Semiconductor device

By forming an inert oxide layer and a migration barrier layer in the aluminum structure, the problem of hollow formation in the aluminum structure after thermal cycling is solved, and the performance and reliability of the semiconductor device are improved.

CN221947155UActive Publication Date: 2024-11-01TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420434337.2
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Priority Date
2023-03-07
Filing Date
2024-03-06
Publication Date
2024-11-01
Estimated Expiration
2034-03-06

AI Technical Summary

Technical Problem

In the semiconductor manufacturing process, aluminum structures are prone to hollows after thermal cycling, resulting in a decrease in yield and an increase in reliability risk, especially in small-width aluminum structures, which leads to serious hollows.

Method used

By forming inert alumina, aluminum nitride or aluminum nitride between the aluminum layers, the formation of voids is reduced and vacuum breaking or plasma treatment is performed in the aluminum deposition process to form a migration barrier layer, separating multiple aluminum layers to alleviate electromigration and stress migration.

Benefits of technology

It effectively reduces the formation of voids, improves the performance and thermal stability of semiconductor devices, and reduces the risk of electromigration and stress migration failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221947155U_ABST
    Figure CN221947155U_ABST
Patent Text Reader

Abstract

A semiconductor device having an aluminum structure is provided. An example apparatus includes an interconnect structure and an aluminum structure electrically connected to the interconnect structure. The aluminum structure includes a first aluminum layer, a migration barrier layer over the first aluminum layer, and a second aluminum layer over the migration barrier layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present disclosure generally relate to a semiconductor device and a method of manufacturing the same, and more particularly to an aluminum structure and a method of manufacturing the same. Background Art

[0002] The semiconductor industry has experienced rapid growth due to the continuous improvement in the integration density of various electronic components (such as transistors, diodes, resistors, capacitors, etc.). In most cases, the increase in integration density comes from the iterative reduction of the minimum feature size, allowing more components to be integrated into a specific area. However, such scaling also increases the complexity of semiconductor manufacturing processes. Therefore, the continuous advancement of semiconductor ICs and devices requires the advancement of semiconductor manufacturing processes and technologies. Utility Model Content

[0003] The present disclosure aims to provide a semiconductor device, comprising: an interconnect structure and an aluminum structure. The aluminum structure is electrically connected to the interconnect structure, and wherein the aluminum structure comprises: a first aluminum layer; a migration barrier layer disposed above the first aluminum layer; and a second aluminum layer disposed above the migration barrier layer.

[0004] Another object of the present disclosure is to provide a semiconductor device, comprising: an interconnect structure, a first aluminum layer disposed above the interconnect structure, a ceramic layer directly above the first aluminum layer, and a second aluminum layer directly above the ceramic layer.

[0005] Another object of the present disclosure is to provide a semiconductor device, comprising: a first aluminum layer, a second aluminum layer, a migration barrier layer, and a conductive structure. The second aluminum layer is disposed above the first aluminum layer. The migration barrier layer is disposed between the first aluminum layer and the second aluminum layer. The conductive structure is electrically connected to the first aluminum layer, the second aluminum layer, and the migration barrier layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] The aspects of the present disclosure will be better understood from the following detailed description in conjunction with the accompanying drawings. It should be noted that, in accordance with standard industry practice, the features are not drawn to scale. In fact, the dimensions of the features may be arbitrarily increased or decreased to make the discussion clearer.

[0007] Figure 1 is a flowchart illustrating a method according to some embodiments;

[0008] Figures 2 to 10 According to some embodiments, Figure 1 a cross-sectional view of a device during a continuous manufacturing stage of the method;

[0009] Figure 11 to Figure 12 According to some embodiments, Fig. 9A focused cross-sectional view of the aluminum structure;

[0010] Figures 13 to 15 is a focused cross-sectional view illustrating an alternative aluminum structure, according to some embodiments.

[0011]

