Method for processing a semiconductor substrate

A two-stage method for separating semiconductor substrates using a breaking device with a defined edge reduces damage, enhancing the functionality and reliability of semiconductor components.

DE102015100827B4Inactive Publication Date: 2024-10-02INFINEON TECHNOLOGIES AG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE102015100827
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2015-01-21
Publication Date
2024-10-02
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for separating semiconductor substrates using saw blades cause damage such as scratches and chipping, affecting the functionality and breaking strength of semiconductor components.

Method used

A method involving a two-stage process where a semiconductor substrate is partially weakened or removed, followed by separation using a breaking device with a defined edge, where a film is bent over the edge until it breaks, minimizing damage.

Benefits of technology

This approach reduces damage to semiconductor substrates and improves the functionality and reliability of individual components by minimizing scratches and chipping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for processing a semiconductor substrate (102), wherein the method comprises: forming a film (104) over a first side (102S1) of a semiconductor substrate (102); forming at least one separation region (108) in the semiconductor substrate (102) between a first region (1021) and a second region (1022) of the semiconductor substrate (102); Arranging the semiconductor substrate (102) on a breaking device (110), wherein the breaking device (110) has a break edge (110B), a first surface (110S1) and a second surface (110S2), wherein the break edge (110B) is a common edge of the first surface (110S1) and the second surface (110S2) and has a length greater than a length of the separation region (108), and wherein the semiconductor substrate (102) is arranged such that the film (104) faces the breaking device and is aligned in at least one alignment position with the at least one separation region at the break edge (110B);and forcing the semiconductor substrate (102) to bend the first region (1021) over the fracture edge (110B) with respect to the second region (1022) until the film (104) is separated between the fracture edge (110B) and the at least one separation region (108).
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] Various embodiments generally relate to a method for processing a semiconductor substrate. background

[0002] A semiconductor device, e.g. a semiconductor chip (also called a semiconductor wafer or ´´die´´), for example on its back, a film for attaching the semiconductor component to a carrier, for example to a lead frame. The film can be referred to as a die attach film (DAF). The film can be non-conductive. Alternatively, it can be electrically conductive, in which case it is used as a conductive chip adhesive film (Conductive Die Attach Film, C-DAF). The film, e.g. the chip adhesive film, can have various materials, e.g. epoxy and / or silver. During a process for separating a wafer using a saw blade, which can be referred to as sawing or dicing the wafer, these materials can Damage to the saw blade, for example a saw blade that contains a nickel binder. In this way, a saw blade quality can quickly This can cause scratches on the side walls of the semiconductor device and / or chipping, the so-called splitting (small semiconductor material fragments that break off from the semiconductor component, e.g. from its backside). Scratches and / or chipping can impair the functionality and / or fracture strength of the semiconductor device affect.

[0003] DE 10 2012 110 603 A1 discloses a method for separating semiconductor dies, which comprises forming a porous area on a semiconductor wafer and separating the die at the porous area by means of mechanical or other means of assistance.

[0004] EP 2 200 074 A1 discloses a method for producing a semiconductor chip with an adhesive film.

[0005] US 2009 / 0 121 337 A1 discloses dicing a semiconductor wafer by stealth dicing.

[0006] US 2014 / 0 127 880 A1 discloses a method for singulating a wafer with a backside layer, in which which localized pressure is exerted on the wafer. Brief description

[0007] A method for processing a semiconductor substrate according to claim 1 is provided. Further Embodiments are described in the dependent claims.

[0008] A method of processing a semiconductor substrate is provided. The method includes applying a film over a first side of a semiconductor substrate, at least one separation region in the semiconductor substrate between a first region and a second region of the semiconductor substrate, the semiconductor substrate on a The breaking device comprises a breaking edge, and the semiconductor substrate is arranged so that the film faces the breaking device, and in at least one alignment position, with the at least one separation region aligned with the fracture edge. The method may further include the semiconductor substrate to force the first area to bend over the break edge in relation to the second area until the film between the fracture edge and at least one separation area. Short description of the drawings

[0009] In the drawings, like reference numerals in the various figures generally refer to the same components. The drawings are not necessarily to scale; rather, they are generally intended illustrate the principles of the invention. In the following description, various embodiments of the invention with reference to the following drawings, in which: Figures 1A to 1C show cross-sectional views of different phases and / or processes of a process for Processing a semiconductor substrate according to various embodiments; Figures 2A to 2D show cross-sectional views of different phases and / or processes of a process for Processing a semiconductor substrate according to various embodiments; and Fig. 3A to 3E show in schematic perspective views 3A to 3C and schematic cross-sectional views 3D to 3E various phases and / or processes of a method for processing a semiconductor substrate according to different embodiments; Figures 4A to 4E illustrate various aspects of a method for processing a semiconductor substrate according to various embodiments; Fig. 5 shows a schematic representation of a method for processing a semiconductor substrate according to different embodiments; Fig. 6 shows a schematic representation of a method for processing a semiconductor substrate according to different embodiments; Fig. 7 shows a schematic representation of aspects of a method for processing a Semiconductor substrate according to various embodiments; and Fig. 8 shows a cross-sectional view of a semiconductor chip according to various embodiments. Description

[0010] The following detailed description refers to the accompanying drawings, which are Illustration showing specific details and embodiments in which the invention may be practiced.

[0011] The term ´´exemplary´´ is used here in the meaning ´´serving as an example, case or illustration´´ Any embodiment or configuration described herein as ´´exemplary´´ is not necessarily to be considered preferred or advantageous over other embodiments or configurations.

[0012] The word ´´over´´, used with respect to an applied material which is ´´over´´ a side or surface can be used here to express that the applied material is ´´directly on´´, e.g. in direct contact with the relevant side or surface. The word ´´over´´ in relation to a applied material which is formed ´´over´´ a side or surface can be used in the meaning that the applied material is formed ´´indirectly on´´ the relevant side or surface, whereby a or several further layers arranged between the relevant side or surface and the applied material can be.

[0013] The word ´´Dicing´´ can be used here to mean a general process of Separating a semiconductor substrate (e.g. a wafer) into a plurality of individual parts (e.g. chips). The word ´´Separation´´ can be used here to mean a process of separating a semiconductor substrate (e.g. a wafers) into a number of individual parts (e.g. chips) by sawing. It is from the respective context to determine whether a particular process is limited to sawing or whether any suitable cutting process can be used.

[0014] Various aspects of the disclosure are provided for devices, and various aspects of the Disclosure are provided for methods. It is understood that the basic properties of the components also apply to the procedures, and vice versa. For the sake of brevity, a twofold description of such Properties may have been waived.

[0015] In various embodiments, a method for processing a semiconductor substrate may be provided which involves a two-part process for separating a semiconductor substrate and a formed film, e.g. a film designed to support the semiconductor substrate on a carrier, e.g. a leadframe (also called chip adhesive film (DAF)). During the first part of the two-stage Process, a semiconductor substrate can be treated to separate it (e.g. by subjecting the semiconductor substrate to at least partially removed or by weakening it to separate it later). During a second part of the two-stage During the process, the film can be separated using a breaking device with a breaking edge. The film can be treated area of ​​the semiconductor substrate and the fracture edge, for example by passing them over the The fracture edge is bent until it breaks.

