Solar cell, cell assembly and photovoltaic system
By providing a second doped layer on the first doped layer of the solar cell and improving its contact surface roughness with the passivation film layer, the problem of insufficient tension on the solder joint is solved, and the reliability of welding is improved.
Patent Information
- Application Number
- CN202420798601.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2034-04-17
AI Technical Summary
The welding joints of existing solar cell cells are prone to the problem of insufficient tension of the welding joints during welding.
By providing a second doping layer on the first doping layer of the solar cell, the contact surface roughness of the second doping layer and the first passivation film layer is greater than that of the first doping layer and the first passivation film. The contact surface roughness of the layer can increase the welding tension of the solder joints and avoid the welding joints from falling apart.
It effectively improves the welding tension of the welding joints, enhances the reliability of welding, and avoids the phenomenon of disengagement of the welding joints during welding.
Smart Images

Figure CN222088615U_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a solar cell sheet, a battery assembly and a photovoltaic system. Background Art
[0002] At present, in solar cells (such as Topcon solar cells, HJT solar cells, back contact solar cells, etc.), a doping layer is provided, and a fine grid and a main grid are also provided on the doping layer. The fine grid penetrates the passivation film layer and contacts the doping layer to collect current, and the main grid is connected to the fine grid to collect the current of the fine grid. When connecting two solar cells, it is necessary to set a solder joint on the cell to weld with the solder strip, and the solder joint is usually set on the passivation film layer. However, in the related art, the tension between the doping layer and the passivation film layer under the solder joint is weak, and the solder joint is prone to detachment due to insufficient solder joint tension during welding. Utility Model Content
[0003] The present application provides a solar cell, a battery assembly and a photovoltaic system, aiming to solve the technical problem in the prior art that the solder joints of the solar cell are prone to insufficient solder joint tension during welding, resulting in solder joint detachment.
[0004] The present application is implemented in this way. The solar cell of the embodiment of the present application includes:
[0005] Silicon wafer;
[0006] A first doped layer stacked on the silicon wafer, wherein the first doped layer has a plurality of first preset regions;
[0007] a second doping layer, wherein the second doping layer is stacked on the first preset region, and the polarity of the second doping layer is opposite to that of the first doping layer;
[0008] a first passivation film layer, wherein the first passivation film layer is stacked on the second doping layer and the first doping layer, and the roughness of a surface of the second doping layer in contact with the first passivation film layer is greater than the roughness of a surface of the first doping layer in contact with the first passivation film layer; and
[0009] A plurality of first welding points, wherein the first welding points are arranged on the first passivation film layer, and an orthographic projection of the first welding points on the first doping layer at least partially overlaps with an orthographic projection of the second doping layer on the first doping layer.
[0010] Furthermore, the solar cell sheet further includes a first isolation layer, which is stacked on the first preset area and located between the first doping layer and the second doping layer.
[0011] Furthermore, the thickness of the first isolation layer is greater than 2 nm.
[0012] Furthermore, the first isolation layer includes at least one of a silicon oxide film layer, a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, a silicon carbide film layer and an intrinsic amorphous silicon film layer.
[0013] Furthermore, the orthographic projection of the first welding point on the first doping layer is completely located within the first preset area.
[0014] Furthermore, the thickness of the second doping layer is 5nm-400nm.
[0015] Furthermore, the first passivation film layer includes at least one of a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, an intrinsic amorphous silicon film layer, and a TCO film layer.
[0016] Furthermore, the solar cell further comprises a third doping layer, a second passivation film layer and a plurality of second solder joints, the polarity of the third doping layer is opposite to the polarity of the first doping layer, and the silicon wafer has a first surface and a second surface opposite to each other;
[0017] wherein the first doped layer is stacked on the first surface, the third doped layer is stacked on the second surface, the second passivation film layer is stacked on the third doped layer, and the second solder joint is arranged on the second passivation film layer; or
[0018] The first doping layer and the third doping layer are both stacked on the first surface, the first passivation film layer is stacked on the first doping layer, the second doping layer and the third doping layer, the second welding point is also arranged on the first passivation film layer, and the second passivation film layer is stacked on the second surface.
[0019] Furthermore, in the case where the third doping layer is stacked on the first surface, on the first surface, a number of the first doping layers and a number of the third doping layers are alternately arranged in sequence along the first direction, and the first doping layers and the third doping layers both extend along the second direction, and the second direction intersects with the first direction.
[0020] Furthermore, in the case where the third doping layer is stacked on the first surface, the first doping layer includes a plurality of first sub-doping layers and a second sub-doping layer, and the third doping layer includes a plurality of third sub-doping layers and a plurality of fourth sub-doping layers;
[0021] A plurality of the first sub-doping layers and a plurality of the third sub-doping layers are alternately arranged in sequence along a first direction and are disposed on the first surface at intervals and extend along a second direction, wherein the second direction intersects the first direction;
[0022] A plurality of the second sub-doping layers and a plurality of the fourth sub-doping layers are arranged alternately and spaced in sequence along the second direction on the first surface and extend along the first direction, the first sub-doping layer is disconnected at the fourth sub-doping layer and contacts the second sub-doping layer, and the third sub-doping layer is disconnected at the second sub-doping layer and contacts the fourth sub-doping layer;
[0023] The second sub-doping layer has a plurality of the first preset regions, and the plurality of the first preset regions are arranged at intervals along the second direction.
[0024] Furthermore, in the first direction, the length of the first solder joint is greater than the length of the second doping layer, and the ratio of the length of the first solder joint above the second doping layer to the total length of the first solder joint is greater than or equal to 20%.
[0025] Furthermore, in the first direction, a ratio of a length of the first welding point located above the second doping layer to a total length of the first welding point is greater than or equal to 50%.
[0026] Furthermore, a ratio of an orthographic projection area of the second doping layer on the second sub-doping layer to an area of the second sub-doping layer is less than or equal to 50%.