Explanation of symbols

[0012] 10: Methods

[0013] 40: Conductive structure

[0014] 41: Upper surface

[0015] 45: uncovered part

[0016] 50: Dielectric layer

[0017] 51: Dielectric segment

[0018] 60: Metal Diffusion Barrier

[0019] 70: Coating

[0020] 80:Mask

[0021] 81: Holes

[0022] 90: Dielectric layer, protective layer

[0023] 91: Upper surface

[0024] 100: Aluminum structure

[0025] 101: Wire

[0026] 102:Through hole

[0027] 108: Plane

[0028] 109: Side wall

[0029] 110: Aluminum, (first) aluminum layer

[0030] 111: Upper surface

[0031] 112: The rest

[0032] 119: Horizontal edge

[0033] 120: Aluminum, (second) aluminum layer

[0034] 121: Upper surface

[0035] 129: Horizontal edge

[0036] 130: (first) migration barrier layer

[0037] 138: Gap

[0038] 139: Horizontal edge

[0039] 140: (Second) Migration Barrier Layer

[0040] 150: Aluminum, (third) aluminum layer

[0041] 160: (Third) Migration Barrier Layer

[0042] 200:Semiconductor devices

[0043] 230,240: Conductive pads

[0044] 250:Solder bump

[0045] 260: Integrated Circuit Die

[0046] T:Thickness

[0047] T1, T2, T3, Tb: thickness

[0048] W1,W9: Width DETAILED DESCRIPTION

[0049] The following disclosure provides many different embodiments or examples to implement different features of the subject matter provided. The specific examples of components and arrangements described below are intended to simplify the disclosure. Of course, these are only examples and are not intended to be limiting. For example, in the following description, a first feature is formed on or above a second feature, which may include an embodiment in which the first feature and the second feature are formed in direct contact, and may also include an embodiment in which additional features may be formed between the first feature and the second feature, so that the first and second features may not be in direct contact. In addition, the disclosure may repeat reference numbers and / or letters in each embodiment. Such repetition is for the purpose of simplicity and clarity, and is not itself intended to limit the relationship between the various embodiments and / or configurations discussed.

[0050] Additionally, spatially relative terms such as "over," "overlying," "above," "upper," "top," "under," "underlying," "beneath," "below," "lower," "bottom," "side" and the like may be used herein to describe the relationship of one element or component to another element(s) or component(s) as illustrated in the accompanying drawings. These spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be oriented in various ways (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should be interpreted accordingly.

[0051] In certain specific embodiments herein, a "layer of material" is a layer comprising at least 50% by weight of a determined material, such as at least 60% by weight of a determined material, at least 75% by weight of a determined material, at least 90% by weight of a determined material, at least 95% by weight of a determined material, at least 99% by weight of a determined material; and a layer of "material" comprises at least 50% by weight of a determined material, such as at least 60% by weight of a determined material, at least 75% by weight of a determined material, at least 90% by weight of a determined material, at least 95% by weight of a determined material, or at least 99% by weight of a determined material. For example, in certain embodiments, each of an aluminum layer and a layer of aluminum is a layer of at least 50% by weight, at least 60% by weight, at least 75% by weight, at least 90% by weight, at least 95% by weight, or at least 99% by weight of aluminum.

[0052] For the sake of brevity, conventional techniques associated with conventional semiconductor device manufacturing may not be described in detail herein. In addition, the various operations and processes described herein may be incorporated into additional functions, more comprehensive procedures or processes that are not described in detail herein. In particular, many processes are well known in the manufacture of semiconductor devices, so for the sake of brevity, many conventional processes will only be briefly mentioned here, or will be omitted entirely without providing well-known process details. As will be apparent to those skilled in the art after a complete reading of the contents of this disclosure, the structures disclosed herein can be used in conjunction with a variety of technologies and can be incorporated into various semiconductor devices and products. In addition, it should be noted that the semiconductor device structure includes different numbers of components, and a single component shown in the accompanying drawings may represent multiple components.

[0053] It should be noted that the present disclosure provides certain embodiments of aluminum structures in the form of conductive lines and / or conductive vias. In addition, certain embodiments of aluminum structures are in the form of aluminum pads for use as under-bump metallization (UBM) and final back-end-of-the-line (BEOL) interconnect layers under the bumps. However, the embodiments herein are not limited thereto.

[0054] Vacancies diffuse through aluminum, which may result in the formation of voids in the aluminum. For example, vacancies may diffuse through thermally induced stress gradients. It has been found that aluminum structures may develop voids after thermal cycling. For example, significant voids were observed when subjected to 300 thermal cycles between -65°C and 150°C. Any aluminum void increases the risk of yield degradation and reliability, for example due to electromigration (EM) or stress migration (SM) failures. Aluminum voids are particularly severe when the aluminum structure has a small width, for example less than two microns, because the stress gradient in the aluminum structure increases with the aspect ratio, i.e., as the width of the aluminum structure decreases. Therefore, it is desirable to prevent vacancy diffusion to minimize voids.

[0055] In this article, embodiments can minimize voids by forming an inert aluminum oxide, aluminum nitride and / or aluminum oxynitride layer between aluminum layers. In addition, embodiments of this article can interrupt the aluminum deposition process by vacuum breaking / air exposure and nitrogen, oxygen and / or nitrous oxide plasma treatment of the upper surface of the deposited aluminum to form such an inert layer, and then continue the aluminum deposition process. Such a process is easily integrated into existing aluminum deposition schemes.

[0056] Presented herein are embodiments of aluminum structures and methods for forming aluminum structures, and / or methods for manufacturing semiconductor devices having aluminum structures. In certain embodiments, electromigration (EM) and / or stress migration (SM) within the aluminum structure are mitigated by including a migration barrier layer in the aluminum structure. In some example embodiments, the migration barrier layer comprises aluminum. For example, the migration barrier layer can be formed by treating the upper surface of the aluminum layer to form a treated aluminum layer, the treated aluminum layer being, for example, a ceramic aluminum layer. In certain embodiments, the migration barrier layer is aluminum oxide, aluminum nitride and / or aluminum oxynitride. The migration barrier layer can be formed by performing a plasma ionization process on the surface of the aluminum layer.

