Method for manufacturing a hybrid-laminated wing body

The method of using displacement bodies to introduce throttle openings non-destructively into undraped fiber composite materials addresses production challenges, enabling efficient and accurate manufacturing of hybrid laminarized wing bodies with maintained load-bearing properties and laminar flow.

DE102018102492B4Active Publication Date: 2024-11-07DEUTSCHES ZENTRUM FÜR LUFT UND RAUMFAHRT E V
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE102018102492
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-02-05
Publication Date
2024-11-07
Estimated Expiration
2038-02-05

AI Technical Summary

Technical Problem

Existing methods for producing hybrid laminarized wing bodies using fiber composite materials face challenges such as impaired load-bearing structure, reduced dimensional accuracy, and increased production complexity due to machining processes for introducing throttle openings, which compromise weight reduction and efficiency.

Method used

A method involving the use of displacement bodies to introduce throttle openings non-destructively into undraped semi-finished fiber products, which are then draped on a shaping tool and integrated with a matrix material to form a support structure without cutting through fibers, allowing for the production of hybrid laminarized wing bodies without machining.

Benefits of technology

Enables efficient production of hybrid laminarized wing bodies with maintained dimensional accuracy and load-bearing properties, reducing production complexity and avoiding the need for additional material compensation, while maintaining a laminar flow for reduced air resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for producing a hybrid-laminarized wing body (1) in which laminar flow around the wing body is to be achieved by shaping and boundary layer extraction, wherein the hybrid-laminarized wing body (1) is produced by arranging a perforated outer skin (2) on an internal support structure (3) forming a plurality of separate extraction chambers (6) such that the extraction chambers (6) are operatively connected to the perforated outer skin (2) for extracting the boundary layer on the one hand and to throttle openings (8) provided in the internal support structure (3) for connecting to an extraction system (9) on the other hand, characterized in that the internal support structure (3) is produced from a fiber composite material in the following steps: - Providing flat, undraped fiber semi-finished products (110) of the fiber composite material, - Introducing displacement bodies (100, 210) into the fiber semi-finished products (110) at the locations where the throttle openings (8) are later to be provided in the internal support structure (3) by non-destructive displacement of the fibers of the respective fiber semi-finished products (110), - Draping the fiber semi-finished products (110) on a shaping tool surface (310) of a forming tool with the displacement bodies (100, 210) introduced into the fiber semi-finished products (110), - Curing of a matrix material of the fiber composite material embedding the fibers of the fiber semi-finished products (110) while the displacement bodies (100, 210) introduced into the fiber semi-finished products (110) remain in the fiber semi-finished products (110), and - Removal of the displacement bodies (100, 210) after the matrix material has hardened to form the throttle openings (8) in the supporting structure (3) - wherein, for the production of the hybrid laminarized wing body, the outer skin (2) is arranged on a wave-shaped profile (4) arranged on the produced supporting structure (3), which has a cavity between two wave crests for the formation of the suction chambers (6).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for manufacturing a hybrid-laminarized wing body, in which a laminar flow around the wing body is to be achieved by shaping and boundary layer suction according to the preamble of claim 1.

[0002] Faced with ever-increasing cost pressures, aircraft manufacturers are striving to make their aircraft more cost-effective to operate through appropriate measures. A key focus here is on significantly reducing the overall weight of commercial aircraft and minimizing drag during flight.

[0003] The consistent use of fiber-reinforced composites, even for critical or load-bearing structures, addresses the issue of weight reduction and thus fuel savings. Furthermore, it has been shown that maintaining a laminar boundary layer on the outer surface of the wing bodies, especially the lift-generating wing bodies, is advantageous for reducing drag during flight, as turbulent flow components significantly increase drag and consequently fuel consumption.

[0004] Airflows encountering an aerodynamic airfoil generally tend towards a laminar boundary layer flow. However, certain shaping features, such as protruding rivets or edges on the aerodynamic airfoil surface, can quickly cause the inherently laminar boundary layer to transition into a turbulent one, thus increasing drag. Therefore, maintaining a laminar boundary layer flow requires that the airfoil shape promotes this flow and minimizes the transition to a turbulent one.Furthermore, it has been shown that by extracting the boundary layer using a suction system integrated into the wing body and a microperforated aerodynamic surface, a laminar flow that lasts as long as possible can be achieved over the airfoil, further reducing drag and thus saving fuel overall. A long-lasting laminar flow in this context means that the flow path along the airfoil surface is as long as possible, ideally extending from the leading edge to the trailing edge of the airfoil.

