METHOD FOR MANUFACTURING A SEMICONDUCTOR DEVICE
The selective removal of oxide film on the trench floor surface using CF-based gases and argon ions addresses contamination issues, enabling deeper P-type implantation and improved semiconductor device performance.
Patent Information
- Application Number
- DE102018200237
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-01-13
- Filing Date
- 2018-01-09
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2038-01-09
AI Technical Summary
Existing semiconductor device manufacturing methods face challenges in forming a floating area without contamination from the P-type impurities during ion implantation, as the oxide film on the trench side surfaces and floor surfaces complicates the process, making it difficult to achieve deeper implantation and maintain device performance.
A method involving the selective removal of the oxide film on the trench floor surface using a CF-based gas with a carbon atomic ring structure and argon ions, allowing for deeper ion implantation while protecting the side surfaces, using a capacitively coupled plasma etching device to control the etching process.
Enables deeper implantation of P-type impurities into the semiconductor substrate without contaminating the trench side surfaces, enhancing the semiconductor device's performance by increasing voltage resistance and reducing resistance issues.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND OF THE INVENTION 1. Field of the Invention
[0001] The present invention relates to a method for manufacturing a semiconductor device. 2. State of the art
[0002] For example, it is known that a semiconductor device such as a metal-oxide-semiconductor field-effect transistor (MOSFET) or an insulated-gate bipolar transistor (IGBT) has a structure in which a p-type floating region is disposed in an n-type drift region of a semiconductor substrate. With this structure, depletion of the drift region is promoted, and thus the voltage resistance of the semiconductor device can be increased.
[0003] The floating region is formed by ion implantation of p-type impurities. The ion implantation is performed over a bottom surface of a trench formed in the semiconductor substrate, and the floating region is formed in a region adjacent to the bottom surface of the trench. At this time, if p-type impurities are implanted into side surfaces of the trench, the characteristics of the semiconductor device, such as on-resistance, may deteriorate. Therefore, during ion implantation, an oxide film is formed in advance on the side surfaces and bottom surface of the trench. As a result, implantation of p-type impurities into the side surfaces of the trench can be further prevented or reduced. P-type impurities penetrate into the bottom surface of the trench at a vertical or substantially vertical angle.Therefore, the p-type impurities pass through the oxide film and are implanted into the semiconductor substrate. An example of this technique is described in JP 2005-116822 A.
[0004] DE 38 32 414 A1 discloses a method for manufacturing a semiconductor device, comprising: preparing a semiconductor substrate; forming a trench on a surface of the semiconductor substrate; forming an oxide film on side surfaces and a bottom surface of the trench; removing at least a part of the oxide film by dry etching from the bottom surface of the trench; and performing ion implantation of conductive impurities into the semiconductor substrate through the bottom surface of the trench after the dry etching, wherein the dry etching is a reactive ion etching.
[0005] In the article by Garozzo, G.; Colombo, S.; Lombardo, SF; La Magna, A.: “A 0-Dimensional Model for Oxide and Nitride Dry Etching”, IEEE Trans. Semicond. Manuf., 28, 2015, 3, 337 - 344, dry etching properties are investigated using different gas mixtures containing fluorocarbon, oxygen gas, and argon gas.
[0006] WO 2006 / 046388 A1 discloses a method for manufacturing a semiconductor device, comprising: preparing a semiconductor substrate in which an n-type drain region, an n-type drift region, and a p-type body region are stacked in this order, and in which a p-type contact region and an n-type source region are arranged along an upper surface of the semiconductor substrate; forming a trench in the semiconductor substrate, the trench extending from the upper surface of the semiconductor substrate into the drift region; forming an oxide film on side surfaces and a bottom surface of the trench; performing ion implantation of conductive impurities into the semiconductor substrate through the bottom surface of the trench; and forming a p-type floating region in the drift region.
[0007] US Pat. No. 6,803,307 B1 describes a method for producing contact holes with spacers on the sidewalls. It also describes the use of etching gases containing a mixture of at least one of oxygen, fluorocarbon, carbon oxide, and argon. SUMMARY OF THE INVENTION
[0008] In the case where the thickness of the oxide film formed on the side surfaces of the trench is insufficient during ion implantation into the floating region, p-type impurities penetrate the oxide film and are implanted into the side surfaces of the trench. Therefore, it is advantageous if the oxide film on the side surfaces of the trench is formed relatively thick. On the other hand, if the oxide film on the bottom surface of the trench is formed thickly, the oxide film interferes with ion implantation into the semiconductor substrate. Therefore, it is difficult to form the floating region further. Therefore, it is advantageous if the oxide film on the bottom surface of the trench is formed extremely thin or even absent. However, in the prior art, the oxide film is formed uniformly on the side surfaces and the bottom surface of the trench, and the oxide film alone cannot be selectively removed from the bottom surface of the trench.Therefore, in order to prevent implantation of p-type impurities into the side surfaces of the trench, the implantation level of ion implantation must be further reduced, and it is difficult to form the floating region even deeper.