[0057] Embodiments of the present disclosure provide advantages over the prior art, and while it is understood that other embodiments may provide different advantages, not all advantages are necessarily discussed herein, and all embodiments do not require a particular advantage. For example, embodiments discussed herein include methods for forming an aluminum structure comprising a plurality of aluminum layers separated by a migration barrier layer. Embodiments are provided herein for treating an aluminum layer to form a migration barrier layer on a surface of the aluminum layer, and embodiments for forming another aluminum layer above the migration barrier layer. The reduction in electromigration and / or stress migration provided by the migration barrier layer can reduce the formation of voids and improve the performance of semiconductor devices. Inert and low coefficient of thermal expansion (CTE) AlO x N y The introduction of double-layer aluminum structures may result in fewer voids. The resulting double-layer aluminum structures may have better thermal stability and SM / EM performance. In addition, the process described here can be easily integrated into existing process flows.

[0058] For the purpose of the following discussion, Figure 1 A flow chart of a method 10 for forming an aluminum structure 100 during a semiconductor manufacturing process is provided. Figures 2 to 10 Describe method 10, which illustrates the method 10 and Figures 11 to 15 FIG. 2 is a diagram of a semiconductor device 200 at various stages of fabrication, and is a focused view of an alternative embodiment of an aluminum structure 100 formed by the method 10 . Figures 2 to 15 1 is a cross-sectional "y-cut" view, wherein the vertical direction (first direction) is defined by the z-axis and the lateral direction (second direction) is defined by the x-axis. It should be understood that method 10 includes steps characteristic of a complementary metal-oxide-semiconductor (CMOS) technology process flow, and thus is only briefly described herein. In addition, additional steps may be performed before, after, and / or during method 10.

[0059] Now refer to Figure 1 and Figure 2, the method 10 for manufacturing the semiconductor device 200 includes S11, forming a conductive structure 40 above a substrate (not shown). In an exemplary embodiment, the conductive structure 40 is formed during a backend-of-the-line (BEOL) process, in which an interconnect is formed within the semiconductor device 200. In other words, the conductive structure 40 is a BEOL interconnect. In an exemplary embodiment, the conductive structure 40 is copper. In an exemplary embodiment, the conductive structure 40 is formed by a damascene process. For example, an etching process forms a gap and a thin barrier layer of tantalum (Ta) and tantalum nitride (TaN) material is deposited using physical vapor deposition (PVD). Tantalum is used to form a liner and tantalum nitride is used for a barrier. The barrier layer is covered with a copper seed barrier. Finally, the structure is electroplated with copper and the structure is polished to an upper surface 41 using chemical mechanical polishing.

[0060] The method 10 further includes S12, forming a dielectric layer over at least a portion of the conductive structure 40. For example, the dielectric layer 50 is deposited over the upper surface 41 of the conductive structure 40 and is patterned to form a dielectric segment 51. As shown, a portion 45 of the upper surface 41 of the conductive structure 40 is not covered by the dielectric segment 51. In an exemplary embodiment, the dielectric layer 50 and the dielectric segment 51 are silicon oxide (SiO2).

[0061] Cross Reference Figure 1 and Figure 3 , the method 10 further includes S13, forming a metal diffusion barrier 60 above the conductive structure 40. For example, the method 10 may include depositing a barrier material, such as tantalum nitride (TaN) or titanium nitride (TiN). In an exemplary embodiment, the barrier material is conformally deposited above the dielectric segment 51 and above the uncovered portion 45 of the upper surface 41 of the conductive structure 40. For example, the barrier material can be deposited by an atomic layer deposition (ALD) process.

[0062] The method 10 further includes S14, forming an aluminum layer 110 above the conductive structure 40. For example, the method 10 may include depositing the aluminum 110 above the metal diffusion barrier 60. In an exemplary embodiment, the aluminum 110 is deposited by a physical vapor deposition (PVD) thermal aluminum reflow process. For example, before reflowing additional aluminum deposited on the compliant PVD aluminum layer by physical vapor deposition, a PVD metal layer of aluminum is deposited. As shown in the figure, the aluminum 110 having an upper surface 111 is formed.

[0063] Cross Reference Figure 1 and Figure 4 , the method 10 further includes S15, processing the aluminum layer 110 to form a migration barrier layer 130. In an exemplary embodiment, the upper surface 111 of the aluminum layer 110 is converted into the migration barrier layer 130. The remaining portion 112 of the aluminum layer 110 below the migration barrier layer 130 is aluminum that remains unchanged. In an exemplary embodiment, processing the upper surface 111 of the aluminum layer 110 to form the migration barrier layer 130 includes forming an aluminum nitride layer, an aluminum oxide layer, and / or an aluminum oxynitride layer as the migration barrier layer 130. In an exemplary embodiment, processing the upper surface 111 of the aluminum layer 110 to form the migration barrier layer 130 includes forming a ceramic layer from the upper surface 111. In certain embodiments, processing the upper surface 111 of the aluminum layer 110 to form the migration barrier layer 130 includes performing a vacuum break. In such an embodiment, native aluminum oxide is thereby formed on the aluminum layer 110. In other embodiments, the upper surface 111 of the aluminum layer 110 is treated to form the migration barrier layer 130, including a plasma ionization process using oxygen (O2), nitrogen (N2) and / or nitrous oxide (N2O). In such a process, oxygen ions and / or nitrogen ions penetrate into the aluminum layer 110 to modify the upper surface 111. The migration barrier layer 130 can be regarded as AlO x N y , wherein one of x or y can be zero, but not both. In an exemplary embodiment, the migration barrier layer 130 comprises passivated Al2O3, passivated AlN, or mixed AlO x N y .

