Method for manufacturing a semiconductor device

By using a tin-based solder with copper dissolution to form (Cu,Ni)6Sn5 barriers, the method addresses bond strength issues in semiconductor devices, enhancing durability against high-temperature exposure.

DE102019135860B4Active Publication Date: 2024-11-07DENSO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE102019135860
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-11
Filing Date
2019-12-30
Publication Date
2024-11-07
Estimated Expiration
2039-12-30

AI Technical Summary

Technical Problem

The bond strength between semiconductor elements connected with a nickel layer and solder decreases due to the formation of intermetallic compounds when exposed to high temperatures, leading to potential metal diffusion and weakened connections.

Method used

A manufacturing method where a tin-based solder with added copper is used, allowing copper to dissolve into the solder during melting, forming intermetallic compounds like (Cu,Ni)6Sn5 on the element surfaces, which act as barriers to suppress metal diffusion and strengthen the bond.

Benefits of technology

The method effectively prevents intermetallic compound formation and enhances bond strength by generating (Cu,Ni)6Sn5 barriers, improving the semiconductor device's durability under high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for manufacturing a semiconductor device (10) comprising a plurality of elements incorporating a semiconductor element (12), wherein the method comprises: Arranging a surface (16a, 18a) of a first element (12), which is one of the plurality of elements, and a surface (20a, 24a) of a second element (20, 24), which is another of the plurality of elements, such that they face each other with an interposed tin-based (Sn-based) solder material (52); and Connecting the first element (12) and the second element (20, 24) by melting and solidifying the Sn-based solder material (52), wherein at least one surface (16a, 18a) of the first element (12) is formed from a nickel-based (Ni-based) metal, and at least one surface (20a, 24a) of the second element (20, 24) is made of copper (Cu), and When the first element (12) and the second element (20, 24) are joined, Cu3Sn and (Cu,Ni)6Sn5 are generated in this order on one surface (20a, 24a) of the second element (20, 24) while the Sn-based solder material (52) solidifies, and the generated (Cu,Ni)6Sn5 contains Ni atoms originating from the Ni-based metal, which are dissolved from the first element (12) into the Sn-based solder material (52).
Need to check novelty before this filing date? Find Prior Art

Description

Technical field

[0001] The disclosure relates to a manufacturing process for a semiconductor device. background

[0002] In a semiconductor device, two or more elements, such as a semiconductor element and a leadframe, are joined with solder. When joining two elements with solder, a surface of the element to be joined is provided with a nickel (Ni) layer, such as a conventional Ni plating, to improve solderability. However, if this Ni layer is exposed to high temperatures for an extended period during use of the semiconductor device, it can disappear, forming an intermetallic compound (e.g., Ni3Sn4) between the Ni layer itself and the solder. In this case, the bond strength between the element and the solder decreases.

[0003] JP 2016-92064A describes a semiconductor device in which a semiconductor element and an element are joined with a solder material consisting mainly of tin (Sn). A method for manufacturing this semiconductor device includes: manufacturing the semiconductor element and the element having a surface provided with a nickel layer, the surface of which is provided with a copper (Cu) layer; placing a solder material between the Cu layer and the semiconductor element; and joining the semiconductor element and the element by melting and solidifying the solder material.

[0004] In the manufacturing process described above, Cu in the Cu layer and Sn in the solder material produce Cu6Sn when the molten solder solidifies. son the surface of the Ni layer. The formation of Cu6Sn5 on the surface of the Ni layer suppresses the interdiffusion of Ni atoms in the Ni layer and Sn atoms in the solder material. This prevents the Ni layer from transforming into an intermetallic compound.

[0005] DE 11 2015 003 845 T5 relates to a bond structure that bonds a Cu wiring conductor and a component electrode to each other, wherein the bond structure is arranged between the Cu wiring conductor and the component electrode and comprises a first intermetallic compound layer (a layer of an intermetallic compound of Cu and Sn) formed on the interface with the Cu wiring conductor, a second intermetallic compound layer (a layer of an intermetallic compound of Cu and Sn) formed on the interface with the component electrode, and an intermediate layer present between the intermetallic compound layers.

[0006] DE 11 2017 000 184 T5 relates to a solder joint comprising: a solder joint layer 10, which has a molten solder material containing more than 5.0 wt% and 10.0 wt% or less Sb, 2.0 to 4.0 wt% Ag, more than 0 and 1.0 wt% or less Ni, and a remainder of Sn and unavoidable impurities, and connecting elements, at least one of which is a Cu element or Cu alloying element, wherein the solder joint layer has a first structure containing (Cu, Ni)6(Sn, Sb)s, and a second structure containing (Ni, Cu)3(Sn, Sb) x (in the formula x is 1, 2 or 4) at an intersection with the Cu element or Cu alloy element and contains an electronic component and a semiconductor component that has the solder joint. Summary

[0007] In the manufacturing process of JP 2016-92064A, the supply of Cu from the Cu layer provided on the surface of the Ni layer enables the production of Cu6Sn5 on the surface of the Ni layer. Depending on conditions, such as the melting temperature and melting time of the solder material, Cu in the Cu layer may not be completely depleted, and the Cu layer may be preserved. The present disclosure provides a method for manufacturing a semiconductor device that is capable of suppressing the diffusion of a metal from a surface of an element used in the semiconductor device by employing a different approach than that in JP 2016-92064A. The present disclosure also discloses the semiconductor device itself.