[0009] The object of the invention is to provide a method for manufacturing a semiconductor device having a floating region in a drift region without a large amount of a reaction product being deposited in the side surfaces of a trench during ion implantation for the floating region, and at the same time an oxide film can be formed extremely thin on a bottom surface of the trench or can be completely removed from the bottom surface.
[0010] The object is achieved according to a method for producing a semiconductor device having the features of claim 1. The dependent claims relate to preferred developments of the invention.
[0011] According to the invention, the oxide film is first formed on the side surfaces and the bottom surface of the trench, and then reactive ion etching is performed to selectively remove the oxide film from the bottom surface of the trench. Reactive ion etching uses an etching gas containing CF-based gas, which has a carbon atom ring structure, oxygen gas, and argon gas. The CF-based gas is a gas that supplies radicals and chemically reacts with oxygen and atoms forming the semiconductor substrate to produce a reaction product. On the other hand, argon is a gas that supplies ions required for an ion-assisted reaction.
[0012] The angle of incidence of ionized argon is relatively small in the oxide film located on the side surfaces of the trench and relatively large in the oxide film located on the bottom surface of the trench. Due to the variation in the angle of incidence, the production of the reaction product (i.e., etching) proceeds in the oxide film located mainly on the bottom surface of the trench. The reaction product evaporates from the bottom surface of the trench and then deposits on the oxide film located on the side surface of the trench to form a protective film that protects the oxide film. At this time, if the CF-based gas supplying radicals has a carbon atom ring structure, the reaction product is likely to deposit.Accordingly, a larger amount of the reaction product deposits on the oxide film located on the side surfaces of the trench before being discharged outside the trench. Thus, the protective film is formed even more effectively. As a result, the oxide film located on the side surfaces of the trench is protected, and the oxide film located on the bottom surface of the trench is selectively removed.
[0013] Preferably, the oxide film can be removed by dry etching until the bottom surface of the trench is exposed. In this aspect of the present invention, the conductive impurities can be implanted through the bottom surface of the trench to a deeper position during subsequent ion implantation.
[0014] Preferably, a capacitively coupled plasma etching apparatus can be used for dry etching, wherein the capacitively coupled plasma etching apparatus includes two AC power sources, each supplying AC power to a pair of electrodes. With the plasma etching apparatus according to the aspect of the present invention, a relatively high electron density can be achieved, and argon or other ions can be drawn even more strongly into the semiconductor substrate.
[0015] Preferably, the CF-based gas having a carbon atom ring structure can be represented by one of the chemical formulas C4F6, C5F8, C5F8, and C5HF7. Here, for example, an attachment coefficient of C4F6 or C4F8 varies depending on different conditions, but is approximately 0.1 to 0.01. On the other hand, an attachment coefficient of CF2 or CF4, which is a CF-based gas that does not have a carbon atom ring structure, is approximately 0.01 to 0.001 under the same conditions.
[0016] Preferably, the semiconductor substrate may be a silicon carbide substrate.
[0017] Preferably, in forming the oxide film, the oxide film may be uniformly formed not only on the side surfaces and the bottom surface of the trench but also on an upper surface of the semiconductor substrate.
[0018] Preferably, in forming the oxide film, the oxide film may be formed such that the thickness of the oxide film in a direction perpendicular to the semiconductor substrate is 1.2 micrometers or more.
