EDGE TRIM METHOD FOR WAFER BONDING AND UNIONING

The pre-bonding edge trimming process for semiconductor wafers addresses inefficiencies in existing methods by reducing edge cutting volume, leading to lower processing costs and tool wear, and achieving a smooth profile during bonding and separation.

DE102020110287B4Active Publication Date: 2024-10-24TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
DE102020110287
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2020-04-15
Publication Date
2024-10-24
Estimated Expiration
2040-04-15

AI Technical Summary

Technical Problem

Existing edge trimming methods for semiconductor wafers during bonding and separation are inefficient, leading to high processing costs, long processing times, and tool wear due to multiple edge trimming processes, which can cause film peeling and splintering.

Method used

A pre-bonding edge trimming process is performed on semiconductor wafers to minimize the volume of edge trims, reducing the depth and width of edge cutting significantly, followed by a post-bonding edge trimming process to achieve a smooth profile, thereby minimizing material removal and tool wear.

Benefits of technology

This approach reduces processing time and costs while extending tool lifespan by minimizing material removal and preventing chipping or flaking during the bonding and separation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for forming a semiconductor structure, comprising: edge trimming (1610) of a front peripheral region of a first wafer (100) by performing a pre-bonding edge trimming process; bonding (1620) of a front surface of the first wafer (100) to a front surface of a second wafer (200); thinning (1630) of a back side of the first wafer (100) by performing at least one wafer thinning process, wherein the at least one wafer thinning process comprises: a first wafer thinning process that thins the first wafer (100) to a first thickness (t1) greater than a first edge-cutting depth (td1); and a second wafer thinning process which thins the first wafer (100) to a second thickness (t2) which is less than the first edge cutting depth (td1) and wherein the first wafer thinning process includes a wafer grinding process and the second wafer thinning process includes an isotropic etching process;and edge trimming (1640) of the first wafer (100) and a front peripheral region of the second wafer (200) by performing a post-bonding edge trimming process.;
Need to check novelty before this filing date? Find Prior Art

Description

GENERAL STATE OF THE ART

[0001] Wafer thinning is used in conjunction with wafer bonding to provide a semiconductor chip that a vertical stack of at least two semiconductor dies. A first wafer comprising first semiconductor devices can be bonded to a second wafer having second semiconductor devices. One of the two Bonded wafers can be thinned after bonding. Bonded and thinned semiconductor wafers can subsequently singulated to form multiple semiconductor chips that offer higher density, multiple functions and / or faster operating speed, which can be achieved by vertical bonding of at least two semiconductor dies Edge regions of a wafer that do not have bonded portions of the semiconductor dies can be edge trimmed during a wafer thinning process to prevent the bonded wafer assembly. Previous edge trimming methods typically use multiple Edge trimming processes after grinding the backside of one of the two wafers in a bonded assembly. Multiple edge trimming processes use a sequential reduction of an edge offset to achieve a to prevent chipping of the wafer. Such wafer edge trimming processes can eliminate more sources of film peeling and have additional problems such as short trim life, long Edge trimming process duration, high processing costs and high demands on Edge trimming tool performance. The document US2014 / 0024170 A1 discloses a method for forming upper metal lines over a semiconductor substrate, with the back of the substrate being formed by processes such as grinding, chemical-mechanical polishing or wet etching. The document US 2005 / 0215056 A1 discloses a Bonded wafer processing method comprising etching the first wafer, bonding the first wafer to a second wafer and thinning the first wafer. US 2008 / 0044984 A1 discloses a method for Forming backlit devices using a pre-ground blade to produce a straight edge around the wafer perimeter or to remove a part of the wafer edge ring that is subject to poor connection quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0002] Aspects of the present disclosure are best understood from the following detailed description in in conjunction with the accompanying drawings. It should be noted that, in accordance with industry practice, various features are not shown to scale. In fact, the dimensions of the various Features may be arbitrarily enlarged or reduced for the sake of clarity. Fig. 1A is a vertical cross-sectional view of a first wafer according to a first embodiment of the this disclosure. Fig. 1B is a top view of the first wafer of Fig. 1A. Fig. 1C is an enlarged vertical cross-sectional view of region C of Fig. 1A. Fig. 2A is a vertical cross-sectional view of the first wafer after a first edge trimming process according to the first embodiment of the present disclosure. Fig. 2B is a top view of the first wafer of Fig. 2A. Fig. 3A is a vertical cross-sectional view of a second wafer according to the first embodiment of the this disclosure. Fig. 3B is a top view of the first wafer of Fig. 3A. Fig. 4A is a vertical cross-sectional view of a first exemplary structure after bonding the first wafer to the second wafer according to the first embodiment of the present disclosure. Fig. 4B is a top view of the first example structure of Fig. 4A. Fig. 5A is a vertical cross-sectional view of the first exemplary structure according to a first Thinning process that grinds the back side of the first wafer according to the first embodiment of the this disclosure. Fig. 5B is a top view of the first example structure of Fig. 5A. Fig. 6A is a vertical cross-sectional view of the first exemplary structure after a second Thinning process that thins the first wafer according to the first embodiment of the present Revelation. Fig. 6B is a top view of the first example structure of Fig. 5A. Fig. 7A is a vertical cross-sectional view of the first exemplary structure after performing a final edge trimming process according to the first embodiment of the present Revelation. Fig. 7B is a top view of the first example structure of Fig. 7A. Fig. 7C is an enlarged vertical cross-sectional view of a peripheral region of the first exemplary Structure of Fig. 7A and Fig. 7B. Fig. 8 is an enlarged vertical cross-sectional view of the first exemplary structure after formation of Substrate via cavities according to the first embodiment of the present disclosure. Fig. 9 is an enlarged vertical cross-sectional view of the first exemplary structure after formation of Substrate via structures and rear bonding pads according to the first embodiment of the this disclosure. Fig. 10A is a vertical cross-sectional view of the first exemplary structure in the processing step of a Die singulation according to the first embodiment of the present disclosure. Fig. 10B is a top view of the first example structure of Fig. 10A. Fig. 11A is a vertical cross-sectional view of a second wafer after a second Edge trimming process according to a second embodiment of the present disclosure. Fig. 11B is a top view of the first wafer of Fig. 11A. Fig. 12A is a vertical cross-sectional view of a second exemplary structure after bonding the first wafer to the second wafer according to the second embodiment of the present disclosure. Fig. 12B is a top view of the second exemplary structure of Fig. 12A. Fig. 13A is a vertical cross-sectional view of the second exemplary structure according to a first Thinning process that grinds the back side of the first wafer according to the second embodiment of the this disclosure. Fig. 13B is a top view of the second exemplary structure of Fig. 13A. Fig. 14A is a vertical cross-sectional view of the second exemplary structure according to a second Thinning process that thins the first wafer according to the second embodiment of the present Revelation. Fig. 14B is a top view of the second exemplary structure of Fig. 14A. Fig. 15A is a vertical cross-sectional view of the second exemplary structure after performing a final edge trimming process according to the second embodiment of the present Revelation. Fig. 15B is a top view of the second exemplary structure of Fig. 15A. Fig. 16 is a first flowchart showing steps for forming an exemplary structure according to a embodiment of the present disclosure. Fig. 17 is a second flowchart showing steps for forming an exemplary structure according to a embodiment of the present disclosure. DETAILED DESCRIPTION