[0016] As a result, damage, e.g. by scratching and / or chipping, of the semiconductor substrate and e.g. individual semiconductor components, e.g. semiconductor chips (also called semiconductor wafers), into which the semiconductor substrate can be separated, can be avoided.

[0017] In various embodiments, functionality, fracture strength and / or Reliability of individual semiconductor components can be improved.

[0018] Figures 1A to 1C show in cross-sectional views various phases and / or processes of a method for Processing a semiconductor substrate 102 according to various embodiments.

[0019] As shown in Fig. 1A, the semiconductor substrate 102 may have a first surface 102S1 and a second surface 102S2 opposite the first surface 102S1. The semiconductor substrate 102 may have at least one (not shown) active region having at least one electronic device extending from the second surface 102S2 into the semiconductor substrate 102. The second area 102S2 can therefore be referred to as the active area 102. The second Surface 102S2 may be arranged on a second side of the semiconductor substrate 102. The first surface 102S1 may also referred to as back surface 102S1. The first surface 102S1 can be formed on a first side of the semiconductor substrate 102 may be arranged.

[0020] In various embodiments, the semiconductor substrate 102 may comprise any type of semiconductor material or consist essentially of, for example, a semiconductor material as is generally used to form integrated circuits, e.g. silicon, germanium, a semiconductor compound material such as gallium arsenide or Silicon carbide or the like.

[0021] In various embodiments, the semiconductor substrate 102 may be a wafer, e.g., a silicon wafer. At least one active region contained on the wafer may be a plurality of active regions. The wafer may be designed to be separated into a plurality of individual chips, each having at least one active area can have.

[0022] In various embodiments, the semiconductor substrate 102 may have a thickness 102T. The thickness 102T of the Semiconductor substrate 102 may be in a range of approximately 50 µm to approximately 2 mm, for example a typical Thickness of a wafer, e.g. about 675 µm, about 725 µm, about 775 µm etc., or another thickness, for example, Thinning a wafer, e.g. by thinning to a thickness in a range of about 50 µm to about 400 µm.

[0023] The method for processing a semiconductor substrate 102 may include forming at least one separation region 108 in the semiconductor substrate 102. The separation region 108 can be formed between a first region 1021 and a second Region 1022 of the semiconductor substrate 102. The at least one separation region 108 can be laterally connected to the first region 1021 and adjoin the second region 1022. The at least one separation region 108 can extend laterally into the Semiconductor substrate 102 extend, e.g. laterally through the semiconductor substrate 102, e.g. from a point of a peripheral surface of the semiconductor substrate 102 to another point on the peripheral surface of the semiconductor substrate 102, for example, as in Substantially straight region. The at least one separation region 108 may be a region in which the semiconductor substrate 102 designed to be separated in order to separate the semiconductor substrate 102, e.g. the wafer, into individual chips. Each Any known process suitable for forming the at least one separation region 108 may be used become.

[0024] The at least one separation region 108 may have a depth 108D. In various embodiments, the at least one separation region 108 from the second surface 102S2 of the semiconductor substrate 102 by the Semiconductor substrate 102 to the first surface 102S1 of the semiconductor substrate 102. In other words: The depth 108D of the at least one separation region 108 may be equal to the thickness 102T of the substrate 102. The at least one Separation region 108 may extend from the second surface 102S2 only partially through the semiconductor substrate 102, for example by less than 100%, for example by between 20% and 99%, for example by between 40% and 80%, of thickness 102T of the semiconductor substrate 102. The at least one separation region 108 may only partially through an initial thickness of the semiconductor substrate 102. Then, the semiconductor substrate 102 can be Surface 102S1 of the semiconductor substrate 102, e.g., the first surface 102S1 can be ground until the (e.g. final) thickness 102T of the semiconductor substrate 102 is reached. This process can also be called ´´Dicing-Before-Grinding´´- Process (DBG, separation before grinding). After thinning, e.g. grinding, the separation area can be 108 partially or completely, e.g. as described above, from the second surface 102S2 of the semiconductor substrate 102 through the semiconductor substrate 102 to the first surface 102S1 of the semiconductor substrate 102.

[0025] In various embodiments, the at least one separation region 108 may be formed by at least one opening, e.g. B. a trench. In other words: The at least one separation region 108 can be formed by removing a part of the semiconductor substrate 102 in the at least one separation region 108. The removal of the part of the semiconductor substrate 102 in the at least one separation region 108 can be, for example, sawing (also called separating or ´´dicing´´), laser ablation and / or etching, e.g. plasma etching, or a combination thereof or in the Essentially consist of this.

[0026] In various embodiments, a cross-section of the at least one separation region 108 may be rectangular, e.g. B. as shown in Fig. 3A. In other words: A bottom side of the at least one separation region 108, e.g. the opening, e.g. B. of the trench, may be flat. The cross-section of the at least one separation region 108 may have a different shape. For example, the underside of the at least one separation region 108, eg the opening, eg the trench, may be V-shaped or concave. This can make the area for separating the semiconductor substrate 102 more restricted.

[0027] In various embodiments, the at least one separation region 108 may be separated as desired from the first side and / or from the second side of the semiconductor substrate 102. For example, in a case where the at least one separation region 108 extends only partially through the semiconductor substrate 102 and / or the first surface 102S1 of the semiconductor substrate 102 is ground after the formation of the at least one separation region 108, the at least one separation region 108 is formed from the first side of the semiconductor substrate 102. In one case for example, that the at least one separation region 108 extends completely through the semiconductor substrate 102 extends, ie from the first surface 102S1 to the second surface 102S2, the at least one separation region 108 can be first side and / or from the second side of the semiconductor substrate 102.

[0028] In various embodiments, before / after the formation of the at least one separation region 108 one or more foils, layers or the like are arranged on the semiconductor substrate 102. For example, Before sawing or laser ablation of the semiconductor substrate 102, a layer which is suitable for the sawing or laser ablation of the semiconductor substrate 102 is designed to the first surface 102S1 of the semiconductor substrate 102. For example, prior to plasma etching of the semiconductor substrate 102, a structured mask, e.g. a masking layer, e.g. a structured photoresist, formed on the semiconductor substrate 102 In various embodiments, a carrier foil for stabilizing the semiconductor substrate 102 and / or to hold parts of the semiconductor substrate 102 in place on the semiconductor substrate 102, e.g. A slide can serve one or more purposes, for example, a Grinding film applied to the second surface 102S2 of the semiconductor substrate 102 to grind the first surface 102S1 sand, also serve as a carrier film.

[0029] As shown in Fig. 1A, the method for processing the semiconductor substrate 102 may include forming a film 104 over the first side 102S1 of the semiconductor substrate 102. The film 104 can, for example, be formed over, e.g., onto, the semiconductor substrate 102. The film 104 may be designed to be laminated on the semiconductor substrate 102. remain. On each part of a plurality of parts of the semiconductor substrate 102 into which the semiconductor substrate 102 is inserted at the at least one separation area 108, a part of the film 104 may remain. For example, in In the case that the semiconductor substrate 102 comprises a wafer or consists essentially of such a wafer, the film 104 form a part of each semiconductor chip to be formed from the wafer.

[0030] In various embodiments, the film 104 may be designed to be used to Semiconductor substrate 102, e.g., any part of the plurality of parts of the semiconductor substrate 102, electrically and / or thermally to a carrier, e.g., a lead frame. In various embodiments, the film 104 may so-called chip adhesive film (Die Attach Film, DAF). In a case where the chip adhesive film is electrically conductive, The chip adhesive film is called conductive die attach film (C-DAF).