[0019] With the method for manufacturing a semiconductor device according to the present invention, an oxide film can be formed relatively thickly on the side surfaces of a trench, and an oxide film can be formed extremely thinly on the bottom surface of the trench, or it can be completely removed from the bottom surface. As a result, even if the implantation level is set relatively high during subsequent ion implantation, conductive impurities can be prevented from being implanted into the side surfaces of the trench. The conductive impurities can be implanted deeper through the bottom surface of the trench. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Features, advantages, and the technical and industrial significance of exemplary embodiments of the invention are described below with reference to the accompanying drawings, in which like reference numerals designate like elements. In the drawings: Fig. 1 is a cross-sectional view showing a structure of a semiconductor device according to an embodiment; Fig. 2 is a flowchart showing a method of manufacturing the semiconductor device according to the embodiment; Fig. 3 is a diagram showing a semiconductor substrate in which a drain region, a drift region, a body region (main region), a contact region, and a source region are formed; Fig. 4 is a diagram showing a state in which a first oxide film is formed on an upper surface of the semiconductor substrate in a step of forming a trench; Fig. 5 is a diagram showing a state in which an opening is formed in the first oxide film corresponding to a position where the trench is to be formed in the trench forming step; Fig. 6 is a diagram showing a state in which the trench is formed on the upper surface of the semiconductor substrate in the trench forming step; Fig. 7 is a diagram showing a state in which a second oxide film is formed on side surfaces and a bottom surface of the trench in a step of forming a floating region; Fig. 8 is a diagram showing a state in which the second oxide film disposed on the bottom surface of the trench is removed by dry etching (i.e., reactive ion etching) in the step of forming the floating region; Fig. 9 is a diagram schematically showing a plasma etching apparatus used for reactive ion etching of the second oxide film in the step of forming the floating region; Fig. 10 is a diagram showing ion implantation of p-type impurities in the step of forming the floating region; Fig. 11 a diagram showing measurement positions of the etching size to illustrate experimental results in combination with Fig. 12 to describe; and Fig. 12 is a table showing the results of measuring the etching size of the second oxide film at the measuring positions of the Fig. 11 shows. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0021] A semiconductor device 10 according to an embodiment and its manufacturing method will be described with reference to the drawings. The semiconductor device 10 according to the embodiment is a power semiconductor device used in a power circuit, and more specifically, has a MOSFET structure. Although not particularly limited thereto, the semiconductor device 10 may be used as a switching element of a power conversion circuit such as a converter or an inverter in an electrically powered vehicle such as a hybrid vehicle, a fuel cell vehicle, or an electric vehicle. Hereinafter, the structure of the semiconductor device 10 will be described first, and then the method of manufacturing the semiconductor device 10 will be described.The semiconductor device 10 and its manufacturing method described below are only exemplary, and various technical features described in the specification are applicable alone or in combination to other various semiconductor devices and their manufacturing methods.
[0022] Fig. 1 is a cross-sectional view showing the structure of the semiconductor device 10 according to the embodiment. Fig. 1 shows a part of the semiconductor device 10. In the semiconductor device 10, the unit structure shown in Fig. 1, is repeatedly formed. As shown in Fig. As shown in FIG. 1, the semiconductor device 10 according to the embodiment includes a semiconductor substrate 12 and a gate electrode 14 disposed in a trench formed in an upper surface 12a of the semiconductor substrate 12. The semiconductor substrate 12 is a silicon carbide (SiC) substrate. The trench 13 has a pair of side surfaces 13a and a bottom surface 13b. A gate insulating film 14a is formed on the side surfaces 13a and the bottom surface 13b of the trench 13, and the gate electrode 14 is located on the opposite side of the gate insulating film 14a from the side surfaces 13a of the trench. The gate electrode 14 is formed, for example, from a conductive material such as polysilicon. The gate insulating film 14a may be formed from an insulating material such as silicon oxide (SiO2). However, specific materials forming the gate electrode 14 and the gate insulating film 14a are not particularly limited.
[0023] The semiconductor device 10 also includes a source electrode 16 disposed on the upper surface 12a of the semiconductor substrate 12 and a drain electrode 18 disposed on a lower surface 12b of the semiconductor substrate 12. The source electrode 16 is in ohmic contact with the upper surface 12a of the semiconductor substrate 12, and the drain electrode 18 is in ohmic contact with the lower surface 12b of the semiconductor substrate 12. An interlayer insulating film 14b is disposed between the source electrode 16 and the gate electrode 14, and the source electrode 16 is electrically insulated from the gate electrode 14. The source electrode 16 and the drain electrode 18 can be formed using a conductive material such as aluminum (Al), nickel (Ni), titanium (Ti), or gold (Au). However, specific materials forming the source electrode 16 and the drain electrode 18 are not particularly limited.
[0024] Here, the upper surface 12a of the semiconductor substrate 12 refers to one surface of the semiconductor substrate 12, and the lower surface 12b of the semiconductor substrate 12 refers to another surface of the semiconductor substrate 12 opposite the upper surface 12a. In the description, "upper surface" and "lower surface" are used for convenience to distinguish between two surfaces arranged opposite each other. For example, the upper surface 12a of the semiconductor substrate 12 is not always arranged vertically upward. Depending on the orientation of the semiconductor substrate 12, the upper surface 12a may be arranged vertically downward, and the lower surface 12b may be arranged upward.
[0025] The semiconductor substrate 12 includes a drain region 32, a drift region 34, a main region or body region 36, a contact region 38, a source region 40, and a floating region 42. The drain region 32 is disposed along the bottom surface 12b of the semiconductor substrate 12 and is exposed to the bottom surface 12b. The drain region 32 is an n-type region. N-type impurities may be formed, for example, from a Group V element (Group 15 element) such as phosphorus. The drain electrode 18 is in ohmic contact with the drain region 32.