[0008] The present disclosure discloses a method for manufacturing a semiconductor device comprising a plurality of elements, each containing a semiconductor element. The method may include arranging a surface of a first element, which is one of the plurality of elements, and a surface of a second element, which is another of the plurality of elements, such that they face each other with a tin-based (Sn-based) solder material placed between them, and joining the first and second elements by melting and solidifying the Sn-based solder material. At least one surface of the first element is formed from a nickel-based (Ni-based) metal, and at least one surface of the second element is formed from copper (Cu).When the first element and the second element are joined, Cu3Sn and (Cu,Ni)6Sn5 are produced in that order on one surface of the second element as the Sn-based solder material solidifies and the (Cu,Ni)6Sn is produced. s contains Ni atoms originating from the Ni-based metal, which are dissolved from the first element into the Sn-based solder material.

[0009] In the manufacturing process described above, one surface of the first element, formed from the nickel-based metal, and one surface of the second element, formed from copper, are positioned opposite each other, with the tin-based solder material placed between them. The first and second elements are then joined by melting and solidifying the tin-based solder material. In this manufacturing process, copper dissolves from the copper surface of the second element into the tin-based solder material as the tin-based solder material melts during the joining of the first and second elements. The dissolution of copper into the tin-based solder material creates an intermetallic compound containing both copper and tin on the nickel-based surface of the first element as the tin-based solder material solidifies.While the Sn-based solder material solidifies, an intermetallic compound with Cu and Sn is also formed on one surface of the second element.

[0010] In the manufacturing process described above, copper is supplied from one surface of the second element, which is the element to be bonded. This creates the intermetallic compound containing copper and tin on one surface of the first element, which is composed of the nickel-based metal. Furthermore, the intermetallic compound containing copper and tin is also created on one surface of the second element, which is composed of copper. Thus, unlike the technology described in JP 2016-92064A, it is not necessary to separately provide a copper layer to serve as the copper source in the manufacturing process described above. This allows the intermetallic compounds containing copper and tin to be more easily created on the surfaces of the elements. This, in turn, suppresses the diffusion of metal atoms from the surfaces of the elements through the intermetallic compounds.

[0011] The term "soldering material" as used here refers to a material that is not yet melted but is to be melted to join two elements. In contrast, the term "solder layer" as used here refers to a bonding layer that joins two elements and is in a state after the two elements have been joined (i.e., after the soldering material has solidified). Brief description of the drawings Fig. Figure 1 is a cross-sectional view of a semiconductor device 10 according to one embodiment. Fig. Figure 2 is an enlarged view that schematically shows a configuration of a dashed rectangular area II in Fig. 1 represents. Fig. Figure 3 is a diagram describing a step for connecting a semiconductor element 12 and a conductor spacer 20. Fig. Figure 4 is a diagram describing the step for connecting the semiconductor element 12 and the conductor spacer 20. Fig. Figure 5 is a graph showing the dissolution rates of Cu and Ni in a Sn-based soldering material. Fig. Figure 6 is a diagram describing the step for connecting the semiconductor element 12 and the conductor spacer 20. Fig. Figure 7A is a graph showing a relationship between the concentrations of Cu in the Sn-Cu solder 72 before and after joining a Ni layer 70 and the Sn-Cu solder 72. Fig. 7B is an electron microscope image of an interface between the Ni layer 70 and the Sn-Cu solder 72 after their joining (which (i) in Fig. 7A corresponds to). Fig. 7C is an electron microscope image of the interface between the Ni layer 70 and the Sn-Cu solder 72 after their joining (which (ii) in Fig. 7A corresponds to). Fig. 7D is an electron micrograph of the interface between the Ni layer 70 and the Sn-Cu solder 72 after their joining (which (iii) in Fig. 7A corresponds to). Fig. 7E is an electron microscope image of the interface between the Ni layer 70 and the Sn-Cu solder 72 after their joining (which (iv) in Fig. 7A corresponds to). Fig. 8A is an electron microscope image of a compound interface in a sample a after a high-temperature endurance test on the sample a (175°C, 1000 hrs); Fig. 8B is an electron microscope image of a compound interface in a sample b after a high-temperature endurance test on the sample b (175°C, 1000 hrs). Fig. 8C is an electron microscope image of the interface in sample b after a further high-temperature endurance test on sample b (200°C, 1000 hrs). Fig. 9A is an electron microscope image of an interface between a Cu element 80 and the Sn-Ag solder 82 (Sn-3.5Ag) after their joining. Fig. 9B is an electron microscope image of an interface between the Cu element 80 and the Sn-Ag solder 82 (Sn-3.5Ag-0.1Ni) after their joining. Fig. Figure 10 is a diagram showing the flow directions of the electrons and a temperature gradient in the semiconductor element 12. Detailed description

[0012] In one embodiment of the present technology, (Cu,Ni)6Sn5 can be generated on one surface of the first element during the joining of the first and second elements as the tin-based solder material solidifies. As the tin-based solder material melts during the joining of the first and second elements, nickel dissolves into the tin-based solder material from the one surface of the first element formed by the nickel-based metal. This dissolution of nickel into the tin-based solder material allows nickel atoms to replace some of the copper atoms in an intermetallic compound containing copper and tin that is generated on one surface of the first element as the tin-based solder material solidifies. That is, (Cu,Ni)6Sn5 is generated on one surface of the first element.This can appropriately suppress the interdiffusion of Ni atoms, which form one surface of the first element, and Sn atoms, which form the Sn-based solder material.

