Method for manufacturing a component, in particular a chassis component, of a motor vehicle
A thermal treatment process for high-strength martensitic steels in vehicle chassis components reduces stress corrosion cracking by forming reconverted austenite as a hydrogen trap, addressing the embrittlement issue without extra protective measures.
Patent Information
- Application Number
- DE102016102770
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2016-02-17
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2036-02-17
AI Technical Summary
High-strength steels used in vehicle chassis components are susceptible to stress corrosion cracking due to hydrogen embrittlement, necessitating costly protective measures.
A method involving the use of corrosion-resistant, pressure-stitched martensitic steels with a specific thermal treatment process, including annealing, quenching in liquid nitrogen, and double tempering, to reduce tensile strength by 2-15% below the maximum achievable, promoting reconverted austenite formation that acts as a hydrogen trap.
Significantly reduces the susceptibility to stress corrosion cracking without additional protective measures, maintaining high tensile strength, particularly effective for mechanically prestressed chassis components.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The present invention relates to a method for producing a component, in particular a chassis component, of a motor vehicle from a high-strength steel, comprising the steps of forming the component in at least one forming step and thermally treating the component for the defined setting of a tensile strength of the component.
[0002] Definition: If reference is made to specific commercially available steel grades in the following description, these are designated by abbreviations according to DIN EN 10027-1:2005-10 and by numbers according to DIN EN 10027-2:2015-07.
[0003] It is already known in the art to use high-strength steels to manufacture components, particularly chassis components, of a motor vehicle. These high-strength steels have a tensile strength that is typically higher than 1400 MPa, preferably higher than 1500 MPa. The use of these high-strength steels to manufacture the components advantageously enables smaller component dimensions and weight savings compared to components made from conventional case-hardening and tempering steels. To adjust certain rheological properties, such as tensile strength, it is generally known in the art to subject components made from high-strength steel to a thermal treatment. Precipitation hardening, which includes the thermal treatment steps of solution annealing, quenching, and ageing, should be mentioned here merely as an example.
[0004] DE 10 2005 054 847 B3 describes a high-strength steel component that exhibits defined deformability in the event of a crash. A defined thermal treatment slightly reduces the strength and increases the ductility to such an extent that targeted wrinkling occurs in the event of a crash.
[0005] A method of the type mentioned above is known from JP S60-234 920 A. Further prior art can be found in the documents JP H04-168 227 A, DE 33 10 693 A1, and US 2010 / 0 037 994 A1.
[0006] Various studies have shown that high-strength steels with a maximum achievable tensile strength greater than 1400 MPa, especially greater than 1500 MPa, exhibit an increased susceptibility to undesirable stress corrosion cracking in this state of maximum tensile strength, which can lead to component damage. This stress corrosion cracking is caused by corrosive processes on the metal surfaces of the component made of the high-strength steel, which are inherently harmless in terms of material removal. However, these corrosive processes generate hydrogen, which penetrates the interior of the component and leads to hydrogen embrittlement, which results in stress corrosion cracking.For this reason, especially when using high-strength steels to manufacture chassis components, additional protective measures are required to effectively reduce the risk of stress corrosion cracking. These protective measures include, in particular, special coatings or encapsulation of the chassis components.
[0007] The present invention has for its object to provide a method for producing a component, in particular a chassis component, of a motor vehicle from a high-strength steel, by means of which the risk of stress corrosion cracking can be effectively reduced without the use of additional time-consuming and costly protective measures.
[0008] This object is achieved by a method of the type mentioned at the outset having the features of the characterizing part of claim 1. The subclaims relate to advantageous developments of the invention.
[0009] A method according to the invention is characterized in that a steel from the group of corrosion-resistant, pressure-nitrided, martensitic steels is used to produce the component and the thermal treatment of the component comprises the steps: - Annealing at a temperature of 970 °C to 1030 °C for 20 minutes, - Quenching in liquid nitrogen at -80 °C to - 120 °C for 1 h, - first tempering at a temperature of 250 °C to 280 °C for 2 h, - second tempering at a temperature of 250 °C to 280 °C for approximately 2 hours, whereby the thermal treatment of the component adjusts the tensile strength to a value at least 2% and at most 15% lower than the maximum achievable tensile strength of the high-strength steel used.
