Laser ablation method and element made of brittle-hard material

The self-regulating laser ablation process with controlled plasma overlap and high pulse frequencies ensures consistent depth and stable fracture points in brittle-hard materials, addressing precision and power fluctuations in existing laser processing methods.

DE102014109791B4Active Publication Date: 2024-10-24SCHOTT AG
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
DE102014109791
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2014-07-11
Publication Date
2024-10-24
Estimated Expiration
2034-07-11

AI Technical Summary

Technical Problem

Existing laser processing methods for brittle-hard materials face challenges in achieving precise and consistent depth of depressions, particularly due to fluctuations in laser power and potential damage to optical elements, especially in the UV wavelength range, leading to inconsistent fracture points and potential destruction.

Method used

A self-regulating laser ablation process using pulsed laser pulses with controlled overlap and frequency, generating plasma to shield material from further ablation, ensuring consistent depth independent of laser power fluctuations, with a feed speed of up to 30 mm/s and pulse frequencies of at least 10 kHz, focusing on wavelengths less than 600 nm for materials like glass.

Benefits of technology

The process achieves consistent depth of depressions between 30 µm and 150 µm, suitable for creating fine structures with controlled fracture points, reducing the risk of laser power variations and ensuring stable, clean breaks over time, even with varying laser performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for producing a depression (6) in an element (2) made of brittle-hard material, in which a laser beam (40) with laser pulses (41) is directed onto the surface (20) of the element (2) by means of a pulsed laser (4), wherein the laser pulses (41) generate a plasma (8) with vaporized material on the surface (20) and thereby ablate material from the surface (20) of the element (2), and wherein the laser beam (40) is guided over the surface (20) of the element (2) at a feed rate of at most 30 mm / s, such that successive laser pulses (41) strike different locations on the surface (20) of the element (2), and wherein the pulse frequency and the feed rate of the laser beam (40) on the surface (20) of the element (2) are adjusted such thatthat the light spots (42) of successive laser pulses (41) of the laser beam (40) overlap on the surface (20) of the element (2) and the plasma (8) generated by the preceding laser pulse (41) still exists when a laser pulse (41) strikes, and wherein material is removed with the laser pulses (41) to a depth in the range between 30 µm and 150 µm.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention generally relates to material processing using lasers. More specifically, the invention relates to the insertion of recesses, such as trenches, into brittle-hard materials, as well as elements made of brittle-hard material with trench-shaped recesses.

[0002] US 2012 / 0 196 454 A1 relates to the laser-based modification of a workpiece, wherein the focusing and directing of laser pulses onto the workpiece is carried out at a pulse repetition rate that is sufficiently high so that material is efficiently removed from the area, reducing the amount of unwanted material compared to a lower repetition rate.

[0003] DE 10 2005 037 412 A1 relates to a laser machining method for forming a laser groove along dividing lines by applying a pulsed laser beam along the dividing lines formed on a workpiece, the method comprising the steps of forming the focal point of the pulsed laser beam in the shape of an oval, positioning the long axis of the oval focal point along each of the dividing lines, and moving the focal point and the workpiece along the dividing line relative to each other.

[0004] JP 2006 - 36 602 A relates to a ceramic component having a recessed part on at least one main surface and being composed of a main component and a plurality of additional components, wherein the recessed part is formed by heat irradiation and wherein there is substantially no melt layer of the ceramic forming the main component on the surface layer of the recessed part.

[0005] EP 2 246 146 A1 relates to a laser processing method comprising directing pulsed laser light onto a surface of a substrate made of brittle material and a laser light scanning step for scanning laser light along a planned scribe line, wherein the method comprises certain parameters for the laser intensity of the pulsed laser light and the value resulting from multiplying the amount of heat supplied by the linear expansion coefficient of the brittle material and the number of pulses within a square that describes the diameter of the condensed light of the pulsed laser.

[0006] EP 0 931 620 A1 describes a device and method for laser ablation of quartz glass using a laser whose light wavelength, at 266 nm, is longer than the absorption edge of quartz glass at 170 nm and less. In this method, the laser is directed through the quartz glass onto a target. This creates a plasma cloud on the target, which spreads between the quartz glass and the target. This secondary plasma cloud is then used to ablate material from the quartz glass. This process is very complex and slow. The laser is operated at a pulse frequency of 1 Hz to provide sufficient pulse energies for indirect ablation.

