodiment of the present invention, a method for manufacturing a photovoltaic cell sheet a having a metal mesh of the present invention comprises:
[0057] First, the metal mesh 2 is unwound by an unwinding device and laid on the surface of the battery cell body 1. While the metal mesh 2 is laid on the surface of the battery cell body 1, the contact between the metal mesh 2 and the battery cell body 1 is irradiated by laser, so that the contact between the metal mesh 2 and the battery cell body 1 is melted;
[0058] Then, the metal mesh is pressed by the pressing roller A so that the metal mesh is pressed against the battery cell body;
[0059] Finally, the redundant part of the metal mesh 2 is cut off, thereby forming a photovoltaic cell sheet a with a metal mesh of the utility model.
[0060] In the first embodiment of the present invention, the metal mesh 2 is laser welded to the battery cell body 1, and the metal mesh 2 is squeezed by the pressure roller A, which can effectively ensure that the metal mesh 2 and the battery cell body 1 are firmly welded, so that the metal mesh 2 is firmly fitted to the battery cell body 1.
[0061] In the first embodiment of the present invention, the metal mesh 2 includes first grid lines 21 and second grid lines 22 that are intersected and fixed together. The plurality of first grid lines 21 may be distributed parallel to each other (eg, Figure 3 As shown in FIG. 1 ), the plurality of first gate lines 21 may also be arranged crosswise with each other (eg Figure 4 As shown); similarly, the plurality of second grid lines 22 may also be parallel to each other or cross each other. In addition, the utility model can unwind the metal mesh 2 and lay it on the surface of the battery cell body 1 through the unwinding device, and can cut off the excess part of the metal mesh 2 after the metal mesh 2 is pressed with the battery cell body 1, so that the utility model can continuously unwind the whole roll of the metal mesh 2 to achieve continuous production.
[0062] In Example 1 of the utility model, the parameters of a photovoltaic cell a with a metal mesh of the utility model are: the width of the first grid line 21 is 20um, and the number density of the first grid line 21 is 5 lines / cm; the width of the second grid line 22 is 80um, and the number density of the second grid line 22 is 4 lines / cm; the shading rate of the metal mesh 2 to the cell body 1 is 4.2%.
[0063] Embodiment 2:
[0064] Cooperate Figure 5 , Figure 6 , Figure 7 and Figure 8 As shown, in the second embodiment of the present invention, a method for manufacturing a photovoltaic cell sheet a having a metal mesh of the present invention comprises:
[0065] First, the whole roll of the metal mesh 2 is unwound by an unwinding device, and at the same time, the silver powder and glass powder mixture 3 placed in the melt tank is melted and then coated on the entire or partial surface of the metal mesh 2 by a transfer roller; the silver powder and glass powder mixture 3 refers to a mixture of silver powder and glass powder;
[0066] Then, a metal mesh 2 whose surface is fully or partially coated with a mixture of silver powder and glass powder 3 is laid on the surface of the battery cell body 1, and the silver powder and glass powder mixture 3 coated on the surface of the metal mesh 2 is melted at the contact point between the metal mesh 2 and the battery cell body 1 by heating;
[0067] Next, the metal mesh 2 is pressed by the pressing roller A so that the metal mesh 2 is pressed together with the battery cell body 1; at the same time, the melted silver powder and glass powder mixture 3 is solidified to form a silver powder and glass powder sintered material 3' located between the metal mesh 2 and the battery cell body 1;
[0068] Finally, the redundant part of the metal mesh 2 is cut off, so as to form a photovoltaic cell sheet a with a metal mesh according to the utility model, and a silver powder and glass powder sintered material 3 ′ is provided between the metal mesh 2 and the cell sheet body 1 .
[0069] In the second embodiment of the utility model, the heating method can be laser heating or oven heating. Through heating, the silver powder and glass powder mixture 3 that is fully or partially coated on the surface of the metal mesh 2 is melted, so that the silver in the silver powder and glass powder mixture 3 begins to diffuse into the silicon matrix inside the battery cell body 1 and contacts with the PN junction inside the battery cell body 1, so that a good ohmic contact is formed between the metal mesh 2 and the battery cell body 1, thereby reducing the contact resistance and improving the conversion efficiency and stability of the photovoltaic cell. At the same time, the glass powder in the silver powder and glass powder mixture 3 will fill the gaps between the silver powder after melting, thereby increasing the stability and conductivity of the first grid line 21 and the second grid line 22 of the metal mesh 2 and the battery cell body 1.
[0070] In the second embodiment of the present invention, the parameters of a photovoltaic cell a with a metal mesh of the present invention are: the width of the first grid line 21 is 35um, and the number density of the first grid line 21 is 10 lines / cm; the width of the second grid line 22 is 60um, and the number density of the second grid line 22 is 2 lines / cm; the shading rate of the metal mesh 2 to the cell body 1 is 4.6%.