[0031] In various embodiments, the film 104 may be any material or any combination of materials or consisting essentially of them, also known as film material, which acts as a layer on the semiconductor substrate 102 and which can have or acquire properties that make it suitable for Process for separating the film 104 as described below, e.g. for breaking the film 104. For example the film 104 with a thickness of 104T may be rigid enough to be broken or designed to to be made rigid accordingly.

[0032] In various embodiments, a modulus of elasticity (also referred to as tension modulus 2 2 2 may) of the film material be higher than approximately 5 kN / mm , e.g. higher than approximately 8 kN / mm , e.g. approximately 8.6 kN / mm , at least during the separation process. The elastic modulus of the film material can be sufficiently high, e.g. in the above-specified range to process the film 104 at a normal processing temperature, e.g. the separation of the semiconductor substrate 102, for example, room temperature. Alternatively, the The elastic modulus of the film material must be sufficiently high, e.g. in the range specified above, to 104 at a lower temperature, e.g. a temperature below room temperature, e.g. at a temperature below about 20 °C, e.g., below about 10 °C, e.g., below 0 °C. The foil 104 can, for example, electrically 2 conductive chip adhesive Loctite Ablestik C130 (which has a modulus of elasticity of approximately 8.666 kN / mm comprises) or consists essentially of.

[0033] The thickness of the film 104 may be in the range of approximately 5 µm to approximately 100 µm, e.g., approximately 20 µm to approximately 50 µm, e.g. approximately 30 µm.

[0034] The film 104 can, for example, consist essentially of the electrically conductive chip adhesive material Loctite Ablestik C130 and can have a thickness of 30 µm.

[0035] In various embodiments, the film 104 may be disposed over the first surface 102S1 of the semiconductor substrate 102 be formed before the at least one separation region 108 is formed, for example in a case that the Process for forming the at least one separation region 108 for the film 104 can not be harmful and from the second side of the semiconductor substrate 102.

[0036] The film 104 may be formed over the first surface 102S1 of the semiconductor substrate 102 after the at least one separation region 108 has been formed, for example in a case that the process for forming the at least one separation region 108 is harmful to the film 104 or the process of forming the at least one separation region 108 must be carried out from the first side of the semiconductor substrate 102.

[0037] A layer 106 may be formed over the film 104. The layer 106 may, for example, be formed on the film 104 The layer 106 can, for example, be laminated to the film 104. The layer 106 can be designed to withstand the process of separating the film 104 without hindering or preventing the process. The layer 106 may, for example, be more flexible than the film 104. It may, for example, be elastic.

[0038] The layer 106 may serve to connect the separated parts of the semiconductor substrate 102 (with the Slide 104) in an orderly arrangement, e.g. fixed to layer 106. The separated parts of the For example, semiconductor substrate 102 may essentially retain its original location and Maintain alignment, e.g. in a case that the layer 106 is flexible but not elastic, or that the layer 106 is elastic, but without using this elasticity to stretch the layer 106. In a case that the layer 106 is elastic, the layer 106 can be stretched to increase a distance between the separated parts, for example, to prevent damage during handling and / or transport or for easier handling of the separated parts, e.g., the chips. Layer 106 can, for example, be an expansion band, as it is generally used in technology, or it can be any other suitable, flexible material or consist essentially of a polymer, e.g. a conventional carrier tape. The film 104 (and the semiconductor substrate 102 on which it is formed) may be releasably fixed to the layer 106. After separation The individual parts can be removed from layer 106 for further processing, for example. The layer 106 (on which the semiconductor substrate 102 with the film 104 can be attached, e.g. fixed) can be mounted in a frame e.g., in a so-called saw frame (not shown). For example, an edge of the layer 106 can be frame must be mounted.

[0039] In various embodiments, the method may include, as shown in Fig. 1B, the semiconductor substrate 102 on a breaking device 110.

[0040] The breaking device 110 may have a breaking edge 110B. The breaking edge 110B may be a straight edge 110B The breaking edge 110B is between a first surface 110S1 and a second surface 110S2 of the breaking device 110. The second surface 110S2 may be substantially planar. The first surface 110S1 may be separated from the plane of the second surface 110S2. The first surface 110S1 and the second surface 110S2 can be connected to form the Break edge 110B as a common edge. The first surface 110S1 and the second surface 110S2 can enclose an angle α. The angle α can be greater than 90° and less than 180°, for example between approximately 110° and 160°. For example, a conventional breaking device, such as that used to cut a laser-cut used for ´´Stealth Laser Dicing´´ of treated wafers (e.g. as shown in Fig. 4E).

[0041] The term ´´Stealth Laser Dicing´´ can refer to a method for treating a semiconductor substrate, e.g. a wafers, with a laser, whereby part of the semiconductor substrate may not be removed, but rather weakened (e.g. by changing a crystal structure) in order to then attach the semiconductor substrate, e.g. the wafer, to to separate the weakened part of the semiconductor substrate, e.g. by stretching or bending the semiconductor substrate.

[0042] The semiconductor substrate 102 may be arranged such that the foil 104 faces the breaking device 110 as shown in Fig. 2. The semiconductor substrate 102 may be at least partially over the second surface 110S2 of the Breaking device 110 may be arranged. The semiconductor substrate 102 may be arranged such that the layer 106 forms the second Surface 110S2 of the breaking device 110 is touched.

[0043] In various embodiments, the semiconductor substrate 102 may be in at least one alignment position be arranged, whereby the at least one separation region 108 is aligned with the break edge 110B. In other words: The method can include arranging the semiconductor substrate in at least one alignment position, wherein the at least one Separation area 108 is aligned with the break edge 110B. The at least one separation area 108 which is aligned with the break edge 110B can be understood to mean that the (e.g. straight) break edge 110B and the (e.g. straight) Separation area 108 are parallel to each other, and that the break edge 110B is at least partially within a vertical projection of the separation region 108. A length of the break edge 110B (which extends into the plane of the paper in Fig. 1B and out of it) is greater than a length of the separation area 108 (which also extends into the plane of the paper in Fig. 1B and out of it), thus the break edge 110B can be formed from ends of the vertical projection of the separation area 108.

[0044] In Fig. 1B, the semiconductor substrate 102 and the breaking device 110 may not be in the at least one The at least one alignment position can be achieved by the semiconductor substrate 102, the breaking device 110 or both are displaced relative to each other, e.g. in a lateral displacement, until At least one alignment position (as shown in Fig. 1C) can be reached. For example, the Breaking device 110 is displaced relative to the semiconductor substrate 102 in a direction as indicated by the arrow 112 As a result, the fracture edge 110B, which in Fig. 1B is shown as parallel to the at least one separation area 108 arranged, but laterally, e.g. horizontally, against the vertical projection of at least one separation area 108 may be shown shifted, be moved horizontally into the at least one alignment position, wherein the Break edge 110B may be arranged at least partially within the vertical projection of the separation region 108.

[0045] In various embodiments, in the at least one alignment position, the first region 1021 of the Semiconductor substrate 102 may be arranged above the first surface 110S1 of the breaking device 110, and the second region 1022 of the semiconductor substrate 102 may be disposed over the second surface 110S2 of the breaking device 110.

