SILICON CARBIDE SEMICONDUCTOR DEVICE
The silicon carbide semiconductor device addresses the challenge of controlling conductivity type concentration profiles by using ion implantation to form a bell-shaped conductivity type profile, reducing gate threshold voltage variation and switch-on resistance, and enhancing channel mobility, thereby increasing yield and reducing defects.
Patent Information
- Application Number
- DE102016226235
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-08-25
- Filing Date
- 2016-12-27
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2036-12-27
AI Technical Summary
Conventional silicon carbide semiconductor devices face challenges in controlling the variation of gate threshold voltage and switch-on resistance due to difficulties in managing the conductivity type concentration profiles, leading to increased defective chips and reduced yield.
A silicon carbide semiconductor device with a first and second semiconductor layer, featuring a first semiconductor region with a bell-shaped conductivity type concentration profile and a gate electrode embedded in a trench, formed through ion implantation to control the conductivity type concentration differences, reducing variations and enhancing channel mobility.
The solution effectively reduces the variation of gate threshold voltage and switch-on resistance, increasing yield by minimizing creep current defects and improving channel mobility, while maintaining low resistance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND OF THE INVENTIONField of the invention
[0001] The embodiments of the invention relate to a silicon carbide semiconductor device and a method for manufacturing a silicon carbide semiconductor device. General state of the art
[0002] Document US 2015 / 0 194 492 A1 discloses a semiconductor device comprising a semiconductor layer of a first conductivity type made of SiC having a Si surface; a gate trench dug downward from the surface of the semiconductor layer; a gate insulating film formed on a bottom surface and a side surface of the gate trench such that the ratio of the thickness of a portion located on the bottom surface to the thickness of a portion located on the side surface is 0.3 to 1.0; and a gate electrode embedded in the gate trench through the gate insulating film.
[0003] The document US 2011 / 0 068 353 A1 describes a semiconductor device comprising a first n-type semiconductor layer, a second n-type semiconductor layer, a p-type semiconductor layer, a trench, an insulating layer, a gate electrode, and an n-type semiconductor region. The p-type semiconductor layer includes a channel region located along the trench and in contact with the second n-type semiconductor layer and the n-type semiconductor region. The size of the channel region in the depth direction x is 0.1 to 0.5 µm. The channel region includes a high-concentration region in which the maximum impurity concentration is approximately 1 × 10 13 cm -3 amounts.
[0004] Silicon carbide (SiC) is considered to be the next-generation semiconductor material compared to silicon (Si). Compared with conventional semiconductor devices using Si as a material, semiconductor devices using silicon carbide (hereinafter referred to as silicon carbide semiconductor devices) offer various advantages, such as reducing the device's on-state resistivity to several hundredths and allowing use in high-temperature environments (200°C or more). These advantages are made possible by the characteristics of the material itself, such as the fact that the band gap of SiC is approximately three times that of Si and the breakdown field strength is about ten times that of Si.
[0005] Schottky diodes (SBDs) and planar vertical metal-oxide-semiconductor field-effect transistors (MOSFETs) have become commercially available SiC semiconductor devices.
[0006] A trench-gate structure is a 3-dimensional structure in which a metal oxide semiconductor (MOS) gate (insulated MOS gate) is embedded in a trench formed in a semiconductor base made of silicon carbide (hereinafter, silicon carbide base), and a portion along a trench sidewall is used as a channel (inversion layer). Therefore, when comparing the device area (chip area) between devices with the same on-resistance (Ron), the device area of the trench-gate structure can be designed significantly smaller than that of a planar gate structure in which a MOS gate is provided in a flat shape on a silicon carbide base, and thus, a trench-gate structure can be considered a promising device structure.
[0007] A structure of a conventional silicon carbide semiconductor device is described, taking a vertical MOSFET with a trench gate structure as an example. Fig. Figure 27 is a cross-sectional view of a structure of a conventional silicon carbide semiconductor device. The conventional silicon carbide semiconductor device shown in Fig. 27 comprises a MOS gate having a typical trench gate structure on the side of a front side (surface on the side of a p-doped base region 104) of a semiconductor base formed of silicon carbide (hereinafter silicon carbide base) 100. The silicon carbide base (semiconductor chip) 100 is formed by epitaxially growing an n + -doped carrier substrate formed from silicon carbide (hereinafter n + -doped silicon carbide substrate) 101, an n -doped drift region 102, an n-doped current spreading region 103 and the p-doped base region 104, which form silicon carbide layers, are formed.
[0008] In the n-doped current spreading region 103, a first p-doped region 111 is selectively provided to completely cover the bottom of a trench 107. The first p-doped region 111 is provided to a depth which covers the n - -doped drift region 102. Furthermore, a second p-doped region 112 is selectively provided between adjacent trenches 107 (mesa part) in the n-doped current spreading region 103. The second p-doped region 112 contacts the p-doped base region 104 and is provided to a depth which covers the n - -doped drift region 102. The reference numerals 105, 106, 108, 109 and 113 to 115 are each an n + -doped source region, a p ++-doped contact region, a gate insulating layer, a gate electrode, an interlayer insulating layer, a source electrode and a drain electrode.
[0009] As such a vertical MOSFET with a trench gate structure, a device has been proposed which includes a p-doped base layer with a 2-layer structure comprising p-doped semiconductor layers with different impurity concentrations formed sequentially by epitaxy (see, for example, Japanese Patent Application Laid-Open No. JP 2012 - 099 601 A (paragraph 0030, Fig. 1) and Japanese Patent Application Laid-Open No. JP 2015-072999 A (paragraph 0060, Fig. 109). In Japanese Patent Application Laid-Open Nos. JP 2012-099601 A and JP 2015-072999 A, between the p-type semiconductor layers forming the p-type base layer, punch-through is suppressed at the p-type semiconductor layer with the higher impurity concentration, and the on-resistance is reduced at the p-type semiconductor layer with the lower impurity concentration.
[0010] Furthermore, a technique for implanting impurity ions (p-conductivity type), such as aluminum (Al) ions, boron (B) ions, etc., on an upper surface of an n-type semiconductor layer in a vertical MOSFET having a trench gate structure to form the p-type semiconductor layer has been proposed (see, for example, Japanese Patent Laid-Open No. JP 2014 - 241435 A (paragraph 0028)). SUMMARY OF THE INVENTION
[0011] According to one aspect of the present invention, a silicon carbide semiconductor device according to claim 1 is provided. The silicon carbide semiconductor device comprises a first semiconductor layer having a first conductivity type formed on a front side of a silicon carbide substrate; a second semiconductor layer having a second conductivity type formed on an opposite side of the first semiconductor layer to a silicon carbide substrate side thereof; a first semiconductor region having the second conductivity type and selectively formed in the second semiconductor layer, the first semiconductor region having an impurity concentration higher than that of the second semiconductor layer; a second semiconductor region having the first conductivity type and selectively formed in the second semiconductor layer at a position shallower than the first semiconductor region;a trench penetrating the second semiconductor region, the first semiconductor region, and the second semiconductor layer and reaching the first semiconductor layer; a gate electrode provided in the trench via a gate insulating layer; a first electrode contacting the second semiconductor region and the second semiconductor layer;and a second electrode provided on a backside of the silicon carbide substrate. The first semiconductor region has an impurity concentration profile with a second conductivity type, in which concentration differences in a depth direction form a bell-shaped curve at a peak of the impurity concentration higher than that of the second semiconductor layer. In the silicon carbide semiconductor device, the peak of the impurity concentration of the impurity concentration profile with a second conductivity type is positioned farther on the first electrode side than the boundary between the second semiconductor layer and the first semiconductor layer.
[0012] Further aspects of the invention are the subject of the subclaims, the drawings and the following description of embodiments.
[0013] In the silicon carbide semiconductor device, the first semiconductor region preferably has the impurity concentration profile with a second conductivity type in which the concentration differences in the depth direction form a plurality of bell-shaped curves at a plurality of peaks of the impurity concentration higher than that of the second semiconductor layer.
[0014] In the silicon carbide semiconductor device, in the impurity concentration profile having a second conductivity type, the impurity concentration preferably decreases sharply at a boundary of the second semiconductor layer and the first semiconductor layer.
[0015] In the silicon carbide semiconductor device, the first semiconductor region is preferably uniformly provided in a direction parallel to the front surface of the silicon carbide substrate.
[0016] The silicon carbide semiconductor device preferably includes a third semiconductor region having the first conductivity type and is formed in the first semiconductor layer, the third semiconductor region having an impurity concentration higher than that of the first semiconductor layer. The third semiconductor region contacts the second semiconductor layer and reaches a position deeper than a bottom of the trench on the second electrode side from a boundary with the second semiconductor layer.
[0017] The silicon carbide semiconductor device preferably comprises a fourth semiconductor region having the second conductivity type selectively formed in the third semiconductor region, the fourth semiconductor region covering the bottom of the trench.
[0018] In the silicon carbide semiconductor device, the fourth semiconductor region preferably penetrates into the third semiconductor region from the bottom of the trench in the depth direction.
[0019] The silicon carbide semiconductor device preferably comprises a fifth semiconductor region having the second conductivity type formed in the third semiconductor region between the trench and an adjacent trench to contact the second semiconductor layer.
[0020] In the silicon carbide semiconductor device, the fifth semiconductor region preferably penetrates into the third semiconductor region in the depth direction.
[0021] A silicon carbide semiconductor device according to another aspect includes a first semiconductor layer having a first conductivity type formed on a front surface of a silicon carbide substrate; a first semiconductor region having a second conductivity type selectively formed in the first semiconductor layer; a second semiconductor region having the first conductivity type selectively formed in the first semiconductor layer at a position shallower than the first semiconductor region; a trench penetrating into the second semiconductor region and the first semiconductor region and reaching the first semiconductor layer; and a gate electrode provided in the trench via a gate insulating film; a first electrode contacting the second semiconductor region and the first semiconductor layer; and a second electrode provided on a back surface of the silicon carbide substrate.The first semiconductor region has an impurity concentration profile with a second conductivity type in which concentration differences in a depth direction form a plurality of bell-shaped curves at a plurality of peaks.
[0022] In the silicon carbide semiconductor device, among the plurality of tips, the impurity concentration at a first tip on the side of a first electrode is higher than that of a second tip on the side of a second electrode.