[0013] In the present technology, when the first and second elements are joined, Cu3Sn and (Cu,Ni)6Sn5 are generated on one surface of the second element in that order as the tin-based solder solidifies. As the tin-based solder melts during the joining process, nickel dissolves into the tin-based solder from the nickel-based metal surface of the first element. This dissolution of nickel into the tin-based solder allows nickel atoms to replace some of the copper atoms in an intermetallic compound containing copper and tin that forms on one surface of the second element as the tin-based solder solidifies. Specifically, Cu3Sn and (Cu,Ni)6Sn5 are generated on one surface of the second element. This (Cu,Ni)6Sn5 then covers the Cu3Sn, thereby suppressing its growth.This can effectively suppress the diffusion of Cu atoms, which form one surface of the second element.

[0014] In one embodiment of the present technology, joining the first and second elements can involve maintaining the temperature of the tin-based solder for a specific period of time within a temperature range higher than the melting point of the tin-based solder. During the joining process, copper dissolves from one surface of the second element into the tin-based solder as the solder melts. Therefore, maintaining the temperature of the tin-based solder as described above allows the copper to dissolve appropriately into the solder.

[0015] In one embodiment of the present technology, while maintaining the temperature of the tin-based solder, the concentration of Cu in the tin-based solder can be increased by dissolving copper from one surface of the second element into the molten tin-based solder. The amount of (Cu,Ni)6Sn5 generated as the tin-based solder solidifies increases with a higher concentration of Cu in the tin-based solder. Therefore, (Cu,Ni)6Sn5 can be suitably generated by increasing the amount of dissolved Cu in the tin-based solder while maintaining the temperature of the tin-based solder as described above.

[0016] In one embodiment of the present technology, the temperature of the tin-based solder material can be maintained under a condition such that the concentration of Cu in the tin-based solder material reaches 0.7 wt% or more. When the concentration of Cu in the tin-based solder material is 0.7 wt% or more, a layer consisting of (Cu,Ni)6Sn can be formed. s The interdiffusion of Ni atoms in the Ni-based metal and the Sn-based solder material (i.e., the formation of an intermetallic compound of Ni and Sn) is sufficiently generated when the first and second elements are joined.

[0017] In one embodiment of the present technology, the temperature of the tin-based solder can be maintained under conditions such that the Cu concentration in the tin-based solder reaches 3.0 wt% or more. According to such a configuration, a large amount of Cu is added to the tin-based solder while maintaining the temperature, allowing the Cu concentration in the tin-based solder to be kept at approximately 0.7 wt% or more until the subsequent joining of the first and second elements is complete. Therefore, the interdiffusion of Ni atoms in the Ni-based metal and Sn atoms in the tin-based solder (i.e., the formation of an intermetallic compound of Ni and Sn) can be further suppressed for almost the entire joining process.

[0018] In one embodiment of the present technology, the first element can be the semiconductor element that includes an electrode, and one surface of the first element can be a surface of the electrode of the semiconductor element.

[0019] Representative, non-limiting examples of the present disclosure are now described in more detail with reference to the accompanying drawings. This detailed description is intended only to provide a person skilled in the art with further details for the application of preferred aspects of the present teaching and is not intended to limit the scope of the present disclosure. Furthermore, each of the additional features and teachings disclosed below can be used individually or in combination with other features and teachings to provide improved semiconductor devices and methods for their use and manufacture.

[0020] Furthermore, combinations of features and steps disclosed in the following detailed description may not be necessary to practice the present disclosure in the broadest sense, but are taught merely to describe representative examples of the present disclosure in a particularly detailed way. Moreover, various features of the representative examples described above and below, as well as of the various independent and dependent claims, can be combined in ways not specifically and explicitly enumerated to provide additional useful embodiments of the present teachings.

[0021] All features disclosed in the description and / or the claims shall be disclosed separately and independently of one another for the purpose of the original written disclosure and for the limitation of the claimed subject matter, irrespective of the combination of features in the embodiments and / or the claims. Furthermore, all ranges of values ​​or statements of groups of things shall disclose any possible intermediate value or intermediate for the purpose of the original written disclosure and for the limitation of the claimed subject matter. embodiment

[0022] Based on the drawings, a semiconductor device 10 is manufactured according to a method for manufacturing the semiconductor device. As in Fig. As shown in Figure 1, the semiconductor device 10 includes a semiconductor element 12, a conductor spacer 20, an upper leadframe 22, a lower leadframe 24 and an insulating resin 26.

[0023] The semiconductor element 12 comprises a semiconductor substrate 14, an upper electrode 16, and a lower electrode 18. In the present embodiment, the semiconductor element 12 is a reverse conducting insulated gate bipolar transistor (RC-IGBT). However, the semiconductor element 12 is not limited to an RC-IGBT and can be a metal-oxide-semiconductor field-effect transistor (MOSFET), a diode, or the like. The semiconductor substrate 14 can be made of any semiconductor material, such as silicon (Si), silicon carbide (SiC), or gallium nitride (GaN).