[0026] The drift region 34 is disposed on the drain region 32 and adjacent to the drain region 32. The drift region 34 is an n-type region. The n-type impurity concentration in the drift region 34 is lower than that in the drain region 32. N-type impurities may be formed, for example, from a Group V element (Group 15 element) such as phosphorus.
[0027] Body region 36 is disposed on and adjacent to drift region 34. Body region 36 is separated from drain region 32 by at least drift region 34. Body region 36 is a p-type region. P-type impurities can be formed from a Group III element (Group 13 element) such as boron (B) or aluminum (Al).
[0028] Contact region 38 is disposed on body region 36 and is exposed to the upper surface 12a of semiconductor substrate 12. Contact region 38 is a p-type region. The p-type impurity concentration in contact region 38 is higher than that in body region 36. P-type impurities may be formed from a Group III element (Group 13 element) such as boron (B) or aluminum (Al). Source electrode 16 is in ohmic contact with contact region 38.
[0029] The source region 40 is disposed on the body region 36 and is exposed to the upper surface 12a of the semiconductor substrate 12. The source region 40 is separated from the drift region 34 by at least the body region 36. The source region 40 is an n-type region. The n-type impurity concentration in the source region 40 is higher than that in the drift region 34. N-type impurities may be formed, for example, from a Group V element (Group 15 element) such as phosphorus. The source electrode 16 is also in ohmic contact with the source region 40.
[0030] The floating region 42 is disposed in the drift region 34 between the bottom surface 13b of the trench 13 and the drain region 32. The floating region 42 is a p-type region. The p-type impurity concentration in the floating region 42 is, for example, equal to that in the body region 36 and lower than that in the contact region 38. P-type impurities may be formed from a Group III element (Group 13 element) such as boron (B) or aluminum (Al). In the case where the p-type floating region 42 is disposed in the n-type drift region 34, depletion of the n-type drift region 34 is promoted, and thus the voltage resistance of the semiconductor device 10 can be further increased.
[0031] The trench 13 extends from the top surface 12a of the semiconductor substrate 12 to the drift region 34 through the source region 40 and the body region 36. The source region 40 is located on opposite sides of the trench 13 and adjacent to the trench 13. The gate electrode 14 in the trench 13 is located on the side of the gate insulating film 14a opposite the source region 40, the body region 36, and the drift region 34. In portions of the body region 36 adjacent to the side surfaces 13a of the trench 13, channels are formed through the gate electrode 14. Although the details will be described below, the floating region 42 is formed by ion implantation of p-type impurities through the bottom surface 13b of the trench 13.During ion implantation, if p-type impurities are implanted into the side surfaces 13a of the trench 13, the impurity concentration in the portions where channels are to be formed inadvertently increases. Therefore, the characteristics (particularly, on-resistance) of the semiconductor device 10 deteriorate. In this regard, with the method for manufacturing the semiconductor device 10 described below, p-type impurities can be prevented from being implanted into the side surfaces 13a of the trench 13 during ion implantation for forming the floating region 42.
[0032] Fig. Figure 2 is a flowchart showing a method for manufacturing the semiconductor device 10 according to the embodiment. First, in step S12, an n-type semiconductor substrate (e.g., a semiconductor wafer) 32 is prepared. Although not particularly limited, a silicon carbide (SiC) substrate is used as the semiconductor substrate 32 in the embodiment. The semiconductor substrate 32 forms the drain region 32, which in Fig. 1, and is thus denoted by the same reference numeral as the drain region 32 for simplicity. Subsequently, in step S14, the n-type drift region 34 is formed on the semiconductor substrate 32 by epitaxial growth of SiC. As described above, the n-type impurity concentration in the drift region 34 is set to be smaller than that in the drain region 32. Subsequently, in step S16, the p-type body region 36 is formed on the drift region 34 by epitaxial growth of SiC.
[0033] Subsequently, in step S18, the p-type contact region 38 is formed in a region including the upper surface 12a of the semiconductor substrate 12. To form the contact region 38, ion implantation of p-type impurities is performed through the upper surface 12a of the semiconductor substrate 12. As described above, the p-type impurity concentration in the contact region 38 is set to be greater than that in the body region 36. Subsequently, in step S20, the n-type source region 40 is formed in a region including the upper surface 12a of the semiconductor substrate 12. To form the source region 40, ion implantation of n-type impurities is performed through the upper surface 12a of the semiconductor substrate 12. As described above, the n-type impurity concentration in the source region 40 is set higher than that in the drift region 34.The steps described above will, as shown in . Fig. 3, the semiconductor substrate 12 is fabricated in which three layers including the drain region 32, the drift region 34 and the body region 36 are stacked on top of each other and in which the contact region 38 and the source region 40 are arranged along the upper surface 12a.