[0023] A method for manufacturing a silicon carbide semiconductor device according to another aspect includes forming a first semiconductor layer having a first conductivity type on a front surface of a silicon carbide substrate; forming a second semiconductor layer having a second conductivity type on the first semiconductor layer; selectively forming a first semiconductor region having the second conductivity type by ion implantation in the second semiconductor layer, the first semiconductor region having an impurity concentration higher than that of the second semiconductor layer; selectively forming a second semiconductor region having the first conductivity type in the second semiconductor layer at a position shallower than the first semiconductor region; forming a trench to penetrate into the second semiconductor region, the first semiconductor region, and the second semiconductor layer and reach the first semiconductor layer;Forming a gate electrode in the trench using a gate insulating layer; Forming a first electrode contacting the second semiconductor region and the second semiconductor layer; and Forming a second electrode on a backside of the silicon carbide substrate. The first semiconductor region is formed to have an impurity concentration profile with a second conductivity type, in which concentration differences in a depth direction form a bell-shaped curve at a peak of the impurity concentration higher than that of the second semiconductor layer.
[0024] In the method for manufacturing a silicon carbide semiconductor device, the first semiconductor region is formed by a plurality of ion implantation phases to have the impurity concentration profile of the second conductivity type in which the concentration differences in the depth direction form a plurality of bell-shaped curves at a plurality of peaks of the impurity concentration higher than that of the second semiconductor layer.
[0025] In the method for manufacturing a silicon carbide semiconductor device, ion implantation is performed using an accelerating voltage so that the peak of the impurity concentration in the impurity concentration profile having a second conductivity type is formed at a position deeper than a surface of the ion implantation.
[0026] The method of manufacturing a silicon carbide semiconductor device includes forming a third semiconductor layer having the second conductivity type on the second semiconductor layer after forming the first semiconductor region and before forming the second semiconductor region.
[0027] In the method for manufacturing a silicon carbide semiconductor device, ion implantation is performed using an accelerating voltage so that the peak of the impurity concentration in the impurity concentration profile having a second conductivity type is formed at a position equal to or deeper than a surface of the ion implantation.
[0028] In the method for manufacturing a silicon carbide semiconductor device, ion implantation is performed using an accelerating voltage so that the peak of the impurity concentration in the impurity concentration profile having a second conductivity type is formed at a depth position further on the side of a first electrode than a boundary of the second semiconductor layer and the first semiconductor layer.
[0029] A method for manufacturing a silicon carbide semiconductor device according to one aspect includes forming a first semiconductor layer having a first conductivity type on a front surface of a silicon carbide substrate; selectively forming a first semiconductor region having a second conductivity type in the first semiconductor layer by ion implantation; selectively forming a second semiconductor region having the first conductivity type in the first semiconductor layer at a position shallower than the first semiconductor region; forming a trench to pass through the second semiconductor region and the first semiconductor region and reach the first semiconductor layer; forming a gate electrode in the trench using a gate insulating film; forming a first electrode contacting the second semiconductor region and the first semiconductor layer; and forming a second electrode on a back surface of the silicon carbide substrate.The first semiconductor region is formed by a plurality of ion implantation phases to have an impurity profile with a second conductivity type in which the concentration differences in a depth direction form a plurality of bell-shaped curves at a plurality of peaks.
[0030] In the method of manufacturing a silicon carbide semiconductor device, the first semiconductor region is formed to have the impurity concentration profile with a second conductivity type in which, among the plurality of peaks, an impurity concentration at a first peak on the first electrode side is higher than that at a second peak on the second electrode side.
[0031] The objects, features and advantages of the present invention will be specifically pointed out or will become apparent from the following detailed description of the invention when read in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] They show: Fig. 1 is a cross-sectional view of a structure of a semiconductor device according to a first embodiment; Fig. 2 a characteristic field showing an impurity concentration profile at the section line AA' in Fig. 1 shows; Fig. 3, Fig. 4, Fig. 5, Fig. 6, Fig. 7, Fig. 8, Fig. 9, Fig. 10, Fig. 11, Fig. 12, Fig. 13 and Fig. 14 shows cross-sectional views of the semiconductor device according to the first embodiment during manufacture; Fig. 15, Fig. 16 and Fig. 17 shows cross-sectional views of the semiconductor device according to a second embodiment during manufacture; Fig. 18 is a cross-sectional view showing a structure of the semiconductor device according to a third embodiment; Fig. 19 is a characteristic diagram illustrating the impurity concentration profile in the case of the semiconductor device according to a fourth embodiment; Fig. 20 is a characteristic diagram illustrating the impurity concentration profile in the case of the semiconductor device according to a fifth embodiment; Fig. 21 is a characteristic diagram showing the impurity concentration profile in the case of the semiconductor device according to a sixth embodiment; Fig. 22 is a characteristic diagram illustrating a frequency of occurrence of leakage current between a drain and a source of the silicon carbide semiconductor device according to a first example; Fig. 23 is a characteristic diagram showing the frequency of occurrence of leakage current between the drain and the source in a conventional example of a silicon carbide semiconductor device; Fig. 24 is a characteristic diagram illustrating the variation of a gate threshold voltage Vth of the silicon carbide semiconductor device according to a second example; Fig. 25A, Fig. 25B and Fig. 25C are diagrams illustrating the conditions of a p-doped base region of silicon carbide semiconductor devices of first and second comparative examples; Fig. 26 Calculation results of on-resistance values when the gate threshold voltage Vth is changed differently by respective conditions; and Fig. 27 is a cross-sectional view of a structure of a conventional silicon carbide semiconductor device. DETAILED DESCRIPTION OF THE INVENTION
[0033] Embodiments of a silicon carbide semiconductor device and a method for manufacturing a silicon carbide semiconductor device according to the present invention will be described in detail with reference to the accompanying drawings. In the present description and the accompanying drawings, layers and regions with the prefix n or p mean that the majority carriers are electrons or holes. In addition, a + or - appended to n or p means that the impurity concentration is higher or lower than in layers and regions without + or -, respectively. In the following description of the embodiments and in the accompanying drawings, identical components are given the same reference numerals and will not be described repeatedly.
[0034] The semiconductor device according to the present invention is configured using a semiconductor material (hereinafter, a wide-gap semiconductor) that has a wider band gap than silicon. A structure of a semiconductor device (silicon carbide semiconductor device) using silicon carbide (SiC) as a wide-gap semiconductor will be described as an example. Fig. 1 is a cross-sectional view of a structure of the semiconductor device according to a first embodiment. In Fig. 1 only 2 unit cells (functional units of an element) are shown, the other unit cells that are adjacent to them are omitted in the drawing (similar to Fig. 18). The semiconductor device according to the first embodiment shown in Fig. 1 is a MOSFET having a MOS gate on a front side (surface on the side of a p-doped base region 4) of a semiconductor base (silicon carbide base: semiconductor chip) 10 formed of silicon carbide.
[0035] The silicon carbide base 10 is formed by depositing on an n + -doped carrier substrate (n + -doped silicon carbide substrate) 1, which is formed of silicon carbide, silicon carbide layers (first and second semiconductor layers) 21, 22, which become an n-doped drift region 2, and the p-doped base region 4 are grown one after the other. Each MOS gate is formed by the p-doped base region 4, an n + -doped source region (second semiconductor region) 5, a p ++-doped contact region 6, a trench 7, a gate insulating layer 8 and a gate electrode 9. In particular, in a surface layer of a source side (a source electrode 16) of the n - An n-type region (hereinafter, n-type current spreading region (third semiconductor region)) 3 is provided on the p-type base region 4 to contact the p-type base region 4. The n-type current spreading region 3 is a so-called current spreading layer (CSL) that reduces carrier spreading resistance. The n-type current spreading region 3 is uniformly provided, for example, in a direction (hereinafter, the horizontal direction) parallel to a base front surface (a front surface of the silicon carbide base 10). Although the n-type current spreading region 3 may be omitted, the provision of the n-type current spreading region 3 enables an improvement in the on-resistance and breakdown voltage.
[0036] The part of the n-doped silicon carbide layer 21 other than the n-doped current spreading region 3 is the n - -doped drift region 2. In the n-doped current spreading region 3, first and second p + -doped regions (fourth and fifth semiconductor regions) 11, 12 are each selectively provided. The first p + -doped region 11 is provided to cover a bottom and a lower corner part of the trench 7. The lower corner part of the trench 7 is the boundary of a sidewall and the bottom of the trench 7. The first p + -doped region 11 is provided from a position deeper than an interface of the p-doped base region 4 and the n-doped current spreading region 3 on the drain side to a depth that does not reach an interface of the n-doped current spreading region 3 and the n-doped drift region 2. The provision of the first p +-doped region 11 enables the formation of a pn junction between the first p + -doped region 11 and the n-doped current spreading region 3 near the bottom of the trench 7.
[0037] The second p + -doped region 12 is formed between adjacent trenches 7 (mesa part), from the first p + -doped region 11 is removed, provided and contacts the p-doped base region 4. Certain parts of the second p + -doped region 12 can extend on the sides of the trench 7 and partially cover the first p + -doped regions 11. Furthermore, the second p + -doped region 12 from the interface of the p-doped base region 4 and the n-doped current spreading region 3 to a depth which reaches the interface of the n-doped current spreading region 3 and the n - doped drift region 2 is not reached. The provision of the second p +doped region 12 enables the formation of a pn junction between the second p + doped region 12 and the n-doped current spreading region 3 between the adjacent trenches 7 in a position that is deeper than the bottom of the trenches 7. The formation of the pn junctions by the first and second p + -doped regions 11, 12 and the n-doped current spreading region 3 makes it possible to prevent a strong electric field from being applied to a lower part of the trench 7 of the gate insulating layer 8.
[0038] In the p-doped silicon carbide layer 22, the n + -doped source region 5 and the p ++ -doped contact region 6 are each selectively provided to contact each other. The depth of the p ++ -doped contact region 6 can, for example, be deeper than the n + -doped source region 5. The part of the p-doped silicon carbide layer 22 other than the n +-doped source region 5 and the p ++ -doped contact region 6 is the p-doped base region 4. In the p-doped base region 4, a p + -doped region (hereinafter highly concentrated implantation region (first semiconductor region)) 13 formed by ion implantation of a p-doped impurity (dashed part).
[0039] The highly concentrated implantation region 13 is provided uniformly, for example, in the horizontal direction to include the parts of the p-type base region 4 in which a channel is formed. The parts of the p-type base region 4 in which the channel is formed are the parts of the p-type base region 4 along the sidewalls of the trench 7. Reference numerals 4a and 4b are respectively a part (hereinafter, the first p-type base part) that is farther on the drain side than the highly concentrated implantation region 13, and a part (hereinafter, the second p-type base part) that is farther on the source side than the highly concentrated implantation region 13 in the p-type base region 4. The first and second p-type base parts 4a, 4b have an impurity concentration lower than that of the highly concentrated implantation region 13.