[0024] The upper electrode 16 is provided on an upper surface 14a of the semiconductor substrate 14. The lower electrode 18 is provided on a lower surface 14b of the semiconductor substrate 14. The upper electrode 16 and the lower electrode 18 are made of a nickel-based (Ni-based) metal. Here, Ni-based metal is defined as any metal that is primarily composed of nickel, and it can be, for example, electroless-plated Ni-P or electroplated Ni. The upper electrode 16 only needs to be made of the Ni-based metal in a region exposed on its upper surface, and the lower electrode 18 only needs to be made of the Ni-based metal in a region exposed on its lower surface.This means that each of the upper electrode 16 and the lower electrode 18 can contain a laminated structure formed from a Ni-based metal layer and another metal layer, such as an aluminum (Al) or aluminum silicon (AlSi) layer.

[0025] The conductor spacer 20 is arranged above the semiconductor element 12. The conductor spacer 20 is connected via a solder layer 28 to an upper surface of the semiconductor element 12 (in particular, the upper surface of the upper electrode 16). The conductor spacer 20 is made of copper (Cu). The conductor spacer 20 only needs to be made of Cu at least on its lower surface.

[0026] The upper leadframe 22 is positioned above the conductor spacer 20. The lower surface of the upper leadframe 22 is connected to an upper surface of the conductor spacer 20 via a solder layer 30. The upper leadframe 22 is made of copper. At least its lower surface of the upper leadframe 22 must be made of copper.

[0027] The lower leadframe 24 is arranged below the semiconductor element 12. The upper surface of the lower leadframe 24 is connected via a solder layer 32 to a lower surface of the semiconductor element 12 (in particular, the lower surface of the lower electrode 18). The lower leadframe 24 is made of copper. The lower leadframe 24 only needs to be made of copper at least on its upper surface.

[0028] The solder layers 28, 30, 32 are formed from a Sn-Cu-based metal in which Cu has been added to the tin (Sn). The concentration of Cu in each of the solder layers 28, 30, 32 is, for example, 0.7 wt% or more, but is not specifically limited to this. Alternatively, the concentration of Cu can be, for example, 1.0 wt% or more, 1.5 wt% or more, 2.0 wt% or more, 2.5 wt% or more, or 3.0 wt% or more.

[0029] Fig. Figure 2 is an enlarged view that schematically shows a configuration of a dashed rectangular area II in Fig. 1 represents. As in Fig. As shown in Figure 2, a first compound layer 40 is provided between the upper electrode 16 and the solder layer 28. In other words, the first compound layer 40 is provided on the Ni-based metal that forms the upper surface of the upper electrode 16. The first compound layer 40 is made of (Cu,Ni)6Sns Furthermore, a second interconnection layer 42 and a third interconnection layer 44 are provided between the conductor spacer 20 and the solder layer 28. The second interconnection layer 42 is provided on the lower surface of the conductor spacer 20, and the third interconnection layer 44 is provided on a lower surface of the second interconnection layer 42. The second interconnection layer 42 is made of Cu3Sn. The third interconnection layer 44 is made of (Cu,Ni)6Sn. s educated.

[0030] A fourth compound layer 46 is provided between the lower electrode 18 and the solder layer 32. In other words, the fourth compound layer 46 is provided on the Ni-based metal that forms the lower surface of the lower electrode 18. The fourth compound layer 46 is made of (Cu,Ni)6Sn sFurthermore, a fifth interconnection layer 48 and a sixth interconnection layer 50 are provided between the lower leadframe 24 and the solder layer 32. The fifth interconnection layer 48 is provided on the upper surface of the lower leadframe 24, and the sixth interconnection layer 50 is provided on the upper surface of the fifth interconnection layer 48. The fifth interconnection layer 48 is made of Cu3Sn. The sixth interconnection layer 50 is made of (Cu,Ni)6Sn. s educated.

[0031] As in Fig. Figure 1 shows a laminate configured with the upper leadframe 22, the conductor spacer 20, the semiconductor element 12, and the lower leadframe 24, covered with the insulating resin 26. The entire surface of the laminate, except for the upper surface of the upper leadframe 22 and the lower surface of the lower leadframe 24, is covered with the insulating resin 26. The insulating resin 26 is made of a thermosetting resin, such as an epoxy resin. The upper surface of the upper leadframe 22 and the lower surface of the lower leadframe 24 are connected to a cooler (not shown). That is, the semiconductor device 10 of the present embodiment includes a so-called double-sided cooling structure, which enables cooling of both the upper and lower surfaces of the insulating resin 26.The semiconductor device 10 can include a one-sided cooling structure in which either the upper surface of the upper leadframe 22 or the lower surface of the lower leadframe 24 is exposed by the insulating resin 26.

[0032] Then, with reference to the Fig. Sections 3 to 6 describe a method for manufacturing the semiconductor device 10. In particular, a method for joining the semiconductor element 12 and the conductor spacer 20 with solder is described below. A method for joining the semiconductor element 12 and the lower leadframe 24 in Fig. 1 is similar to the method for connecting the semiconductor element 12 and the conductor spacer 20, so its description is omitted. Furthermore, the conductor spacer 20 and the upper leadframe 22 can be connected according to the method described below or according to a conventionally known method.