[0034] Subsequently, in step S22, the trench 13 is formed on or in the upper surface 12a of the semiconductor substrate 12. The trench 13 is mainly formed by processes described in the Fig. 4 to 6. First, as shown in Fig. 4, a first oxide film 50 is formed on the upper surface 12a of the semiconductor substrate 12. The first oxide film 50 is, for example, a silicon oxide film and can be formed by chemical vapor deposition using tetraethyl orthosilicate (TEOS) as a source gas. The thickness of the first oxide film 50 can be set to, for example, 1.5 micrometers. In the step (S24) of forming the floating region 42, which will be described below, the first oxide film 50 serves as a mask that restricts implantation of p-type impurities into the upper surface 12a of the semiconductor substrate 12. Therefore, the first oxide film 50 can be formed relatively thick.
[0035] Then, as described in Fig. 5, a resist mask 52 is formed on the first oxide film 50, the resist mask 52 is patterned, and then the first oxide film 50 is etched. As a result, an opening 50a is formed in the first oxide film 50 at a position where the trench 13 is to be formed. The etching of the first oxide film 50 can be a wet etching or a dry etching. After the etching of the first oxide film 50, the resist mask 52 is removed. Subsequently, as shown in Fig. As shown in Figure 6, the semiconductor substrate 12 is etched using the first oxide film 50, in which the opening 50a is formed, as a mask. As a result, the trench 13 is formed in the upper surface 12a of the semiconductor substrate 12. The etching of the semiconductor substrate 12 can be performed, for example, by dry etching using an etching gas containing sulfur hexafluoride (SF6).
[0036] During the etching of the semiconductor substrate 12, the first oxide film 50 is etched simultaneously. Therefore, the thickness of the first oxide film 50 is reduced. As described above, in the step (S24) of forming the floating region 42, which will be described below, the first oxide film 50 serves as a mask for p-type impurities. Accordingly, the thickness of the first oxide film 50 must be maintained at the same level even after the etching of the semiconductor substrate 12. For example, in the embodiment, the desired thickness of the first oxide film 50 after etching is 1.2 micrometers or more. The depth of the trench 13 is 3 micrometers, and the etching selectivity of the semiconductor substrate 12 for the first oxide film 50 is 10. That is, during the formation of the trench 13 having a depth of 3 micrometers, the thickness of the first oxide film 50 is reduced by about 0.3 micrometers.Therefore, the first oxide film 50 is initially formed with a thickness of 1.5 micrometers. As can be seen from the above description, the thickness of the first oxide film 50 can be appropriately adjusted during formation, taking into account the depth of the trench 13, the etch selectivity of the semiconductor substrate 12 for the first oxide film 50, and a respective index (e.g., implantation level) of the ion implantation for forming the floating region 42.
[0037] According to Fig. 2, in the subsequent step S24, the floating region 42 is formed in the semiconductor substrate 12. The floating region 42 is mainly formed by the processes described in the Fig. 7 to 10. First, as shown in Fig. 7, a second oxide film 54 is formed on the side surfaces 13a and the bottom surface 13b of the trench 13. The second oxide film 54 can be uniformly formed not only in the trench 13 but also on the first oxide film 50 disposed on the upper surface 12a of the semiconductor substrate 12. The second oxide film 54 is, for example, a silicon oxide film and can be formed by chemical vapor deposition using tetraethyl orthosilicate (TEOS) as a source gas. In this case, in particular, low-pressure chemical vapor deposition (LP-CVD) has superior step coverage and thickness uniformity, and thus can be advantageously used to form the second oxide film 54.
[0038] During the ion implantation of p-type impurities described below, the second oxide film 54 serves as a mask that prevents p-type impurities from being implanted into the side surfaces 13a of the trench 13. The direction in which p-type impurities penetrate into the semiconductor substrate 12 is perpendicular to the semiconductor substrate 12 (specifically, perpendicular to the bottom surface 12b of the semiconductor substrate 12). Therefore, to prevent p-type impurities from being implanted into the side surfaces 13a of the trench 13, the dimension of the second oxide film 54 disposed on the side surfaces 13a of the trench 13 in the direction perpendicular to the semiconductor substrate 12 is important. In the embodiment, the desired value of the dimension is set to 1.2 micrometers or larger.Accordingly, if it is assumed that the side surfaces 13a of the trench 13 are not perpendicular to the semiconductor substrate 12 and form an angle of 85 degrees with respect to the semiconductor substrate 12, the thickness of the second oxide film 54 must be equal to or greater than 105 nanometers according to the expression “1.2 / tan85° = 0.105 µm = 105 nm”.