[0071] Embodiment three:
[0072] Cooperate Fig. 9 As shown, in the third embodiment of the present invention, a method for manufacturing a photovoltaic cell sheet a having a metal mesh of the present invention comprises:
[0073] First, the silver powder and glass powder mixture 3 is distributed on the entire cell body 1 or only on the portion of the cell body 1 that is in contact with the metal mesh 2;
[0074] Then, the whole roll of metal mesh 2 is unwound by an unwinding device and laid on the surface of the battery cell body 1, and the silver powder and glass powder mixture 3 is melted by heating;
[0075] Next, the metal mesh 2 is pressed by the pressing roller A so that the metal mesh 2 is pressed together with the battery cell body 1; at the same time, the melted silver powder and glass powder mixture 3 is solidified to form a silver powder and glass powder sintered material 3' located between the metal mesh 2 and the battery cell body 1;
[0076] Finally, the excess part of the metal mesh 2 is cut off and the excess silver powder and glass powder mixture 3 is removed by a suction device, thereby forming a photovoltaic cell a with a metal mesh of the utility model, and a silver powder and glass powder sintered material 3' is present between the metal mesh 2 and the cell body 1.
[0077] In the third embodiment of the present invention, the heating can be laser heating or oven heating. Through heating, the silver powder in the silver powder and glass powder mixture 3 begins to melt and diffuse into the silicon matrix inside the cell body 1, and contacts the PN junction inside the cell body 1, so that a good ohmic contact is formed between the metal mesh 2 and the cell body 1, thereby reducing the contact resistance and improving the conversion efficiency and stability of the photovoltaic cell. In addition, the metal mesh 2 does not need to be surface coated. The metal mesh 2 can be a copper mesh, a silver mesh or an alloy metal mesh. The surface of the metal mesh 2 can be plated with a coating as needed, and the coating can be a silver coating, a tin coating or a nickel coating.
[0078] In the third embodiment of the utility model, the parameters of a photovoltaic cell a with a metal mesh of the utility model are: the width of the first grid line 21 is 16um, and the number density of the first grid line 21 is 8 lines / cm; the width of the second grid line 22 is 50um, and the number density of the second grid line 22 is 3 lines / cm; the shading rate of the metal mesh 2 to the cell body 1 is 2.8%.
[0079] Embodiment 4:
[0080] Cooperate Fig.10 and Fig.11 As shown, in the fourth embodiment of the present invention, a method for manufacturing a photovoltaic cell sheet a having a metal mesh of the present invention comprises:
[0081] First, the whole roll of metal mesh 2 is unrolled by an unwinding device and laid on the surface of the battery cell body 1;
[0082] Then, glass powder 4 is added between the metal mesh 2 and the battery cell body 1, and laser heating or oven heating is performed to melt the glass powder 4 between the metal mesh 2 and the battery cell body 1;
[0083] Next, the metal mesh 2 is pressed by the pressing roller A so that the metal mesh 2 is pressed together with the battery cell body 1;
[0084] Finally, the redundant part of the metal mesh 2 is cut off, thereby forming a photovoltaic cell sheet a with a metal mesh of the utility model.
[0085] In the fourth embodiment of the utility model, the added glass powder 4 melts at the contact point between the metal mesh 2 and the battery cell body 1, and the melted glass powder 4 can fill the gap between the metal mesh 2 and the battery cell body 1, so that the metal mesh 2 and the battery cell body 1 form a good contact, and effectively prevent the metal mesh 2 and the battery cell body 1 from delamination; wherein, the first grid line 21 of the metal mesh 2 plays the role of a fine grid line, and the second grid line 22 of the metal mesh 2 plays the role of a main grid line, thereby also increasing the stability and conductivity of the grid line.
[0086] In the fourth embodiment of the utility model, the parameters of a photovoltaic cell a with a metal mesh of the utility model are: the width of the first grid line 21 is 15um, and the number density of the first grid line 21 is 12 lines / cm; the width of the second grid line 22 is 70um, and the number density of the second grid line 22 is 1 line / cm; the shading rate of the metal mesh 2 is 2.5%.
[0087] Embodiment five:
[0088] Cooperate Fig.12 and Fig.13 As shown, in the fifth embodiment of the present invention, a method for manufacturing a photovoltaic cell sheet a having a metal mesh of the present invention comprises:
[0089] First, the whole roll of metal mesh 2 is unrolled by an unwinding device and laid on the surface of the battery cell body 1;
[0090] Then, glass powder 4 is added to the surface of the metal mesh 2, and is heated in an oven or by laser, so that the glass powder 4 is melted and coated on the surface of the metal mesh 2;
[0091] Next, the metal mesh 2 is pressed by the pressing roller A so that the metal mesh 2 is pressed together with the battery cell body 1;
[0092] Finally, the redundant part of the metal mesh 2 is cut off, thereby forming a photovoltaic cell sheet a with a metal mesh of the utility model.