[0007] JP 2000-348621 A discloses a process in which a glass solder joint between the screen and the funnel of cathode-ray tubes is loosened or separated using a laser. The separation or separation occurs by briefly evaporating the glass inside the glass joint.

[0008] This procedure therefore results in immediate, deep damage, which in itself is advantageous in order to be able to easily separate the two parts.

[0009] The process described in JP 2000-348 621 A is intended to separate the canopy and funnel for recycling. The exact shape of the break line is not important here.

[0010] However, the process will therefore not be suitable for reliably ensuring a very precise fracture edge. Furthermore, difficulties arise if the ablation and separation of the parts are to be separated in time. Aging phenomena can occur in this case, especially with glass. Chemical changes in the surface cause a change in the fracture force. This change can also be inhomogeneous, so that the required fracture force varies locally, and thus the fracture edge can be disturbed.

[0011] It would therefore be desirable to be able to introduce predetermined breaking points into an element made of brittle material in such a way that a clean division of the element with a defined breaking force is possible even long after the predetermined breaking point has been inserted.

[0012] Even with depressions for purposes other than inserting a predetermined breaking point, the laser ablation process presents the problem that the depth of such a depression depends on the laser power. However, the laser power can fluctuate considerably during operation, particularly with lasers in the UV wavelength range due to the higher energy density and the resulting negative impact on the optical elements (even to the point of destruction). In this case, it would be desirable if the depth of an ablated depression could be adjusted as independently as possible from the laser power.

[0013] This object is achieved by the subject matter of the independent claims. Advantageous embodiments and further developments of the invention are specified in the dependent claims.

[0014] It was found that by choosing the right process parameters for laser ablation, a self-regulating process is obtained that remains stable even when the laser power drops by more than 40%, provided the pulse energy does not fall below the ablation threshold.

[0015] Accordingly, the invention provides a method for producing a recess in an element made of brittle material, in which a laser beam with laser pulses is directed onto the surface of the element by means of a pulsed laser, wherein the laser pulses generate a plasma with vaporized material on the surface and thus material is ablated from the surface of the element, and wherein the laser beam is guided over the surface of the element at a feed rate of at most 30 mm / s so that successive laser pulses impinge on different locations on the surface of the element, and wherein the pulse frequency and the feed rate of the laser beam on the surface of the element are adjusted such that the light spots of successive laser pulses of the laser beam overlap on the surface of the element and the plasma generated by the respective previous laser pulse still exists when a laser pulse impinges,and wherein the laser pulses are used to remove material with a thickness or depth in the range between 30 µm and 150 µm.,

[0016] During laser ablation with a pulsed laser, particularly an ultrashort pulse laser, the aforementioned self-regulating process occurs at very low scanning speeds because the impact points of the pulses overlap. Surprisingly, when the plasma generated by a previous pulse overlaps with the subsequent pulse in time and space, the ablation depth is almost independent of the laser power over a wide power range. The following mechanism is suspected: The first pulses evaporate the material to a certain depth, creating a plasma. When a certain energy level is reached, this plasma shields the underlying material from further laser irradiation. Thus, even with a sharp decrease in laser power, the ablation depth decreases only slightly or not at all.

[0017] It has also been shown that the stability of the process, or rather the constancy of the removal depth, is particularly pronounced when the laser spot is held at a fixed location / point, i.e., the laser beam is stationary, and the element to be processed is moved. In other words, according to a further development of the invention, the element made of brittle material is moved relative to the laser beam to generate a feed rate of the laser beam.

[0018] According to one embodiment of the invention, without limitation to a specific embodiment, a pulsed Nd-YAG laser is used as the laser.

[0019] According to another preferred embodiment of the invention, the laser beam is frequency multiplied. A frequency multiplier is provided for this purpose. If an Nd:YAG laser with a wavelength of 1064 nm is used, a KDP crystal, for example, is suitable as a frequency doubler to generate green light with a wavelength of 532 nm. The laser beam is then directed onto the surface of a brittle-hard material to be treated using focusing optics.