[0040] The first and second p-doped base portions 4a, 4b and the high-concentration implantation region 13 configure the p-doped base region 4. In the portions of the first and second p-doped base portions 4a, 4b and the high-concentration implantation region 13 along the sidewalls of the trenches 7, an n-doped inversion layer (channel) is formed during the ON state. Although in Fig. 1 and Fig. 2, the highly concentrated implantation region 13 is depicted as having a predetermined thickness t1 to clarify the arrangement of the highly concentrated implantation region 13, the highly concentrated implantation region 13 is a part formed by ion implantation of a p-type impurity and has a p-type impurity concentration profile 31 with Gaussian distribution (impurity concentration distribution) (see Fig. 2).
[0041] In particular, the highly concentrated implantation region 13 has a p-doped impurity concentration profile 31 in which the concentration differences in the depth direction form a bell-shaped curve at a peak 13a of the impurity concentration, which is higher than that of the p-doped silicon carbide layer 22 forming the p-doped base region 4. In other words, the peak 13a of the p-doped impurity concentration profile 31 lies in the p-doped base region 4, and the impurity concentration decreases from the position of the peak 13a on both sides of the main surface (source side and drain side) of the base via respective predetermined slopes. The depth of the position of the peak 13a of the highly concentrated implantation region 13 is in a range from a position deeper than or equal to the depth of the position of the interface of the n +-doped source region 5 and the p-doped base region 4, and a position shallower than the depth of the position of the interface of the p-doped base region 4 and the n-doped current spreading region 3.
[0042] Preferably, the depth of the position of the tip 13a of the high concentration implantation region 13 can be in a range from the interface of the n + -doped source region 5 and the p-doped base region 4 to a depth of approximately 80% of a thickness t2 of the p-doped base region 4 (= 0.8xt2), and the tip 13a may be in a range from the interface of the n +-doped source region 5 and the p-doped base region 4 to a depth that is approximately 10% to 70% of the thickness t2 of the p-doped base region 4. The reason for this is to further improve the trade-off between the reduced on-resistance and the reduced variation of the gate threshold voltage Vth. The thickness t2 of the p-doped base region 4 is a thickness from the interface of the n + -doped source region 5 and the p-doped base region 4 to the interface of the p-doped base region 4 and the n-doped current spreading region 3.
[0043] In other words, the tip 13a of the highly concentrated implantation region 13 is located in a position that is shallower than the n-doped current spreading region 3 relative to the base front and is distant from the n-doped current spreading region 3 in depth. If the depth of the position of the tip 13a of the highly concentrated implantation region 13 is the depth of the position of the interface of the n + -doped source region 5 and the p-doped base region 4, the highly concentrated implantation region 13 contacts the n + -doped source region 5 and the p ++ doped contact region 6, whereby the second p-doped base portion 4b is not formed. The p-doped impurity concentration profile resulting from the ion implantation of a p-doped impurity to form the highly concentrated implantation region 13 will be described in detail below.
[0044] The highly concentrated implantation region 13 may have a plurality of impurity concentration peaks 13a at different depths. In this case, the depths of the positions of all impurity concentration peaks 13a of the highly concentrated implantation region 13 are in the previously described ranges. Disturbance in the crystal structure (for example, defects such as dislocations) partially occurs in the p-doped base region 4 to a greater extent with the ion implantation for forming the highly concentrated implantation region 13 than in a case with only epitaxy. Therefore, when the p-doped base region 4 is formed only by epitaxy without ion implantation of an impurity (ie, the conventional structure used in Fig. 27), the layer quality is sometimes different.
[0045] Trench 7 penetrates the n +-doped source region 5, the highly concentrated implantation region 13, and the p-doped base region 4 from the base front side and reaches the n-doped current spreading region 3. In the trench 7, the gate insulating film 8 is provided along the sidewalls of the trench 7, and the gate electrode 9 is provided on the gate insulating film 8. A source-side end of the gate electrode 9 may or may not protrude outward from the base front side. The gate electrode 9 is electrically connected to a gate pad (not shown) at a part not shown. An interlayer insulating film 14 is provided on the entire base front side to cover the gate electrode 9 embedded in the trench 7.
[0046] The source electrode (first electrode) 16 contacts the n + -doped source region 5 and the p ++-doped contact region 6 via a contact hole in the interlayer insulating layer 14 and is electrically insulated from the gate electrode 9 by the interlayer insulating layer 14. Between the source electrode 16 and the interlayer insulating layer 14, for example, a barrier metal 15 can be provided, which prevents the spread of metal atoms from the source electrode 16 to the side of the gate electrode 9. A source contact area 17 is provided at the source electrode 16. On a back side of the silicon carbide base 10 (back side of the n + -doped silicon carbide substrate 1, which contains the n + -doped drain region) a drain electrode (second electrode) 18 is provided.
[0047] The p-doped impurity concentration profile resulting from the ion implantation of a p-doped impurity to form the high-concentration implantation region 13 is described. Fig. 2 is a characteristic field showing the impurity concentration profile at the section line AA' in Fig. 1. In Fig. 2, a horizontal axis represents the depth from the base front (the interface of the source electrode 16 and the silicon carbide base 10), and a vertical axis represents the impurity concentration. In addition to the p-doped impurity concentration profile 31 resulting from the ion implantation of a p-doped impurity to form the high-concentration implantation region 13, Fig. 2 an n-doped impurity concentration profile 32 resulting from the ion implantation of an n-doped impurity to form the n + -doped source region 5. In Fig. 2, the n-doped impurity (n-type dopant) is assumed to be phosphorus (P), and the p-doped impurity (p-type dopant) is assumed to be aluminum (Al).
[0048] As in Fig. 2, the impurity concentration (background impurity concentration) of the p-doped silicon carbide layer 22, which forms the p-doped base region 4 on the epitaxially grown n-doped silicon carbide layer 21, is approximately 4×10 16 atoms / cm 3 . As a result of the ion implantation of an n-doped impurity to form the n +-doped source region 5 in the p-doped silicon carbide layer 22, the n-doped impurity concentration profile 32 is formed, which has a peak 32a impurity concentration higher than that of the p-doped silicon carbide layer 22 in a relatively shallow position. In the n-doped impurity concentration profile 32, the impurity concentration decreases from the position of the peak 32a on the drain side over a predetermined slope. A part of the base front side (the opposite side of the p-doped silicon carbide layer 22 from the side of the n-doped silicon carbide layer 21) up to an intersection point 30a of the n-doped impurity concentration profile 32 and the p-doped impurity concentration profile 31 is the n + -doped source region 5. The peak 32a of the n-doped impurity concentration profile 32 is a peak 5a of the impurity concentration profile of the n + -doped source region 5.
[0049] Furthermore, as a result of the ion implantation of a p-type impurity to form the high-concentration implantation region 13 in the p-type silicon carbide layer 22, the p-type impurity concentration profile 31 is formed, which has a peak 31a of the impurity concentration at a position deeper than the peak 32a of the n-type impurity concentration profile 32 of the base front. The peak 31a of the p-type impurity concentration profile 31 is the peak 31a of the impurity concentration profile of the high-concentration implantation region 13. Furthermore, in the p-type impurity concentration profile 31, the impurity concentration on the source side and the drain side decreases by respective predetermined slopes from the position of the peak 31a in a bell-shaped curve.In addition, in the p-doped impurity concentration profile 31, the impurity concentration at an interface 30b of the p-doped silicon carbide layer 22 and the n. - -doped silicon carbide layer 21, and the impurity concentration decreases by a predetermined gradient from the interface 30b toward the drain side. The peak 31a of the impurity concentration of the p-doped impurity concentration profile 31 is, for example, 6×10 17 atoms / cm 3 .
[0050] Such a p-doped impurity concentration profile 31 is achieved by performing ion implantation of a p-doped impurity to form the high-concentration implantation region 13 after the p-doped silicon carbide layer 22 forming the p-doped base region 4 is formed by epitaxy. When the p-doped base region 104 is formed only by epitaxy, such as in the conventional structure (see Fig. 27), the control of the impurity concentration is difficult, and the p-doped impurity concentration profile 31 is not achieved. A part from the intersection point 30a of the profile 32 of an n-doped impurity concentration and the p-doped impurity concentration profile 31 to the interface 30b of the p-doped silicon carbide layer 22 and the n - -doped silicon carbide layer 21 is the p-doped base region 4. A part which is deeper on the drain side than the interface 30b of the p-doped silicon carbide layer 22 and the n - -doped silicon carbide layer 21, the n - doped silicon carbide layer 21, which forms the n-doped current spreading region 3 and the n - -doped drift region 2.
[0051] The impurity concentration of the p-doped silicon carbide layer 22 forming the p-doped base region 4 may, for example, preferably be in a range of 1×10 16atoms / cm 3 or more up to 2×10 17 atoms / cm 3 or less, since the same effects as those of the above example are achieved within this range. Furthermore, the impurity concentration of the peak 31a of the p-doped impurity concentration profile 31 may preferably be in a range of 2×10 16 atoms / cm 3 or more up to 5×10 13 atoms / cm 3or less. If the peak 31a of the impurity concentration of the p-doped impurity concentration profile 31 is set to be higher than the impurity concentration of the p-doped silicon carbide layer 22, the same effects as those of the above example are achieved. Although a channel length L of 0.6 μm is assumed, the configuration is not limited thereto, and the channel length L may preferably be 0.3 μm or more and 1 μm or less. The channel length L is a length from the intersection point 30a of the n-doped impurity concentration profile 32 and the p-doped impurity concentration profile 31 to the interface 30b of the p-doped silicon carbide layer 22 and the n - -doped silicon carbide layer 21.
[0052] The method for manufacturing a silicon carbide semiconductor device according to the first embodiment will be described. Fig. 3, Fig. 4, Fig. 5, Fig. 6, Fig. 7, Fig. 8, Fig. 9, Fig. 10, Fig. 11, Fig. 12, Fig. 13 and Fig. 14 are cross-sectional views of the semiconductor device according to the first embodiment during manufacture. As shown in Fig. 3, the n + -doped silicon carbide substrate 1, which contains the n + -doped drain region. Then, on the front side of the n + -doped silicon carbide substrate 1 the n - doped silicon carbide layer 21a, which forms the n - -doped silicon carbide layer 21 is formed by epitaxy. Subsequently, the first p + -endowed regions 11 and the p + -endowed regions (hereinafter p + -doped subregions) 12a each selectively in the surface layer of the n - -doped silicon carbide layer 21a by photolithography and ion implantation of a p-doped impurity. The p+ -doped subregions 12a are part of the second p + -endowed Region 12.