[0064] In an exemplary embodiment, the plasma ionization process is performed at a temperature ranging from 25° C. to 400° C., a pressure ranging from 0.001 Torr to 10 Torr, and a duration ranging from 10 seconds to 120 seconds.

[0065] Cross Reference Figure 1 and Figure 5 , the method 10 further includes S16, forming an aluminum layer 120 above the conductive structure 40. For example, the method 10 may include depositing the aluminum 120 above the migration barrier layer 130. In an exemplary embodiment, the aluminum 120 is deposited by a physical vapor deposition (PVD) hot aluminum reflow process. For example, before reflowing additional aluminum deposited on the compliant PVD aluminum layer by physical vapor deposition, a PVD metal layer of aluminum is deposited. As shown, the aluminum 120 having an upper surface 121 is formed. In some embodiments, the aluminum layer 110, the migration barrier layer 130, and the aluminum layer 120 are used for the aluminum structure 100.

[0066] The method 10 includes S17, determining whether more aluminum layers are needed, that is, whether the aluminum structure 100 formed by the aluminum layers is completed. If not, the method 10 continues from S15, wherein the upper surface of the last deposited aluminum layer, such as the upper surface 121 of the aluminum layer 120, is processed to form another migration barrier layer 130.

[0067] When a sufficient aluminum layer is formed, the method 10 may proceed to S18 to selectively process the last deposited aluminum layer to form another migration barrier layer 130, for example, using the process described above with respect to S15. Figures 1 to 10 In the embodiment shown, only two aluminum layers are needed and the method 10 proceeds directly from S17 to S18. In addition, in the illustrated embodiment, no additional migration barrier layer 130 is formed in S18.

[0068] Cross Reference Figure 1 and Figure 6 The method 10 further includes S19, forming a coating 70 on the aluminum structure 100, for example, on the aluminum layer 120. In an example embodiment, the coating 70 is an antireflective coating (ARC). An example coating 70 is silicon oxycarbide (SiOC).

[0069] Cross Reference Figure 1 and Figure 7 , the method 10 further includes S20, forming a mask 80 above the coating layer 70. For example, a photoresist layer may be coated / deposited on the semiconductor device 200, and exposed and developed according to a conventional lithography patterning process to form the mask 80, the mask 80 defining an anisotropic etched pattern having holes 81 for openings, such as high aspect ratio through-hole openings. In an exemplary embodiment, a deep ultraviolet (DUV) chemically amplified photoresist for patterning the openings may include an activating radiation source having a wavelength of less than about 250 nanometers, such as about 193 nanometers to about 250 nanometers, to expose the photoresist layer. The photoresist layer may be any conventional DUV photoresist layer, including a multilayer photoresist, including, for example, a chemically amplified photoresist that generates photogenerated acid.

[0070] Cross Reference Figure 1 and Figure 8, the method 10 further comprises S21, etching the aluminum structure 100 through the hole 81 in the mask 80. In an exemplary embodiment, the etching process also etches through the metal diffusion barrier 60. An exemplary etching process is a wet etching with a suitable chemistry. As a result of the etching process, the aluminum structure 100 is formed with a sidewall 109 formed by the aluminum layer 110, the aluminum layer 120 and the migration barrier layer 130.

[0071] like Figure 8 As shown, the method 10 further includes S22 , after etching the aluminum structure 100 , removing the mask 80 . The coating 70 may remain on the aluminum structure 100 .

[0072] Cross Reference Figure 1 and Fig. 9 The method 10 further includes S23, forming a dielectric layer 90, such as a protective layer (passivation layer) 90, above the aluminum structure 100. In an exemplary embodiment, the protective layer 90 is silicon oxide (SiO2) or silicon nitride (SiN). In an exemplary embodiment, forming the protective layer 90 includes depositing a protective material and planarizing an upper surface 91 of the protective material.

[0073] Method 10 Figures 2 to 10 It is illustrated that the aluminum structure 100 is formed into a conductive line 101, which is isolated from the underlying conductive structure 40 in the provided cross-sectional view and is electrically connected to the underlying conductive structure 40 as a conductive via 102 in the provided cross-sectional view.

[0074] The method 10 may continue with further processing at S24 to complete the semiconductor device 200 .

[0075] For example, Fig.10 As shown, during the advanced packaging process, the protective layer 90 can be etched over selected portions of the aluminum structure 100, such as over the wire 101 as shown, and conductive pads 230 and 240 can be formed to contact the aluminum structure 100. In some embodiments, other layers can be formed as needed, such as a sealing layer, a phosphor-silicate glass (PSG) layer, or other dielectric layer. Example conductive pads 230 and 240 can be independently chromium, copper, or aluminum. As further shown, a solder bump 250 can be formed over the conductive pad 240 and electrically connected to the aluminum structure 100. Further processing can electrically connect the solder bump 250 to additional conductive structures. For example, an integrated circuit die 260 can be electrically connected to the solder bump 250.