[0020] According to a further development of the invention, the frequency of the laser beam is tripled. If an Nd:YAG laser is tripled using the frequency multiplier, the wavelength of the laser pulses impinging on the surface of the element is 355 nm, i.e., a wavelength in the ultraviolet spectral range. In general, the two aforementioned light wavelengths, generally light wavelengths of less than 600 nm, are particularly suitable for processing glass, a brittle material. In general, without being limited to a specific embodiment, a development of the invention therefore provides for the recess to be created using a laser beam with a light wavelength of less than 600 nm.

[0021] In general, without limitation to a specific embodiment, the method according to the invention is particularly suitable for creating a recess in a glass element. Preferred glass types for this purpose are borosilicate glasses, including aluminoborosilicate glasses.

[0022] With the invention, virtually any desired geometry of depressions can be created by appropriately guiding the laser beam over the surface. However, it is generally preferred that a depression be inserted into the element in the form of a trench.

[0023] With the invention, virtually any desired geometry of depressions can be created by appropriately guiding the laser beam over the surface. However, it is generally preferred that a depression be inserted into element 2 in the form of a trench.

[0024] In general, without limitation to a specific embodiment, a laser is operated at a pulse frequency of at least 10 kHz, preferably at least 50 kHz. These high pulse frequencies allow the process to be carried out economically with sufficient feed rates. In particular, these pulse frequencies ensure that the plasma is maintained between individual pulses.

[0025] The plasma still present above the surface when the next laser pulse hits counteracts variations in laser power. If the laser power decreases, the plasma is weaker when the next laser pulse arrives. This also weakens the shielding effect of the plasma, allowing the laser light to penetrate more easily to the surface of the element being processed.

[0026] In this way, the laser pulses can be used to remove material with a thickness or depth ranging between 30 µm and 150 µm. The self-regulating mechanism allows the removal depth to be kept very constant within the above-specified range. Thus, according to one embodiment of the invention, the removal depth is approximately 80 µm. The invention is therefore generally particularly suitable for introducing extremely small structures into the material.

[0027] In order to ensure a spatial overlap of small light spots for inscribing fine structures in the element to be processed, it is generally preferred according to the invention, without limitation to a specific example, if the laser beam is guided over the surface of the element at a feed rate of at most 22 mm / s.

[0028] Furthermore, it is preferred that the laser beam is focused so that the light spot on the surface of the element has a diameter of at most 70 µm, preferably at most 50 µm, in order to be able to produce fine structures.

[0029] According to a further development of the invention, it is generally provided that an element in the form of a tube is provided which has an axial section with an enlarged circumference, wherein a circumferentially extending recess is inserted in the axial section with an enlarged circumference.

[0030] Without being limited to a specific embodiment, according to a preferred embodiment of the invention, a recess having a width of at most 50 µm is produced.

[0031] Due to the comparatively slow ablation process according to the invention due to the spatial overlap of the laser pulses, a deep depression can generally be created in a single pass of the laser beam, without being limited to specific exemplary embodiments. In general, a further development of the invention provides for a depression of at least 30 µm, preferably at least 50 µm, to be created in a single pass of the laser beam. According to the invention, the feed rates are 30 mm / s or less. According to one exemplary embodiment, the ablation takes place at a feed rate of 15 mm / s with a laser repetition frequency of approximately 100 kHz. At first glance, this slow processing appears disadvantageous.However, especially when processing thin tubes, especially capillaries, the slow processing time is hardly significant, since the circumference and thus the distance to be covered by the laser beam are correspondingly short.

[0032] The method, in particular, produces depressions that have a high aspect ratio between width and depth. Generally, without limitation to specific embodiments, an element made of brittle-hard material is provided, which has at least one trench-shaped depression whose depth is at least as great as its width. The width of the depression, as already stated above, is at most 50 µm and the depth is between 30 µm and 150 µm, preferably between 50 µm and 100 µm.

[0033] Without being limited to specific embodiments, a further development of the invention provides that the side walls of the recess have an opening angle on the surface of the element which is at most 45°.

[0034] The invention is described in more detail below, also using exemplary embodiments and with reference to the figures. Like reference numerals in the figures designate like or corresponding elements.

[0035] They show: Fig. 1 schematically shows a structure for carrying out the method according to the invention, Fig. 2 an alternative structure, Fig. 3 schematically shows a cross-section of a pipe processed according to the process, Fig. 4 a microscopic side view of a tube, Fig. 5 a microscopic image of the fracture edge of a pipe broken at the recess, Fig. 6 a cross-section through an element made of brittle material, preferably glass.