[0053] Then, as in Fig. 4, an n-doped impurity in the entire n-doped silicon carbide layer 21a, which forms an n-doped region (hereinafter n-doped sub-region) 3a in the entire surface layer of the n - -doped silicon carbide layer 21a is ion-implanted. The n-doped subregion 3a is a part of the n-doped current spreading region 3. Now, the depth of the n-doped subregion 3a becomes deeper than the first p + -doped regions 11, and the entire drain side (the side of the n + -doped silicon carbide substrate 1) of the first p + -endowed regions 11 and the p +-doped subregions 12a are covered by the n-doped subregion 3a. A part of the n-doped silicon carbide layer 21a, which is further away on the drain side than the n-doped subregion 3a, forms the n - -doped drift region 2. The order in which the n-doped subregion 3a and the first p + -endowed regions 11 and the p + The doped subregions 12a are formed can be interchanged. The ion implantation can be performed at ambient temperature (less than 200 °C) or at a high temperature (200 °C to 500 °C). For ion implantation at ambient temperature, a resist layer is used as a mask, and for ion implantation at high temperature, an oxide layer is used as a mask (the same applies to all ion implantations discussed below).
[0054] As in Fig. 5, will next be shown on the n --doped silicon carbide layer 21a an n - -doped silicon carbide layer 21b, which has the previously described n - doped silicon carbide layer 21 is formed by epitaxy. Next, as shown in Fig. 6 shown, the p + -doped subregions 12b by photolithography and ion implantation of a p-doped impurity in a part of the n--doped silicon carbide layer 21b opposite the p + -doped subregions 12a to a depth which corresponds to the p + doped subregions 12a are selectively formed. The width and the impurity concentration of the p + -doped subregions 12b, for example, are essentially the same as those of the p + -endowed subregion 12a. The p + -doped subregions 12a, 12b are joined together in the depth direction (vertical direction), whereby the second p + -doped region 12 is formed.
[0055] Next, as in Fig. 7, an n-doped impurity is ion-implanted into the entire n-doped silicon carbide layer 21b, forming an n-doped sub-region 3b in the entire n-doped silicon carbide layer 21b, to a depth that reaches the n-doped sub-region 3a. The impurity concentration of the n-doped sub-region 3b can be substantially the same as that of the n-doped sub-region 3a. The n-doped sub-regions 3a, 3b are joined together in the depth direction, thereby forming the n-doped current spreading region 3. The order in which the p + -doped subregions 12b and the n-doped subregion 3b can be exchanged. Next, as shown in Fig. 8, the p-doped silicon carbide layer 22 is formed by epitaxy on the n-doped silicon carbide layer 21. Through the previous process steps, the n +-doped silicon carbide substrate 1 the n - doped silicon carbide layer 21 and the p-doped silicon carbide layer 22 are deposited in sequence, thereby forming the silicon carbide base (semiconductor wafer) 10.
[0056] Next, as in Fig. 9, a p-doped impurity is fully ion-implanted in the p-doped silicon carbide layer 22 to form the highly concentrated implantation region 13 to the predetermined thickness t1 at a predetermined depth in the p-doped silicon carbide layer 22. As a result, for example, in the p-doped silicon carbide layer 22, a part that is farther away on the drain side than the highly concentrated implantation region 13 forms the first p-doped base part 4a, and a part that is farther away on the source side (relative to the n +-doped silicon carbide substrate 1) is farther away than the highly concentrated implantation region 13, forms the second p-doped base part 4b. The p-doped base region 4 is formed by the first and second p-doped base parts 4a, 4b and the highly concentrated implantation region 13.
[0057] Next, as in Fig. 10, by photolithography and ion implantation of an n-doped impurity the n + -doped source region 5 is selectively formed in the surface layer of the p-doped silicon carbide layer 22. The n + doped source region 5 can contact the high concentration implantation region 13. Next, as shown in Fig. 11, by photolithography and ion implantation of a p-doped impurity each p ++ -doped contact region 6 is selectively formed in the surface layer of the p-doped silicon carbide layer 22 to form the n+ doped source regions 5. In other words, the n + -doped source regions 5 and the p ++ -doped contact regions 6 are each selectively formed in the second p-doped base part 4b. The order in which the n + -doped source region 5 and the p ++ -doped contact region 6 can be interchanged. After all ion implantations have been completed, an activation annealing step is performed. The temperature of the activation annealing step can preferably be between 1500 °C and 1900 °C. During activation annealing, for example, the formation of a carbon (C) layer on the surface by sputtering, etc., and annealing is desired.
[0058] Next, as in Fig. 12, by photolithography and etching each trench 7 is formed to enter the n +-doped source region 5, the first and second p-doped base parts 4a, 4b and the highly concentrated implantation region 13 to form the corresponding first p + -doped region 11 in the n-doped current spreading region 3. An oxide layer is used as a mask during trench formation. Furthermore, after the trench etching, an isotropic etching may be performed to remove damage to the trenches 7, a hydrogen annealing may be performed to round the corners of an open part of the trenches 7 and the bottom of the trenches, etc. Only one of the isotropic etching and the hydrogen annealing may be performed. Alternatively, after the isotropic etching is performed, the hydrogen annealing may be performed. Next, as shown in Fig. As shown in Figure 13, the gate insulating layer 8 is formed along the front surface (the surface of the p-type silicon carbide layer 22) of the silicon carbide base 10 and an inner wall of each of the trenches 7. Next, for example, polysilicon (polySi) may be deposited and etched to be embedded in the trenches 7, leaving the polysilicon in the trenches 7 to form the gate electrode 9. In this case, etching and etching may be performed to leave the polysilicon on an inner surface of a base surface portion; patterning and etching may be performed so that the polysilicon protrudes from the base surface portion.
[0059] Next, as in Fig. 14, the interlayer insulating layer 14 is formed on the entire front surface of the silicon carbide base 10 to cover the gate electrode 9. The interlayer insulating layer 14 is formed, for example, by an undoped silicate glass (NSG), a phosphosilicate glass (PSG), a borophosphosilicate glass (BPSG), a high-temperature oxide (HTO), or a combination thereof. Next, the interlayer insulating layer 14 and the gate insulating layer 8 are patterned, and contact holes are formed, which form the n + -doped source region 5 and the p ++ -doped contact region 6. Next, the barrier metal 15 is formed and patterned to cover the interlayer insulating layer 14, and the n + -doped source region 5 and the p ++ -doped contact region 6 are exposed again. Next, the source electrode 16 is formed to form the n + -doped source region 5 and the p ++-doped contact region 6. The source electrode 16 may be formed to cover the barrier metal 15; the source electrode 16 may be formed to remain only in the contact hole.
[0060] Next, the source contact pad 17 is formed so that it is embedded in the contact hole. A portion of a metal layer deposited to form the source contact pad 17 can be used as a gate contact pad. In the back of the n +On the doped silicon carbide substrate 1, a metal layer made of a nickel (Ni) layer, a titanium (Ti) layer, etc., is formed in a contact portion of the drain electrode 18 using sputtering. The metal layer may be a combination of stacked Ni layers and Ti layers. Annealing, such as rapid thermal annealing (RTA), is then performed to convert the metal layer into a silicide and form a current junction. Then, for example, a thick layer such as a stacked layer is formed by sequentially stacking a Ti layer, a Ni layer, and a gold (Au) layer by electron beam (EB) deposition, etc., to form the drain electrode 18.
[0061] In the epitaxy and ion implantation described above, nitrogen (N) and / or phosphorus (P), for example, can be used as n-doped impurities (n-type dopants), which are n-doped relative to silicon carbide, arsenic (As), antimony (Sb), etc. As p-doped impurities (p-dopants), boron (B) and / or aluminum (Al), for example, can be used, which are p-doped relative to silicon carbide, gallium (Ga), indium (In), thallium (Ti), etc. Thus, the Fig. 1 MOSFET shown completed.
[0062] As described above, according to the first embodiment, the formation of the highly concentrated implantation region by ion implantation in the p-type base region formed by epitaxy generates the bell-shaped impurity concentration profile in which the impurity concentration in the p-type base region is different in the depth direction. In addition, the formation of the highly concentrated implantation region by ion implantation in the p-type base region generates an incomplete crystal structure disorder in the p-type base region. This can be achieved compared to the impurity concentration profile in the depth direction in the case of a structure formed by only one semiconductor layer, such as a conventional structure (see Fig. 25A, Fig. 25B and Fig. 25C), the leakage current between the drain and source can be reduced more than in the case of the uniform p-type base region. Therefore, for a product unit that includes all products (semiconductor chips) to be manufactured within a predetermined period of time as a single unit, defective chips having leakage current defects between the drain and source can be reduced, and the yield can be increased. All products to be manufactured within a predetermined period of time are all products to be manufactured within a period for completing all manufacturing processes in the semiconductor wafer surface in each batch process of the manufacturing process and the inter-batch processes.In a batch process of the manufacturing process and the inter-batch processes, the negative effects that occur according to the product unit include, for example, the condition of the equipment, as well as the negative effects resulting from property fluctuations caused by the batch of semiconductor wafers. Furthermore, if the product unit includes all products to be manufactured that are present only in the surface of the semiconductor wafer, the yield can be further increased.
[0063] Furthermore, although the smaller the variations in the channel carrier density are, the smaller the variations in the gate threshold voltage can be made, in the epitaxial growth of silicon carbide, the control of the impurity concentration becomes difficult, and the variations in the channel carrier density increase. Therefore, in a conventional structure (see Fig. 27) configured by a p-type base region composed of only one semiconductor layer, the variations in the channel carrier density and the gate threshold voltage are large. In contrast, according to the first embodiment, by forming the highly concentrated implantation region in the p-type base region, the variation in the gate threshold voltage is rate-limited by the variation in the impurity concentration of the highly concentrated implantation region, which has a higher impurity concentration than the p-type base region. A variation in the impurity concentration of the highly concentrated implantation region formed by ion implantation is much smaller than the variation in the impurity concentration of a region formed only by epitaxy.Therefore, by forming the highly concentrated implantation region in the p-type base region, the gate threshold voltage variation can be made smaller than that of the conventional structure configured by a p-type base region formed only by epitaxy. Furthermore, according to the first embodiment, the p-type silicon carbide layer formed by epitaxy serves as the p-type base region, thereby achieving a channel with favorable crystallinity from the features of the semiconductor layer and enabling a lower on-resistance due to high carrier mobility.