[0010] Surprisingly, it has been shown that the defined thermal treatment, in which a tensile strength of at least 2% and at most 15% lower than the maximum achievable tensile strength of the high-strength steel is set, can significantly reduce the component's susceptibility to stress corrosion cracking. According to the invention, it is therefore deliberately accepted that the thermal treatment will not adjust the component's tensile strength to the maximum achievable tensile strength for this steel material. However, this supposed disadvantage proves to be an advantage according to the present invention, since the component's susceptibility to stress corrosion cracking can be effectively reduced while the tensile strength can still be adjusted to a high level.According to current knowledge, the mechanism that significantly reduces the component's susceptibility to stress corrosion cracking most likely lies in the thermal treatments tailored to high-strength steels that generate re-transformed austenite in the steel matrix. This re-transformed austenite is present, at least in part, between the martensite needles. Austenite has greater solubility for hydrogen than martensite. Furthermore, hydrogen diffusion rates are lower in austenite than in martensite. Advantageously, hydrogen has little or no embrittlement effect in austenite, thus reducing the risk of undesirable stress corrosion cracking.The austenite re-transformed by the defined thermal treatment of the component acts as a diffusion barrier, preventing the penetration and spread of hydrogen within the steel matrix. The re-transformed austenite thus acts as a hydrogen trap, effectively preventing corrosive damage to the component. In corrosion-resistant, compressive-resistant, martensitic steels, residual austenite, which remains in the structure during hardening of the steel, has a similar effect. The process according to the invention has the advantage that the risk of stress corrosion cracking can be effectively reduced without the use of additional time-consuming and costly protective measures. The process is particularly suitable for the production of chassis components of a motor vehicle that are mechanically prestressed and are therefore subject to permanent tensile stress.These landing gear components include bearing journals, connecting elements and tripod stars.
[0011] In a preferred embodiment, it is proposed that a corrosion-resistant, pressure-nitrided, martensitic steel of the X30CrMoN15-1 grade according to DIN EN 10027-1:2005-10 be used to manufacture the component. This steel has significantly higher carbon and chromium contents than maraging and aerospace steels.
[0012] Typical values for the chemical composition of a steel grade X30CrMoN15-1, 1.4108, which is commercially available from various manufacturers, are: 0.30 wt% C, 0.60 wt% Si, 0.40 wt% Mn, 15.00 wt% Cr, 1.00 wt% Mo, 0.40 wt% N, Rest: Iron including impurities resulting from smelting.
[0013] Investigations have shown that by thermal treatment, the tensile strength of the component can be adjusted to be at least 2% and at most 15% lower than the maximum achievable tensile strength of the corrosion-resistant, pressure-nitrided, martensitic steel.
[0014] Further features and advantages of the present invention will become clear from the following description of preferred embodiments with reference to the accompanying drawings. Fig. 1 a diagram illustrating the dependence of the tensile strength of a component made of a precipitation-hardening maraging steel on the aging temperature, Fig. 2 a diagram showing the influence of the aging temperature on the notch tensile strength and the threshold load of the component made of maraging steel, Fig. 3 a diagram illustrating the dependence of the tensile strength of a component made of a precipitation-hardening, corrosion-resistant aerospace steel on the aging temperature.
[0015] A method for producing a component, in particular a chassis component, of a motor vehicle from a high-strength steel having a maximum achievable tensile strength higher than 1400 MPa, preferably higher than 1500 MPa, comprises the steps - Forming the component in at least one forming step and - thermal treatment of the component to define the tensile strength of the component.
[0016] The parameters of the component's thermal treatment are selected for each steel so that the tensile strength is deliberately set to a value that is at least 2% and at most 15% lower than the maximum achievable tensile strength of the steel material in question. Various studies have surprisingly shown that the defined thermal treatment, which sets a tensile strength that is at least 2% and at most 15% lower than the maximum achievable tensile strength of the high-strength steel, can significantly reduce the component's susceptibility to stress corrosion cracking.
[0017] For many steel grades, the aging temperature has a significant influence on the tensile strength.
[0018] In Fig. Figure 1 shows the dependence of the aging temperature on the tensile strength of a component, in particular a chassis component of a motor vehicle, made of a precipitation-hardening maraging steel. This embodiment is not the subject of the invention. The high-strength steel in this case is a maraging steel of the grade X3NiCoMoTi18-9-5, 1.6354. This is commercially available from various suppliers and has the following alloy composition: 17 - 19 wt% Ni, 8.00 - 9.50 wt% Co, 4.6 - 5.20 wt% Mo, 0.60 - 0.90 wt% Ti, 0.05 - 0.15 wt% Al, ≤ 0.25 wt% Cr, ≤ 0.03 wt% C, ≤ 0.1 wt% Mn and Si each, ≤ 0.01 wt% P and S each, Rest: iron.
[0019] It is clear that the tensile strength of the tested specimens, starting from low aging temperatures, reaches a range of maximum tensile strength in a temperature range between 480 °C and 540 °C. In this aging temperature range, the tensile strength is > 1900 MPa and < 1950 MPa. In an aging temperature range between 540 °C and 560 °C, the tensile strength drops to a value that is at least 2% and at most 15% lower than the maximum achievable tensile strength of this maraging steel. The component made from the maraging steel is deliberately aged in this temperature range because this can significantly reduce the component's susceptibility to stress corrosion cracking.
[0020] In Fig. Figure 2 shows the results of load increase tests on specimens made from the above-mentioned maraging steel grade X3NiCoMoTi18-9-5, 1.6354, and aged at various temperatures. This embodiment is also not subject to the invention. In the tests, the notch tensile strength R mk in a dry state of the test specimens and the threshold load L in a salt solution with 5% NaCl and a pH value of 3. The test results show that at an aging temperature of 485 °C the difference between the notched tensile strength R mk and the threshold load L is significantly higher than at an aging temperature of 550 °C. The greater the difference between the threshold load L and the notched tensile strength R mk The higher the temperature, the greater the component's susceptibility to stress corrosion cracking. Higher aging temperatures therefore counteract stress corrosion cracking.