[0036] Fig. Figure 1 shows a schematic structure of a device 1 for carrying out the method according to the invention for producing a recess in an element 2 made of brittle material. The device 1 comprises a laser 4 for emitting a pulsed laser beam 40. The laser beam 40 is therefore composed of a sequence of laser pulses 41. For example, a laser with an output power of approximately 40 µJ per pulse can be used.

[0037] A pulsed Nd-YAG laser is used as laser 40.

[0038] In the Fig. In the example shown in Figure 1, the laser beam 40 is frequency multiplied. A frequency multiplier 43 is provided for this purpose. If an Nd:YAG laser with a wavelength of 1064 nm is used, a KDP crystal, for example, is suitable as a frequency doubler to generate green light with a wavelength of 532 nm. The laser beam 40 is then directed onto the surface 20 of an element 2 to be treated, made of brittle material, by means of a focusing optics 44.

[0039] For example, it is proposed to triple the frequency of the laser beam 40. If an Nd:YAG laser is tripled using the frequency multiplier 43, the resulting wavelength of the laser pulses 40 impinging on the surface 20 of the element 2 is 355 nm, i.e., a wavelength in the ultraviolet spectral range. In general, the two aforementioned light wavelengths, generally light wavelengths of less than 600 nm, are particularly suitable for processing glass, a brittle material. Therefore, it is proposed, for example, that the recess 6 be created with a laser beam 40 with a light wavelength of less than 600 nm.

[0040] The method is particularly suitable for producing a recess 6 in a glass element. Preferred glass types for this purpose are borosilicate glasses, including aluminoborosilicate glasses.

[0041] By appropriately guiding the laser beam over the surface, virtually any desired geometry of recesses 6 can be created. It is preferred that a recess 6 be inserted into the element 2 in the form of a trench.

[0042] In the Fig. In the example shown in Figure 1, three laser pulses 41 are shown for illustration purposes only, which are located between the laser 4 and the surface 20 of the element 2. Typically, however, repetition frequencies and distances are used that are so low that the laser pulse 20 fills the optical path between the laser 4 and the surface 20.

[0043] The focusing optics 44 now collimates the laser beam 40 onto a light spot 42 on the surface 20 of the element. The light spot 42 is preferably as small as possible, so that the light spot 42 represents the focus of the laser beam 40 generated by the focusing optics. The laser pulses 41 generate a plasma 8 with vaporized material of the element 2 on its surface 20, so that material is ablated from the surface 20 of the element 2. To create an elongated recess 6, the laser beam 4 is guided over the surface 20 of the element so that successive laser pulses 41 impinge on different locations on the surface 20 of the element 2.

[0044] One possibility is to deflect the laser beam 40. According to a preferred embodiment of the invention, however, the element 2 made of brittle material is moved relative to the laser beam 4 to generate a feed of the laser beam 40. For this purpose, in the Fig. In the example shown in Figure 1, a device 10 is provided for guiding the laser beam 40 over the surface 20 of the element 2. In this example, the device 10 comprises a carriage 101 on which the element 2 is arranged. The carriage 101, and thus also the element 2, is moved relative to the stationary laser 4 in a direction transverse to the direction of incidence of the laser 4, so that an elongated depression 6 is created which extends along the direction of movement of the element 2.

[0045] After the end of a laser pulse 41, the plasma 8 collapses due to the lack of heating power from the laser beam 4, until the next impinging laser pulse 41 generates a new plasma 8, and the ablation process continues. According to the invention, however, the pulse frequency and the feed rate of the laser beam 40 on the surface 20 of the element 2 are adjusted such that the light spots 42 of successive laser pulses 41 of the laser beam 40 overlap on the surface 20 of the element 2, and the plasma 8 generated by the preceding laser pulse 41 still exists when a laser pulse 41 impinges.

[0046] Laser 4 is operated at a pulse frequency of at least 10 kHz, preferably at least 50 kHz. These high pulse frequencies allow the process to be carried out economically with sufficient feed rates. In particular, these pulse frequencies ensure that the plasma is maintained between individual pulses.