[0064] Furthermore, according to the first embodiment, even when a commercially available silicon carbide base is used on which a p-type silicon carbide layer is formed by epitaxy on an n-type silicon carbide substrate to become the p-type base region, by forming the high-concentration implantation region by ion implantation in the p-type base region, the same effects as described above are achieved.
[0065] A method for manufacturing a silicon carbide semiconductor device according to a second embodiment will be described. Fig. 15, Fig. 16 and Fig. 17 are cross-sectional views of the semiconductor device according to the second embodiment during manufacturing. The structure of the semiconductor device according to the second embodiment is the same as that of the first embodiment (see Fig. 1 and Fig. 2).
[0066] The method for manufacturing a silicon carbide semiconductor device according to the second embodiment differs from the method for manufacturing a silicon carbide semiconductor device according to the first embodiment in the process for forming the p-doped base region 4. Specifically, the epitaxial growth of the p-doped silicon carbide layer 22 (22a, 22b) forming the p-doped base region 4 is separated into two treatments spanning the ion implantation process for forming the high-concentration implantation region 13.
[0067] In particular, first, similar to the first embodiment, the n + doped silicon carbide substrate 1 is prepared and the processes up to the formation process of the n-doped current spreading region 3 are carried out sequentially (see Fig. 3 to 7). Next, as in Fig. 15, a p-doped silicon carbide layer (second semiconductor layer) 22a, which becomes the previously described p-doped silicon carbide layer 22, on which n - -doped silicon carbide layer (the first semiconductor layer) 21 is formed by epitaxy. The thickness of the p-doped silicon carbide layer 22a is the same thickness as the total thickness of the first p-doped base part 4a and the high-concentration implantation region 13. Next, as shown in Fig. 16, a p-type impurity is ion-implanted into the entire p-type silicon carbide layer 22a, and the high-concentration implantation region 13 having the predetermined thickness t1 is formed in the entire surface layer of the p-type silicon carbide layer 22a. A portion of the p-type silicon carbide layer 22a that is farther on the drain side than the high-concentration implantation region 13 becomes the first p-type base portion 4a. Now, a portion of the p-type silicon carbide layer 22a that is farther on the source side than the high-concentration implantation region 13 and that becomes the second p-type base portion 4b can also be formed.
[0068] Next, as in Fig. 17, on the p-type silicon carbide layer 22a (i.e., on the high-concentration implantation region 13), a p-type silicon carbide layer (third semiconductor layer) 22b, which becomes the previously described p-type silicon carbide layer 22, is formed by epitaxy. The p-type silicon carbide layer 22b becomes the second p-type base part 4b. Although the p-type silicon carbide layer 22 is formed only by epitaxy and has a uniform impurity concentration profile in the depth direction similar to the first embodiment, this is now sufficient provided the high-concentration implantation region 13 has the impurity concentration peak 13a.When the p-doped silicon carbide layer 22b is formed by epitaxy, the impurity concentration can be controlled, and an impurity concentration profile for which the impurity concentration increases over a predetermined gradient in the depth direction can be formed. Thus, the p-doped base region 4, which consists of the first and second p-doped base portions 4a, 4b and the high-concentration implantation region 13, is formed.
[0069] Furthermore, the silicon carbide base (semiconductor wafer) 10 is formed by the previous processes, in which the n - -doped silicon carbide layer 21 and the p-doped silicon carbide layer 22 successively on the n + -doped silicon carbide substrate 1. Subsequently, similar to the first embodiment, the processes that determine the formation process of the n +-doped source region 5, and the subsequent processes are carried out in sequence (see Fig. 10 to 14), whereby the Fig. 1 MOSFET shown is completed.
[0070] As described above, according to the second embodiment, the same effects as those of the first embodiment can be achieved. Furthermore, conventionally, when performing ion implantation so that the impurity reaches a deep position relative to the ion implantation surface, problems arise, for example, that special equipment capable of ion implantation (mega-implantation) with high acceleration energy is required, that the ion implantation takes a long time, and so on. According to the second embodiment, on the other hand, epitaxy is divided and performed into multiple treatments, and based on the thickness of each p-type silicon carbide layer, the depth of the position of the high-concentration implantation region can be freely determined.As a result, without the use of special equipment capable of mega-implantation, a highly concentrated implantation region can be formed in the base region at a deep position opposite to the side of the base front.
[0071] The structure of the semiconductor device according to a third embodiment will be described. Fig. Fig. 18 is a cross-sectional view of a structure of the semiconductor device according to the third embodiment. The semiconductor device according to the third embodiment differs from the semiconductor device according to the first embodiment in that the first and second p + -doped regions 11, 12 are provided at a depth that is further on the drain side than the interface of the n-doped current spreading region 3 and the n - -doped drift region 2.
[0072] In particular, the first p +-doped region 11 into the n-doped current spreading region 3 from the bottom of the trench 7 in the depth direction and is in the n - -doped drift region 2. The second p + -doped region 12 penetrates into the n-doped current spreading region 3 from the interface of the p-doped base region 4 and the n-doped current spreading region 3 in the depth direction and projects into the n-doped drift region 2. The depth of the position of the drain side ends of the first and second p + -doped regions 11, 12 may be the same as that of the interface of the n-doped current spreading region 3 and the n - -doped drift region 2.
[0073] The method for manufacturing a silicon carbide semiconductor device according to the third embodiment is sufficient to achieve the depth of the first p in the method for manufacturing a silicon carbide semiconductor device according to the first embodiment. +-doped region 11 and the depth of the p + -doped subregion 12a, which is part of the second p + -doped region 12 becomes deeper than the n-doped sub-region 3a, which becomes part of the n-doped current spreading region 3.
[0074] As described above, according to the third embodiment, regardless of the depths of the first and second p + -doped regions, the same effects as those of the first and second embodiments are achieved.
[0075] A semiconductor device according to a fourth embodiment will be described. The structure of the semiconductor device according to the fourth embodiment is the same as that of the first embodiment (see Fig. 1). In the semiconductor device according to the fourth embodiment, a p-doped impurity concentration profile 41 of the high-concentration implantation region 13 differs from the impurity concentration in the semiconductor device according to the first embodiment. In particular, the p-doped impurity concentration profile 41 has two Gaussian distribution shapes formed by two ion implantation treatments of a p-doped impurity (see Fig. 19).
[0076] Specifically, the highly concentrated implantation region 13 has the p-type impurity concentration profile 41, in which the concentration differences in the depth direction form two bell-shaped curves at the peaks 13b, 13c where the impurity concentration is higher than that of the p-type silicon carbide layer 22 forming the p-type base region 4. In other words, the p-type impurity concentration profile 41 has the peaks 13b, 13c in the p-type base region 4, and from the respective positions of the peaks 13b, 13c, the impurity concentration decreases via respective predetermined slopes on both sides (the source side and the drain side) of the base. The depths of the positions of the deep peaks 13b, 13c of the highly concentrated implantation region 13 are preferably the same depth as that of the peak 13a in the first embodiment.
[0077] Next, the p-doped impurity concentration profile 41 resulting from the ion implantation of a p-doped impurity to form the high-concentration implantation region 13 will be described in detail. Fig. 19 is a characteristic field showing the impurity concentration profile at the section line AA' in Fig. 1 for the case of the semiconductor device according to the fourth embodiment. Fig. 19 depicts the p-type impurity concentration profile 41 for the case where the depth of the position of a peak 41b of the highly concentrated implantation region 13 is the depth of the position of the interface between the n+-type source region 5 and the p+-type base region 4, the highly concentrated implantation region 13 contacts the n+-type source region 5 and the p++-type contact region 6, and the second p-type base part 4b is not provided. Among the peaks 41b, 41c of the highly concentrated implantation region 13, the peak 41b is the one for which the depth of the position thereof is close to the n+-type source region 5.
[0078] Below, the description of Fig. 19 parts dealing with description of Fig. 2 covers, omitted. In Fig. 19, the horizontal axis is the depth from the base front, and the vertical axis is the impurity concentration. In addition to the p-doped impurity concentration profile 41 resulting from the ion implantation of a p-doped impurity to form the high-concentration implantation region 13, Fig. 19 depicts an n-doped impurity concentration profile 42 resulting from the ion implantation of an n-doped impurity to form the n+-doped source region 5. By ion implanting an n-doped impurity to form the n+-doped source region 5, the n-doped impurity concentration profile 42 is formed in the p-doped silicon carbide layer 22. A portion from the base front side to an intersection point 40a of the n-doped impurity concentration profile 42 and the p-doped impurity concentration profile 41 is the n+-doped source region 5.
[0079] Furthermore, by ion implanting a p-type impurity to form the high-concentration implantation region 13, the p-type impurity concentration profile 41, which has the impurity concentration peaks 41b, 41c at positions deeper from the base front than a peak 42a of the n-type impurity concentration profile 42, is formed in the p-type silicon carbide layer 22. The peaks 41b, 41c of the p-type impurity concentration profile 41 are, respectively, the peaks 13b, 13c of the impurity concentration profile of the high-concentration implantation region 13. Furthermore, in the p-type impurity concentration profile 41, the impurity concentration decreases in a bell-shaped curve from the positions of the peaks 41b, 41c by respective predetermined slopes on the source side and the drain side.In addition, in the p-doped impurity concentration profile 41, the impurity concentration at an interface 40b of the p-doped silicon carbide layer 22 and the n-doped silicon carbide layer 21 decreases sharply, and the impurity concentration decreases from the interface 40b toward the drain side by a predetermined slope.
[0080] Such a p-type impurity concentration profile 41 is obtained by performing ion implantation of a p-type impurity similar to the p-type impurity concentration profile 31, and is not obtained only by epitaxy. Furthermore, the impurity concentration of the p-type silicon carbide layer 22 and the impurity concentration of the peaks 41b, 41c of the p-type impurity concentration profile 41 preferably have the same values as those of the impurity concentration of the p-type silicon carbide layer 22 of the first embodiment and the peak 31a of the p-type impurity concentration profile 31, respectively. Furthermore, in the fourth embodiment, although there is a case where the p-type impurity concentration profile 41 includes the peaks 41b, 41c, the p-type impurity concentration profile 41 may have more than two peaks.
[0081] The method for manufacturing a silicon carbide semiconductor device according to the fourth embodiment will be described. The method for manufacturing a silicon carbide semiconductor device according to the fourth embodiment differs from the method for manufacturing a silicon carbide semiconductor device according to the first embodiment in the process for forming the high-concentration implantation region 13. Specifically, in the ion implantation process for forming the high-concentration implantation region 13, the ion implantation is divided and performed into two treatments.