[0046] As shown in Fig. 1C, the method involves forcing the semiconductor substrate 102 to form the first region 1021 in With respect to the second region 1022, the foil 104 is bent over the break edge 110B until the foil 104 is between the break edge 110B and the at least one separation area 108.

[0047] When the semiconductor substrate 102 and the breaking device 110 are in the at least one alignment position force can be applied, e.g. in the direction indicated by arrows 116, 118 in Fig. 1C, to move the first Region 1021 of the semiconductor substrate 102 towards the first surface 110S1 of the breaking device 110 (e.g. pull, e.g. suck, or push), and to move the second region 1022 of the semiconductor substrate 102 towards the second Surface 110S2 of the breaking device 110 (e.g. pulling, sucking, or pushing). This allows the Semiconductor substrate 102 is forced to bend over the break edge 110B. One or more of the various Parameters, e.g. properties of the separation area 108 (e.g. a depth 108D and / or a shape), an amount of force, a Geometry of the breaking device 110, e.g. the breaking edge 110B, a material of the film 104, a thickness 104T of the film 104 and optionally a temperature of the film 104 can be adjusted in various embodiments so that that the film 104 breaks. These various parameters can be adjusted so that the film 104 breaks between the at least one separation area 108 and the break edge 110B, but not in areas of the Semiconductor substrate 102 and / or the film, positioned, e.g. laterally, next to the at least one separation region 108, e.g. in first area 1021 or in the second area 1022.

[0048] As described above, the film 104 may be rigid, at least while the semiconductor substrate 102 is forced to bend the first region 1021 with respect to the second region 1022 over the break edge 110B until the Film 104 is separated between the break edge 110B and the at least one separation region 108.

[0049] In other words, the film 104 may be rigid, e.g. brittle, enough to be in an area between the fracture edge 110B and the separation region 108 when the force is applied as described above.

[0050] In various embodiments, the film 104 may be sandwiched between a first surface 104S1 and a second Surface 104S2 of the film. In other words: The film 104 can be separated between the breaking edge 110B and the at least one separation area 108 when it is forced to extend over the break edge 110B to bend.

[0051] In various embodiments, moving apart the first part 1021 and the second part 1022 of the semiconductor substrate 102 can be prevented by the layer 106 to which the semiconductor substrate 102 is fixed can.

[0052] Forcing the semiconductor substrate 102 to bend the first region 1021 with respect to the second region 1022 may include applying the force 116, 118, e.g. a vacuum suction force, to the semiconductor substrate 102. The Vacuum suction force may be provided at the break edge 110B to seal the first region 1021 of the semiconductor substrate 102 in the direction of the first surface 110S1 of the breaking device 110 and the second region 1022 of the semiconductor substrate 102 towards the second surface 110S2 of the crushing device 110. Channels 436, 438 (not shown here, but in Fig. 3D ) may be formed in the breaking device 110, which are designed to reduce the vacuum suction force to provide.

[0053] Figures 2A to 2D show in cross-sectional views various phases and / or processes of a method for Processing a semiconductor substrate 102 according to various embodiments.

[0054] The processes, materials, properties, parameters, etc. shown in Fig. 2A to Fig. 2D can generally similar to or identical to those described above, and their description may be omitted.

[0055] The method shown in Figs. 2A to 2D can be used in various embodiments from those shown in Figs. 1A to 1D. 1C in that at least one separation region 108 within a semiconductor substrate 102, ie by partially modifying the semiconductor substrate 102 instead of partially removing it In the at least one separation region 108, the semiconductor material of the semiconductor substrate 102 can be separated in such a way, e.g. by means of a laser, that a structural strength, in other words: a resistance, e.g. a breaking strength and / or tensile strength may be reduced. In other words, the semiconductor substrate 102 may the at least one separation region 108. In other words: The formation of the at least one Separation region 108 in the semiconductor substrate 102 may include separating the semiconductor substrate 102 in the at least one to weaken separation area 108.

[0056] A laser may be used to separate the semiconductor substrate 102 in the at least one separation region 108. The laser can be used to separate the semiconductor substrate 102 in the at least one separation region 108 The laser can be used for a so-called ´´Stealth Laser Dicing´´ process in which at least one separation area can be used.

[0057] In various embodiments, the weakened at least one separation region 108 may be separated from a first Surface 102S1 to a second surface 102S2 of the semiconductor substrate 102.

[0058] In various embodiments, while the semiconductor substrate 102 is forced to form the first region 1021 of the semiconductor substrate 102 with respect to the second region 1022 of the semiconductor substrate 102 over the break edge 110B until the film 104 is separated between the breaking edge 110B and the at least one separation region 108, the semiconductor substrate 102 is separated at the at least one separation region 108. In other words: In the exemplary case that the semiconductor substrate 102 is not (or only partially) separated before the semiconductor substrate 102 is forced to bend the first region 1021 with respect to the second region 1022 over the break edge 110B until the film 104 is separated between the break edge 110B and the at least one separation area 108, the separation of the semiconductor substrate 102 at the at least one separation region 108 (e.g. in the at least one separation region and / or between the at least one separation region 108 and the first surface 102S1) during the same process as separating the film 104 between the break edge 110B and the at least one separation region 108.

[0059] In the embodiments shown in Fig. 2A and Fig. 2B, the film 104 (and a layer 106) may be applied over the Semiconductor substrate 102 after the at least one separation region 108 in the semiconductor substrate 102 has been trained.

[0060] The film 104 (and optionally the layer 106) may be formed over the semiconductor substrate 102 before the at least one separation region 108 is formed, for example by modifying the semiconductor substrate 102 in Separation area 108.

[0061] Fig. 3A to Fig. 3E show, in schematic perspective views Fig. 3A to Fig. 3C and schematic Cross-sectional views Fig. 3D and Fig. 3E, different phases and / or processes of a method for machining a Semiconductor substrate 102 according to various embodiments.

[0062] The processes, materials, properties, parameters, etc. shown in Fig. 3A to Fig. 3E can generally similar to or identical to those described above, and their description may be omitted.

[0063] In various embodiments, as shown in Figure 324 of Figure 3A, the formation of the at least a separation region 108 in the semiconductor substrate 102 between a first region 1021 and a second region 1022 of the semiconductor substrate 102, a plurality of separation regions 108 in semiconductor substrate 102.

[0064] The semiconductor substrate 102 may be or comprise a wafer in various embodiments.

[0065] In various embodiments, the plurality of separation regions 108 can be formed by sawing, e.g., with a Saw blade. Alternatively, the plurality of separation regions 108 can be formed by etching or by irradiation with a laser, e.g. as described above.

[0066] As shown in image 324 of Fig. 3A, the plurality of separation regions 108 may be separated from a second surface 102S2 of the semiconductor substrate 102.