[0093] In the fifth embodiment of the present invention, since the glass powder 4 is added to the surface of the metal mesh 2, the heated and melted glass powder 4 can wrap the metal mesh 2 and then adhere and fix it to the battery cell body 1. Since the glass powder 4 is transparent after solidification, it can wrap the metal mesh 2 and make the metal mesh 2 not easily oxidized to improve the stability of the photovoltaic battery cell a with a metal mesh of the present invention, and will not affect the shading rate and conductivity of the photovoltaic battery cell a with a metal mesh of the present invention.
[0094] In the fifth embodiment of the present invention, the parameters of a photovoltaic cell a with a metal mesh of the present invention are: the width of the first grid line 21 is 30um, and the number density of the first grid line 21 is 15 lines / cm; the width of the second grid line 22 is 120um, and the number density of the second grid line 22 is 0.2 lines / cm; the shading rate of the metal mesh 2 to the cell body 1 is 4.8%.
[0095] Embodiment six:
[0096] Cooperate Fig.14 , Fig.15 and Fig.16 As shown, in the sixth embodiment of the present invention, a method for manufacturing a photovoltaic cell sheet a having a metal mesh of the present invention comprises:
[0097] First, the whole roll of metal mesh 2 is unrolled by an unwinding device and laid on the surface of the battery cell body 1;
[0098] Then, the molten thermoplastic resin 5 is melt-extruded and pressed onto the surface of the cell body 1 by a pressing roller A. After the thermoplastic resin 5 is cooled, a transparent photovoltaic film 5' covering the metal mesh 2 is formed, that is, the metal mesh 2 is pressed onto the cell body 1 through the transparent photovoltaic film 5'.
[0099] Finally, the redundant parts of the metal mesh 2 and the transparent photovoltaic film 5' are cut off, thereby forming a photovoltaic cell sheet a with a metal mesh of the utility model.
[0100] In the sixth embodiment of the present invention, a photovoltaic cell a with a metal mesh of the present invention also includes a transparent photovoltaic film 5' connected to the surface of the cell body 1. The transparent photovoltaic film 5' covers the metal mesh 2 and fixes the metal mesh 2 to the surface of the cell body 1, which can effectively prevent the metal mesh 2 from falling off; at the same time, the transparent photovoltaic film 5' can also effectively protect the metal mesh 2, prevent the metal mesh 2 from being directly in contact with the external environment and oxidized, thereby increasing the service life of the photovoltaic cell a. The material of the transparent photovoltaic film 5' can be EVA or POE. The transparent photovoltaic film 5' can completely cover the metal mesh 2 or partially cover the metal mesh 2. The transparent photovoltaic film 5' partially covering the metal mesh 2 can effectively reduce the material used for the transparent photovoltaic film 5' and reduce costs.
[0101] Embodiment seven:
[0102] Cooperate Fig.17 As shown, in the seventh embodiment of the present invention, a photovoltaic cell a with a metal mesh of the present invention comprises a cell body 1 and a metal mesh 2 fixedly matched on the cell body 1, the metal mesh 2 comprises a first grid line 21 and a second grid line 22 intersecting and consolidating each other, the first grid line 21 is used to collect current and acts as a fine grid line, and the second grid line 22 is used to collect current and acts as a main grid line; the metal mesh 2 also comprises at least one third grid line 23 interspersed between the first grid lines 21 and having a width greater than the first grid line 21; when the number of the third grid lines of the metal mesh is greater than or equal to two, at least one first grid line 21 is spaced between adjacent third grid lines 23. The metal mesh 2 can be fixed to the surface of the cell body 1 by gluing, spot welding, laser heating, and the manufacturing methods in the above-mentioned embodiments 1 to 6.
[0103] In the seventh embodiment of the present invention, the third grid line 23 is thicker than the first grid line 21, that is, the metal mesh 2 has grid lines of different thicknesses, and the widths of the plurality of third grid lines 23 may be the same or completely different or not exactly the same. The plurality of thicker third grid lines 23 of the metal mesh 2 may effectively improve the strength of the metal mesh 2, prevent the photovoltaic cell piece a with a metal mesh of the present invention from being broken during assembly and use, and make the assembly of the photovoltaic cell piece a with a metal mesh of the present invention easier.