[0082] Specifically, first, similarly to the first embodiment, the n+-doped silicon carbide substrate 1 is prepared, and the processes up to the formation process of the p-doped silicon carbide layer 22 are carried out sequentially (see Fig. 3 to 8). Next, a p-doped impurity is implanted into the entire p-doped silicon carbide layer 22 by two ion implantation treatments to form the high-concentration implantation region 13 to the predetermined thickness t1 at a predetermined depth in the p-doped silicon carbide layer 22 (see Fig. 9). This ion implantation performs ion implantation using different accelerating voltages and is carried out in such a way that one type of ion is implanted at different depths in the p-doped silicon carbide layer 22.
[0083] For example, in the first ion implantation, the acceleration voltage is adjusted to implant the ion species at a depth corresponding to the peak 41b of the p-type impurity concentration profile 41. Further, in the second ion implantation, the acceleration voltage is adjusted to implant the ion species at a depth corresponding to the peak 41c of the p-type impurity concentration profile 41. The order of the acceleration voltages can be reversed. In other words, in the first ion implantation, the acceleration voltage can be adjusted to implant the ion species at a depth corresponding to the peak 41c, and in the second ion implantation, the acceleration voltage can be adjusted to implant the ion species at a depth corresponding to the peak 41b.As a result, for example, in the p-type silicon carbide layer 22, a portion located further on the drain side than the high-concentration implantation region 13 becomes the previously described first p-type base portion 4a, and a portion located further on the source side (the opposite side relative to the side of the n+-type silicon carbide substrate 1) than the high-concentration implantation region 13 becomes the previously described second p-type base portion 4b. The p-type base region 4 is formed by the first and second p-type base portions 4a, 4b and the high-concentration implantation region 13. Furthermore, although the high-concentration implantation region 13 is formed by two ion implantation treatments here, the high-concentration implantation region 13 may be formed by more than two ion implantation treatments.Furthermore, the highly concentrated implantation region 13 having the p-doped impurity concentration profile 41 can be formed by ion implanting several kinds of different p-doped ions.
[0084] Subsequently, similar to the first embodiment, the formation process of the n+-doped source region 5 and the processes thereafter are carried out sequentially (see Fig. 10 to 14), thereby completing the MOSFET according to the fourth embodiment.
[0085] As described above, according to the fourth embodiment, the same effects as those of the first embodiment can be achieved. In the fourth embodiment, although the high-concentration implantation region 13 of the first embodiment is formed by two ion implantation treatments, the high-concentration implantation region 13 of the second embodiment and the third embodiment can be formed by two ion implantation treatments. Even in these cases, the same effects as those of the second embodiment and the third embodiment can be achieved.
[0086] A semiconductor device according to a fifth embodiment will be described. The structure of the semiconductor device according to the fifth embodiment is the same as that of the first embodiment (see Fig. 1). In the semiconductor device according to the fifth embodiment, a p-type impurity concentration profile 51 of the high-concentration implantation region 13 differs from the impurity concentration in the semiconductor device according to the first embodiment. Specifically, the p-type impurity concentration profile 51 has two Gaussian distribution shapes formed by two p-type impurity ion implantation treatments similar to the fourth embodiment (see Fig. 20).
[0087] Fig. 20 is a characteristic field showing the impurity concentration profile at the section line AA' in Fig. 1 for the case of the semiconductor device according to the fifth embodiment. In Fig. 20, the p-doped impurity concentration profile 51, an n-doped impurity concentration profile 52, the peaks 51b, 51c, an intersection 50a, and an interface 50b are respectively the same as the p-doped impurity concentration profile 41, the n-doped impurity concentration profile 42, the peaks 41b, 41c, the intersection 40a, and the interface 40b in Fig. 19, and therefore their description is omitted.
[0088] Although in the p-type impurity concentration profile 41, the impurity concentration decreases sharply at the interface 40b, in the p-type impurity concentration profile 51, the impurity concentration decreases at a predetermined slope from the position of the drain-side peak 51c. Furthermore, the source-side peak 51b is a factor that determines the gate threshold voltage Vth, and the higher the impurity concentration of the peak 51b, the more the gate threshold voltage Vth can be raised. The drain-side peak 51c is a factor that determines the short-channel effects, and the closer the position of the peak 51c is to the n-type current spreading region 3, the more the short-channel effects can be suppressed.
[0089] Next, the method for manufacturing a silicon carbide semiconductor device according to the fifth embodiment will be described. In the method for manufacturing a silicon carbide semiconductor device according to the fifth embodiment, the processes for forming the first p-type base portion 4a, the second p-type base portion 4b, and the highly concentrated implantation region 13 are different from those of the method for manufacturing a silicon carbide semiconductor device according to the fourth embodiment. Specifically, instead of forming the p-type silicon carbide layer 22 by epitaxy, an n-type silicon carbide layer 22' is formed by epitaxy. By ion implanting a p-type impurity into the n-type silicon carbide layer 22', the first p-type base portion 4a, the second p-type base portion 4b, and the highly concentrated implantation region 13 are formed by returning to the p-type conductivity type.
[0090] Specifically, first, similarly to the first embodiment, the n+ doped silicon carbide substrate 1 is prepared, and the processes up to the formation process of the n-doped current spreading region 3 are carried out sequentially (see Fig. 3 to 7). Next, the n-doped silicon carbide layer 22' is formed by epitaxy on the n-doped silicon carbide layer 21. The n-doped silicon carbide layer 22' is formed in the same position as the p-doped silicon carbide layer 22 and is therefore not shown. Through the previous processes, the silicon carbide base (semiconductor wafer) 10 is formed, in which the n-doped silicon carbide layer 21 and the n-doped silicon carbide layer 22' are deposited sequentially on the n+-doped silicon carbide substrate 1 (see Fig. 8).
[0091] Next, a p-doped impurity is implanted into the entire n-doped silicon carbide layer 22' by two ion implantation treatments to form the highly concentrated implantation region 13 having the predetermined thickness t1 at a predetermined depth in the n-doped silicon carbide layer 22' (see Fig. 9). This ion implantation is performed by the same method as in the fourth embodiment. However, in the fifth embodiment, the impurity dose used in the ion implantation to return the n-type silicon carbide layer 22' to the p-type conductivity type is larger than that in the fourth embodiment. The thickness of the n-type silicon carbide layer 22' is the sum of the channel length L and the thickness of the n+ type source region 5 (approximately 0.3 μm or more and 0.5 μm or less). Therefore, the n-type silicon carbide layer 22' is returned to the p-type conductivity type and becomes the p-type silicon carbide layer 22 by the overlap of the two p-type regions formed by the two ion implantation treatments at different implantation depths.In the p-type silicon carbide layer 22, a portion located further on the drain side than the high-concentration implantation region 13 becomes the previously described first p-type base portion 4a, and a portion located further on the source side than the high-concentration implantation region 13 (the opposite side relative to the n+-type silicon carbide substrate 1 side) becomes the previously described second p-type base portion 4b. The p-type base region 4 is formed by the first and second p-type base portions 4a, 4b and the high-concentration implantation region 13. Furthermore, similar to the fourth embodiment, the formation may be performed by more than two ion implantation treatments.The p-type impurity concentration profile 51 may be a profile approximately close to a box profile (a uniform impurity concentration profile in the depth direction), and the number of ion implantation treatments may preferably be in a range of 2 to 5, for example. In this case, one or more peaks are formed in the p-type impurity concentration profile 51 between the peak 51b on the source side and the peak 51c on the drain side. Furthermore, similar to the fourth embodiment, the high-concentration implantation region 13 having the p-type impurity concentration profile 51 may be formed by ion implanting a plurality of different p-type ion species.
[0092] Subsequently, similar to the first embodiment, the formation process of the n+-doped source region 5 and the processes thereafter are carried out sequentially (see Fig. 10 to 14), whereby the MOSFET according to the fifth embodiment is completed.
[0093] As described above, according to the fifth embodiment, the same effects as those of the first embodiment can be achieved. Furthermore, similar to the second embodiment, the n-doped silicon carbide layer 22' can be formed by epitaxy separated into two treatments. In this case, the same effects as those of the second embodiment can be achieved.
[0094] Next, the semiconductor device according to a sixth embodiment will be described. The structure of the semiconductor device according to the sixth embodiment is the same as that of the first embodiment (see Fig. 1). In the semiconductor device according to the sixth embodiment, a p-doped impurity concentration profile 61 of the high-concentration implantation region 13 differs from the profile of the semiconductor device according to the fifth embodiment. In particular, the p-doped impurity concentration profile 61 has two Gaussian distribution shapes formed by two ion implantation treatments of a p-doped impurity (see Fig. 21).
[0095] Specifically, the high-concentration implantation region 13 has the p-type impurity concentration profile 61, in which the concentration differences in the depth direction form two bell-shaped curves at the peaks 13b, 13c where the impurity concentration is higher than that of the p-type silicon carbide layer 22 forming the p-type base region 4. In other words, the p-type impurity concentration profile 61 has the peaks 13b, 13c in the p-type base region 4, and the depths of the positions of the peaks 13b, 13c are different. Furthermore, in the p-type impurity concentration profile 61, from the respective positions of the peaks 13b, 13c, the impurity concentration on both sides (source side and drain side) of the base decreases by respective predetermined slopes.The depth of the position of one of the peaks 13b, 13c of the high concentration implantation region 13 may preferably be the depth of the position of the peak 13a in the first embodiment.
[0096] The p-doped impurity concentration profile 61 resulting from the ion implantation of a p-doped impurity to form the high-concentration implantation region 13 is described in detail. Fig. 21 is a characteristic field showing an impurity concentration profile at the section line AA' in Fig. 1 for the case of the semiconductor device according to the sixth embodiment. In Fig. 21, the p-doped impurity concentration profile 61, an n-doped impurity concentration profile 62, the peaks 61b, 61c, an intersection 60a, and an interface 60b are the same as the p-doped impurity concentration profile 41, the n-doped impurity concentration profile 42, the peaks 41b, 41c, the intersection 40a, and the interface 40b in Fig. 19, and therefore their description is omitted.
[0097] In the p-type impurity concentration profile 61, similar to the p-type impurity concentration profile 51, the impurity concentration decreases by a predetermined slope from the position of the peak 61c on the drain side. Furthermore, the depths of the positions of the peaks 61b, 61c in the p-type impurity concentration profile 61 are the same as the depths of the peaks 51b, 51c in the p-type impurity concentration profile 51. The impurity concentration of the peak 61b on the source side is higher than the impurity concentration of the peak 61c on the drain side. In particular, the impurity concentration of the peak 61c on the drain side may preferably be 10% to 70% of the impurity concentration of the peak 61b on the source side.