[0067] As shown in image 324 of Fig. 3A, the plurality of separation regions 108 may, for example, have a depth 108D which may be smaller than an initial thickness of the semiconductor substrate 102. Thereafter, as shown in the images 326 and 328 of Fig. 3A, a temporary layer 334 on the second surface 102S2 of the semiconductor substrate 102 attached, e.g., fixed thereto. The temporary layer 334 can, for example, be designed to Semiconductor substrate 102 from a first surface 102S1 opposite the second surface 102S2. The temporary Layer 334 may, for example, be a so-called grinding layer, e.g. a grinding layer as used in the art is known. The first surface 102S1 can be ground, e.g., with a grinding tool 336. The semiconductor substrate 102 can be ground until a thickness of 102T is reached. The thickness of 102T can be as large as the depth 108D of the plurality of separation areas 108, e.g. as shown in Figure 328 of Figure 3A. In this case, the Semiconductor substrate 102 may be separated into individual parts after grinding. Alternatively, the thickness 102T may depend on the depth 108D may be different, e.g. smaller (in this case, the grinding of the semiconductor substrate 102 may be continued, after a separation of the semiconductor substrate 102 at the plurality of separation regions 108 is achieved) or greater (in In this case, a part of the semiconductor substrate 102 may be disposed between the plurality of separation regions 108 and the first surface 102S1 of the semiconductor substrate 102 remain).

[0068] Alternatively, the plurality of separation regions 108 may, for example, have a depth 108D that is smaller than the Thickness 102T of the semiconductor substrate 102. In other words: The majority of separation regions 108 can only extend partially through the semiconductor substrate 102, or the plurality of separation regions 108 may extend completely through the semiconductor substrate 102, in other words: The depth 108D of the plurality of separation regions 108 may be equal to the thickness 102T of the semiconductor substrate 102.

[0069] Damage to and / or below the surface caused by sawing and / or grinding can be reduced or removed, e.g. by means of a so-called stress relief process. Reducing or removing damage can be achieved by dry polishing with a ´´Polygrind´´ grinding wheel and / or a Dry etching process, whereby the dry etching process not only repairs damage to the polished surface, e.g. first surface 102S1 (the back surface) of the semiconductor substrate 102, but also Damage to side walls, e.g. side walls of the separation areas 108, caused by the process of mechanical sawing may have been caused.

[0070] The plurality of separation regions 108 may comprise a first plurality 108P1 of substantially parallel separation regions 108. The plurality of separation regions 108 may comprise a second plurality 108P2 of substantially parallel separation areas 108, and the second plurality 108P2 of substantially parallel separation areas 108 may be Substantially orthogonal to the first plurality 108P1 of substantially parallel separation regions 108. Otherwise In various embodiments, the formation of the at least one separation region 108 in the Semiconductor substrate 102 include a first plurality 108P1 of substantially parallel separation regions 108 and a second plurality 108P2 of substantially parallel separation regions 108, wherein the second plurality 108P2 of substantially parallel separation regions 108 substantially orthogonal to the first plurality 108P1 of Essentially parallel separation areas 108.

[0071] A distance between the substantially parallel separation regions 108 may correspond to a lateral size of a It can be in a range from approximately 100 µm to approximately 2 cm, e.g. approximately 1 mm to approximately 5 mm. The first plurality 108P1 and the second plurality 108P2 of substantially parallel separation regions 108, the semiconductor substrate 102, e.g. the wafer, can be divided into a plurality of semiconductor chips separate.

[0072] As shown in Fig. 3B, a film 104, e.g. a chip adhesive film, e.g. an electrically conductive chip adhesive film, be attached to the semiconductor substrate 102, e.g., to the first surface 102S1 of the semiconductor substrate 102. The film 104 can for example, laminated over, e.g. on, the semiconductor substrate 102.

[0073] A plurality of active regions (not shown) may extend from the first surface 102S1 into the extend into the semiconductor substrate 102. Thus, the second surface 102S2 of the semiconductor substrate 102 can be ground, and / or the film, which may remain, e.g. permanently, on the semiconductor substrate 102, may be arranged over the second surface 102S2 of the semiconductor substrate 102.

[0074] In various embodiments, the film 104 may be a preformed film applied to the second surface 102S2 of the semiconductor substrate 102, e.g., fixed thereto. An adhesive, e.g., an adhesive, can used to attach the film 104 to the semiconductor substrate 102. Alternatively, other known Methods, e.g. depositing the film 104 on the second surface 102S2 of the semiconductor substrate 102, to arrange the film 104 over the semiconductor substrate 102.

[0075] In various embodiments, as shown in image 338 of Figure 3C, a layer 106 may be deposited over the second surface 102S2 of the semiconductor substrate 102, for example above the film 104, which is above the semiconductor substrate 102 can be arranged.

[0076] The layer 106 may be a preformed layer, e.g. a stretch band, arranged on the film 104, e.g. An adhesive, e.g. an adhesive, can be used to fix the layer 106 to the film 104. Alternatively, other known methods can be used to apply the layer 106 over the film 104 to arrange.

[0077] In image 340 of Fig. 3C, the semiconductor substrate 102 may be arranged with respect to the position shown in image 338 of Fig. 3C. Orientation may be reversed. Thus, in Figure 340, layer 106 may be arranged below semiconductor substrate 102. The temporary layer 334 may be provided on a top surface of the semiconductor substrate 102. The method may include removing, e.g., peeling off, the temporary layer 334 from the semiconductor substrate 102. Alternatively, other suitable methods may be used to remove the temporary layer from the semiconductor substrate 102.

[0078] As shown in Fig. 3D, the method may include placing the semiconductor substrate 102 on a breaking device 110. Arranging the semiconductor substrate 102 on the breaking device 110 includes placing the semiconductor substrate 102 on the breaking device 110 so that the film 104 faces the breaking device 110, e.g. so that the layer 106 touches the breaking device 110. In Fig. 3D, the semiconductor substrate 102 and the formed film 104 may be represented as an integral element, which is referred to as the semiconductor substrate 102, 104 can be made, with specific reference to the slide where necessary.

[0079] The breaking device 110 may have a breaking edge 110B. The breaking device 110 may further comprise a first surface 110S1 and a second surface 110S2. The break edge 110B is between the first surface 110S1 and the second surface 110S2 of the breaking device 110. The breaking edge 110B is the common edge of the first Surface 110S1 and the second surface 110S2. As shown in Fig. 3D, the second surface 110S2 of the breaking device 110 may be substantially flat. In other words, the second surface 110S2 may be arranged in a plane. The first surface 110S1 may recede from the plane of the second surface 110S2. For example, as shown in Fig. 3D shown, the first surface 110S1 slopes away from the second surface 110S2, e.g. away from the fracture edge 110B.

[0080] The method may include placing the semiconductor substrate 102 over the breaking device 110 in at least one Alignment position with the at least one separation area 108 aligned with the break edge 110B, e.g. as described above. The at least one alignment position may comprise a plurality of alignment positions A number of alignment positions may, for example, be equal to a number of separation regions 108.