[0027] Furthermore, in the first direction, a distance between two adjacent first welding points is 3 mm-40 mm.
[0028] Furthermore, the third doping layer has a plurality of second preset regions, and the solar cell further comprises a fourth doping layer, the fourth doping layer is stacked on the second preset regions, and the fourth doping layer has an opposite polarity to the third doping layer;
[0029] In the case where the third doped layer is stacked on the second surface, the second passivation film layer covers the third doped layer and the fourth doped layer, the roughness of the surface of the fourth doped layer in contact with the second passivation film layer is greater than the roughness of the surface of the third doped layer in contact with the second passivation film layer, and the orthographic projection of the second welding point on the third doped layer at least partially overlaps with the orthographic projection of the fourth doped layer on the third doped layer;
[0030] In the case where the third doped layer is stacked on the first surface, the first passivation film layer covers the first doped layer, the second doped layer, the third doped layer and the fourth doped layer, the roughness of the surface of the fourth doped layer in contact with the first passivation film layer is greater than the roughness of the surface of the third doped layer in contact with the first passivation film layer, and the orthographic projection of the second welding point on the third doped layer at least partially overlaps with the orthographic projection of the fourth doped layer on the third doped layer.
[0031] Furthermore, the solar cell sheet further includes a second isolation layer, which is stacked on the second preset area and located between the third doping layer and the fourth doping layer.
[0032] Furthermore, the orthographic projection area of the second preset region on the silicon wafer is greater than or equal to the orthographic projection area of the second welding point on the silicon wafer, and the second welding point is completely located in the second preset region.
[0033] Furthermore, in the case where the third doping layer is stacked on the first surface, the first doping layer includes a plurality of first sub-doping layers and a second sub-doping layer, and the third doping layer includes a plurality of third sub-doping layers and a plurality of fourth sub-doping layers;
[0034] A plurality of the first sub-doping layers and a plurality of the third sub-doping layers are alternately arranged in sequence along a first direction and are disposed on the first surface at intervals and extend along a second direction, wherein the second direction intersects the first direction;
[0035] A plurality of the second sub-doping layers and a plurality of the fourth sub-doping layers are arranged alternately and spaced in sequence along the second direction on the first surface and extend along the first direction, the first sub-doping layer is disconnected at the fourth sub-doping layer and contacts the second sub-doping layer, and the third sub-doping layer is disconnected at the second sub-doping layer and contacts the fourth sub-doping layer;
[0036] The second sub-doping layer has a plurality of the first preset regions, which are spaced apart along the first direction; the fourth sub-doping layer has a plurality of the second preset regions, which are spaced apart along the first direction.
[0037] The present application also provides a battery assembly, which includes a plurality of solar cells as described in any one of the above items.
[0038] The present application also provides a photovoltaic system, which includes the above-mentioned battery assembly.
[0039] In the solar cell, battery assembly and photovoltaic system of the embodiment of the present application, a second doping layer is provided on the first preset area of the first doping layer, the second doping layer is covered with a first passivation film layer, the roughness of the surface of the second doping layer in contact with the first passivation film layer is greater than the roughness of the surface of the first doping layer in contact with the first passivation film layer, and the orthographic projection of the first welding point on the first doping layer and the orthographic projection of the second doping layer on the first doping layer at least partially overlap. In this way, by providing the second doping layer on the first doping layer, and the roughness of the surface of the second doping layer in contact with the first passivation film layer is greater than the roughness of the surface of the first doping layer in contact with the first passivation film layer, the bonding tension between the first passivation film layer and the second doping layer can be greater than the bonding tension between the first passivation film layer and the first doping layer. In this way, the first welding point is provided above the second doping layer, which can effectively increase the welding tension of the first welding point during welding, thereby effectively avoiding the first welding point from being separated during welding, and improving the reliability of welding.
[0040] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 is a module schematic diagram of a photovoltaic system provided in an embodiment of the present application;
[0042] Figure 2 is a module schematic diagram of a battery assembly provided in an embodiment of the present application;
[0043] Figure 3 is a schematic diagram of the structure of a solar cell provided in an embodiment of the present application;
[0044] Figure 4 is another structural schematic diagram of a solar cell provided in an embodiment of the present application;
[0045] Figure 5 is a schematic diagram of the planar structure of a solar cell provided in an embodiment of the present application;
[0046] Figure 6 yes Figure 5 Schematic diagram of the cross section of the back contact cell along line VI-VI;
[0047] Figure 7 yes Figure 5 Another schematic cross-sectional view of the back contact cell along line VI-VI;
[0048] Figure 8 is another schematic diagram of the planar structure of a solar cell provided in an embodiment of the present application;
[0049] Fig. 9 yes Figure 8Schematic diagram of the cross section of the back contact cell along line IX-IX;
[0050] Fig.10 yes Figure 8 Schematic cross-sectional view of the back contact cell along line XX;
[0051] Fig.11 This is another schematic diagram of the planar structure of the solar cell provided in the embodiment of the present application.
[0052] Description of main component symbols:
[0053] Photovoltaic system 1000, battery assembly 200, solar cell 100, silicon wafer 10, first surface 11, second surface 12, first doping layer 20, first preset area 201, first sub-doping layer 21, second sub-doping layer 22, second doping layer 30, first passivation film layer 40, first welding point 50, first isolation layer 60, third doping layer 70, second preset area 701, third sub-doping layer 71, fourth sub-doping layer 72, second passivation film layer 80, second welding point 90, fourth doping layer 110, second isolation layer 120. Specific embodiments
[0054] In order to make the purpose, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. In addition, it should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0055] In the description of the present application, it should be understood that the terms "length", "width", "up", "down", "top", "bottom", "lateral", "longitudinal", etc., indicating orientation or positional relationships, are based on the orientation or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0056] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0057] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0058] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0059] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, and does not indicate the relationship between the various embodiments and / or settings discussed in itself. In addition, the various specific processes and examples of materials provided by the present application, but those of ordinary skill in the art can be aware of the application of other processes and / or the use scenarios of other materials.