[0047] The plasma still present above the surface when the next laser pulse 41 hits counteracts variations in laser power. If the laser power decreases, the plasma is weaker when the next laser pulse arrives. This also weakens the shielding effect of plasma 8, allowing the laser light to penetrate more easily to the surface 20 of the element 2 to be processed.

[0048] In this way, laser pulses 41 can be used to remove material with a thickness or depth in the range between 30 µm and 150 µm. The self-regulating mechanism allows the removal depth to be kept very constant within the range specified above. For example, the removal depth is approximately 80 µm. The process is therefore particularly suitable for introducing the smallest structures into the material.

[0049] Fig. 2 shows a variant of the Fig. 1 device 1 shown.

[0050] In order to ensure a spatial overlap of small light spots 42 for inscribing fine structures in the element to be processed, it is preferred if the laser beam 40 is guided over the surface 20 of the element 2 at a feed rate of at most 22 mm / s.

[0051] Furthermore, it is preferred that the laser beam 40 is focused such that the light spot 42 on the surface 20 of the element 2 has a diameter of at most 70 µm, preferably at most 50 µm, in order to be able to produce fine structures.

[0052] Fig. 2 shows a variant of the Fig. 1. This variant is generally based on the fact that the element 2 made of brittle material is rotated in order to guide the laser beam 40 over the surface of the element 2. The device for guiding the laser beam 40 over the surface 20 of the element 2 comprises a rotation device 102, for example with a chuck, in which the element 2 is clamped and which is driven by a motor with a gear reduction. This embodiment of the invention is particularly suitable, as also in Fig. 2, circumferentially extending recesses are inserted into the lateral surface of an element 2 in the form of a tube 22, particularly preferably in a glass tube.

[0053] The application of the method according to the invention results in a further advantage that makes the invention particularly suitable for processing tubular elements. The plasma, which still exists during the subsequent laser pulse 41, also suppresses ablation of material on the surface facing away from the laser beam due to the shielding. For an element 2 in the form of a tube, this surface is its inner surface. If ablation occurs on the inner surface, particles can be deposited inside the tube. Depending on the application, such particles and other deposits from the ablation can be very disruptive.

[0054] A recess 6, such as that introduced using the method according to the invention, can form a predetermined breaking point according to one embodiment of the invention. The element 2 can then be separated at the predetermined breaking point after the recess 6 has been introduced. A recess in the form of a trench is particularly suitable for forming a predetermined breaking point.

[0055] Glass elements that are to be cut at a defined point are used in the analytical and medical fields, among others. Ampoules are one example. As already explained above, one problem is being able to introduce predetermined breaking points into an element made of brittle material in such a way that the element can be cleanly cut with a defined breaking force even long after the predetermined breaking point has been inserted. It turns out that the method according to the invention is particularly suitable for inserting predetermined breaking points that meet this requirement.

[0056] The problem of creating a clean break edge is further exacerbated when the element is to be cut at a particularly stable point. This is the case, for example, with capillary tubes that have a sectionally enlarged diameter. Such glass capillaries, cut at the section of maximum diameter, are used in chemical analysis, particularly in immunological tests. The section serves as a reaction reservoir, and the adjacent, thinner capillary section absorbs particles formed during the reaction, such as agglutinates.

[0057] For example, it is provided that an element 2 is provided in the form of a tube 22, which has an axial section 23 with an enlarged circumference, wherein a circumferentially extending recess 6 is inserted in the axial section 23 with an enlarged circumference. Fig. Figure 3 shows a schematic cross-section of such a tube 22. The tube 22 has the shape of a capillary. In the axial section 23, the inner and outer diameters of the capillary expand. At the same time, the wall thickness of the tube 22 also tapers toward the axial position with the maximum outer diameter.

[0058] Such a tube 22 can be produced in particular by a method for forming a glass tube, in particular a capillary tube, in a forming section, wherein the tube 22 is one or two open ends. The tube 22 is held and fixed by a holding device. The holding device preferably comprises a first fixing section 14 and a second fixing section. The tube 22 is then heated between the first and second fixing sections. The heating is preferably carried out with a A heating tube is arranged in the second fixing section, which surrounds the tube 22 in a ring-like manner. A gas flow is provided by a gas source and introduced into the tube 22 via at least one of the open ends with a connector communicating with the gas source. In other words, the pressure inside the tube 22 is increased relative to the ambient temperature by means of a gas source. The set pressure inside causes a radial expansion of the tube 22 in the forming section softened by the heating. This forming section is thus formed into the axial section 23 with an enlarged diameter.