[0076] Reference Fig.11, illustrates details of an exemplary aluminum structure 100, such as a conductive line 101. As shown, the aluminum layer 110 has a lateral edge 119, the aluminum layer 120 has a lateral edge 129, and the migration barrier layer 130 has a lateral edge 139. In the etching process for etching the aluminum structure 100, the etchant may have different selectivities for the materials of the aluminum and the migration barrier layer. Specifically, the migration barrier layer 130 may be etched faster. Therefore, a cutout portion or a gap 138 may be formed in the migration barrier layer 130. For example, the lateral edges 119 and 129 of the aluminum layer 110 and the aluminum layer 120 define a plane 108. The lateral edge 139 of the migration barrier layer 130 is away from the plane 108 by the cutout portion, and the cutout portion has a width W9 in the x-direction (second direction). In an exemplary embodiment, the width W9 is less than 10 nanometers (nm).

[0077] Reference Fig.12 , depicting more details of an example aluminum structure 100. As shown, the aluminum structure 100 has a thickness or height T in the z direction. Further, the aluminum layer 110 has a thickness or height T1 in the z direction, and the aluminum layer 120 has a thickness or height T2 in the z direction (first direction). Similarly, the migration barrier layer 130 has a thickness or height Tb in the z direction (first direction).

[0078] In an example embodiment, the total thickness T is 0.5 micrometers (500 nanometers) to 5 micrometers (5000 nanometers). For example, the total thickness T may be 1 micrometer (1000 nanometers) to 3 micrometers (3000 nanometers). In an example embodiment, the thickness Tb of the migration barrier layer is less than 20 nanometers, such as less than 10 nanometers, such as less than 8 nanometers, or less than 6 nanometers. In an example embodiment, the thickness Tb of the migration barrier layer 130 is 2 nanometers to 6 nanometers. In an example embodiment, the migration barrier layer 130 has a thickness of at least 0.2 nanometers, such as at least 0.5 nanometers, at least 1 nanometer, at least 1.5 nanometers, at least 1.75 nanometers, or at least 2 nanometers. In an example embodiment, the migration barrier layer 130 has a thickness of no more than 5 nanometers, such as no more than 4 nanometers, no more than 3 nanometers, or no more than 2 nanometers. In an example embodiment, the migration barrier layer has a thickness of 2 nanometers. Therefore, compared with the rest of the aluminum structure 100, the migration barrier layer 130 is very thin.

[0079] When referring to the total thickness or thickness ratio between the aluminum layer 110 and the aluminum layer 120, the thickness of the migration barrier layer can be neglected because it is within the error range. Therefore, it is generally considered that the total thickness T is equal to the sum of T1 and T2.

[0080] In an example embodiment, aluminum 110 may form 25% of the total thickness T of aluminum structure 100, and aluminum 120 may form 75% of the total thickness T of aluminum structure 100. In such structure 100, the ratio of T1:T is 1:4 and the ratio of T1:T2 is 1:3. In an example embodiment, aluminum layer 110 may form 75% of the total thickness T of aluminum structure 100, and aluminum 120 may form 25% of the total thickness T of aluminum structure 100. In such structure 100, the ratio of T1:T is 3:4 and the ratio of T1:T2 is 3:1. In an example embodiment, aluminum 110 may form 50% of the total thickness T of aluminum structure 100, and aluminum 120 may form 50% of the total thickness T of aluminum structure 100. In such structure 100, the ratio of T1:T is 1:2 and the ratio of T1:T2 is 1:1. Typically, the ratio T1:T may be from 1:4 to 3:4, and the ratio T1:T2 may be from 1:3 to 3: 1. In a specific embodiment, for process control purposes, T1 / T is from 25% to 75%, and T2 / T is from 25% to 75%.

[0081] In example embodiments, the thickness of the aluminum layer 110 or the aluminum layer 120 may be 125 nanometers to 3750 nanometers.

[0082] like Fig.12 As shown, the aluminum structure 100 has a width W1 extending between the opposite sidewalls in the x-direction (second direction), wherein the aluminum layer 110 and the aluminum layer 120 also have a width W1 in the x-direction (second direction). In an exemplary embodiment, the width W1 is less than 2 microns. The migration barrier layer 130 has the same width W1, or, as described above, may have a width slightly less than the width W1 due to the cutout portion. Assuming that the migration barrier layer 130 has a cutout portion at each end, the width of the migration barrier layer 130 will be within 20 nanometers of the width W1, that is, less than the width W1 by no more than 20 nanometers, or not less than the width W1 minus 20 nanometers.

[0083] Although Figures 2 to 12 An aluminum structure 100 is shown including two aluminum layers 110 and 120 and a migration barrier layer 130, but other embodiments are contemplated. Fig.13 , the second migration barrier layer 140 is formed from the upper surface 121 of the aluminum layer 120. Therefore, the aluminum structure 100 includes the first aluminum layer 110, the first migration barrier layer 130, the second aluminum layer 120, and the second migration barrier layer 140. The second migration barrier layer 140 can be formed according to the process used to form the first migration barrier layer 130, and can have the same characteristics as the first migration barrier layer 130, including thickness and width.