[0060] See also Figure 1-Figure 2 , the photovoltaic system 1000 in the embodiment of the present application may include the battery assembly 200 in the embodiment of the present application, the battery assembly 200 in the embodiment of the present application may include a plurality of battery strings, and the battery string may include a plurality of solar cells 100 in the embodiment of the present application. In the present application, the plurality of solar cells 100 in the battery assembly 200 may be connected in series in sequence through welding strips to form a battery string. The battery strings in the battery assembly 200 may be connected in series, in parallel, or in series-parallel combination to realize the bus output of current, for example, the connection between the battery strings may be realized through bus bars.
[0061] See also Figure 3The solar cell 100 in this embodiment may include a silicon wafer 10 , a first doping layer 20 , a second doping layer 30 , a first passivation film layer 40 and a first solder joint 50 .
[0062] The first doping layer 20 is stacked on the silicon wafer 10 and has a plurality of first preset regions 201. The second doping layer 30 is stacked on the first preset regions 201 and has a polarity opposite to that of the first doping layer 20.
[0063] The first passivation film layer 40 is stacked on the second doping layer 30 and the first doping layer 20. Specifically, the first passivation film layer 40 can cover the entire first doping layer 20 and the second doping layer 30 (that is, the first passivation film layer 40 covers the second doping layer 30 and the area of the first doping layer 20 that is not covered by the second doping layer 30).
[0064] like Figure 3 As shown, the roughness of the surface 301 of the second doping layer 30 in contact with the first passivation film layer 40 is greater than the roughness of the surface 202 of the first doping layer 20 in contact with the first passivation film layer 40, and the first solder joint 50 can be arranged on the first passivation film layer 40, and the orthographic projection of the first solder joint 50 on the first doping layer 20 at least partially overlaps with the orthographic projection of the second doping layer 30 on the first doping layer 20.
[0065] It should be noted that, in the present application, “orthographic projection” refers to the orthographic projection along the thickness direction of the solar cell 100 . In the following text, if there is the same description, please refer to this for understanding.
[0066] In the solar cell of the embodiment of the present application, a second doping layer 30 is provided on the first preset area 201 of the first doping layer 20, and the second doping layer 30 is covered with a first passivation film layer 40, the roughness of a surface 301 of the second doping layer 30 in contact with the first passivation film layer 40 is greater than the roughness of a surface 202 of the first doping layer 20 in contact with the first passivation film layer 40, and the orthographic projection of the first solder joint 50 on the first doping layer 20 at least partially overlaps with the orthographic projection of the second doping layer 30 on the first doping layer 20. In this way, by arranging the second doping layer 30 on the first doping layer 20, and the roughness of the surface 301 of the second doping layer 30 in contact with the first passivation film layer 40 is greater than the roughness of the surface 202 of the first doping layer 20 in contact with the first passivation film layer 40, the bonding tension between the first passivation film layer 40 and the second doping layer 30 can be made greater than the bonding tension between the first passivation film layer 40 and the first doping layer 20. In this way, arranging the first welding point 50 above the second doping layer 30 (that is, the orthographic projection of the first welding point 50 on the first doping layer 20 at least partially overlaps with the orthographic projection of the second doping layer 30 on the first doping layer 20) can effectively increase the welding tension of the first welding point 50 during welding, thereby effectively avoiding the first welding point 50 from detaching during welding, thereby improving the reliability of welding.
[0067] Specifically, in the present application, the solar cell 100 may be a back contact cell, a Topcon solar cell, an HJT solar cell, or the like having a first doping layer 20 and requiring solder joints to be set on the first doping layer 20, and no specific limitation is made here.
[0068] In the present application, the first doping layer 20 and the second doping layer 30 can be a P-type doping layer and an N-type doping layer, respectively, as long as the polarities of the two are opposite. For example, in some embodiments, the first doping layer 20 can be a P-type polysilicon layer, a P-type amorphous silicon layer, or a P-type microcrystalline silicon layer, which is not specifically limited here. Similarly, the second doping layer 30 can be an N-type polysilicon layer, an N-type amorphous silicon layer, or an N-type microcrystalline silicon layer, which is not specifically limited here.
[0069] In some embodiments, a tunneling oxide layer or an intrinsic amorphous silicon layer (not shown) may be provided between the first doped layer 20 and the silicon wafer 10. Specifically, when the solar cell is a Topcon solar cell or a back contact cell, a tunneling oxide layer may be provided between the first doped layer 20 and the silicon wafer 10, and when the solar cell is a HJT solar cell, an intrinsic amorphous silicon layer may be provided between the first doped layer 20 and the silicon wafer 10.
[0070] See also Figure 4In some embodiments, the solar cell 100 may further include a first isolation layer 60 . The first isolation layer 60 may be stacked on the first preset region 201 and located between the first doping layer 20 and the second doping layer 30 .
[0071] In this way, the second doping layer 30 can be separated from the first doping layer 20 by the first isolation layer 60 to avoid direct contact between the two, while also ensuring the passivation effect of the first doping layer 20 .
[0072] Of course, it is understandable that in some embodiments, it is not necessary to set the first isolation layer 60 to separate the first doped layer 20 and the second doped layer 30. It is only necessary to set the metal grid line in contact with the first doped layer 20 in the solar cell 100 to be not in contact with the second doped layer 30. No specific limitation is made here.
[0073] In some embodiments, the thickness of the first isolation layer 60 may be greater than 2 nm. In this way, it is possible to avoid a situation where the thickness of the first isolation layer 60 is too small, which would significantly increase the difficulty of the process.
[0074] Furthermore, in some embodiments, the first isolation layer 60 may include at least one of a silicon oxide film layer, a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, a silicon carbide film layer, and an intrinsic amorphous silicon film layer.