[0033] First, as in Fig. Figure 3 shows the semiconductor element 12 and the conductor spacer 20 arranged opposite each other, with a tin-based solder material 52 positioned between them. Specifically, the semiconductor element 12 and the conductor spacer 20 are arranged such that an upper surface (nickel-based metal) 16a of the upper electrode 16 of the semiconductor element 12 faces a lower surface 20a of the conductor spacer 20a, and the tin-based solder material 52 is positioned between them. The term "tin-based solder material" here refers to a solder material that is primarily composed of tin and is, for example, a solder material to which a certain amount of copper has been added. The concentration of copper in the tin-based solder material 52 may be lower than the concentration of copper in a conventional solder material, as will be described in detail later. Furthermore, the tin-based solder material 52 may optionally contain no copper.The upper surface 16a of the upper electrode 16 can be covered with another metal layer, such as a gold (Au) or silver (Ag) layer, to prevent corrosion of the Ni-based metal. In a subsequent joining step, such a metal layer diffuses into the Sn-based solder material 52 while the Sn-based solder material 52 is melted.

[0034] The joining step is then performed on a laminate 100, which consists of the semiconductor element 12, the tin-based solder material 52, and the conductor spacer 20. In the joining step, the laminate 100 is first heated, as shown in Fig. Figure 4 illustrates this process. The laminate 100 is heated to a specific temperature such that the tin-based solder material 52 melts. That is, the tin-based solder material 52 is heated to its melting temperature (liquid phase point) or higher. Before heating to the melting temperature or higher, the laminate 100 can be heated for a specific period of time to a temperature slightly lower than the melting temperature. That is, a pre-joining step can be performed in which the laminate 100 is heated until the entire laminate 100 has an approximately uniform temperature. By performing the pre-joining step, it is less likely that the tin-based solder material 52 will have a temperature difference when heated to its melting temperature or higher and can be melted at an approximately uniform temperature.

[0035] When the Sn-based solder material 52 is melted, Cu from the lower surface 20a of the conductor spacer 20 begins to dissolve into the Sn-based solder material 52, as shown by the arrows 102 in Fig. 4 show. Furthermore, when the Sn-based solder material 52 melts, the Ni-based metal from the upper surface 16a of the upper electrode 16 of the semiconductor element 12 begins to dissolve into the Sn-based solder material 52, as shown by arrows 104 in Fig. Figure 4 shows that the melting points of Cu and the Ni-based metal are higher than the melting point of the Sn-based solder 52. However, when the Sn-based solder 52 is melted, the Cu and the Ni-based metal in contact with it begin to dissolve into the Sn-based solder 52. Specifically, when the Sn-based solder 52 is melted at a certain temperature, the Cu and the Ni-based metal continue to dissolve into the Sn-based solder 52 until they saturate it at that temperature. This involves maintaining a temperature at which the Sn-based solder 52 is in a molten state (hereafter referred to as the heating temperature) until a certain amount of Cu dissolves into the Sn-based solder 52.For example, the heating temperature is maintained until the concentration of Cu in the Sn-based solder material 52 reaches 3.0 wt%. Alternatively, the heating temperature can be maintained until the concentration of Cu reaches, for example, 3.5 wt%, 4.0 wt%, 4.5 wt%, or 5.0 wt%.

[0036] Fig. Figure 5 shows the dissolution rates of Cu and Ni into the Sn-based solder material 52 at each temperature T. As in Fig. As shown in Figure 5, the dissolution rate of Cu is approximately 40 times higher than the dissolution rate of Ni. Since the dissolution rate of Cu is higher than that of the Ni-based metal, the amount of Cu dissolving into the Sn-based solder material 52 from the conductor spacer 20 is greater than the amount of Ni-based metal dissolving into the Sn-based solder material 52 from the upper electrode 16. Therefore, the amount of Ni-based metal dissolving into the Sn-based solder material 52 is relatively small. As shown in Fig. As shown in Figure 5, the dissolution rate of Cu, for example, in a case where the Sn-based solder material 52 is melted at approximately 230°C, is about 0.1 µm / sec. Therefore, maintaining the temperature at approximately 230°C for about 40 seconds in the present embodiment allows the amount of Cu to dissolve into the Sn-based solder material 52 to be about 3.0 wt%. Furthermore, the dissolution rate of Cu, for example, in a case where the Sn-based solder material 52 is melted at approximately 300°C, is about 0.4 µm / sec. Therefore, maintaining the temperature at approximately 300°C for about 10 seconds in the present embodiment allows the amount of Cu to dissolve into the Sn-based solder material 52 to be about 3.0 wt%. Thus, the heating temperature and the time period for holding the heating temperature can be set so that the concentration of Cu in the Sn-based solder material 52 reaches a target value.

[0037] Subsequently, heat is extracted from the laminate 100 to solidify the molten tin-based solder material 52. Cu, which detached from the conductor spacer 20 during the melting step of the tin-based solder material 52, moves to the upper surface 16a of the upper electrode 16 of the semiconductor element 12. Then, as in Fig. 6 shown, while the Sn-based solder material 52 solidifies, (Cu,Ni)6Sn s(Reference numeral 40) is generated on the upper surface 16a of the upper electrode 16. This process firmly bonds the semiconductor element 12 and the solder layer 28 (i.e., the solidified Sn-based solder material 52). This (Cu,Ni)6Sn5 covers the upper surface 16a (the Ni-based metal) of the upper electrode 16, thereby acting as a barrier layer that suppresses the interdiffusion of Ni in the upper electrode 16 and Sn in the solder layer 28 (i.e., the formation of Ni3Sn4).