[0084] exist Fig.14, the third aluminum layer 150 is formed above the second migration barrier layer 140. Therefore, the aluminum structure 100 includes the first aluminum layer 110, the first migration barrier layer 130, the second aluminum layer 120, the second migration barrier layer 140, and the third aluminum layer 150. The third aluminum layer 150 has an upper surface 151, and may be formed according to the process for forming the aluminum layers 110 and / or 120, and may have the same characteristics as the aluminum layer 110 and / or the aluminum layer 120, including thickness and width. In example embodiments, the thicknesses of the aluminum layer 110, the aluminum layer 120, and the aluminum layer 150 may be different. For example, the first aluminum layer 110 may have a thickness T1, the second aluminum layer 120 may have a thickness T2, and the third aluminum layer 150 may have a thickness T3, wherein each of T1, T2, and T3 is at least 1 / 6 of the total thickness T of the aluminum structure 100, and does not exceed 2 / 3 of the total thickness T of the aluminum structure 100.

[0085] exist Fig.15 , the third migration barrier layer 160 is formed by the upper surface 151 of the aluminum layer 150. Therefore, the aluminum structure 100 includes the first aluminum layer 110, the first migration barrier layer 130, the second aluminum layer 120, the second migration barrier layer 140, the third aluminum layer 150, and the third migration barrier layer 160. The third migration barrier layer 160 can be formed according to the process used to form the first migration barrier layer 130 and / or the second migration barrier layer 140, and can have the same characteristics as the migration barrier layers 130 and / or 140, including thickness and width.

[0086] It will be appreciated that the aluminum structure may be formed from any suitable desired number of aluminum layers separated by migration barrier layers, and may or may not include a migration barrier layer above the uppermost aluminum layer.

[0087] Differences in the coefficient of thermal expansion (CTE) between adjacent materials may lead to stress-driven void merging during thermal cycling. Aluminum has a CTE of 20ppm to 25ppm, such as 23ppm. SiO2 has a CTE of 0.25ppm to 1ppm, such as 0.5ppm; and SiN has a CTE of 2ppm to 3ppm, such as 2.4ppm. AlN has a CTE of 4.5ppm to 6ppm, such as 5.3ppm, and Al2O3 has a CTE of 6.5ppm to 8ppm, such as 7.3ppm. Therefore, providing a migration barrier layer 130 of AlN or Al2O3 can reduce the diffusion of vacancies, which would otherwise merge to form voids. Specifically, the migration barrier layer 130 can block the diffusion of vacancies.

[0088] Therefore, one embodiment of the present disclosure describes a device including an interconnect structure and an aluminum structure electrically connected to the interconnect structure. The aluminum structure includes a first aluminum layer; a migration barrier layer above the first aluminum layer; and a second aluminum layer above the migration barrier layer.

[0089] In certain embodiments, the device further includes a dielectric layer over the interconnect structure, wherein the dielectric layer includes silicon oxide (SiO 2 ).

[0090] In certain embodiments of the device, the aluminum structure has a height in the z-direction (first direction) of 0.5 micrometers to 5 micrometers, and wherein the migration barrier layer has a thickness in the z-direction (first direction) of 2 nanometers to 6 nanometers.

[0091] In certain embodiments of this device, the first aluminum layer has a thickness T1 in the z-direction (first direction), wherein the second aluminum layer has a thickness T2 in the z-direction (first direction), and wherein T1:T2 is 3:1 to 1:3.

[0092] In certain embodiments of the device, the migration barrier layer comprises aluminum oxide, aluminum nitride and / or aluminum oxynitride.

[0093] In certain embodiments of the device, the migration barrier layer is a first migration barrier layer, and the device further comprises a second migration barrier layer over the second aluminum layer; and a third aluminum layer over the second migration barrier layer.

[0094] In certain embodiments of the device, the migration barrier layer is a ceramic layer.

[0095] In certain embodiments of this device, the first aluminum layer has a first lateral edge; the second aluminum layer has a second lateral edge; the migration barrier layer has a barrier lateral edge; the first lateral edge and the second lateral edge define a plane; and the distance between the barrier lateral edge and the plane is less than 10 nanometers (nm).

[0096] In another embodiment, a semiconductor device is provided and includes a first aluminum layer; a ceramic layer directly above the first aluminum layer, wherein the ceramic layer is composed of aluminum oxide, aluminum nitride and / or aluminum oxynitride; and a second aluminum layer directly above the ceramic layer.

[0097] In some embodiments, the device further comprises an interconnect structure; and a dielectric layer located above the interconnect structure, wherein the first aluminum layer, the ceramic layer, and the second aluminum layer comprise a conductive line, and wherein the conductive line is located above the dielectric layer.

[0098] In certain embodiments of this device, the first aluminum layer has a thickness in the z-direction (first direction) of 125 nanometers to 3750 nanometers; the ceramic layer has a thickness in the z-direction (first direction) of 2 nanometers to 6 nanometers; and the second aluminum layer has a thickness in the z-direction (first direction) of 125 nanometers to 3750 nanometers. In such embodiments, the first aluminum layer may have a first width in the x-direction (second direction) of less than 2 micrometers; the ceramic layer may have a ceramic width in the x-direction (second direction) of less than 2 micrometers; and the second aluminum layer may have a second width in the x-direction (second direction) of less than 2 micrometers. In such embodiments, the ceramic width is no less than the first width and the second width by no more than 20 nanometers.