[0075] Specifically, in such an embodiment, the first isolation layer 60 may or may not have a tunneling function, and may be an insulating layer or a non-insulating layer. There is no specific limitation here, and the specific film layer may be selected according to different types of battery cells.
[0076] For example, when the cell is a Topcon solar cell and a back contact cell, the first isolation layer 60 may be at least one of a silicon oxide film layer, a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, and a silicon carbide film layer, and the first isolation layer 60 may or may not have a tunneling function.
[0077] When the cell is a HJT solar cell, the first isolation layer 60 may be an intrinsic amorphous silicon layer. It is understood that the specific selection of the first isolation layer 60 is merely an exemplary description here, but it cannot be understood as a limitation to the present application.
[0078] like Figure 3 and Figure 4 As shown, in some embodiments, the orthographic projection of the first solder joint 50 on the first doping layer 20 is completely located within the first preset area 201 , that is, in the thickness direction of the solar cell 100 , the first solder joint 50 is completely located above the second doping layer 30 .
[0079] In this way, the first welding point 50 is completely located in the first preset area 201, and the entire bottom of the first welding point 50 has the second doping layer, which can maximize the welding tension at the first welding point 50, thereby ensuring the reliability of welding.
[0080] Specifically, in such an embodiment, the area of the first preset region 201 may preferably be just equal to the orthographic projection area of the first welding point 50 or slightly larger than the orthographic projection area of the first welding point 50 .
[0081] Of course, in some embodiments, the orthographic projection area of the first solder joint 50 on the first doping layer 20 may also be larger than the orthographic projection area of the second doping layer 30 on the first doping layer 20 (that is, the area of the first preset area 201). For example, a single first solder joint 50 may correspond to multiple second doping layers 30. In this case, the first solder joint 50 may completely cover the second doping layer 30. In this case, the ratio of the overlapping area of the second doping layer 30 and the first solder joint 50 to the total area of the first solder joint 50 may be greater than 20% to avoid too small welding tension.
[0082] In addition, in some embodiments, the first solder joint 50 may be bonded to the first passivation film layer 40, may be partially embedded in the first passivation film layer 40, or may at least partially penetrate the first passivation film layer 40 to contact the second doping layer 30. When the first solder joint 50 contacts the second doping layer 30, the first doping layer 20 and the second doping layer 30 may be isolated by setting a first isolation layer 60. No specific limitation is made here.
[0083] In some embodiments, the thickness of the second doping layer 30 may be 5 nm-400 nm.
[0084] In this way, it is possible to effectively avoid the second doping layer 30 being too thin to cause poor tensile reinforcement effect, the second doping layer 30 being too thin to cause increased process difficulty, and the second doping layer 30 being too thick to cause increased cost.
[0085] Specifically, the thickness of the second doping layer 30 may be 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm or any value between 5nm and 400nm, and is not limited here.
[0086] In some embodiments, the first passivation film layer 40 may include at least one of a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, an intrinsic amorphous silicon film layer, and a TCO film layer.
[0087] Specifically, in such an embodiment, the type of the first passivation film layer 40 can also be selected according to different types of battery cells. For example, when the battery is a Topcon solar cell and a back contact battery, the first passivation film layer 40 can be at least one of a silicon oxide film layer, a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, and a silicon carbide film layer.
[0088] When the cell is a HJT solar cell, the first passivation film layer 40 may be a TCO film layer, which is not specifically limited here. It is understandable that the specific selection of the first passivation film layer 40 is merely exemplified here, but it cannot be understood as a limitation to the present application.
[0089] See also Figure 5-Figure 9 In some embodiments, the silicon wafer 10 has a first surface 11 and a second surface 12 relative to each other, and the solar cell 100 may further include a third doping layer 70, a second passivation film layer 80 and a plurality of second solder joints 90, and the polarity of the third doping layer 70 is opposite to the polarity of the first doping layer 20.
[0090] like Figure 5 and Figure 6 As shown, in some embodiments, the first doping layer 20 may be stacked on the first surface 11, the third doping layer 70 may be stacked on the second surface 12, the second passivation film layer 80 is stacked on the third doping layer 70, and the second solder joint 90 is disposed on the second passivation film layer 80. In this case, the solar cell 100 is a double-sided solar cell, such as a Topcon solar cell, an HJT solar cell, etc.
[0091] Similarly, in the present application, the second passivation film layer 80 may also include at least one of a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, an intrinsic amorphous silicon film layer, and a TCO film layer.
[0092] like Figure 8 and Fig. 9 As shown, in some embodiments, the first doping layer 20 and the third doping layer 70 may also be stacked on the first surface 11, the first passivation film layer 40 is stacked on the first doping layer 20, the second doping layer 30 and the third doping layer 70, the second solder joint 90 is also disposed on the first passivation film layer 40, and the second passivation film layer 80 is stacked on the second surface 12. In this case, the solar cell 100 is a back contact cell, the first surface 11 is the back side of the cell, and the second surface 12 is the front side of the cell.
[0093] In the embodiment of the present application, in the solar cell 100, the second doping layer 30 can be obtained by partially removing the plating layer formed on the first doping layer 20 in the process of forming the third doping layer 70 mentioned above, and the roughness of the second doping layer 30 can be controlled by controlling the temperature and time of deposition or by etching. Of course, in some embodiments, the second doping layer 30 can also be directly obtained by deposition, and similarly, the roughness of the second doping layer 30 can also be controlled by controlling the temperature and time of deposition or by etching, which is not limited here.