[0038] Furthermore, Ni, which detached from the upper electrode 16 during the melting step of the Sn-based solder material 52, moves to the lower surface 20a of the conductor spacer 20. Then, as in Fig. 6 shown, while the Sn-based solder material 52 solidifies, Cu3Sn (reference numeral 42) and (Cu,Ni)6Sn s(Reference numeral 44) is generated on the lower surface 20a of the conductor spacer 20. This results in a strong bond between the conductor spacer 20 and the solder layer 28 (i.e., the solidified tin-based solder material 52). This (Cu,Ni)6Sn5 covers the lower surface 20a of the conductor spacer 20, thereby acting as a barrier layer that suppresses the growth of Cu3Sn.

[0039] As described above, the laminated structure of the semiconductor element 12 and the conductor spacer 20 with the intermediate solder layer 28, as shown in the above, can be produced by the steps described above. Fig. 1 and Fig. Figure 2 shows how this can be achieved. As mentioned earlier, the semiconductor element 12 and the lower leadframe 24 can be connected via the solder layer 32 by performing steps similar to those described above. That is, by following steps similar to those described above, a Fig. The layer structure shown in section 2 is obtained, in which (Cu,Ni)6Sn s (reference 46) is produced on a lower surface 18a of the lower electrode 18 of the semiconductor element 12 and Cu3Sn (reference 48) and (Cu,Ni)6Sn5 (reference 50) are produced on an upper surface 24a of the lower leadframe 24.

[0040] As described above, in the manufacturing process of the present invention, the lower surface 20a of the conductor spacer 20, which is one of the elements to be joined, provides Cu for the generation of (Cu,Ni)6Sn5 on the upper surface 16a of the upper electrode 16, which is formed from the Ni-based metal. This eliminates the conventional need to provide a separate Cu layer to serve as a Cu source. Accordingly, (Cu,Ni)6Sn5 can be more easily generated on the upper surface 16a of the upper electrode 16. Since (Cu,Ni)6Sn5 acts as a barrier for the upper surface 16a of the upper electrode 16, the diffusion of Ni atoms from the upper surface 16a of the upper electrode 16 can be suppressed.

[0041] Furthermore, in the manufacturing process of the present embodiment, Cu is supplied by the conductor spacer 20 while the Sn-based solder material 52 is being melted. The concentration of Cu in the Sn-based solder material 52 thus increases as it melts. Therefore, even if the concentration of Cu in the Sn-based solder material 52 is relatively low before the joining step, a desired amount of (Cu,Ni)6Sn5 can be produced on the upper surface 16a of the upper electrode 16. Sn-based solder with a higher concentration of Cu has a higher melting point. In the manufacturing process of the present embodiment, the concentration of Cu in the Sn-based solder material 52 can be set low before the joining step, which allows the melting point of the Sn-based solder material 52 to be low. This reduces the energy consumption required for the joining step.Furthermore, the impact on various elements that are heated together with the Sn-based solder material 52 can be mitigated.

[0042] Furthermore, saturated solubility in the tin-based solder 52 depends on the melting temperature of the tin-based solder 52. Therefore, by adjusting the melting temperature of the tin-based solder 52, the amount of copper supplied by the conductor spacer 20 can be controlled. This can prevent excessive copper consumption by the conductor spacer 20.

[0043] Next, the concentration of copper in the solder layer after the joining step will be discussed. Fig. Figures 7A to 7E show results of experiments carried out by the inventor of the present disclosure. Fig. Figure 7A shows a relationship between the concentrations of Cu in solder 72, which is formed from a Sn-Cu-based metal (hereinafter referred to as Sn-Cu solder 72), before and after joining a Ni layer 70 and the Sn-Cu solder 72 (i.e., before the Sn-Cu solder 72 melts and after it solidifies (after joining)). Furthermore, the Fig. 7B to 7E Electron microscope images of an interface between the Ni layer 70 and the Sn-Cu solder 72 after their joining or for concentrations of Cu at points (i) to (iv) in Fig. 7A. These experiments were carried out using a Ni-P electroless plating layer as Ni-layer 70.

[0044] As in the Fig. As shown in Figures 7B to 7D, it was confirmed that when the concentration of Cu in the Sn-Cu solder 72 after joining was less than 0.7 wt%, not only (Cu,Ni)6Sn5 but also (Ni,Cu)3Sn4 was formed at the joint interface. On the other hand, as shown in Fig. Figure 7E shows that when the concentration of Cu in the Sn-Cu solder 72 was 0.7 wt% or more after joining, no (Ni,Cu)3Sn4 was produced at the joining interface and only (Cu,Ni)6Sn5 was produced there.

[0045] The experimental results confirmed that even when the concentration of Cu in the Sn-Cu solder 72 is less than 0.7 wt% after joining, (Cu,Ni)6Sn5, which acts as a barrier layer, is formed. The influence of (Ni,Cu)3Sn4, which is formed when the concentration of Cu in the Sn-Cu solder 72 is less than 0.7 wt% after joining, on the joint interface is then discussed further.

[0046] The Fig. Figures 8A to 8C show the results of experiments conducted by the inventor. For these experiments, a sample a and a sample b were prepared. In sample a, (Ni,Cu)3Sn4 was produced at a bonding interface between the Sn-Cu solder 72 and a Cu element 68, the surface of which was provided with the Ni layer 70. In sample b, (Cu,Ni)6Sn5 was produced at a bonding interface between the Sn-Cu solder 72 and the Cu element 68, the surface of which was provided with the Ni layer 70. These samples were then subjected to a high-temperature endurance test, in which the samples were stored for 1000 hours under a high-temperature atmosphere of 175°C. In addition, sample b was subjected to a further high-temperature endurance test, in which the sample was placed for 1000 hours under a high-temperature atmosphere of 200°C. Fig. Figures 8A to 8C show electron microscope images of the interfaces in the samples after the high-temperature endurance tests on the samples.