[0059] The thus formed tube 22 can then be provided with a recess 6 in the axial section 23 with the aforementioned circumferentially extending recess 6 by laser ablation using the method according to the invention. Preferably, the recess extends completely around the entire circumference and thus has the shape of a closed, annular notch or a closed, annular groove.

[0060] Furthermore, it is also preferred that the recess 6 is inserted at or near the axial position of the tube 22 with the maximum diameter of the section 23.

[0061] This creates a predetermined breaking point which, after the tube has been broken at the recess 6, provides two glass parts with essentially equal-sized extensions at their respective ends, preferably serving as a reaction space.

[0062] Fig. Figure 4 shows a microscopic image of such a tube 22. Specifically, a section of the tube 22 with the axial section 23 is shown. The circumferential recess 6 in the form of an annular groove in the region of the maximum diameter of the axial section 23 is clearly visible. It is also evident from the scale of 500 µm that the recess 6 is very narrow. For example, it is envisaged that a recess 6 with a maximum width of 50 µm is created.

[0063] The recesses 6 that can be produced using the method according to the invention are typically also characterized by steep walls, so that the recesses 6, for a given width, extend deep into the brittle material of the element 2. This is also demonstrated by the example of Fig. 5 clearly. Fig. 5 shows a plan view of the front side of a Fig. 4 machined tube 22. The tube 22 was broken into two parts. The end face of the resulting tube 22 thus extends along the plane perpendicular to the longitudinal axis of the tube 22 at the axial position of the maximum diameter of the region 23.

[0064] The recess 6 extends as in the Fig. 3 and Fig. 4, from the outer side 25 of the tube 22 to a depth that is less than the wall thickness of the tube 22. When the element 2, or here the tube 22, breaks at the predetermined breaking point formed by the recess 6, a fracture surface 26 is created which extends from the recess 6 to the side of the element 2 opposite the side with the recess 6. In the case of a tube 22, this opposite side is formed by the inner side 24 of the tube 22.

[0065] The fracture surface 26 and the wall of the former depression 6 are shown in the image of the Fig. 5 can be clearly seen due to the different surface textures. The fracture surface 26, which appears bright in the image, is very smooth, while the wall remaining from the depression 6 exhibits a certain roughness due to the ablation process.

[0066] Due to the comparatively slow ablation process according to the invention due to the spatial overlap of the laser pulses, a deep depression can be created in a single pass of the laser beam. For example, it is provided that a depression of at least 30 µm, preferably at least 50 µm, is created in a single pass of the laser beam. According to the invention, the feed rates are 30 mm / s or less. According to one embodiment, the ablation is carried out at a feed rate of 15 mm / s at a laser repetition frequency of approximately 100 kHz. At first glance, this slow processing appears disadvantageous. However, particularly when processing thin tubes 22, in particular capillaries, as shown in the examples of Fig. As shown in Figures 3 to 5, the slow processing time is of little consequence, since the circumference and thus the distance to be covered by the laser beam are correspondingly short. Thus, the tube 22 of the Fig. In the example shown in Figure 4, the recess 6 has a diameter of only approximately 1.5 mm. At a feed rate of 15 mm / s, the machining time is therefore only approximately 0.3 s. This machining time is therefore typically less than the time required to fix the tube.

[0067] The removal depth D is in Fig. 5 is marked with a double arrow and is approximately 80 µm. Such a removal depth is typical for the above-mentioned pulse frequencies of at least 50 kHz.

[0068] A trench-shaped depression created using the method according to the invention has several characteristics that make it particularly suitable as a long-term stable predetermined breaking point. In particular, the breaking force required for breaking can be kept essentially constant almost independently of the storage period. In comparison, this is not the case with conventional scoring, as the score can partially heal, particularly under the influence of moisture. This can cause the required breaking force to increase locally. Conversely, storage under tension can lead to stress corrosion cracking, which can lead to a locally reduced required breaking force or even to premature fracture. Both effects can occur simultaneously, so that the overall required breaking force becomes inhomogeneous along the predetermined breaking point. If there is a time delay between scoring and breaking, this can lead to blurred and unclean fracture edges.