[0099] A method for manufacturing a semiconductor device is also provided, and includes depositing a first layer of aluminum, wherein the first layer of aluminum has an upper surface; processing the upper surface of the first layer of aluminum to form a migration barrier layer, wherein the remaining portion of the first layer of aluminum below the migration barrier layer remains unchanged; and depositing a second layer of aluminum above the migration barrier layer.

[0100] In certain embodiments of this method, the migration barrier layer is a first migration barrier layer, the second layer of aluminum has an upper surface, and the method further includes processing the upper surface of the second layer of aluminum to form a second migration barrier layer, wherein the remaining portion of the second layer of aluminum below the second migration barrier layer remains unchanged; and depositing a third layer of aluminum above the second migration barrier layer.

[0101] In some embodiments, the method further includes etching the second layer of aluminum, the migration barrier layer, and the first layer of aluminum to form a conductive line having a first sidewall and a second sidewall; wherein the conductive line has a line width from the first sidewall to the second sidewall in the x-direction (second direction), and wherein the line width is less than 2 microns.

[0102] In some embodiments, the method further includes etching the second layer of aluminum, the migration barrier layer, and the first layer of aluminum to form a conductive structure having a first sidewall; and depositing a dielectric material over the conductive structure. In some embodiments, when etching the second layer of aluminum, the migration barrier layer, and the first layer of aluminum to form the conductive structure having the first sidewall, a kerf gap is formed from an edge of the migration barrier layer, and wherein the kerf gap has a width of less than 10 nanometers (nm). In some embodiments, after etching the second layer of aluminum, the migration barrier layer, and the first layer of aluminum to form the conductive structure having the first sidewall, the first layer of aluminum has a first lateral edge, the second layer of aluminum has a second lateral edge, the migration barrier layer has a barrier lateral edge, the first lateral edge and the second lateral edge define a plane, and the barrier lateral edge is less than 10 nanometers (nm) from the plane.

[0103] In certain embodiments of the method, processing the upper surface of the first layer of aluminum to form a migration barrier layer includes forming an aluminum nitride layer, an aluminum oxide layer, or an aluminum oxynitride layer.

[0104] In certain embodiments of the method, treating the upper surface of the first layer of aluminum to form the migration barrier layer includes forming a ceramic layer from the upper surface of the first layer of aluminum.

[0105] In certain embodiments of the method, treating the upper surface of the first layer of aluminum to form the migration barrier layer includes: performing a vacuum break on the upper surface of the first layer of aluminum and forming native aluminum oxide.

[0106] In certain embodiments of the method, treating the upper surface of the first layer of aluminum to form the migration barrier layer includes performing a plasma ionization process using oxygen (O2), nitrogen (N2) or nitrous oxide (N2O).

[0107] The present disclosure provides a semiconductor device, comprising an interconnect structure and an aluminum structure. The aluminum structure is electrically connected to the interconnect structure, wherein the aluminum structure comprises a first aluminum layer, a migration barrier layer and a second aluminum layer. The migration barrier layer is disposed above the first aluminum layer. The second aluminum layer is disposed above the migration barrier layer.

[0108] In an embodiment of the semiconductor device, the aluminum structure has a height of 0.5 micrometers to 5 micrometers in the first direction, and the migration barrier layer has a thickness of 2 nanometers to 6 nanometers in the first direction.

[0109] In an embodiment of the semiconductor device, the first aluminum layer has a thickness T1 in the first direction, the second aluminum layer has a thickness T2 in the first direction, and T1:T2 is 3:1 to 1:3.

[0110] In an embodiment of the semiconductor device, the migration barrier layer is a first migration barrier layer, and the device further comprises a second migration barrier layer and a third aluminum layer, wherein the second migration barrier layer is above the second aluminum layer, and the third aluminum layer is above the second migration barrier layer.

[0111] In an embodiment of this semiconductor device, the first aluminum layer has a first lateral edge; the second aluminum layer has a second lateral edge; the migration barrier layer has a barrier lateral edge; the first lateral edge and the second lateral edge define a plane; and the distance between the barrier lateral edge and the plane is less than 10 nanometers (nm).

[0112] The present disclosure provides a semiconductor device, comprising an interconnection structure, a first aluminum layer, a ceramic layer, and a second aluminum layer. The first aluminum layer is disposed above the interconnection structure. The ceramic layer is directly above the first aluminum layer. The second aluminum layer is directly above the ceramic layer.

[0113] In the embodiment of the semiconductor device, a dielectric layer is further included. The dielectric layer is located above the interconnect structure, wherein the first aluminum layer, the ceramic layer and the second aluminum layer include conductive lines, and wherein the conductive lines are located above the dielectric layer.