[0094] It can be understood that when the solar cell 100 is a double-sided solar cell, a plurality of first sub-grids (not shown in the figure) are arranged on the first passivation film layer 40, and the first sub-grids penetrate the first passivation film layer 40 and contact the first doped layer 20, and a plurality of second sub-grids (not shown in the figure) are also arranged on the second passivation film layer 80, and the second sub-grids penetrate the second passivation film layer 80 and contact the third doped layer 70. In the double-sided solar cell, a first main grid (not shown in the figure) cross-contacting with the first auxiliary grid and a second main grid (not shown in the figure) cross-contacting with the second auxiliary grid are also provided. The first welding point 50 can be provided on the first main grid, which can be located on the first passivation film layer 40 or partially embedded in the first passivation film layer 40 or penetrate the first passivation film layer 40 and contact the second doping layer 30 below the first passivation film layer 40. The first welding point 50 is used for welding with the welding strip. Similarly, the second welding point 90 can be provided on the second main grid, which can be located on the second passivation film layer 80 or partially embedded in the second passivation film layer 80 or penetrate the second passivation film layer 80. The second welding point 90 is also used for welding with the welding strip.
[0095] When the solar cell 100 is a back contact cell, the first passivation film layer 40 is provided with a third sub-grid (not shown in the figure) and a fourth sub-grid (not shown in the figure), the third sub-grid penetrates the first passivation film layer 40 and contacts the first doped layer 20, and the fourth sub-grid penetrates the first passivation film layer 40 and contacts the third doped layer 70.
[0096] When the solar cell 100 is a back contact cell, it can be divided into the following two cases:
[0097] The first type: Figure 8 As shown, in some embodiments, on the first surface 11, a plurality of first doped layers 20 and a plurality of third doped layers 70 may be arranged alternately in sequence along the first direction, and the first doped layers 20 and the third doped layers 70 both extend along the second direction, the second direction intersects the first direction, and the two directions may be the longitudinal direction and the transverse direction of the solar cell 100, respectively. Figure 8 It can be seen that in this embodiment, the first doping layer 20 and the third doping layer 70 are doping layers that are continuous and unbroken along the second direction, and the two are alternately arranged along the first direction.
[0098] In a back-contact battery, a main grid may be set or not. When a main grid is set, it includes a plurality of third main grids (not shown) and a plurality of fourth main grids (not shown). The plurality of third main grids and the plurality of fourth main grids are alternately arranged along the second direction. The third auxiliary grid is connected to the third main grid and disconnected at the fourth main grid. The fourth auxiliary grid is connected to the fourth main grid and disconnected at the third main grid. The first welding point 50 is set at the third main grid and connected to the third main grid. The second welding point 90 is set at the fourth main grid and connected to the fourth main grid. A plurality of first welding points 50 may be set along the extension direction of the third main grid, and a plurality of second welding points 90 may be set along the extension direction of the fourth main grid.
[0099] When the main grid is not provided, the first welding point 50 and the second welding point 90 can be directly provided in the area covered by the welding strip of the battery. For example, the first welding point 50 can be provided at the disconnection of the third auxiliary grid, and the second welding point 90 can be provided at the disconnection of the fourth auxiliary grid. In this way, the welding point can be directly connected to the welding point through the welding strip in the absence of the main grid. It can be understood that in this case, the welding strip welded to the first welding point 50 can be electrically connected to all the third auxiliary grids, and the welding strip welded to the second welding point 90 can be electrically connected to all the fourth auxiliary grids. Of course, in some embodiments, the third auxiliary grid and the fourth auxiliary grid may not be disconnected, but an insulating glue is provided at the main grid or welding strip of opposite polarity for isolation, which is not specifically limited here.
[0100] The second type: Fig.11 As shown, in some embodiments, the first doping layer 20 may include a plurality of first sub-doping layers 21 and a second sub-doping layer 22, and the third doping layer 70 may include a plurality of third sub-doping layers 71 and a plurality of fourth sub-doping layers 72. The plurality of first sub-doping layers 21 and the plurality of third sub-doping layers 71 are arranged alternately and spaced in sequence along the first direction on the first surface 11 and extend along the second direction. The plurality of second sub-doping layers 22 and the plurality of fourth sub-doping layers 72 are arranged alternately and spaced in sequence along the second direction on the first surface 11 and extend along the first direction, the first sub-doping layer 21 is disconnected at the fourth sub-doping layer 72 and contacts the second sub-doping layer 22, and the third sub-doping layer 71 is disconnected at the second sub-doping layer 22 and contacts the fourth sub-doping layer 72. The second sub-doping layer 22 has a plurality of first preset regions 201, and the plurality of first preset regions 201 are arranged at intervals along the second direction, and the number of the first solder joints 50 may correspond to the number of the first preset regions 201. In this case, the first solder joint 50 may be disposed on the second sub-doping layer 22 , and the second solder joint 90 may be disposed on the fourth sub-doping layer 72 .
[0101] Specifically, it is not difficult to understand that the first sub-doping layer 21 and the second sub-doping layer 22 together form a comb-shaped first doping layer 20, and the third sub-doping layer 71 and the fourth sub-doping layer 72 together form a comb-shaped third doping layer 70. The first sub-doping layer 21 and the second sub-doping layer 22 can be formed by the same process, and the third doping layer 71 and the fourth sub-doping layer 72 can be formed by the same process.
[0102] Further, in such an embodiment, in the first direction, the length of the first solder joint 50 is greater than the length of the second doping layer 30, and the ratio of the length of the first solder joint 50 above the second doping layer 30 to the total length of the first solder joint 50 is greater than or equal to 20%.
[0103] In this way, when the length of the first solder joint 50 in the first direction is relatively large, setting the ratio between the length of the first solder joint 50 above the second doping layer 30 (i.e., the length of the orthographic projection of the first solder joint 50 in the thickness direction overlapping with the second doping layer 30) and the total length of the first solder joint 50 to be greater than or equal to 20% can effectively ensure the welding tension of the first solder joint 50 and avoid insufficient welding tension.
[0104] Preferably, in such an embodiment, in order to ensure the welding tension of the first welding spot 50 , the ratio of the length of the first welding spot 50 located above the second doping layer 30 to the total length of the first welding spot 50 is greater than or equal to 50%.