[0069] In contrast, a recess 6 inserted according to the invention serves as a predetermined breaking point suitable for delayed breaking, whereby further processing steps can also be performed between the insertion of the recess and the breaking. In particular, a cleaning step with an aqueous medium and / or a coating step can be performed between the scoring and the breaking. Water, in particular, otherwise leads to the aforementioned phenomena of crack healing and stress corrosion cracking. A preferred application of such a product is a sample carrier (also in the form of a sample container) for medical, biological, or chemical samples.

[0070] According to one embodiment of the invention, a method is therefore provided for further processing and use of a sample carrier with an element made of brittle-hard material, wherein an element 2 made of brittle-hard material, preferably made of glass, is provided with at least one recess 6 serving as a predetermined breaking point using the method according to the invention, is cleaned with an aqueous medium after insertion of the recess 6, is subsequently coated if necessary, and is then broken at the predetermined breaking point. In the case of tubular sample carriers, as also the Fig. 3 to Fig. As shown in Figure 5, after breaking, a further cleaning step can be carried out before filling the tube with a sample.

[0071] The following are based on Fig. 6 describes the characteristics of a product that can be produced using the process according to the invention. Fig. 6 shows a cross section through an element 2 made of brittle material, preferably glass, wherein a section of the element 2 is shown with two examples of depressions 6 according to the invention which are designed in the form of a trench for the purpose of a predetermined breaking point.

[0072] The method is used to create depressions 6 that have a high aspect ratio between width and depth. In both cases Fig. 6, the depth D is greater than the width B of the depression 6. For example, an element 2 made of brittle material is provided, which has at least one trench-shaped depression 6, the depth of which is at least as great as its width, wherein the width of the depression, as already stated above, is at most 50 µm and the depth is between 30 µm and 150 µm, preferably between 50 µm and 100 µm. Furthermore, as in both Fig.In the examples shown in Figure 6, the two side walls 60, 61 extend toward each other from the surface of the element 2. The side walls can extend toward each other essentially in a straight line, as in the embodiment shown on the right, or with a curve, as in the example shown on the left.

[0073] In both cases, the opening angle α of the side walls 60, 61 is marked on the surface 20 of the element 2. The opening angle α, i.e. the angle between opposite wall sections of the walls 60, 61, is smaller in the case of the curved side walls shown on the left than in the case of straight side walls.

[0074] For example, it is provided that the side walls 60, 61 of the recess have an opening angle α at the surface 20 of the element 2 of a maximum of 45°. Assuming a typical depth D of the recess 6 of approximately 80 µm and a width of 50 µm, the embodiment shown on the right results in an opening angle of approximately 35°.

[0075] The comparatively small opening angle is advantageous for generating high tensile stresses at the tip 63 of the recess 6 when the element 2 is subjected to a bending stress and thus enabling the element 2 to be easily separated at the recess.

[0076] On the other hand, a very pointed depression 6 can lead to phenomena similar to crack healing. In depressions produced according to the invention, however, a rounding of the tip 63 is evident. While this rounding leads to slightly increased fracture stresses, it also results in a predetermined breaking point that is long-term stable, even during cleaning processes and in contact with aqueous media. The radius R of the tip 63 is generally less than 1 µm, but at least 50 nm.

[0077] In summary, the method according to the invention can be used to produce an element 2 made of brittle-hard material which has a trench-shaped depression 6, wherein the trench-shaped depression is produced with a width of at most 50 µm and a depth of at most 150 µm, preferably at most 100 µm, wherein the side walls of the depression 6 on the surface 20 of the element 2 have an opening angle of less than 45° and wherein the two side walls 60, 61 of the depression 6 converge in a tip 63 which has a radius in the range from 0.05 µm to 1 µm.

[0078] For the purpose of a predetermined breaking point, it is still less sensible to provide very thick walls or thicknesses of element 2, in order to avoid excessively high breaking forces. Element thicknesses at recess 6 in the range of 200 µm to 2 mm are preferred. The depth of the recess is not included in this specification; therefore, the thickness is measured from a point adjacent to the recess.