[0005] Aerodynamic airfoils or wing bodies designed to maintain a laminar flow for as long as possible, both through their shape and with the aid of boundary layer suction, are also known as hybrid laminar flow airfoils or airfoils and are currently known, at least in the experimental stage, under the name HLFC technology. Such a wing body has a structure in which a perforated outer skin, e.g., made of an erosion-resistant material such as metal or aluminum, is applied to a supporting structure. Due to its shape, this supporting structure, together with the perforated outer skin, forms individual suction chambers beneath the perforated outer skin, thus enabling the extraction of airflow from the boundary layer region.The individual suction chambers each have one or more throttle openings, through which the respective suction chamber communicates with a suction system to generate a negative pressure. The suction chambers can be created, for example, by giving the supporting structure a wave-like structure or shape on the side facing the perforated outer skin, so that when the perforated outer skin is placed on top, chambers are formed between the supporting structure and the perforated outer skin due to the wave-like structure.

[0006] If such a support structure for HLFC technology is to be manufactured from a fiber composite material for further weight reduction, the problem arises that the throttle openings provided in the support structure must be introduced into the load-bearing fiber composite structure of the support structure using machining processes, which in principle represents an impairment of the supporting structure and places corresponding demands on industrial manufacturing.

[0007] Machining processes cut load-bearing fibers and thus weaken the structure, which must be compensated for with additional material. This, however, partially negates the weight advantage gained through the use of fiber-reinforced composites. Furthermore, fiber-reinforced plastics are usually inhomogeneous and therefore mechanically difficult to machine, resulting in reduced dimensional accuracy across a large number of bores. Tool life is limited, as are feed rates, leading to long machining times for creating the throttle openings. Additionally, lubricated machining of fiber-reinforced plastic structures has not yet been implemented industrially, meaning that dust is released during machining, which must be contained.

[0008] Furthermore, the insertion of the throttle openings can only take place after the curing reaction has been completed and therefore must be carried out on geometrically complex structures, which can sometimes lead to collisions between the tool and the fiber composite structures.

[0009] German patent DE 10 2013 109 995 A1 discloses a manufacturing process for producing a fiber composite component in which, prior to the curing of the matrix material, a mandrel is inserted into the fiber material. This mandrel does not cut the fibers but merely displaces them to create an opening in the fiber composite component. The mandrel remains in the fiber composite component until the matrix material has fully cured and is then drilled out. The resulting opening in the fiber composite component is then fitted with an insert, a bolt, or a rivet to connect the fiber composite component to other components. However, the subsequent drilling out of the mandrel necessitates a machining process, which entails the aforementioned disadvantages in industrial manufacturing.

[0010] Similar manufacturing processes for producing openings using a mandrel are known from DE 2 944 371 A1, DE 3 715 409 A1 and DE 10 2013 201 963 A1.

[0011] Furthermore, a laminar flow wing is known from EP 2 687 439 A1, which consists of an outer layer, a middle support layer, and a bottom layer. The outer layer has perforations that open into the middle layer, which can be made of, for example, an air-permeable or impermeable material. The bottom layer has openings to allow boundary layer extraction via the perforations in the outer layer.

[0012] It is therefore an object of the present invention to provide an improved method for producing a hybrid-laminated wing body, with which such wing bodies can also be efficiently produced in an industrial context.

[0013] The problem is solved by the method according to claim 1 according to the invention. Advantageous embodiments are found in the corresponding dependent claims.

[0014] According to claim 1, a method for manufacturing a hybrid-laminarized wing body is proposed, in which laminar flow around the wing body is to be at least partially achieved by shaping and boundary layer extraction. The hybrid-laminarized wing body is manufactured by arranging a perforated outer skin onto an internal support structure, forming a plurality of separate extraction chambers such that the extraction chambers are operatively connected to the perforated outer skin for extracting the boundary layer on the one hand, and to throttle openings provided in the internal support structure for connecting to an extraction system on the other.

[0015] According to the invention, the manufacturing process is characterized in that the internal support structure is made of a fiber-reinforced composite material, wherein the throttle openings provided in the internal support structure are specifically not to be introduced by a machining process. The fiber-reinforced composite material comprises, on the one hand, a fiber material and, on the other hand, a matrix material as essential components, wherein the matrix material embeds the fiber material and, after curing, forms an integral unit with the fiber material.