[0105] In some embodiments, the ratio of the orthographic projection area of the second doping layer 30 on the second sub-doping layer 22 to the area of the second sub-doping layer 22 is less than 50%. In this way, it is possible to avoid the second doping layer 30 being too large in area, which may cause the second doping layer 30 to be more easily recombined with the second sub-doping layer 22 and cause a large recombination loss.
[0106] Specifically, in such an embodiment, "the ratio of the area of the orthographic projection of the second doping layer 30 on the second sub-doping layer 22 to the area of the second sub-doping layer 22 is less than 50%" can mean that the ratio of the area of all second doping layers 30 on a single second sub-doping layer 22 to the single second sub-doping layer 22 is less than 50%, or it can mean that the ratio of the sum of the areas of all second doping layers 30 on the entire back contact battery to the sum of the areas of all second sub-doping layers 22 is less than 50%. There is no specific limitation here, and the first one is preferred.
[0107] Furthermore, if Fig.11 As shown, in such an embodiment, in the first direction, the distance between two adjacent first welding points 50 may be 3 mm-40 mm.
[0108] In this way, by setting the distance between two adjacent first solder joints 50 within this reasonable range, the first solder joints 50 can be basically within a reasonable distance, so that there can be enough first solder joints 50 on the same second sub-doping layer 22, thereby avoiding cold solder joints when welding solder strips and ensuring the reliability of welding.
[0109] Specifically, in such an embodiment, the spacing between two adjacent first welding points 50 may be, for example, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, 15mm, 20mm, 25mm, 30mm, 35mm, 40mm or any value between 3mm-40mm, and is not limited here.
[0110] like Figure 7 and Fig.10 As shown, in some embodiments, the third doping layer 70 has a plurality of second preset regions 701, and the solar cell 100 may further include a fourth doping layer 110, which is stacked on the second preset regions 701, and the fourth doping layer 110 has an opposite polarity to the third doping layer 70;
[0111] like Figure 7 As shown, in the case where the third doping layer 70 is stacked on the second surface 12, the second passivation film layer 80 covers the third doping layer 70 and the fourth doping layer 110, the roughness of the surface 111 of the fourth doping layer 110 in contact with the second passivation film layer 80 is greater than the roughness of the surface 702 of the third doping layer 70 in contact with the second passivation film layer 80, and the orthographic projection of the second solder joint 90 on the third doping layer 70 at least partially overlaps with the orthographic projection of the fourth doping layer 110 on the third doping layer 70.
[0112] like Fig.10 As shown, in the case where the third doping layer 70 is stacked on the first surface 11, the first passivation film layer 40 covers the first doping layer 20, the second doping layer 30, the third doping layer 70 and the fourth doping layer 110, the roughness of the surface 111 of the fourth doping layer 110 in contact with the first passivation film layer 40 is greater than the roughness of the surface 702 of the third doping layer 70 in contact with the first passivation film layer 40, and the orthographic projection of the second solder joint 90 on the third doping layer 70 at least partially overlaps with the orthographic projection of the fourth doping layer 110 on the third doping layer 70.
[0113] In this way, while increasing the tensile force of the first welding point 50 during welding, the tensile force of the second welding point 90 during welding can also be effectively increased, thereby effectively preventing the second welding point 90 from detaching during welding.
[0114] See also Figure 7 and Fig.10In some embodiments, the solar cell 100 may further include a second isolation layer 120 , which is stacked on the second preset region 701 and located between the third doping layer 70 and the fourth doping layer 110 .
[0115] In this way, the fourth doping layer 110 can be separated from the third doping layer 70 by the second isolation layer 120 to avoid direct contact between the two, while also ensuring the passivation effect of the third doping layer 70 .
[0116] Of course, it is understandable that, in some embodiments, it is not necessary to provide the second isolation layer 120 to separate the third doping layer 70 and the fourth doping layer 110 , and this is not specifically limited herein.
[0117] In some embodiments, the thickness of the second isolation layer 120 may be greater than 2 nm. In this way, it is possible to avoid a situation where the thickness of the second isolation layer 120 is too small, which would significantly increase the difficulty of the process.
[0118] Furthermore, in some embodiments, the second isolation layer 120 may include at least one of a silicon oxide film layer, a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, a silicon carbide film layer, and an intrinsic amorphous silicon film layer.
[0119] Specifically, in such an embodiment, the second isolation layer 120 may or may not have a tunneling function, and may be an insulating layer or a non-insulating layer. There is no specific limitation here, and the specific film layer may be selected according to different types of battery cells.
[0120] For example, when the cell is a Topcon solar cell and a back contact cell, the second isolation layer 120 may be at least one of a silicon oxide film layer, a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, and a silicon carbide film layer, and the second isolation layer 120 may or may not have a tunneling function.
[0121] When the cell is a HJT solar cell, the second isolation layer 120 may be an intrinsic amorphous silicon layer. It is understood that the specific selection of the second isolation layer 120 is merely exemplified herein, but it cannot be construed as a limitation to the present application.
[0122] In some embodiments, the orthographic projection of the second solder joint 90 on the third doping layer 70 is completely located in the second preset area 701 , that is, in the thickness direction of the solar cell 100 , the second solder joint 90 is completely located above the fourth doping layer 110 .
[0123] In this way, the second welding point 90 is completely located in the second preset area 701, and the entire bottom of the second welding point 90 has the fourth doping layer 110, which can maximize the welding tension at the second welding point 90, thereby ensuring the reliability of welding.
[0124] Specifically, in such an embodiment, the area of the second preset region 701 may preferably be just equal to the orthographic projection area of the second welding point 90 or slightly larger than the orthographic projection area of the second welding point 90 .
[0125] Of course, in some embodiments, the orthographic projection area of the second solder joint 90 on the third doping layer 70 may also be greater than the orthographic projection area of the fourth doping layer 110 on the third doping layer 70 (that is, the area of the second preset area 701). For example, a single second solder joint 90 may correspond to multiple fourth doping layers 110. In this case, the second solder joint 90 may completely cover the fourth doping layer 110. In this case, the ratio of the overlapping area of the fourth doping layer 110 and the second solder joint 90 to the total area of the second solder joint 90 may be greater than 20% to avoid too small welding tension.