[0039] During the dry etching of the second oxide film 54 described below, the second oxide film 54 disposed on the bottom surface 13b of the trench 13 is mainly etched, but the second oxide film 54 disposed on the side surfaces 13a of the trench 13 is also etched simultaneously. Accordingly, the etching size is also taken into account to adjust the thickness of the second oxide film 54 during formation. For example, assuming the etching size is 30 nanometers, the thickness of the second oxide film 54 during formation can be adjusted to 135 nanometers or greater.
[0040] Then, as described in Fig. 8, the second oxide film 54 formed on the bottom surface 13b of the trench 13 is removed by dry etching. Although there is no particular limitation, the second oxide film 54 is removed by dry etching until the bottom surface 13b of the trench 13 is exposed. As a result, an opening 54a through which the bottom surface 13b of the trench 13 is exposed is formed in the second oxide film 54. As shown Fig. As shown in Figure 9, the dry etching of the second oxide film 54 is reactive ion etching, and the etching gas 112 contains octafluorocyclobutane (C4F8), oxygen (O2), and argon (Ar). For example, in the case where the flow rate of octafluorocyclobutane is 20 standard cubic centimeters per minute (sccm), the flow rate of oxygen gas can be set to 10 to 15 sccm, and the flow rate of argon gas can be set to about 300 sccm. That is, the oxygen supply amount is preferably 50 percent to 75 percent of the octafluorocyclobutane supply amount (or other CF-based gas).
[0041] Octafluorocyclobutane is an example of a CF-based gas that has a carbon atom ring structure. Instead of octafluorocyclobutane, or instead of it, another CF-based gas that has a carbon atom ring structure can be used. As another CF-based gas that has a carbon atom ring structure, a CF-based gas represented by any of the chemical formulas C4F6, C4F8, C5F8, and C5HF7 can be used.
[0042] Octafluorocyclobutane (C4F8), a CF-based gas, is a radical-generating gas that chemically reacts with oxygen and atoms (Si, C) forming the semiconductor substrate 12 to produce a reaction product. On the other hand, argon is a gas that contributes ions required for an ion-assisted reaction. The incident angle of ionized argon is relatively small in the second oxide film 54 located on the side surfaces 13a of the trench 13 and relatively large in the second oxide film 54 located on the bottom surface 13b of the trench 13. Due to the variation in the incident angle, the production of the reaction product (i.e., etching) progresses in the second oxide film 54 located mainly on the bottom surface 13b of the trench 13.The reaction product is volatilized from the bottom surface 13b of the trench 13 and then deposited on the second oxide film 54 disposed on the side surface 13a of the trench 13 to form a protective film that protects the second oxide film 54. The protective film is, for example, a fluorocarbon film, contains carbon and fluorine as components, and optionally also contains oxygen.
[0043] At this time, in the case where the CF-based radical-supplying gas has a carbon atom ring structure, the reaction product is less likely to decompose into small molecules and is likely to precipitate. Accordingly, a large amount of the reaction product deposits on the second oxide film 54 disposed on the side surface 13a of the trench 13 before being discharged to the outside of the trench 13. Thus, the protective film is formed even more effectively. As a result, the second oxide film 54 disposed on the side surfaces 13a of the trench 13 is protected, and the second oxide film 54 disposed on the bottom surface 13b of the trench 13 is selectively removed.As a result, the second oxide film 54 can be formed relatively thick on the side surfaces 13a of the trench 13, whereas the second oxide film 54 can be formed extremely thin on the bottom surface 13b of the trench 13 or completely removed from the bottom surface 13.
[0044] As described above, the CF-based gas, which has a carbon atom ring structure, is less likely to decompose. This indicates that the electron density required for the dissociation of the CF-based gas is relatively high, making control of reactive ion etching difficult. In this regard, the embodiment uses a capacitively coupled plasma etching apparatus 100 including two alternating current sources, as shown in Fig. 9. The plasma etching apparatus 100 includes an etching chamber 102 and a pair of electrodes 104, 106 disposed opposite each other in the etching chamber 102, as well as two alternating current sources 108, 110. The electrode 104, located at the bottom, has a step, and the semiconductor substrate 12 is disposed on the electrode 104. The alternating current source 108 is electrically connected to the electrode 104, located at the bottom, and supplies alternating current to the electrode 104. The alternating current source 110 is electrically connected to the electrode 106, located at the top, and supplies alternating current to the electrode 106. The electrode 106, located at the top, must be supplied with electrical energy or power capable of generating a plasma. For example, an alternating current power of 1000 watts or higher can be supplied to the electrode 106. On the other hand, the electrode 104, which is arranged below, must be supplied with electrical energy orPower is supplied to attract ions. If the electrical energy or power supplied to the electrode 104 is excessively high, the formed protective film will be inadvertently etched. Therefore, it is preferable that an AC power of, for example, 600 watts or less be supplied to the electrode 104 located below. The plasma etching apparatus 100 is not limited to the configuration described in the embodiment and may have other configurations.