[0016] According to the invention, it is further provided that, to implement a non-machining process, the throttle openings are introduced by first providing flat, undraped fiber semi-finished products of the fiber composite material. Displacement elements are then inserted into these flat, undraped fiber semi-finished products at the locations where the throttle openings are later to be provided in the internal support structure, the insertion of the displacement elements being carried out in such a way that the fibers of the respective fiber semi-finished products are displaced without damage.

[0017] The fiber preforms, along with the integrated displacement bodies, are then draped onto a shaping tool surface of a mold, thus forming the final component shape of the supporting structure. Subsequently, a matrix material of the fiber composite, which embeds the fibers of the fiber preforms, is cured, for example, by tempering and, if necessary, pressurization. During the curing process, which can take some time, the displacement bodies remain in the fiber preforms.

[0018] After the matrix material has hardened and an integral unit has formed between the matrix material and the fiber material, the displacement bodies are removed from the manufactured component, thus forming the corresponding throttle openings in the supporting structure.

[0019] To produce the hybrid laminar wing body, the outer skin is then placed on a wave-shaped profile arranged on the supporting structure thus produced, wherein the wave-shaped profile has a cavity between two wave crests for forming the suction chambers.

[0020] With such a method according to the invention, it becomes possible to produce a supporting structure for wing bodies with HLFC technology from a fiber composite material without having to introduce the required throttle openings for the extraction system by means of a machining process.

[0021] According to the invention, it was discovered that displacement bodies can be introduced into the flat, undraped fiber semi-finished products, and that these fiber semi-finished products, now equipped with the displacement bodies, can then be draped onto the corresponding shaping tool surface without the inserted displacement bodies damaging the fibers or rendering the fiber semi-finished product unusable. This is because the draping process is a very critical step in the entire manufacturing process, as fibers are frequently displaced or sheared, and material compression or stretching often occurs, which can later lead to structural defects.According to the invention, however, the displacement bodies can remain in the fiber semi-finished products during the draping process without negatively affecting the draping process, thus offering the advantage that the displacement bodies do not have to be introduced into the already draped fiber semi-finished products and thus into the complex geometric structure later.

[0022] Furthermore, the inventor recognized that such a throttle opening, produced using a displacement body as described according to the invention, is suitable as a throttle opening for extracting the boundary layer, even if the inner wall of the throttle opening is not lined with an insert. In fact, with the aid of such a displacement body, a throttle opening can be produced in such a way that it conforms to the specified tolerance values ​​and dimensions, and this dimensional accuracy can be maintained across a large number of these throttle openings, even when the displacement bodies are inserted into the flat, undraped fiber semi-finished products and the fiber semi-finished products are subsequently draped.

[0023] A further advantage is that no fiber ends are exposed through the throttling openings created by the displacement bodies. Subsequent edge sealing of the throttling openings to minimize water absorption by fiber composite components in humid environments is therefore unnecessary.

[0024] The term "flat" refers specifically to a fiber semi-finished product that has a flat shape and a relatively small thickness or height. The term "undraped" further implies that the fiber semi-finished product has not yet been formed into its final component shape and is preferably still in a flat, undeformed state.

[0025] In an advantageous embodiment, one or more fiber layer packages are first formed from the provided, undraped fiber semi-finished products. These packages are produced from several layers of the provided fiber semi-finished products. The displacement bodies are then inserted into these layer-by-layer fiber layer packages. Following the preform production step and the insertion of the displacement bodies, the fiber layer packages, or the single fiber layer package, are then draped onto the mold.

[0026] It was recognized here that such a displacement body in the undraped state can also be introduced through several layers or strata of fiber material without destroying the fibers, while still complying with the boundary conditions imposed on the throttle openings.

[0027] In a further advantageous embodiment, several different displacement bodies are provided, each having different cross-sectional sizes and / or cross-sectional shapes, wherein each throttle opening is specified with a certain opening size and / or opening shape, and a displacement body is selected for a certain location where a throttle opening is to be formed, depending on the opening size and / or opening shape specified for the respective throttle opening at that location.

[0028] This allows for the integration of various throttle openings with different cross-sectional sizes and / or shapes across the entire length of the supporting structure, thereby influencing the strength of the suction at the aerodynamic surface of the airfoil. Larger throttle openings are generally provided in the leading edge region to enhance the suction effect, while the openings become smaller towards the trailing edge of the wing to reduce the suction force.