[0126] In some embodiments, the thickness of the fourth doping layer 110 may be 5 nm-400 nm.
[0127] In this way, it is possible to effectively avoid the fourth doping layer 110 being too thin to cause poor tensile reinforcement effect, the fourth doping layer 110 being too thin to cause increased process difficulty, and the fourth doping layer 110 being too thick to cause increased cost.
[0128] Specifically, the thickness of the fourth doping layer 110 may be 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm or any value between 5nm and 400nm, and is not limited here.
[0129] Furthermore, if Fig.11 As shown, in the case where the third doping layer 70 is disposed on the first surface 11 and the first doping layer 20 includes a plurality of first sub-doping layers 21 and a second sub-doping layer 22, and the third doping layer 70 includes a plurality of third sub-doping layers 71 and a plurality of fourth sub-doping layers 72, the second sub-doping layer 22 has a plurality of first preset regions 201, the plurality of first preset regions 201 are arranged at intervals along the second direction, and the number of the first welding points 50 corresponds to the number of the first preset regions 201. The fourth sub-doping layer 72 has a plurality of second preset regions 701, the plurality of second preset regions 701 are arranged at intervals along the first direction, and the number of the second welding points 90 pairs corresponds to the number of the second preset regions 701, that is, in such a case, the fourth doping layer 110 is stacked on the second preset regions 701 of the fourth sub-doping layer 72.
[0130] like Fig.11As shown, in such an embodiment, in the first direction, the length of the second solder joint 90 may be greater than the length of the fourth doping layer 110, and the ratio of the length of the second solder joint 90 located above the fourth doping layer 110 to the total length of the second solder joint 90 is greater than or equal to 20%.
[0131] In this way, when the length of the second solder joint 90 in the first direction is relatively large, setting the ratio between the length of the second solder joint 90 above the fourth doping layer 110 (i.e., the length of the orthographic projection of the second solder joint 90 in the thickness direction overlapping with the fourth doping layer 110) and the total length of the second solder joint 90 to be greater than or equal to 20% can effectively ensure the welding tension of the second solder joint 90 and avoid insufficient welding tension.
[0132] Preferably, in such an embodiment, in order to ensure the welding tension of the second welding spot 90 , the ratio of the length of the second welding spot 90 located above the fourth doping layer 110 to the total length of the second welding spot 90 is greater than or equal to 50%.
[0133] In some embodiments, the ratio of the orthographic projection area of the fourth doping layer 110 on the fourth sub-doping layer 72 to the area of the fourth sub-doping layer 72 is less than 50%. In this way, it is possible to avoid the fourth doping layer 110 being more likely to recombine with the fourth sub-doping layer 72 due to the large area ratio of the fourth doping layer 110, thereby preventing the fourth doping layer 110 from being more likely to recombine with the fourth sub-doping layer 72 and causing a large recombination loss.
[0134] Specifically, in such an embodiment, “the ratio of the area of the orthographic projection of the fourth doping layer 110 on the fourth sub-doping layer 72 to the area of the fourth sub-doping layer 72 is less than 50%” may mean that the ratio of the area of all fourth doping layers 110 on a single fourth sub-doping layer 72 to the area of a single fourth sub-doping layer 72 is less than 50%, or it may mean that the ratio of the sum of the areas of all fourth doping layers 110 on the entire back contact battery to the sum of the areas of all fourth sub-doping layers 72 is less than 50%. There is no specific limitation here, and the first one is preferred.
[0135] Furthermore, if Fig.11 As shown, in such an embodiment, in the first direction, the distance between two adjacent second welding points 90 may be 3 mm-40 mm.
[0136] In this way, by setting the distance between two adjacent second solder joints 90 within this reasonable range, the second solder joints 90 can be basically within a reasonable distance, so that there can be enough second solder joints 90 on the same fourth sub-doping layer 72, thereby avoiding cold solder joints when welding solder strips and ensuring the reliability of welding.
[0137] Specifically, in such an embodiment, the spacing between two adjacent second welding points 90 may be, for example, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, 15mm, 20mm, 25mm, 30mm, 35mm, 40mm or any value between 3mm-40mm, and is not limited here.
[0138] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0139] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A solar cell, characterized in that: include: Silicon wafer; A first doped layer stacked on the silicon wafer, wherein the first doped layer has a plurality of first preset regions; a second doping layer, wherein the second doping layer is stacked on the first preset region, and the polarity of the second doping layer is opposite to that of the first doping layer; a first passivation film layer, wherein the first passivation film layer is stacked on the second doping layer and the first doping layer, and the roughness of a surface of the second doping layer in contact with the first passivation film layer is greater than the roughness of a surface of the first doping layer in contact with the first passivation film layer; and A plurality of first welding points, wherein the first welding points are arranged on the first passivation film layer, and an orthographic projection of the first welding points on the first doping layer at least partially overlaps with an orthographic projection of the second doping layer on the first doping layer.
2. The solar cell according to claim 1, characterized in that: The solar cell sheet further includes a first isolation layer, which is stacked on the first preset area and located between the first doping layer and the second doping layer.
3. The solar cell according to claim 2, characterized in that: The thickness of the first isolation layer is greater than 2 nm.
4. The solar cell according to claim 2, characterized in that: The first isolation layer includes at least one of a silicon oxide film layer, a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, a silicon carbide film layer and an intrinsic amorphous silicon film layer.
5. The solar cell according to claim 1, characterized in that: The orthographic projection of the first welding point on the first doping layer is completely located within the first preset area.