[0045] In the case where the temperature of the semiconductor substrate 12 is excessively high during reactive ion etching, the protective film deposited on the side surfaces 13a of the trench 13 may be dissociated by thermal energy. Therefore, the temperature of the semiconductor substrate 12 is as low as possible and may be set to, for example, 25 degrees Celsius (°C) or lower. In addition, the internal pressure of the etching chamber 102 is as high as possible to maintain a relatively high electron density and may be set to, for example, 5 Pascals (Pa) or higher. However, various indices of reactive ion etching are not limited to the values described in the specification and may be appropriately changed.
[0046] In reactive ion etching, argon is used as a gas that supplies ions required for an ion-assisted reaction. Generally, a gas that supplies ions, for example, helium (He), is used. However, in the case where helium is used in the embodiment, the dissociation degree of the CF-based gas that supplies radicals becomes excessively high, and thus the formation of the protective film is further suppressed. On the other hand, in the case where argon is used, the dissociation degree of the CF-based gas is limited to within a suitable range, and thus the formation of the protective film can be promoted. That is, in the case where the dissociation degree of the CF-based gas is suitably low, the radical energy is also suitably reduced. Therefore, the reaction product remains in the trench 13 and is likely to be attached to the side surfaces 13a of the trench 13.
[0047] Then, as described in Fig. 10, ions of p-type impurities are implanted through the upper surface 12a of the semiconductor substrate 12. A group of arrows P in Fig. 10 schematically shows p-type impurities implanted into the semiconductor substrate 12. The top surface 12a of the semiconductor substrate 12 and the side surfaces 13a of the trench 13 are covered with the first oxide film 50 or the second oxide film 54. On the other hand, the bottom surface 13b of the trench 13 is exposed through the opening 54a of the second oxide film 54. Accordingly, the p-type impurities pass through the bottom surface 13b of the trench 13 alone and are introduced into the semiconductor substrate 12. As a result, p-type impurities are introduced into a region where the floating region 42 is to be formed. As described above, the second oxide film 54 is formed relatively thick on the bottom surface 13b of the trench 13. As a result, the ion implantation of the p-type impurities can be performed with a relatively high implantation level by selecting a relatively high acceleration energy.For example, in the embodiment, the dimension of the second oxide film 54 in the direction in which the p-type impurities are implanted is 1.2 micrometers or more. Therefore, the acceleration energy can be increased to a maximum of 300 kiloelectronvolts (keV). By further increasing the thickness of the second oxide film 54 disposed on the bottom surface 13b of the trench 13, the acceleration energy can be further increased. As a result, the floating region 42 can be formed at a deeper position. The p-type impurities implanted into the semiconductor substrate 12 are activated by subsequent annealing.
[0048] According to Fig. 2, in the subsequent step S26, the gate electrode 14 is formed in the trench 13. In this step, first, the gate insulating film 14a is formed on the side surfaces 13a and the bottom surface 13b of the trench 13. Subsequently, the gate electrode 14 is formed in the trench 13. Subsequently, the interlayer insulating film 14b is formed such that it covers the gate electrode 14 in the trench 13. Subsequently, in step S28, the source electrode 16 (see Fig. 1) is formed on the upper surface 12a of the semiconductor substrate 12. In step S30, the drain electrode 18 (see Fig. 1) is formed on the lower surface 12b of the semiconductor substrate 12. Subsequently, the semiconductor device 10 is manufactured through various steps such as dicing. Further additional steps may optionally be performed in the method for manufacturing the semiconductor device 10.
[0049] As described above, in the method for manufacturing the semiconductor device 10 according to the embodiment, in the step (S24) of forming the floating region 42, the second oxide film 54 is formed on the side surfaces 13a and the bottom surface 13b of the trench 13, and then the second oxide film 54 is removed from the bottom surface 13b of the trench 13 by dry etching. The dry etching is a reactive ion etching using the etching gas 112 containing CF-based gas having a carbon atom ring structure, oxygen gas, and argon gas. As a result, the second oxide film 54 on the side surfaces 13a of the trench 13 can be formed relatively thick, whereas the second oxide film 54 on the bottom surface 13b of the trench 13 can be formed extremely thin or can be completely removed from the bottom surface 13b.