[0047] In sample a, as from Fig. As can be seen in sample 8A, the Ni layer 70 almost completely disappeared after the high-temperature endurance test at 175°C for 1000 hours. Furthermore, it was confirmed that a Ni3SnP layer was formed and a phosphorus-rich layer (Ni3P layer) grew significantly. The thickness of the phosphorus-rich layer was correlated with the amount of Ni consumed from the Ni layer 70, and a greater thickness of the phosphorus-rich layer indicates that a greater amount of Ni was consumed from the Ni layer 70. In contrast, in sample b, as shown in the Fig. 8B and Fig. The detection of 8C confirms that the Ni layer 70 was preserved and that the growth of the P-rich layer was suppressed even after the high-temperature endurance tests at 175°C for 1000 hours and at 200°C for 1000 hours. These results lead to the conclusion that in a semiconductor device incorporating a connection interface where only (Cu,Ni)6Sn5 is provided between the Ni layer 70 and the Sn-Cu solder 72, the disappearance of the Ni layer 70 can be suppressed, and thus the semiconductor device can adequately withstand repeated heat generation caused by its operation.

[0048] As described above, a suitable barrier layer can be produced by adjusting the concentration of Cu in the solder layer 28 (the Sn-based solder material 52 after solidification) to 0.7 wt% or more. The concentration of Cu in the solder layer 28 can be adjusted by setting a dissolution rate of Cu in the Sn-based solder material 52 during the joining step. As described in Fig. As shown in Figure 7A, if the solder material has a Cu concentration of approximately 3.2 wt% or more before melting, the Cu can remain at a concentration of 0.7 wt% or more. In this case, during the joining step, while the Sn-based solder material 52 is melting, Cu dissolves from the conductor spacer 20 into the Sn-based solder material 52, and (Cu,Ni)6Sn5 begins to form on the upper surface 16a of the upper electrode 16. That is, while the Sn-based solder material 52 is melting, the supply of Cu from the conductor spacer 20 and the consumption of Cu through the formation of (Cu,Ni)6Sn5 can occur simultaneously. Therefore, by increasing the Cu concentration to approximately 3.0 wt% or more while the Sn-based solder material 52 is melting in the joining step, the solder layer 28 with a Cu concentration of 0.7 wt% or more can be achieved.

[0049] Next, an intermetallic compound is discussed that is formed at a connection interface between the conductor spacer 20 and the solder layer 28. Fig. 9A and Fig. Figures 9B each show an electron microscope image of a bonding interface between a Cu element 80 and the solder 82, which is formed from a Sn-Ag-based metal (hereinafter referred to as Sn-Ag solder 82) (cited from CE Ho, SC Yang and CR Kao: J. Mater. Sci.: Mater. Electron. 18 (2007) 155-174). For the Sn-Ag solder 82 in Fig. In 9A, a Sn-3.5Ag solder is used, in which 3.5 wt% Ag has been added to the Sn. Meanwhile, for solder 82 in Fig. 9B Sn-3,5Ag-0,1Ni, in which 3.5 wt% Ag and 0.1 wt% Ni were added to the Sn, is used as soldering material.

[0050] As in Fig. As shown in 9A, when using the Sn-Ag solder 82, which does not contain Ni, Cu3Sn and Cu6Sn are formed in this order. s on an upper surface of the Cu element 80. On the other hand, as in Fig. As shown in Figure 9B, when using the Sn-Ag solder 82 to which Ni is added, (Cu,Ni)6Sn5 is formed instead of Cu6Sn5. Fig. 9A is produced. That is, a layer in which Ni atoms replace some of the Cu atoms in Cu6Sn. s have been substituted. Furthermore, when focusing on the Cu3Sn layers, a thickness of Cu3Sn in Fig. 9A greater than a thickness of Cu3Sn in Fig. 9B. As such, it can be understood that the addition of Ni to the solder material results in the production of (Cu,Ni)6Sn s and the presence of (Cu,Ni)6Sn5 suppresses the growth of Cu3Sn.

[0051] It is known that at a junction between a copper (Cu) and a tin (Sn) element, the diffusion rate of Cu in Sn is much higher than the diffusion rate of Sn in Cu. For this reason, an intermetallic compound with the composition Cu3Sn, as described above, is formed between the Cu and Sn elements. At this point, due to the unbalanced interdiffusion of Cu and Sn across the junction, atomic vacancies are created in the Cu element at the interface between the Cu element and Cu3Sn. If these atomic vacancies accumulate without disappearing, a so-called Kirkendall vacancy is formed. The formation of a Kirkendall vacancy leads to a decrease in bond strength. Therefore, the growth of Cu3Sn should be suppressed.