[0079] It will be apparent to those skilled in the art that the invention can be varied in many ways within the scope of the subject matter of the patent claims. In particular, the features of the individual embodiments can also be combined with one another. List of reference symbols 1 Device for producing a recess 2 Element made of brittle material 4 lasers 6 Deepening 8 Plasma 10 Device for guiding the laser beam 40 over the surface 20 of the element 2 20 surface of 2 22 pipe 23 axial section of 22 with extended circumference 24 Inside of 22 25 outside of 22 26 Fracture surface 40 laser beam 41 laser pulses 42 light spot 43 frequency multipliers 44 Focusing optics 60, 61 side walls of 6 63 top of 6 101 sleds 102 Rotation device

Claims

[1] Method for producing a depression (6) in an element (2) made of brittle material, in which a laser beam (40) with laser pulses (41) is directed onto the surface (20) of the element (2) by means of a pulsed laser (4), wherein the laser pulses (41) generate a plasma (8) with vaporized material on the surface (20) and thus material is ablated from the surface (20) of the element (2), and wherein the laser beam (40) is guided over the surface (20) of the element (2) at a feed rate of at most 30 mm / s so that successive laser pulses (41) strike different locations on the surface (20) of the element (2), and wherein the pulse frequency and the feed rate of the laser beam (40) on the surface (20) of the element (2) are adjusted so thatthat the light spots (42) of successive laser pulses (41) of the laser beam (40) overlap on the surface (20) of the element (2) and the plasma (8) generated by the respective preceding laser pulse (41) still exists when a laser pulse (41) impinges, and wherein the laser pulses (41) remove material to a depth in the range between 30 µm and 150 µm., [2] Method according to the preceding claim, characterized by that the element (2) made of brittle material is moved relative to the laser beam (40) to generate a feed of the laser beam (40). [3] Method according to the preceding claim, characterized by that the element (2) made of brittle material is rotated. [4] Method according to one of the preceding claims, wherein the recess (6) is produced in a glass element. [5] Method according to one of the preceding claims, characterized bythat a recess (6) in the form of a trench is inserted into the element (2). [6] Method according to one of the preceding claims, characterized by that the recess (6) forms a predetermined breaking point and the element (2) is separated at the predetermined breaking point after the recess (6) has been inserted. [7] Method according to one of the preceding claims, characterized by that an element (2) in the form of a tube (22) is provided which has an axial section (23) with an enlarged circumference, wherein a circumferential recess (6) is inserted in the axial section (23) with an enlarged circumference. [8] Method according to one of the preceding claims, characterized by that the laser beam (40) is guided over the surface (20) of the element (2) at a feed rate of not more than 22 mm / s. [9] Method according to one of the preceding claims, characterized bythat the laser (4) is operated with a pulse frequency of at least 10 kHz, preferably at least 50 kHz. [10] Method according to one of the preceding claims, characterized by that the recess (6) is produced with a laser beam (40) with a light wavelength of less than 600 nm. [11] Method according to one of the preceding claims, characterized by that the laser beam (40) is focused such that the light spot (42) on the surface (20) of the element (2) has a diameter of at most 70 µm, preferably at most 50 µm. [12] Method according to one of the preceding claims, characterized by that a recess (6) with a width of at most 50 µm is created. [13] Method according to one of the preceding claims, characterized by that a depression of at least 30 µm, preferably at least 50 µm, is created with a single pass of the laser beam. [14] Element (2) made of brittle material, which has a trench-shaped depression (6), wherein the trench-shaped depression (6) has a width of at most 50 µm and a depth of at most 150 µm, preferably at most 100 µm, wherein the side walls of the depression (6) on the surface (20) of the element (2) have an opening angle of less than 45° and wherein the two side walls (60, 61) of the depression 6 converge in a tip (63) which has a radius in the range from 0.05 µm to 1 µm. [15] Element (2) according to the preceding claim, wherein its thickness at the recess (6) is in the range of 200 µm to 2 mm.

Citation Information

Patent Citations

  • laser processing process

    DE102005037412A1

  • Laser machining method and apparatus

    EP0931620A1

  • Laser machining method and laser machining apparatus

    EP2246146A1

  • Separating method and separating device for cathode-ray tube

    JP2000348621A

  • Ceramic member, its producing method, and electronic component using the same

    JP2006036602A