[0081] In Fig. 3D, each separation region 108 of the (e.g. first) plurality of separation regions 108 can extend into the plane of the The break edge 110B can also extend into the plane of the paper and out of it. A separation area 108A (which may be marked by the triangular arrows 434) of the (e.g. first) plurality of Separation areas 108 can be displayed in one alignment position of the plurality of alignment positions. The Separation areas 108 of the (e.g. first) plurality of separation areas 108 which are arranged above the first surface 110S1 of the breaking device 110 may already have been in one of the plurality of alignment positions, whereas the separation areas 108 of the (e.g. first) plurality of separation areas 108 located above the second surface 110S2 of the Breaking device 110 are shown, have not yet been in an alignment position of the plurality of alignment positions Each separation area 108 of the (e.g. first) plurality of separation areas 108 can subsequently be Alignment position of the majority of alignment tion positions, for example, by the breaking device 110 and the semiconductor substrate 102 (with the foil 104) are moved relative to each other, e.g. by moving the breaking device in a direction indicated by the arrow 112 direction shown, while the semiconductor substrate 102 can remain in its position. Alternatively the semiconductor substrate 102 can be moved or both the semiconductor substrate 102 and the Breaking device 110. The direction indicated by arrow 112 can be substantially orthogonal to the direction in which each of the separation regions 108 of the (e.g. first) plurality of separation regions 108 extends, and substantially parallel to the semiconductor substrate 102, e.g. to the first surface 102S1 and / or to the second surface 102S2 of the semiconductor substrate 102. By moving the breaking device 110 (and with it the breaking edge 110D) in the direction of Arrow 112 is moved, each alignment position of the (eg first) plurality of Alignment positions can be achieved. In various embodiments, the displacement of the breaking device 110 relative to the semiconductor substrate 102 in at least one lateral direction 112 successively each separation region 108 of the Align the plurality of separation areas 108 at the break edge 110B.

[0082] In various embodiments of the plurality of separation regions 108 including the first plurality 108P1 of separation regions 108 and the second plurality 108P2 of separation regions 108, the semiconductor substrate 102 may first successively in each of the alignment positions corresponding to the first plurality 108P1 of separation regions 108, In this case, the direction of the arrow 112 may correspond to a first direction 1121, for example as shown in Fig. 4B, which shows an example of moving the breaking device 110 in the direction 1121 over the Semiconductor substrate 102 with the film 104 arranged thereon.

[0083] In various embodiments, the semiconductor substrate 104 and the breaking device 110 rotated relative to each other. For example, the breaking device 110 can be rotated, the semiconductor substrate 102 can be rotated or both can be rotated. Each rotation can be essentially in the plane of the semiconductor substrate 102 and / or the breaking device 110. An angle of rotation may be an angle between a direction in which the first plurality 108P1 of separation regions 108 can extend and a direction into which the second plurality 108P2 of separation regions 108 can extend. The semiconductor substrate 102 and the breaking device 110 can be rotated relative to each other into a position in which the breaking edge 110D in the Substantially parallel to the second plurality 108P2 of separation regions 108.

[0084] Thereafter, in various embodiments, the breaking device 110 (including the breaking edge 110D) relative to the semiconductor substrate 102 in the direction of arrow 112, which may correspond to a second direction 1122, The semiconductor substrate 102 can then be successively moved into each of the alignment positions that the second plurality 108P2 of separation areas 108.

[0085] In other words: The displacement of the semiconductor substrate 102 and the breaking device 110 relative to each other may include moving the breaking device 110 relative to the semiconductor substrate 102 in at least one lateral direction (also referred to as channel 1). The displacement of the breaking device 110 relative to the semiconductor substrate 102 in at least one lateral direction 112 may include moving the breaking device 110 relative to the semiconductor substrate 102 in a first lateral direction 1121 and then the breaking device 110 relative to the semiconductor substrate 102 in a second lateral direction 1122 (also referred to as channel 2).

[0086] In various embodiments, an angle between the direction in which the first plurality 108P1 of separation areas 108 and the direction in which the second plurality 108P2 of separation areas 108, may be approximately 90°, as shown for example in Fig. 3A to Fig. 3B. The first lateral Direction 1121 may thus be substantially orthogonal to the second lateral direction 1122. Alternatively, the Angle may be different, for example approximately 45°.

[0087] The displacement of the breaking device 110 relative to the semiconductor substrate 102 can be referred to as scanning, and the direction of displacement can be called the scanning direction.

[0088] The method may include when the semiconductor substrate 102 is in an alignment position of the plurality of Alignment positions, to force the semiconductor substrate 102, a first region 1021 of the semiconductor substrate 102 with respect to a second region 1022 of the semiconductor substrate 102, wherein each separation region 108 of the plurality of Separation areas 108 may have an adjacent first area 1021 and an adjacent second area 1022, over which Break edge 110B until the film 104 is between the break edge 110B and the at least one separation area 108 is separated.

[0089] In various embodiments illustrated in Fig. 3D, the plurality of separation regions 108 formed in a part of the semiconductor substrate 102, which is above the second surface 110S2 of the breaking device 110 is arranged, not be shown, in order to allow the separation of the film 104 over the breaking edge 110B, which is caused by free spaces between individual separate parts of the semiconductor substrate 102 (on which the film 104 may be attached) Nevertheless, in the (eg first) majority of separation areas 108, the Semiconductor material of the semiconductor substrate 102 can be removed, e.g., as described above. Alternatively, the (e.g., first) plurality of separation regions 108 comprise modified, but not removed, semiconductor material as above described. A distance between the individual parts of the semiconductor substrate 102 (with the film arranged thereon 104) may be essentially the same before and after the break line. Alternatively, the distance for example, increase.

[0090] In various embodiments, while the semiconductor substrate 102 is forced to form the first region 1021 with respect to the second region 1022 over the breaking edge 110B until the film 104 is between the breaking edge 110B and the respective aligned separation area 108 of the plurality of separation areas 108, for each Alignment position of the plurality of alignment positions, the semiconductor substrate 102 at the at least one Separation area 108, e.g. in the respective aligned separation area 108 and / or between the respective aligned separation region 108 and the first surface 102S1, for example as described above.

[0091] In various embodiments, the layer 106 may be formed after breaking the film 104 between each Separation area of ​​the majority of separation areas 108 and the break edge 110B remain intact. The majority of individual Parts of the semiconductor substrate 102, which is obtained by separating the semiconductor substrate 102, can be applied to the layer 106 remain attached. The layer 106 may, in various embodiments, comprise the majority of individual parts of the semiconductor substrate 102 in their original relative positions and orientations. The layer 106 can For example, prevent the majority of individual parts of the semiconductor substrate 102 from falling down and Disorder arises after they are separated from each other.

[0092] The layer 106 may (e.g., as described above and below) be removed during the process of separating the semiconductor substrate 102. While a stretching force applied to the layer 106 results in an increased Distance between the individual parts of the semiconductor substrate 102 above the first surface 110S1 of the breaking device the stretching force may not be strong enough to separate the film 104 between the separation areas 108 and the second surface 110S2 of the breaking device 110.

[0093] As shown in Fig. 3D, a plurality of channels 436, 438 may be formed in the breaking device 110. Through the plurality of channels 436, 438, a vacuum suction force (e.g. in directions 116, 118) can be applied to the fracture edge 110B, the first surface 110S1 and / or the second surface 110S2 of the breaking device 110. As As described above, the vacuum suction force may be provided at the break edge 110B to seal the first area 1021 of the semiconductor substrate 102 in the direction of the first surface 110S1 of the breaking device 110 and the second region 1022 of the semiconductor substrate 102 towards the second surface 110S2 of the breaking device 110, for each of the Plurality of separation areas 108 with their respective first area 1021 and second area 1022.

[0094] In various embodiments, the vacuum suction force 116, 118 may be substantially constant provided while the semiconductor substrate 102 and the breaking device 110 are displaced relative to each other Alternatively, the vacuum suction force 116, 118 may be weaker or non-existent if the Semiconductor substrate 102 is not in one of the plurality of alignment positions. As a breaking device 110, e.g. Breaking device that provides the vacuum suction force 116, 118, a breaking device can be used, such as used in the technique for breaking wafers in ´´stealth laser dicing´´, e.g. as shown in Fig. 4E.