[0052] As described above, if a layer consisting of (Cu,Ni)6Sn sSince (Cu,Ni)6Sn5 is formed on a Cu3Sn surface, it acts as a barrier layer, thus suppressing the growth of Cu3Sn. In the manufacturing process of the present embodiment, the upper surface 16a of the upper electrode 16 of the semiconductor element 12, which is one of the elements to be joined, supplies Ni to generate (Cu,Ni)6Sn5 on the lower surface 20a of the Cu-based conductor spacer 20. By dissolving Ni into the Sn-based solder material 52, Cu3Sn and (Cu,Ni)6Sn5 are generated in that order on the lower surface 20a of the conductor spacer 20. Because (Cu,Ni)6Sn5 is generated on a Cu3Sn surface, the growth of Cu3Sn is suppressed.As a result, the Kirkendall vacancy is less likely to be generated in the manufacturing process of the present embodiment, and a suitable bond strength can be achieved between the conductor spacer 20 and the solder layer 28. Cu3Sn can also grow due to repeated heat generation from operation of the semiconductor device. However, since (Cu,Ni)6Sn. s In the semiconductor device 10 of the present embodiment, the interdiffusion of Cu and Sn is suppressed and the growth of Cu3Sn is suppressed.

[0053] In the embodiment described above, an RC-IGBT is used for the semiconductor element 12. It is generally a known problem that in a semiconductor device, the atomic diffusion described above is caused by electromigration (hereinafter referred to as EM) or thermomigration (hereinafter referred to as TM), and that an electrode is thereby damaged. EM is caused by an electron flow in the electrode, and the EM level rises according to a temperature and current density. TM is caused by a temperature gradient across the electrode and an adjacent component (e.g., solder layer), and the TM level rises according to a temperature and the temperature gradient.

[0054] As in Fig.As shown in Figure 10, in the semiconductor element 12, which, as in the present embodiment, includes an IGBT region 90 and a diode region 92, when functioning as an IGBT, a direction in which electrons flow coincides with a direction of the temperature gradient on a lower electrode side 18 (a receiver electrode side), as shown in a dashed line region 94. Accordingly, it is likely that both EM and TM will cause damage to the lower electrode 18. When the semiconductor element 12 functions as a diode, a direction in which electrons flow coincides with a direction of the temperature gradient on an upper electrode side 16 (i.e., an anode electrode side), as shown in a dashed line region 96. Accordingly, it is likely that both EM and TM will cause damage to the upper electrode 16.Therefore, the technology disclosed herein is particularly useful when applied to a semiconductor device that includes a region in which atoms can diffuse due to EM and TM. (Correspondence relationships)

[0055] The semiconductor element 12 is an example of a “first element”. The conductor spacer 20 and the lower leadframe 24 are examples of a “second element”. The upper surface 16a of the upper electrode 16 and the lower surface 18a of the lower electrode 18 are examples of a “surface of a first element”. The lower surface 20a of the conductor spacer 20 and the upper surface 24a of the lower leadframe 24 are examples of a “surface of a second element”.

Claims

[1] A method of manufacturing a semiconductor device (10) comprising a plurality of elements including a semiconductor element (12), the method comprising: Arranging a surface (16a, 18a) of a first element (12), which is one of the plurality of elements, and a surface (20a, 24a) of a second element (20, 24), which is another of the plurality of elements, so that they face each other with a tin-based (Sn-based) solder material (52) arranged therebetween; and Joining the first element (12) and the second element (20, 24) by melting and solidifying the Sn-based solder material (52), wherein at least one surface (16a, 18a) of the first element (12) is formed from a nickel-based (Ni-based) metal, and at least one surface (20a, 24a) of the second element (20, 24) is formed of copper (Cu), and when joining the first element (12) and the second element (20, 24), Cu3Sn and (Cu,Ni)6Sn5 are produced in this order on one surface (20a, 24a) of the second element (20, 24) while the Sn-based solder material (52) is solidifying, and the produced (Cu,Ni)6Sn5 contains Ni atoms originating from the Ni-based metal which are dissolved from the first element (12) into the Sn-based solder material (52). [2] The method of claim 1, wherein in joining the first member (12) and the second member (20, 24), (Cu,Ni)6Sn5 is generated on the one surface (16a, 18a) of the first member (12) while the Sn-based solder material (52) solidifies. [3] The method of claim 1 or 2, wherein joining the first member (12) and the second member (20, 24) comprises maintaining a temperature of the Sn-based solder material for a predetermined period of time within a temperature range higher than a melting temperature of the Sn-based solder material (52). [4] The method of claim 3, wherein maintaining the temperature of the Sn-based solder material (52) comprises increasing a concentration of Cu in the Sn-based solder material (52) by dissolving copper from the one surface (20a, 24a) of the second member (20, 24) into molten Sn-based solder material (52). [5] The method according to claim 4, wherein maintaining the temperature of the Sn-based solder material (52) is performed under the condition that the concentration of Cu in the Sn-based solder material reaches 0.7 mass% or more. [6] The method according to claim 4, wherein maintaining the temperature of the Sn-based solder material (52) is performed under the condition that the concentration of Cu in the Sn-based solder material reaches 3.0 mass% or more. [7] The method according to any one of claims 1 to 6, wherein the first element is the semiconductor element (12) including an electrode (16, 18), and the one surface of the first element is a surface (16a, 18a) of the electrode (16, 18) of the semiconductor element (12).

Citation Information

Patent Citations

  • bond structure, bond material and bonding process

    DE112015003845T5

  • solder joint

    DE112017000184T5

  • Semiconductor device and manufacturing method of the same

    JP2016092064A

  • Semiconductor device and method of manufacturing semiconductor device