[0098] Furthermore, in the sixth embodiment, although a case is depicted where the p-type impurity concentration profile 61 has two peaks (the peaks 61b, 61c), the p-type impurity concentration profile 61 may have more than two peaks. In this case, the impurity concentration of the peak closest to the source side is higher than the impurity concentration of the peak closest to the drain side. Specifically, the impurity concentration of the peak closest to the drain side may preferably be 10% to 70% of the impurity concentration of the peak closest to the source side. Furthermore, the impurity concentrations of peaks other than the peak closest to the source side and the peak closest to the drain side may be the same, or the impurity concentrations may gradually decrease toward the drain side.
[0099] The method for manufacturing a silicon carbide semiconductor device according to the sixth embodiment will be described. In the method for manufacturing a silicon carbide semiconductor device according to the sixth embodiment, the ion implantation process differs from that in the method for manufacturing a silicon carbide semiconductor device according to the fifth embodiment. Specifically, the high-concentration implantation region 13, which has the p-type impurity concentration profile 61 in which the impurity concentration of the peak 61b is higher than the impurity concentration of the peak 61c, is formed by ion implantation.
[0100] Specifically, first, similarly to the fifth embodiment, the n+ doped silicon carbide substrate 1 is prepared, and the processes up to the formation process of the n-doped silicon carbide layer 22' are carried out sequentially (see Fig. 3 to 8). Next, two ion implantation treatments of a p-doped impurity are carried out into the entire n-doped silicon carbide layer 22' to form the high-concentration implantation region 13 to the predetermined thickness t1 at a predetermined depth in the n-doped silicon carbide layer 22' (see Fig. 9). This ion implantation performs ion implantation at different accelerating voltages and is performed to implant one type of ion at different depths in the n-doped silicon carbide layer 22'. In this case, the ion implantation is performed such that the impurity concentration at a shallower position (near the source side) in the n-doped silicon carbide layer 22' is higher than the impurity concentration at a deeper position (near the drain side).
[0101] Thereby, similarly to the fifth embodiment, the n-type silicon carbide layer 22' is returned to the p-type conductivity type to become the p-type silicon carbide layer 22; and in the p-type silicon carbide layer 22, a part located further on the drain side than the high-concentration implantation region 13 becomes the previously described first p-type base part 4a, and a part located further on the source side (the opposite side relative to the n+-type silicon carbide substrate 1) than the high-concentration implantation region 13 becomes the previously described second p-type base part 4b. The p-type base region 4 is formed by the first and second p-type base parts 4a, 4b and the high-concentration implantation region 13. Furthermore, similar to the fourth embodiment, the formation may be carried out by more than two ion implantation treatments.The number of ion implantation treatments may, for example, preferably be in a range of 2 to 5, similar to the fifth embodiment. Further, similar to the fourth embodiment, the high-concentration implantation region 13 having the p-type impurity concentration profile 61 may be formed by ion implanting a plurality of different p-type ion species.
[0102] Subsequently, similar to the first embodiment, the formation process of the n+-doped source region 5 and the processes thereafter are carried out sequentially (see Fig. 10 to 14), whereby the MOSFET according to the sixth embodiment is completed.
[0103] As described above, according to the sixth embodiment, the same effects as those of the first embodiment can be achieved. Further, according to the sixth embodiment, in the p-type impurity concentration profile, the impurity concentration of the peak on the source side is higher than the impurity concentration of the peak on the drain side. Thereby, the on-resistance can be reduced without changing the gate threshold voltage and without varying the gate threshold voltage. That is, because the gate threshold voltage is determined by the impurity concentration of the peak on the source side and by causing the impurity concentration of the peak on the drain side to be a small impurity concentration of a magnitude that makes it possible to suppress the short-channel effect, the increase in the channel resistance can be suppressed.The short-channel effect is a sharp decrease in the gate threshold voltage due to a shortening of the channel length. Furthermore, similar to the second embodiment, the n-doped silicon carbide layer 22' can be formed by epitaxy, separated into two treatments. In this case, the same effects as those of the second embodiment can be achieved.
[0104] The frequency of leakage current between the drain and the source was checked. Fig. 22 is a characteristic diagram illustrating the frequency of occurrence of leakage current between the drain and the source of the silicon carbide semiconductor device according to a first example. Fig. Figure 23 is a characteristic diagram showing the frequency of leakage current occurrence between the drain and the source in a conventional example of a silicon carbide semiconductor device. Fig. 22 and Fig. 23, the vertical axis represents the frequency of leakage current occurrence for a semiconductor wafer area, and the horizontal axis represents the magnitude (current value) of the leakage current Idds between the drain and source of each product (semiconductor chip) formed from a semiconductor wafer area. On the horizontal axes in Fig. 22 and Fig. 23, if the leakage current Idds between the drain and the source is 1×10 -8 A or less, the leakage current Idds is “1×10 -8 A". If the leakage current Idds between the drain and source is greater than 1×10 x A and 1×10 x+1 A or less, the leakage current Idds is defined as “~1×10 x+1 A" (x = -8 to -4). If the leakage current Idds between the drain and source is greater than 1×10 3 A, the leakage current Idds is expressed as “1×10 -3 A~“ is indicated.
[0105] Several MOSFET chips (see Fig. 1) having the highly concentrated implantation region 13 in the p-doped base region 4 were formed from a semiconductor wafer according to the method for manufacturing a silicon carbide semiconductor device according to the first embodiment described above (hereinafter the EXAMPLE). Several MOSFET chips (see Fig. 27) with a conventional structure configured by the p-doped base region 104 formed only by epitaxy were fabricated from a semiconductor wafer for comparison (hereinafter, the first conventional example). The leakage current Idds between the drain and the source in several MOSFET chips as well as in the first conventional example and the EXAMPLE were measured. The results are shown in Fig. 22 and Fig. 23. From the Fig. 22 and Fig. 23 results shown, it was confirmed that in the EXAMPLE the impurity concentration profile (see Fig. 2) resulting from the highly concentrated implantation region 13 in the p-doped base region 4, whereby the frequency of occurrence of the leakage current Idds between the drain and the source and the magnitude of the leakage current Idds can be significantly reduced to a greater extent than in the first conventional example.
[0106] The variation of the gate threshold voltage Vth was checked. Fig. 24 is a characteristic diagram illustrating a variation of the gate threshold voltage Vth of the silicon carbide semiconductor device according to a second example. Fig. 24, the horizontal axis represents a standard deviation σ of the variation in the channel carrier density, and the vertical axis represents a variation in the gate threshold voltage Vth for a case where the gate threshold voltage Vth = 5 V. In the second example, in addition to the first example and the first conventional example, a plurality of MOSFET chips having the high-concentration implantation region 13 in the p-type base region 4 were manufactured from a semiconductor wafer according to the method for manufacturing a silicon carbide semiconductor device according to the fourth embodiment and the sixth embodiment described above (hereinafter, the second example). The measurement results of the variation in the gate threshold voltage Vth in the first example, the second example, and the first conventional example described above are shown in Fig. 24 shown.
[0107] From the Fig. From the results shown in Figure 24, it was confirmed that, in the first conventional example of a semiconductor wafer surface, the variation in the impurity concentration of the p-type base region 104 was ±30% within a standard deviation of ±3σ of the mean value. Furthermore, it was confirmed that the gate threshold voltage Vth varied within a standard deviation of ±3σ of the mean value in a range of 3.5 V to 6.5 V.
[0108] In contrast, in the first semiconductor wafer area example, although the variation in the impurity concentration of the p-type base region 4 was ±30% within a standard deviation of ±3σ of the mean value as in the first conventional example, the variation in the impurity concentration of the high-concentration implantation region 13 was confirmed to be ±10%. Furthermore, it was confirmed that the gate threshold voltage Vth could be controlled within a standard deviation of ±3σ of the mean value to be within a range of 4.4 V to 5.6 V.
[0109] Similarly, in the second example of a semiconductor wafer surface, although the variation in the impurity concentration of the p-type base region 4 was ±30% within a standard deviation of ±3σ of the mean value, as in the first conventional example, the variation in the impurity concentration of the high-concentration implantation region 13 was confirmed to be ±10% for both the fourth embodiment and the sixth embodiment. Furthermore, it was confirmed that the gate threshold voltage Vth could be controlled within a standard deviation of ±3σ of the mean value to be in a range of 4.35 V to 5.6 V. These results explain that by forming the high-concentration implantation region 13 in the p-type base region 4, the variation in the gate threshold voltage Vth is rate-limited by the variation in the impurity concentration of the high-concentration implantation region 13.
[0110] Although not shown, for MOSFET chips manufactured according to the method for manufacturing a silicon carbide semiconductor device according to the fifth embodiment described above, it was confirmed by the inventor that the same effects as those of the second example could be obtained.
[0111] The optimal depth of the position of the tip 13a of the high concentration implantation region 13 was verified. Fig. 25A, Fig. 25B and Fig. 25C are diagrams illustrating the conditions of the p-doped base region of the silicon carbide semiconductor devices of the first and second comparative examples. In Fig. 25A, Fig. 25B and Fig. 25C, the horizontal axis is the depth of the base front, and the vertical axis is the impurity concentration. In Fig. 25A, Fig. 25B and Fig. 25C, depth = 0 µm is an interface of a source electrode (not shown) and an n+ -doped source region 35. Fig. 25A, Fig. 25B and Fig. 25C are characteristic diagrams illustrating the relationships between the gate threshold voltage Vth and the on-resistance of the silicon carbide semiconductor devices of the first and second comparative examples. The simulation results of the relationships between the gate threshold voltage Vth and the on-resistance (RonA) in the second conventional example and the first and second comparative examples are shown in Fig. 26 shown.
[0112] In the second conventional example and the first and second comparative examples, the channel carrier mobility and the channel dependence of the gate threshold voltage Vth are different and were therefore qualitatively evaluated. For the second conventional example and the first and second comparative examples, the channel carrier mobility was assumed for a case where the channel carrier mobility was set to 2.0×10 17 / cm 3 Since the respective subthreshold current values for the second conventional example and the first and second comparative examples were also different, the gate threshold voltage Vth was also qualitatively evaluated. The cell pitch (arrangement interval of the unit cells) was set to 6.0 µm, and the drain voltage Vd was set to 20 V.