[0114] In an embodiment of the semiconductor device, a dielectric layer is further included. The dielectric layer is located above the interconnect structure, wherein the first aluminum layer has a thickness of 125 nanometers to 3750 nanometers in the first direction; the ceramic layer has a thickness of 2 nanometers to 6 nanometers in the first direction; the second aluminum layer has a thickness of 125 nanometers to 3750 nanometers in the first direction; the first aluminum layer has a first width of less than 2 micrometers in the second direction; the ceramic layer has a ceramic width of less than 2 micrometers in the second direction; and the second aluminum layer has a second width of less than 2 micrometers in the second direction.

[0115] In an embodiment of the semiconductor device, the ceramic width is less than the first width and the second width by no more than 20 nanometers.

[0116] In an embodiment of the semiconductor device, the first aluminum layer has a thickness T1 in the first direction, the second aluminum layer has a thickness T2 in the first direction, and T1:T2 is 3:1 to 1:3.

[0117] The present disclosure provides a semiconductor device, comprising a first aluminum layer, a second aluminum layer, a migration barrier layer, and a conductive structure. The second aluminum layer is disposed above the first aluminum layer. The migration barrier layer is disposed between the first aluminum layer and the second aluminum layer. The conductive structure is electrically connected to the first aluminum layer, the second aluminum layer, and the migration barrier layer.

[0118] In an embodiment of the semiconductor device, the first aluminum layer has a thickness T1 in the first direction, the second aluminum layer has a thickness T2 in the first direction, and T1:T2 is 3:1 to 1:3.

[0119] In an embodiment of the semiconductor device, the migration barrier layer is a first migration barrier layer, and the device further comprises a second migration barrier layer and a third aluminum layer, wherein the second migration barrier layer is above the second aluminum layer, and the third aluminum layer is above the second migration barrier layer.

[0120] In an embodiment of this semiconductor device, the first aluminum layer has a first lateral edge; the second aluminum layer has a second lateral edge; the migration barrier layer has a barrier lateral edge; the first lateral edge and the second lateral edge define a plane; and the distance between the barrier lateral edge and the plane is less than 10 nanometers (nm).

[0121] The foregoing summarizes the features of several embodiments so that those skilled in the art can better understand the various aspects of the present disclosure. It should be understood by those skilled in the art that they can easily use the present disclosure as a basis to design or modify other processes and structures to perform the same purpose and / or achieve the same advantages of the embodiments described herein. It should also be recognized by those skilled in the art that such equivalent structures do not depart from the spirit and scope of the present disclosure, and various modifications, substitutions and changes may be made herein without departing from the spirit and scope of the present disclosure.

Claims

1. A semiconductor device, characterized in that: Include: an interconnect structure; and an aluminum structure electrically connected to the interconnect structure, wherein the aluminum structure comprises: a first aluminum layer; a migration barrier layer disposed above the first aluminum layer; and A second aluminum layer is disposed on the migration barrier layer.

2. The semiconductor device according to claim 1, wherein The aluminum structure has a height of 0.5 micrometers to 5 micrometers in a first direction, and the migration barrier layer has a thickness of 2 nanometers to 6 nanometers in the first direction.

3. A semiconductor device, characterized in that: Include: an interconnect structure; a first aluminum layer disposed above the interconnect structure; a ceramic layer directly over the first aluminum layer; and A second aluminum layer is directly above the ceramic layer.

4. The semiconductor device according to claim 3, wherein: Also includes: a dielectric layer located above the interconnect structure, The first aluminum layer, the ceramic layer and the second aluminum layer include a wire, and the wire is located above the dielectric layer.

5. The semiconductor device according to claim 3, wherein: in: The first aluminum layer has a thickness in a first direction of 125 nanometers to 3750 nanometers; The ceramic layer has a thickness in a first direction of 2 nm to 6 nm; The second aluminum layer has a thickness in the first direction of 125 nm to 3750 nm; The first aluminum layer has a first width less than 2 micrometers in a second direction; The ceramic layer has a ceramic width less than 2 microns in the second direction; as well as The second aluminum layer has a second width in the second direction that is less than 2 micrometers.

6. The semiconductor device according to claim 5, wherein: The ceramic width is smaller than the first width and the second width is no more than 20 nanometers.

7. A semiconductor device, characterized in that: Include: a first aluminum layer; a second aluminum layer disposed on the first aluminum layer; a migration barrier layer disposed between the first aluminum layer and the second aluminum layer; and A conductive structure electrically connects the first aluminum layer, the second aluminum layer and the migration barrier layer.

8. The semiconductor device according to claim 1, 3 or 7, wherein: The first aluminum layer has a thickness T1 in a first direction, the second aluminum layer has a thickness T2 in the first direction, and T1:T2 is 3:1 to 1:

3.

9. The semiconductor device according to claim 1 or 7, wherein: wherein the migration barrier layer is a first migration barrier layer, and wherein the device further comprises: a second migration barrier layer on the second aluminum layer; and A third aluminum layer is formed on the second migration barrier layer.

10. The semiconductor device according to claim 1 or 7, wherein: in: The first aluminum layer has a first lateral edge; The second aluminum layer has a second lateral edge; The migration barrier layer has a barrier lateral edge; The first lateral edge and the second lateral edge define a plane; and The distance between the lateral edge of the barrier and the plane is less than 10 nanometers (nm).