[0021] Fig. Figure 3 shows the dependence of tensile strength on the aging temperature of a corrosion-resistant, precipitation-hardening aerospace steel of the X1CrNiMoAlTi12-11-1 grade. This embodiment is also not the subject of the invention. This steel grade, which exhibits high toughness and low tensile stress sensitivity, is commercially available from various manufacturers and typically has the following alloy composition: max. 0.02 wt.% C, max. 0.25 wt.% Si, max. 0.25 wt% Mn, max. 0.015 wt.% P, max. 0.010 wt.% S, 11.00 to 12.50 wt% Cr, 0.75 to 1.25 wt% Mo, 10.75 to 11.25 wt% Ni, 1.50 to 1.80 wt% Ti, Rest: iron.
[0022] A test specimen made from this steel material achieves a tensile strength of approximately 1740 MPa at an aging temperature of 510 °C. If the aging temperature of the test specimens is increased to more than 520 °C up to 550 °C, the resulting tensile strength is at least 2% and at most 15% lower than the maximum tensile strength achievable with this steel material. For example, at an aging temperature of around 540 °C, a tensile strength of approximately 1600 MPa is achieved.
[0023] According to one embodiment of the invention, components made of a corrosion-resistant, pressure-nitrided martensitic steel of grade X30CrMoN15-1, 1.4108 are subjected to a thermal treatment. This commercially available steel exhibits improved corrosion and toughness properties with high hardness and compressive strength compared to conventionally produced Cr or CrMo steels. Typical values for the chemical composition of a steel of grade X30CrMoN15-1, 1.4108 are: 0.30 wt% C, 0.60 wt% Si, 0.40 wt% Mn, 15.00 wt% Cr, 1.00 wt% Mo, 0.40 wt% N, Rest: Iron including impurities resulting from smelting.
[0024] A thermal treatment of a component made of this high-strength steel comprises the following steps: - Annealing at a temperature of 970 °C to 1030 °C for 20 minutes, - Quenching in liquid nitrogen at -80 °C to - 120 °C for 1 h, - first tempering at a temperature of 250 °C to 280 °C for 2 h, - second tempering at a temperature of 250 °C to 280 °C for 2 h.
[0025] Through this thermal treatment, the tensile strength can also be adjusted to a value that is at least 2% and at most 15% lower than the maximum achievable tensile strength of the steel.
[0026] The mechanism that significantly reduces the tendency of the components tested to stress corrosion cracking is most likely due to the thermal treatments tailored to the high-strength steels that generate re-transformed austenite in the steel matrix. This re-transformed austenite is present, at least in part, between the martensite needles. Austenite has greater solubility for hydrogen than martensite. Furthermore, hydrogen has a lower diffusion rate in austenite than in martensite. Advantageously, hydrogen embrittlement in austenite is either non-existent or very minimal, thus reducing the risk of undesirable stress corrosion cracking. The re-transformed austenite, created by the specific thermal treatment of the component, acts as a diffusion barrier, preventing the penetration and spread of hydrogen within the steel matrix.The re-transformed austenite thus acts as a kind of hydrogen trap. In corrosion-resistant, compressive-resistant, martensitic steels, residual austenite, which remains in the structure during hardening, has a similar effect.
[0027] The process presented here is particularly suitable for the production of chassis components of a motor vehicle that are mechanically prestressed and subject to permanent tensile stress, as stress corrosion cracking is particularly critical for these chassis components. These chassis components include bearing journals, connecting elements, and tripod spiders.
Claims
[1] Method for producing a component, in particular a chassis component, of a motor vehicle, comprising the steps - Forming the component in at least one forming step and - thermal treatment of the component to define the tensile strength of the component, characterized by that a steel from the group of corrosion-resistant, pressure-nitrided, martensitic steels is used to manufacture the component and the thermal treatment of the component comprises the following steps: - Annealing at a temperature of 970 °C to 1030 °C for 20 minutes, - Quenching in liquid nitrogen at -80 °C to - 120 °C for 1 h, - first tempering at a temperature of 250 °C to 280 °C for 2 h, - second tempering at a temperature of 250 °C to 280 °C for approximately 2 hours, whereby the thermal treatment of the component adjusts the tensile strength to a value at least 2% and at most 15% lower than the maximum achievable tensile strength of the high-strength steel used. [2] Method according to claim 1, characterized by that a corrosion-resistant, pressure-nitrided, martensitic steel of the type X30CrMoN15-1 according to DIN EN 10027-1:2005-10 is used to manufacture the component.
Citation Information
Patent Citations
high-strength steel component with targeted deformation in the event of a crash
DE102005054847B3
Corrosion-resistant chromium steel, process for its production and use of the corrosion-resistant chromium steel
DE3310693A1
Manufacture of ultrahigh tensile maraging cold rolled steel plate
JP1985234920A
Production of austenitic stainless steel sheet or strip
JP1992168227A
Method of processing maraging steel
US20100037994A1