[0113] The conditions of the second conventional example and the first and second comparative examples were as follows. As in Fig. As shown in Figure 25A, the second conventional example includes a p-type base region 34 having an impurity concentration profile uniform in the depth direction. A thickness t0 of the p-type base region 34 was set to 0.55 μm, and a depth D of an interface between the p-type base region 34 and an n-type current spreading region (not shown) from the base front side was set to 1.1 μm. Fig. Figure 26 shows the calculation results of on-resistance values when the gate threshold voltage Vth is changed differently by respective conditions, where the impurity concentration of the p-doped base region 34 is set to 1.5×10 17 / cm 3 , 2.0×10 17 / cm 3 , 2.5×10 17 / cm 3 and 3.0×10 17 / cm 3 is assumed.
[0114] As in Fig. 25B, the first comparative example differs from the second conventional example in that, in the p-type base region 34, the impurity concentration of a part (hereinafter, the second part) 34b on the source side is made higher than that of a part on the drain side (hereinafter, the first part) 34a. Fig. 26 shows the calculation results of on-resistance values when the gate threshold voltage Vth is changed differently by respective conditions, wherein the impurity concentration of the second part 34b of the p-doped base region 34 is set to 2.0×10 17 / cm 3 , 2.5×10 17 / cm 3 and 3.0×10 17 / cm 3 is assumed. Furthermore, Fig. 26 cases where the impurity concentration of the first part 34a of the p-doped base region 34 is 1.0×10 17 / cm 3 and 1.5×10 17 / cm 3amounts.
[0115] As in Fig. 25C, the second comparative example differs from the second conventional example in that, in the p-type base region 34, the impurity concentration of a part on the source side (hereinafter, the second part) 34d is made lower than that of a part on the drain side (hereinafter, the first part) 34c. Fig. 26 depicts the calculation results of on-resistance values when the gate threshold voltage Vth is changed differently by respective conditions, wherein the impurity concentration of the first part 34c of the p-doped base region 34 is set to 2.0×10 17 / cm 3 , 2.5×10 17 / cm 3 and 3.0×10 17 / cm 3 is assumed. Furthermore, Fig. 26 cases where the impurity concentration of the second part 34d of the p-doped base region 34 is 1.0×10 17 / cm 3 and 1.5×10 17 / cm3 amounts.
[0116] In the first and second comparative examples, the thicknesses t11, t12 of the first and second parts of the p-type base region 34 were the same, namely 0.275 μm. Furthermore, in the first and second comparative examples, although the impurity concentration profile of the p-type base region 34 is changed to be stepped in the depth direction, the second and first high-impurity concentration parts 34b, 34c are assumed to have impurity concentration profiles having a Gaussian distribution formed as a result of ion implantation. In other words, the second and first parts 34b, 34c of the p-type base region 34 in the first and second comparative examples assume the high-concentration implantation region 13 of the present invention.
[0117] From the Fig. From the results shown in Figure 26, it was confirmed that in the first comparative example (segment indicated by the dashed lines 41), on-resistance characteristics comparable to the second conventional example could be maintained. In other words, the results illustrate that in the present invention, the highly concentrated implantation region 13 can preferably be arranged in a depth position as close as possible to the n +-doped source region 5. On the other hand, in the second comparative example (segment indicated by a single-dotted dashed line and a double-dotted dashed line 42), it was confirmed that when the conditions of the gate threshold voltage Vth are the same, the on-resistance becomes higher than in the second conventional example. Therefore, the results illustrate that, in the present invention, it is favorable if the depth of the position of the tip 13a is set such that the highly concentrated implantation region 13 is located at a depth position that does not reach the depth of the interface of the p-type base region 4 and the n-type current spreading region 3 from the base front side (that is, a depth that is shallower than the second comparative example).Although the EXAMPLE shows simulation results for a case where the cell pitch is 6 µm, even if the cell pitch ranges from 1.5 µm to 10 µm, for example, the same effects are achieved.
[0118] Although in the first to third examples, a case where aluminum is used as a p-type dopant (p-type impurity) constituting the p-type base region 4 and the high-concentration implantation region 13 is described as an example, the p-type dopant is not limited to this, and even if the above p-type dopant that is p-doped relative to silicon carbide is used, the same effects are achieved. Furthermore, the same effects are achieved even if the p-type dopant used when the p-type base region 4 is formed by epitaxy and the p-type dopant used when the high-concentration implantation region 13 is formed by ion implantation are different ion types.
[0119] In the above description, various changes are possible without departing from the spirit of the present invention. In the described embodiments, for example, the dimensions, impurity concentrations, etc. of the constituent elements can be varied according to the necessary specifications. Furthermore, in the described embodiments, although a MOSFET is described as an example without limitation, various silicon carbide semiconductor devices that conduct and block current by gate driving based on a predetermined gate threshold voltage are widely applicable. A gate-driven silicon carbide semiconductor device may be, for example, an insulated-gate bipolar transistor (IGBT) or the like.Furthermore, in the described embodiments, although a case where silicon carbide is used as a wide-gap semiconductor is described as an example, a wide-gap semiconductor other than silicon carbide, such as gallium nitride (GaN) and the like, may be used. In the described embodiments, a first conductivity type is assumed to be n-type, and a second conductivity type is assumed to be p-type; however, the present invention also applies when the first conductivity type is p-type and the second conductivity type is n-type. In this case, an n-type ion is formed in an n-type base region. + -doped highly concentrated implantation region is formed, which has an impurity concentration profile that is comparable to the p-doped impurity concentration profile in Fig. 2 by ion implantation is identical.
[0120] Although the described conventional structure achieves a channel with favorable crystallinity by forming the p-type base region 104 through epitaxy and enables reduced on-resistance due to high carrier mobility, controlling the impurity concentration during epitaxy of the silicon carbide layer is extremely difficult. The variation in the impurity concentration with current epitaxy techniques is ±30% for a unit product (including a semiconductor wafer area, each batch process of the manufacturing process, and inter-batch processes), which includes all products to be manufactured as a single unit within a predetermined period of time. When the variation in the p-type impurity concentration of the p-type base region 104 is ±30%, a problem arises that the variation in the gate threshold voltage Vth increases.Furthermore, when a vertical MOSFET with a trench gate structure is manufactured (produced), there arises a problem that defective chips due to the leakage current between the drain and the source (hereinafter leakage defect) increase and the yield decreases.
[0121] The silicon carbide semiconductor device and the method for manufacturing a silicon carbide semiconductor device according to the present invention enable a reduction in gate threshold voltage variation while maintaining a low on-resistance. Furthermore, it achieves the effect of reducing leakage defects and increasing yield.
[0122] As described, the silicon carbide semiconductor device and the method for manufacturing a silicon carbide semiconductor device according to the present invention are useful, for example, for semiconductor devices used in power conversion equipment such as converters and inverters and power supply devices such as various industrial machines, and are particularly suitable for the silicon carbide semiconductor devices of a trench gate structure.
Claims
[1] A silicon carbide semiconductor device comprising: a first semiconductor layer (21) having a first conductivity type formed on a front surface of a silicon carbide substrate (1); a second semiconductor layer (22) having a second conductivity type formed on an opposite side of the first semiconductor layer (21) of a silicon carbide substrate side thereof; a first semiconductor region (13) having the second conductivity type and selectively formed in the second semiconductor layer (22), the first semiconductor region (13) having an impurity concentration higher than that of the second semiconductor layer (22); a second semiconductor region (5) having the first conductivity type selectively formed in the second semiconductor layer (22) in a position shallower than the first semiconductor region (13); a trench (7) penetrating into the second semiconductor region (5), the first semiconductor region (13) and the second semiconductor layer (22) and reaching the first semiconductor layer (21); a gate electrode (9) provided by a gate insulating layer (8) in the trench (7); a first electrode (16) contacting the second semiconductor region (5) and the second semiconductor layer (22); and a second electrode (18) provided on a back side of the silicon carbide substrate (1), wherein: the first semiconductor region (13) has an impurity concentration profile with a second conductivity type in which the concentration differences in a depth direction form a bell-shaped curve at an impurity concentration peak higher than that of the second semiconductor layer (22); and the peak of the impurity concentration of the impurity concentration profile having a second conductivity type is positioned further on the side of a first electrode (16) than the boundary of the second semiconductor layer (22) and the first semiconductor layer (21). [2] The silicon carbide semiconductor device according to claim 1, wherein the first semiconductor region (13) has the impurity concentration profile with a second conductivity type in which the concentration differences in the depth direction form a plurality of bell-shaped curves at a plurality of peaks of the impurity concentration higher than that of the second semiconductor layer (22). [3] A silicon carbide semiconductor device according to claim 1 or 2, in which the impurity concentration profile having a second conductivity type, the impurity concentration decreases sharply at a boundary of the second semiconductor layer (22) and the first semiconductor layer (21). [4] A silicon carbide semiconductor device according to any one of claims 1 to 3, wherein the first semiconductor region (13) is provided in a direction parallel to the front side of the silicon carbide substrate (1). [5] A silicon carbide semiconductor device according to any one of claims 1 to 4, comprising a third (3) semiconductor region having the first conductivity type formed in the first semiconductor layer (21), wherein the third semiconductor region (3) has an impurity concentration higher than that of the first semiconductor layer (21), wherein the third semiconductor region (3) contacts the second semiconductor layer (22) and reaches a position which is deeper than a bottom of the trench (7) on the side of a second electrode (18) from a boundary with the second semiconductor layer (22). [6] A silicon carbide semiconductor device according to claim 5, comprising a fourth semiconductor region (11) having the second conductivity type selectively formed in the third semiconductor region (3), the fourth semiconductor region covering the bottom of the trench (7). [7] The silicon carbide semiconductor device according to claim 6, wherein the fourth semiconductor region (11) penetrates into the third semiconductor region (3) from the bottom of the trench (7) in the depth direction. [8] A silicon carbide semiconductor device according to any one of claims 5 to 7, comprising a fifth semiconductor region (12) having the second conductivity type formed in the third semiconductor region (3) between the trench (7) and an adjacent trench (7) to contact the second semiconductor layer (22). [9] A silicon carbide semiconductor device according to claim 8, wherein the fifth semiconductor region (12) penetrates into the third semiconductor region (3) in the depth direction.
Citation Information
Patent Citations
Semiconductor device and method of manufacturing the same
JP2012099601A
Semiconductor device
JP2014241435A
Silicon carbide semiconductor device
JP2015072999A
Semiconductor device
US20110068353A1
Semiconductor device and method of manufacturing semiconductor device
US20150194492A1