[0029] It is conceivable that a mandrel with a conical tip could be used as the displacement body, allowing it to be inserted into the fiber material without causing damage. Alternatively, a thread could be used as the displacement body, which could, for example, have different thicknesses.

[0030] In a further advantageous embodiment, at least dry fiber semi-finished products are provided as fiber semi-finished products, which are not yet impregnated or pre-impregnated with a matrix material. After draping the fiber semi-finished products onto the predetermined tool surface, the dry fiber semi-finished products are infused with a matrix material. For this purpose, it is advantageous, for example, if the fiber material draped onto the mold is vacuum-sealed using a vacuum setup and the component is then evacuated to improve the infusion of the matrix material into the fiber material. However, it is also conceivable to provide pre-impregnated fiber semi-finished products (so-called prepregs) that do not necessarily require infusion with a matrix material in the further manufacturing process.

[0031] Furthermore, it has proven advantageous if the displacement bodies are coated or provided with a release agent, or supplied with such an agent, so that the displacement bodies can be removed from the formed openings without damage and without excessive adhesion to the hardening matrix material. It is also conceivable, however, that the displacement bodies consist of a material that inherently has the property of only forming an adhesive bond with the matrix material with difficulty.

[0032] Another aspect of the present invention is the use of a fiber composite component as a supporting structure of a hybrid laminated wing body, wherein the fiber composite component contains a plurality of throttle openings formed by displacement bodies which are introduced into the fiber semi-finished products at the locations where the throttle openings are to be provided in the internal supporting structure by non-destructive displacement of the fibers of the respective fiber semi-finished products and are removed after the curing of a matrix material embedding the fibers of the fiber semi-finished products.

[0033] The invention is explained in more detail using the attached figures as examples. They show: Fig. 1 Schematic representation of a partial section of a hybrid-laminarized wing body; Fig. 2. Schematic representation of the insertion of a displacement body into fiber semi-finished products; Fig. 3 exemplary schematic representations of the manufacturing process in one aspect.

[0034] Fig. Figure 1 shows a section of a hybrid-laminated wing body 1, which has an outer skin 2 and a supporting structure 3. The supporting structure 3 has a wave-shaped profile 4 on its side facing the outer skin 2, whereby a cavity 5 is formed between two wave crests, from which the suction chambers 6 can then be formed by arranging the outer skin 2 onto this wave-shaped profile 4 of the supporting structure 3.

[0035] The outer skin 2 is perforated, particularly in the micro-perforation area, and can, for example, have openings of less than 100 µm. This perforated outer skin 2 allows for the extraction of a fluid flowing around the suction chambers 6 by creating a negative pressure within them, as schematically indicated by arrows 7.

[0036] In order to generate a negative pressure in the extraction chambers 6, each extraction chamber 6 is also connected to an extraction system 9 via a throttle opening 8, wherein the extraction system 9 can be, for example, a negative pressure chamber within the leading edge of the wing, which is connected to the respective extraction chambers 6 via the throttle openings 8.

[0037] The throttle openings 8 can have different diameters in order to adjust the suction power accordingly.

[0038] With such a wing body 1, it is possible to selectively extract the boundary layer during the flow towards the aerodynamic wing body 1 and thus maintain a long-lasting laminar boundary layer across the cross-section of the wing body.

[0039] According to the invention, the supporting structure 3 with the throttle openings 8 is to be manufactured from a fiber-reinforced composite material, whereby the throttle openings 8 are specifically not to be produced by means of a machining process, as would be the case, for example, with drilling. According to the invention, it is now proposed that a displacement body 100, as described in Fig. As schematically indicated in Figure 2, the fibers are displaced non-destructively by introducing the displacement body 100 into the fiber semi-finished product 110, whereby the displacement body 100 remains in the fiber material 110 during the curing of the matrix material. It is schematically indicated that in the displacement area 120, the fibers of the fiber material 110 are not destroyed, but merely deflected from their path, thus preserving the load-bearing capacity of the component.

[0040] Fig. Figure 3 schematically shows the planar fiber layer package 200, which is composed of several layers of fiber semi-finished product 110. In the displacement area 120, where the corresponding throttle opening will later be located, a displacement body 210 is now inserted. This displacement body has a flange at its upper end and thus terminates flush with the upper fiber layer package 200. On its underside, which will later be brought into contact with a forming tool, the displacement body 210 terminates flush with the underside of the fiber layer package.