[0095] In various embodiments, the force to push the semiconductor substrate 102 over the break edge 110B bend until it breaks, can be provided in different ways, e.g. a mechanical force can be used.

[0096] In various embodiments, as shown in Fig. 3E, a distance between the separated parts of the semiconductor substrate 102 (with a part of the film 104 attached to each of the parts of the semiconductor substrate 102) be increased. In a case that the layer 106 is elastic, the layer 106 can be stretched, for example, B. in directions indicated by an arrow 446, to determine the distance between the separated parts of the semiconductor substrate 102. In various embodiments, for example, in a case where the semiconductor substrate 102 is two, e.g. orthogonal, directions, stretching of the layer 106 can further be carried out in directions orthogonal (within a plane of layer 106) to the directions indicated by arrow 446. To move layer 106 stretch, the layer 106 can be fixed in a holding device 440B, 440T, 442. For example, the layer 106 can be the holding device 440B, 440T, 442 may be clamped as shown in Fig. 4A (which holds the layer 106 and the separated Semiconductor device 102 with the separated film 104 arranged thereon in a fixed, but not stretched arrangement). By moving an expansion element 443 in a direction 444 as shown in Fig. 3E, e.g. B. pressing against the layer 106 and displacing the layer 106 orthogonal to its lateral direction, while a Edge of the layer 106 remains fixed in the holding device 440B, 440T, 442, the layer 106 can be stretched, e.g. in the directions 446. The stretching of the layer 106 can be carried out as known in the art. Alternatively, the Stretching should be avoided.

[0097] As shown in Fig. 4D, after stretching, the layer 106 (with the semiconductor substrate 102 with the arranged film 104) on a frame 550. Alternatively, the frame 550 can be mounted on the layer 106 mounted, e.g. as shown in Fig. 4D. This prevents the layer 106 from shrinking and the individual parts of the semiconductor substrate 102, e.g. the individual chips (semiconductor wafers), can be Position with the increased distance between them.

[0098] Regarding the breaking device 110 and the separation and stretching process as described above, different parameters can be adjusted. For example, a strain rate, in other words, a Speed ​​at which the layer 106 can be stretched and / or a degree of stretching, in other words, a Factor by which the layer 106 can be stretched; the stretching of the layer 106 can be done, after the breaking device 110 has been removed, or alternatively while the breaking device 110 is further in Contact with the semiconductor substrate 102 (or the film 104). Furthermore, a speed of the breaking device 110, e.g. of a crushing bar, in other words, a speed with which the crushing device 110 is displaced The direction(s) 112 in which the breaking device 110 is displaced can be adjusted be adapted, e.g. requirements that are determined by the plurality of separation regions 108 of the semiconductor substrate 102 For example, the breaking device 110 can be moved in one, two or three directions, e.g. B. 0°, 90° and / or 45°, and in a case that more than one direction is scanned, a sequence of directions be selected, e.g. first scan along the 0° direction, then in the 45° direction, or first in the 90° direction, then with 0°, etc. The breaking device 110, e.g. the breaking bar, can be used in conjunction with the above-described Alternatively, the breaking device 110, e.g. the breaker bar, can be used without vacuum force Instead, the semiconductor substrate 102 may be forced in another way to extend over the to bend the breaking edge 110B, for example by applying a mechanical force. Furthermore, Parameters for frame mounting, e.g. the diameter of the frame 550, can be adjusted.

[0099] Fig. 5 shows a schematic representation of a method 500 for processing a semiconductor substrate according to different designs.

[0100] In various embodiments, the method includes applying a film over a first side of a semiconductor substrate (in 510). The method may further include forming at least one separation region in the semiconductor substrate between a first region and a second region of the semiconductor substrate (in 520), to arrange the semiconductor substrate on a breaking device, wherein the breaking device comprises a breaking edge and wherein the semiconductor substrate is arranged such that the foil faces the breaking device, and in at least an alignment position, wherein the at least one separation region is aligned with the break edge (in 530), and to force the semiconductor substrate to bend the first region with respect to the second region over the fracture edge bend until the film is separated between the break edge and the at least one separation area (in 540).

[0101] Fig. 6 shows a schematic representation 600 of a method for processing a semiconductor substrate according to different designs.

[0102] The method may include a so-called ´´Dicing-Before-Grinding´´ (DBG) process (in 610) which is carried out on the semiconductor substrate, e.g. as shown in Fig. 3A. The method may further comprise forming a film to laminate over the semiconductor substrate, e.g. a chip adhesive film, e.g. a conductive chip adhesive film (in 620), e.g. as in Fig. 3B shows how to mount the semiconductor substrate on a strain gauge, whereby the semiconductor substrate is positioned on the The film can be mounted so that the film faces the expansion band (which is called top-facing orientation). top side) (in 630), e.g. as shown in Fig. 3C. The method may further include breaking the chip adhesive film, for example as described above, e.g. in connection with Fig. 3D, e.g. by means of a breaking device (in 640). The method may further include stretching the expansion band (in 650), e.g. as shown in Fig. 3E, and thereby creating a distance between individual parts of the separated semiconductor substrate (where the chip adhesive film is attached to each of the individual parts is attached).

[0103] Fig. 7 shows a schematic representation 700 of aspects of a method for processing a Semiconductor substrate according to various embodiments.

[0104] The method may include attaching a wafer (in 710), e.g., securing the wafer to a holding device e.g., fixing the wafer to a holding device, e.g. as shown in Fig. 4A. The method can further include a breaking device, e.g. a breaking bar, relative to the wafer in a first direction, also as channel 1 referred to, to move (in 720), e.g., as shown in Fig. 4B. The method may further include Breaking device, e.g. the breaker bar, relative to the wafer in a second direction, also referred to as channel 2, (in 730), e.g. as shown in Fig. 4C. This allows the wafer to be separated into semiconductor dies. The The method may optionally include stretching the separated semiconductor die, in other words, a distance between the separated semiconductor dies (in 740), e.g. as shown in Fig. 3E. The process can optionally include mounting a frame, e.g. a frame with a diameter of approximately 8" (approx. 20 cm) up to approximately 12" (approx. 31 cm) (in 750), e.g. as shown in Fig. 4D.

[0105] Fig. 8 shows a cross-sectional view of a semiconductor chip 900 according to various embodiments.

[0106] In various embodiments, a semiconductor chip 990 may be provided. The semiconductor chip 990 may formed by one of the methods described above for processing a semiconductor substrate, and Methods, parameters, materials, etc. described therein may be applicable to the semiconductor chip 990.

[0107] In various embodiments, the semiconductor chip 990 may include a foil 104 disposed over a surface of the semiconductor substrate 102, wherein a side surface 992 of the film 104 is formed by breaking the film 104 can be.

[0108] The surface may be a first surface 102S1 of the semiconductor substrate 102. The semiconductor substrate 102 may have a second surface 102S2 opposite the first surface 102S1. The semiconductor chip 990 may have at least one active region extending from the second surface 102S2 into the semiconductor substrate 102.

[0109] In various embodiments, the film 104 may be a die attach film (DAF).