6. The solar cell according to claim 1, characterized in that: The thickness of the second doping layer is 5nm-400nm.
7. The solar cell according to claim 1, characterized in that: The first passivation film layer includes at least one of a silicon nitride film layer, an aluminum oxide film layer, a silicon oxynitride film layer, an intrinsic amorphous silicon film layer, and a TCO film layer.
8. The solar cell according to claim 1, characterized in that: The solar cell further comprises a third doping layer, a second passivation film layer and a plurality of second solder joints, the polarity of the third doping layer is opposite to the polarity of the first doping layer, and the silicon wafer has a first surface and a second surface opposite to each other; wherein the first doped layer is stacked on the first surface, the third doped layer is stacked on the second surface, the second passivation film layer is stacked on the third doped layer, and the second solder joint is arranged on the second passivation film layer; or The first doping layer and the third doping layer are both stacked on the first surface, the first passivation film layer is stacked on the first doping layer, the second doping layer and the third doping layer, the second welding point is also arranged on the first passivation film layer, and the second passivation film layer is stacked on the second surface.
9. The solar cell according to claim 8, characterized in that: In the case where the third doping layer is stacked on the first surface, on the first surface, a plurality of the first doping layers and a plurality of the third doping layers are alternately arranged in sequence along a first direction, and both the first doping layers and the third doping layers extend along a second direction, and the second direction intersects with the first direction.
10. The solar cell according to claim 8, characterized in that: In the case where the third doping layer is stacked and arranged on the first surface, the first doping layer includes a plurality of first sub-doping layers and a second sub-doping layer, and the third doping layer includes a plurality of third sub-doping layers and a plurality of fourth sub-doping layers; A plurality of the first sub-doping layers and a plurality of the third sub-doping layers are alternately arranged in sequence along a first direction and are disposed on the first surface at intervals and extend along a second direction, wherein the second direction intersects the first direction; A plurality of the second sub-doping layers and a plurality of the fourth sub-doping layers are arranged alternately and spaced in sequence along the second direction on the first surface and extend along the first direction, the first sub-doping layer is disconnected at the fourth sub-doping layer and contacts the second sub-doping layer, and the third sub-doping layer is disconnected at the second sub-doping layer and contacts the fourth sub-doping layer; The second sub-doping layer has a plurality of the first preset regions, and the plurality of the first preset regions are arranged at intervals along the second direction.
11. The solar cell according to claim 10, characterized in that: In the first direction, the length of the first solder joint is greater than the length of the second doping layer, and a ratio of a length of the first solder joint located above the second doping layer to a total length of the first solder joint is greater than or equal to 20%.
12. The solar cell according to claim 10, characterized in that: In the first direction, a ratio of a length of the first solder joint located above the second doping layer to a total length of the first solder joint is greater than or equal to 50%.
13. The solar cell according to claim 10, characterized in that: A ratio of an orthographic projection area of the second doping layer on the second sub-doping layer to an area of the second sub-doping layer is less than or equal to 50%.
14. The solar cell according to claim 10, characterized in that: In the first direction, the distance between two adjacent first welding points is 3 mm-40 mm.
15. The solar cell according to claim 8, characterized in that: The third doping layer has a plurality of second preset regions, and the solar cell further comprises a fourth doping layer, the fourth doping layer is stacked on the second preset regions, and the fourth doping layer has a polarity opposite to that of the third doping layer; In the case where the third doped layer is stacked on the second surface, the second passivation film layer covers the third doped layer and the fourth doped layer, the roughness of the surface of the fourth doped layer in contact with the second passivation film layer is greater than the roughness of the surface of the third doped layer in contact with the second passivation film layer, and the orthographic projection of the second welding point on the third doped layer at least partially overlaps with the orthographic projection of the fourth doped layer on the third doped layer; In the case where the third doped layer is stacked on the first surface, the first passivation film layer covers the first doped layer, the second doped layer, the third doped layer and the fourth doped layer, the roughness of the surface of the fourth doped layer in contact with the first passivation film layer is greater than the roughness of the surface of the third doped layer in contact with the first passivation film layer, and the orthographic projection of the second welding point on the third doped layer at least partially overlaps with the orthographic projection of the fourth doped layer on the third doped layer.
16. The solar cell according to claim 15, characterized in that: The solar cell further includes a second isolation layer, which is stacked on the second preset area and located between the third doping layer and the fourth doping layer.
17. The solar cell according to claim 15, characterized in that: The orthographic projection area of the second preset region on the silicon wafer is greater than or equal to the orthographic projection area of the second solder joint on the silicon wafer, and the second solder joint is completely located within the second preset region.
18. The solar cell according to claim 15, characterized in that: In the case where the third doping layer is stacked and arranged on the first surface, the first doping layer includes a plurality of first sub-doping layers and a second sub-doping layer, and the third doping layer includes a plurality of third sub-doping layers and a plurality of fourth sub-doping layers; A plurality of the first sub-doping layers and a plurality of the third sub-doping layers are alternately arranged in sequence along a first direction and are disposed on the first surface at intervals and extend along a second direction, wherein the second direction intersects the first direction; A plurality of the second sub-doping layers and a plurality of the fourth sub-doping layers are arranged alternately and spaced in sequence along the second direction on the first surface and extend along the first direction, the first sub-doping layer is disconnected at the fourth sub-doping layer and contacts the second sub-doping layer, and the third sub-doping layer is disconnected at the second sub-doping layer and contacts the fourth sub-doping layer; The second sub-doping layer has a plurality of the first preset regions, which are spaced apart along the first direction; the fourth sub-doping layer has a plurality of the second preset regions, which are spaced apart along the first direction.
19. A battery assembly, characterized in that: The invention comprises the solar cell sheets as described in any one of claims 1 to 18.
20. A photovoltaic system, characterized in that: A battery assembly comprising the battery assembly of claim 19.
Citation Information
Cited By
Solar cell sheet, cell assembly and photovoltaic system
EP4590093B1
Solar cell sheet, cell assembly and photovoltaic system
WO2025218816A1