[0041] After the formation of such fiber layer packages and the introduction of the respective displacement bodies 210, the fiber layer package 200 is placed on a shaping tool surface 310 of a molding tool 300, which in the lower part of the Fig.This is shown schematically in Figure 3. Here, the fiber layer package 200 is brought into its final component shape and can now be referred to as component 320. In this process, the fiber layer package 200 is bent, particularly from its original fiber plane, even multiple times, thus acquiring its final component shape. Reference symbol list 1 hybrid laminarized wing body 2 Outer skin 3 Supporting structure 4 wave-shaped profiling 5-cavity 6 extraction chambers 7 Extraction 8 Throttle opening 9 Extraction system 100 displacement bodies 110 fiber semi-finished products 120 Displacement area 200 fiber layer package 210 Displacement bodies 300 tools 310 shaping tool surface 320 component

Claims

[1] Method for producing a hybrid-laminarized wing body (1), in which a laminar flow around the wing body is to be achieved by shaping and boundary layer extraction, wherein the hybrid-laminarized wing body (1) is produced by arranging a perforated outer skin (2) on an internal support structure (3) to form a plurality of separate extraction chambers (6) in such a way that the extraction chambers (6) are in operative connection with the perforated outer skin (2) for extracting the boundary layer on the one hand and with throttle openings (8) provided in the internal support structure (3) for connecting to an extraction system (9) on the other hand, characterized by that the internal supporting structure (3) is made of a fiber composite material with the following steps: - Providing flat, undraped semi-finished fiber products (110) of the fiber composite material, - introducing displacement bodies (100, 210) into the semi-finished fibre products (110) at the locations where the throttle openings (8) are to be provided later in the internal support structure (3), by non-destructively displacing the fibres of the respective semi-finished fibre products (110), - draping the semi-finished fiber products (110) on a shaping tool surface (310) of a molding tool with the displacement bodies (100, 210) introduced into the semi-finished fiber products (110), - curing a matrix material of the fiber composite material embedding the fibers of the semi-finished fiber products (110) while the displacement bodies (100, 210) introduced into the semi-finished fiber products (110) remain in the semi-finished fiber products (110), and - removing the displacement bodies (100, 210) after the matrix material has hardened to form the throttle openings (8) in the supporting structure (3) - wherein, for the production of the hybrid laminated wing body, the outer skin (2) is arranged on a wave-shaped profile (4) arranged on the manufactured support structure (3), which has a cavity between two wave crests for forming the suction chambers (6). [2] Method according to claim 1, characterized by that one or more fiber layer packages (200) are first formed from the provided, undraped fiber semi-finished products (110), wherein the displacement bodies (100, 210) are subsequently introduced into the fiber layer package(s) (200). [3] Method according to claim 1 or 2, characterized bythat several different displacement bodies (100, 210) are provided, each having different cross-sectional sizes and / or cross-sectional shapes, wherein each throttle opening (8) is predetermined with a specific opening size and / or opening shape, and a displacement body (100, 210) is selected for a certain location at which a throttle opening (8) is to be formed, depending on the opening size and / or opening shape predetermined for the respective throttle opening (8) at this location. [4] Method according to one of the preceding claims, characterized by that a mandrel and / or a thread are introduced as a displacement body (100, 210). [5] Method according to one of the preceding claims, characterized bythat dry semi-finished fiber products are provided as semi-finished fiber products (110), wherein after draping the semi-finished fiber products (110) on the shaping tool surface (310), the dry semi-finished fiber products are infused with a matrix material. [6] Method according to claim 5, characterized by that after draping the semi-finished fiber products (110) and before infusing the matrix material, the semi-finished fiber products (110) are closed or sealed in a vacuum-tight manner and then the semi-finished fiber products (110) are evacuated by means of a vacuum pump. [7] Method according to one of the preceding claims, characterized by that the displacement bodies (100, 210) are provided with a release agent or coated before being introduced into the semi-finished fiber products (110) or are provided with such a release agent.

Citation Information

Patent Citations

  • Method for manufacturing a component from a fiber composite material with a hole

    DE102013109995A1

  • Method for manufacturing a fiber-reinforced plastic component

    DE102013201963A1

  • Hole piercing method for fibre reinforced components - consists of inserting heated spike before hardening and removing after hardening

    DE2944371A1

  • Process for producing fibre-reinforced composite material with fastening holes

    DE3715409A1

  • Laminar flow panel

    EP2687439A1