[0110] In various embodiments, a method for processing a semiconductor substrate is provided. The method includes forming a film over a first side of a semiconductor substrate, at least one separation region in the semiconductor substrate between a first region and a second region of the semiconductor substrate, the to arrange a semiconductor substrate on a breaking device, wherein the breaking device comprises a breaking edge and wherein the semiconductor substrate is arranged such that the foil faces the breaking device, and in at least one Alignment position, wherein the at least one separation area is aligned with the break edge, and the semiconductor substrate to bend the first region with respect to the second region over the break edge until the film between the fracture edge and the at least one separation area.

[0111] In various embodiments, the film may be rigid, at least while the semiconductor substrate is forced to bend the first area with respect to the second area over the break edge until the film between the The foil can be a chip adhesive foil. The forcing of the semiconductor substrate, bending the first region with respect to the second region may include bending the semiconductor substrate with a vacuum suction force. The breaking device may further comprise a first surface and a second surface which are joined at the fracture edge, and the vacuum suction force can be provided at the fracture edge to move the first area towards the first surface and the second area towards the second surface The first surface may be recessed from a plane of the second surface. The semiconductor substrate may be a wafer be.

[0112] Arranging the semiconductor substrate on the breaking device in the at least one alignment position can include placing the semiconductor substrate on the breaking device and the semiconductor substrate and the Breaking device relative to each other into at least one alignment position. The displacement of the half conductor substrate and the breaking device relative to each other may include moving the breaking device relative to the semiconductor substrate in at least one lateral direction. The displacement of the breaking device relative to the semiconductor substrate in at least one lateral direction may include moving the breaking device relative to the semiconductor substrate in a first lateral direction and then to move the breaking device relative to the semiconductor substrate in a second lateral direction. The first lateral direction can be essentially be orthogonal to the second lateral direction.

[0113] The at least one separation region may comprise a plurality of separation regions. The plurality of separation regions may comprise a first plurality of substantially parallel separation regions. The plurality of separation regions may a second plurality of substantially parallel separation areas, and the second plurality of Substantially parallel separation regions may be substantially orthogonal to the first plurality of substantially parallel separation areas. The displacement of the breaking device relative to the semiconductor substrate in at least one lateral direction, each of the separation areas of the plurality of separation areas can be successively separated at the fracture edge align.

[0114] Forming the at least one separation region in the semiconductor substrate may include forming at least one trench in the semiconductor substrate. Forming the at least one separation region in the semiconductor substrate may include to weaken the semiconductor substrate in the at least one separation region. During the forcing of the semiconductor substrate, to bend the first area in relation to the second area over the break edge until the film is between the break edge and the at least one separation region, the semiconductor substrate can be separated in the at least one separation region be separated.

[0115] In various embodiments, a semiconductor chip may be provided. The semiconductor chip may have a film formed over a surface of a semiconductor substrate, wherein a side surface of the film is thereby can be formed so that the film is broken.

[0116] In various embodiments, the film may be a chip adhesive film.

[0117] The scope of the invention is defined by the appended claims.

Claims

1. A method for processing a semiconductor substrate (102), the method comprising: Forming a film (104) over a first side (102S1) of a semiconductor substrate (102); Forming at least one separation region (108) in the semiconductor substrate (102) between a first region (1021) and a second region (1022) of the semiconductor substrate (102); Arranging the semiconductor substrate (102) on a breaking device (110), wherein the breaking device (110) has a breaking edge (110B), a first surface (110S1) and a second surface (110S2), wherein the breaking edge (110B) has a common edge of the first surface (110S1) and the second surface (110S2) and has a length which is greater than a length of the separation region (108), and wherein the semiconductor substrate (102) is arranged such that the Foil (104) facing the breaking device, and in at least one alignment position with the at least one Separation area is aligned with the break edge (110B); and Forcing the semiconductor substrate (102) to move the first region (1021) relative to the second region (1022) over the break edge (110B) until the film (104) between the breaking edge (110B) and the at least one separation area (108) is separated.

2. The method of claim 1, wherein the film (104) is rigid, at least during the forcing of the semiconductor substrate (102) to bend the first region (1021) with respect to the second region (1022) over the breaking edge until the film (104) between the fracture edge (110B) and the at least one separation region (108).

3. The method according to claim 1 or 2, wherein the film (104) is a chip adhesive film.

4. The method according to any one of claims 1 to 3, wherein forcing the semiconductor substrate (102) to move the first region with respect to bend to the second region, comprises applying a negative pressure suction force to the semiconductor substrate (102).

5. The method of claim 4, wherein the vacuum suction force is provided at the break edge (110B) to press the first area towards the first surface and the second area towards the second surface.

6. The method of claim 5, wherein the first surface recedes from a plane of the second surface.

7. The method according to any one of claims 1 to 6, wherein the semiconductor substrate (102) is a wafer.

8. Method according to one of claims 1 to 7, wherein the arranging of the semiconductor substrate (102) on the breaking device (110) in the at least one alignment position, to place the semiconductor substrate on the breaking device and the semiconductor substrate and the breaking device (110) relative to each other into the at least one alignment position move.

9. The method according to claim 8, wherein the displacement of the semiconductor substrate (102) and the breaking device (110) relative to each other, the breaking device relative to the semiconductor substrate in at least one lateral direction move.

10. The method according to claim 9, wherein the displacement of the breaking device (110) relative to the semiconductor substrate (102) in at least one lateral direction: to displace the breaking device (110) relative to the semiconductor substrate (102) in a first lateral direction; and subsequently moving the breaking device (110) relative to the semiconductor substrate (102) in a second lateral direction move.

11. The method of claim 10, wherein the first lateral direction is substantially orthogonal to the second lateral direction is.

12. The method according to any one of claims 1 to 11, wherein the at least one separation region (108) comprises a plurality of separation areas (108).

13. The method according to claim 12, wherein the plurality of separation regions (108) comprises a first plurality (108P1) of essentially parallel dividing areas.

14. The method according to claim 13, wherein the plurality of separation regions (108) comprises a second plurality (108P2) of substantially parallel separation regions, and wherein the second plurality of substantially parallel Separation areas substantially orthogonal to the first plurality (108P1) of substantially parallel separation areas is.

15. The method according to claim 12, wherein the displacement of the breaking device (110) relative to the semiconductor substrate (102) in at least one lateral direction successively each of the separation areas (108) of the plurality of separation areas on the Aligns the break edge (110B).

16. The method according to any one of claims 1 to 15, wherein the formation of the at least one separation region (108) in the Semiconductor substrate (102) has at least one trench formed in the semiconductor substrate (102).

17. The method according to any one of claims 1 to 16, wherein the formation of the at least one separation region (108) in the Semiconductor substrate (102) to weaken the semiconductor substrate in the at least one separation region.

18. The method according to claim 17, wherein, during the forcing of the semiconductor substrate (102), the first region (1021) in With respect to the second area (1022) over the breaking edge (110B) until the film (104) is between the breaking edge and the at least one separation region (108), the semiconductor substrate (102) is separated at the at least one separation region (108) is separated.

Citation Information

Patent Citations

  • Method for separating semiconductor dies by means of material modification

    DE102012110603A1

  • Method for producing semiconductor chip with adhesive film, adhesive film for semiconductor used in the method, and method for producing semiconductor device

    EP2200074A1

  • Semiconductor device manufacturing method and semiconductor

    US20090121337A1

  • Semiconductor die singulation method and apparatus

    US20140127880A1