[0104] Embodiment eight:
[0105] Cooperate Fig.18 As shown, in the eighth embodiment of the present invention, a photovoltaic cell a with a metal mesh of the present invention comprises a cell body 1 and a metal mesh 2 fixedly fitted on the cell body 1, the metal mesh 2 comprises a first grid line 21 and a second grid line 22 which are cross-fixed together, the first grid line 21 is used to collect current and acts as a fine grid line, the second grid line 22 is used to collect current and acts as a main grid line; the metal mesh 2 also comprises a metal frame 24 with a width greater than or equal to 200um, the metal frame 24 is fixedly connected to each first grid line 21 and each second grid line 22; the metal mesh 2 can be fixed to the surface of the cell body 1 by gluing, spot welding, laser heating and the manufacturing methods in the above-mentioned embodiments one to six.
[0106] The metal frame 24 in the eighth embodiment of the utility model can improve the strength and stiffness of the metal mesh 2, and effectively reduce the risk of the first grid line 21 and the second grid line 22 of the metal mesh 2 being broken by external forces during the assembly and use of the photovoltaic cell piece a with a metal mesh of the utility model, making the photovoltaic cell piece a with a metal mesh of the utility model easier to assemble.
[0107] Embodiment nine:
[0108] Cooperate Fig.19 As shown, in the ninth embodiment of the present invention, a method for manufacturing a photovoltaic cell a with a metal mesh of the present invention comprises: first, coating the metal mesh 2 with a conductive adhesive 6; then, laying the metal mesh 2 on the surface of the cell body 1; finally, waiting for the conductive adhesive 6 to solidify, so that the metal mesh 2 and the cell body 1 are glued and fixed together.
[0109] Embodiment ten:
[0110] Cooperate Fig. 20As shown, in the tenth embodiment of the present invention, a manufacturing method of a photovoltaic cell a with a metal mesh of the present invention includes: first, coating a conductive adhesive 6 on the surface of the cell body 1 corresponding to the layout position of the metal mesh 2; then, laying the metal mesh 2 on the surface of the cell body 1; finally, waiting for the conductive adhesive 6 to solidify, so that the metal mesh 2 and the cell body 1 are glued and fixed together.
[0111] Embodiment eleven:
[0112] Cooperate Fig.21 As shown, in the eleventh embodiment of the present invention, a method for manufacturing a photovoltaic cell a with a metal mesh of the present invention comprises: first, laying the metal mesh 2 on the surface of the cell body 1; then, welding the metal mesh 2 to the cell body 1 by spot welding.
[0113] The above embodiments and drawings do not limit the product form and style of the present utility model. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present utility model.
Claims
1. A photovoltaic cell with a metal mesh, characterized in that: It includes a battery cell body and a metal mesh fixedly matched to the battery cell body; The metal mesh includes first grid lines and second grid lines that are cross-connected and solidified with each other, the number density of the first grid lines is 5-15 / cm, and the number density of the second grid lines is 0.2-4 / cm; the shading rate of the metal mesh to the battery cell body is less than or equal to 6%.
2. A photovoltaic cell with a metal mesh as claimed in claim 1, characterized in that: The metal mesh is a copper mesh, a silver mesh, an aluminum mesh, a nickel mesh or an alloy metal mesh.
3. A photovoltaic cell with a metal mesh as claimed in claim 1, characterized in that: The surface of the metal mesh is plated with a coating.
4. A photovoltaic cell with a metal mesh as claimed in claim 3, characterized in that: The coating is a silver coating, a tin coating or a nickel coating; the metal mesh is a copper mesh, a silver mesh, an aluminum mesh, a nickel mesh or an alloy metal mesh.
5. The photovoltaic cell with a metal mesh according to claim 1, characterized in that: The width of the first grid line of the metal mesh is less than or equal to 35 um.
6. The photovoltaic cell with a metal mesh according to claim 1, characterized in that: The width of the first grid line of the metal mesh is less than or equal to 20 um.
7. The photovoltaic cell with a metal mesh according to claim 1, characterized in that: The width of the second grid line of the metal mesh is greater than 35 um.
8. The photovoltaic cell with a metal mesh according to claim 1, characterized in that: The shading rate of the metal mesh to the battery cell body is ≤4%.
9. The photovoltaic cell with a metal mesh according to claim 1, characterized in that: The metal mesh also includes at least one third grid line with a width greater than that of the first grid lines, and the third grid lines are interspersed between the first grid lines; and when the number of the third grid lines of the metal mesh is greater than or equal to two, at least one first grid line is spaced between adjacent third grid lines.
10. A photovoltaic cell with a metal mesh as claimed in claim 9, characterized in that: When the number of the third grid lines of the metal mesh is greater than or equal to two, the widths of the third grid lines of the metal mesh are the same, completely different, or not exactly the same.
11. The photovoltaic cell with a metal mesh according to claim 1, characterized in that: The metal mesh further includes a metal frame with a width greater than or equal to 200 um, and the metal frame is fixedly connected to each first grid line and each second grid line.