[0050] The experimental results of measuring the thickness of the second oxide film 54 before and after dry etching are presented with reference to Fig. 11 and Fig. 12, although the results are only examples. As described in Fig. 11, in the experiment, the thickness of the second oxide film 54 before and after dry etching was measured at four positions including: an upper portion (A) of the side surface 13a of the trench 13; an intermediate portion (B) of the side surface 13a of the trench 13; a lower portion (C) of the side surface 13a of the trench 13; and the bottom surface 13b (D) of the trench 13. In addition, in order to investigate effects depending on positions on a semiconductor wafer, the same measurement was performed in the trench 13 located in the central portion of the semiconductor wafer and in the trench 13 located in a peripheral edge portion of the semiconductor wafer. Fig. 12 shows the results. As in Fig. As shown in Fig. 12, it was found that the second oxide film 54 disposed on the bottom surface 13b of the trench 13 is selectively removed, regardless of the positions on or in the semiconductor wafer, compared to the second oxide film 54 disposed on the side surfaces 13a of the trench 13. Specifically, it was found that even in the case where the second oxide film 54 is dry-etched, the second oxide film 54 has a sufficient thickness remaining on the side surfaces 13a of the trench 13 until the second oxide film 54 disposed on the bottom surface 13b of the trench 13 is completely removed.
[0051] The technique described in the embodiment, particularly the method of step (S24) of forming the floating region 42, can be applied not only to the formation of the floating region 42, but also to steps of forming any type of region in semiconductor devices having various other structures. In particular, the technique of the embodiment can be preferably applied to a case where ion implantation of conductive impurities needs to be performed through a bottom surface of a trench formed in a semiconductor substrate.
[0052] The technique described in the embodiment is not limited to a case where the material constituting the semiconductor substrate 12 is silicon carbide. The technique described in the embodiment can be applied, for example, to a case where the material constituting the semiconductor substrate 12 is silicon or another semiconductor material. In the case where the material constituting the semiconductor substrate 12 is silicon, even if conductive impurities are inadvertently implanted into the side surfaces of the trench 13, it is easy to remove the side surfaces 13a of the trench by dry etching or sacrificial oxidation. On the other hand, in the case where the material constituting the semiconductor substrate 12 is silicon carbide, the bonding energy between atoms is relatively high. Therefore, it is difficult to remove the side surfaces 13a of the trench 13 by dry etching or sacrificial oxidation.Therefore, the technique described in the embodiment can be particularly advantageously used for a case where the material constituting the semiconductor substrate 12 is silicon carbide.
Claims
[1] A method of manufacturing a semiconductor device (10), comprising: Producing a semiconductor substrate (12) in which an n-type drain region (32), an n-type drift region (34) and a p-type body region (36) are stacked in this order, and in which a p-type contact region (38) and an n-type source region (40) are arranged along an upper surface (12a) of the semiconductor substrate (12), Forming a trench (13) in the semiconductor substrate (12), the trench extending from the upper surface (12a) of the semiconductor substrate (12) into the drift region (34); Forming an oxide film (54) on side surfaces (13a) and a bottom surface (13b) of the trench (13); Removing at least a portion of the oxide film (54) by dry etching from the bottom surface (13b) of the trench (13), and performing ion implantation of conductive impurities into the semiconductor substrate (12) through the bottom surface (13b) of the trench (13) after dry etching, so that a p-type floating region (42) is formed in the drift region (34), wherein the dry etching is a reactive ion etching using etching gas (112) containing fluorocarbon-based gas having a carbon atom ring structure, oxygen gas, and argon gas. [2] The method according to claim 1, wherein the oxide film (54) is removed by dry etching in the removal of the oxide film (54) until the bottom surface (13b) of the trench (13) is exposed. [3] The method of claim 1 or 2, wherein a capacitively coupled plasma etching apparatus (100) is used for the dry etching, the capacitively coupled plasma etching apparatus (100) including two alternating current sources (108, 110) supplying alternating current to a pair of electrodes (104, 106). [4] The method according to any one of claims 1 to 3, wherein the fluorocarbon-based gas having the carbon atom ring structure is represented by any one of the chemical formulas C4F6, C4F8, C5F8 and C5HF7. [5] The method according to any one of claims 1 to 4, wherein the semiconductor substrate (12) is a silicon carbide substrate. [6] The method according to any one of claims 1 to 5, wherein the oxide film (54) is uniformly formed not only on the side surfaces (13a) and the bottom surface (13b) of the trench (13) but also on the upper surface (12a) of the semiconductor substrate (12) in the formation of the oxide film (54). [7] The method according to any one of claims 1 to 6, wherein the oxide film (54) is formed in the formation of the oxide film (54) such that a dimension of the oxide film (54) disposed on the side surfaces (13a) of the trench (13) in a direction perpendicular to the semiconductor substrate (12) is 1.2 micrometers or more.
Citation Information
Patent Citations
Insulated-gate semiconductor device and its manufacturing method
JP2005116822A
semiconductor memory device
DE3832414A1
Method of avoiding enlargement of top critical dimension in contact holes using spacers
US6803307B1
Insulated gate semiconductor device and method for producing the same
WO2006046388A1