[0003] The following disclosure provides many different embodiments or examples for implementing various features of the provided article. Specific examples of components and arrangements are described below to simplify the present disclosure. These are, of course, merely examples and not intended as a limitation. For example, the formation of a first feature over or on a second feature in the following description contains embodiments in which the first and second features are in direct contact formed, and may also include embodiments in which additional features are arranged between the first and second feature, so that the first and second feature may not be in direct contact. In addition, the present disclosure may use reference numbers and / or letters in the various examples This repetition serves the purpose of simplicity and clarity and does not itself imply any relationship between the various discussed embodiments and / or configurations.

[0004] Furthermore, spatial terms such as ´´below´´, ´´beneath´´, ´´lower´´, ´´above´´, ´´upper´´ and the like are used here for simple description to indicate a relationship of an element or feature to a or several other element(s) or feature(s) shown in the figures. The Spatial terms are intended to describe different orientations of the device in use or operation in addition to the orientation shown in the figures. The device can be oriented differently (90 degrees or in other orientations) and the spatial descriptors used here can also be be interpreted accordingly.

[0005] The present disclosure relates generally to semiconductor devices and, more particularly, to a method for Edge trimming of wafers during a wafer bonding and dicing process.

[0006] In general, the methods of the present disclosure minimize the volume of edge-trimmed Sections of semiconductor substrates during a wafer bonding process. A front peripheral section of a first semiconductor substrate can be edge trimmed in a pre-bonding edge trimming process without Edge trimming of a rear peripheral portion of the first semiconductor substrate. Compared with a A method according to the prior art in which an entire periphery of a semiconductor substrate is bonded to a other substrate and before thinning the semiconductor substrate, the depth of a Edge trimming into the first semiconductor substrate can be significantly smaller, such as less than 50 micrometers. As such the volume of a peripheral portion of the first semiconductor substrate which is formed during the pre-bonding edge trimming process of the present disclosure can be significantly reduced. For example, a typical state-of-the-art edge trimming process performed on a bonded pair of wafers with a diameter of 450 mm with an edge cutting width of about 3 mm, a removal volume 3 3 of π × 450 mm × 3 mm × 0.825 mm ≅ 3.500 mm = 3.5 cm for one of the two bonded wafers. Comparison, a pre-bonding edge trimming process on a 450 mm diameter wafer with a Edge trimming depth of 30 micrometers and an edge cutting width of 3 mm according to a Illustrative example of an embodiment of the present disclosure removes only π × 450 mm × 3 mm × 3 3 0.030 mm ≅ 127 mm = 0.127 cm . As such, the methods of the present disclosure can reduce the amount of Such a reduction in the amount of cut material sections of a wafer. Material sections reduces the processing time and processing costs for the wafer Edge trimming processes used during a bonding process and increases the lifetime of a Edge cutting tool.

[0007] Furthermore, in various embodiments, peripheral portions of material layers located at Bonding sides of the wafers are effectively removed before bonding a pair of wafers. In one embodiment a second semiconductor substrate to be bonded to the first semiconductor substrate may optionally be bonded to the first semiconductor substrate. Material sections located at peripheral portions of the semiconductor wafers and have weaker adhesion to the semiconductor substrates, can be bonded during Pre-bonding edge trimming processes can be removed. Thus, the pre-bonding edge trimming processes Reduce chipping or flaking of material sections during or after the wafer bonding process. Various features and aspects of the methods of the present disclosure will now be described in detail under Described with reference to the drawings.

[0008] Referring to Figs. 1A-1C, a first wafer 100 according to an embodiment of the present disclosure. The first wafer 100 includes a first semiconductor substrate 108 comprising a commercially available semiconductor substrate, such as a single-crystalline silicon substrate with a diameter of 200 mm, 300 mm or 450 mm and with a thickness in a range of 600 micrometers to 1 mm, although smaller and larger thicknesses can also be used. The first semiconductor substrate 108 can have a planar front surface and a planar rear surface that are parallel to each other. The edge of the first semiconductor substrate 108 can In other words, a convex surface that changes direction by 180 degrees in a vertical cross-sectional view may extend around the entire periphery of the first semiconductor substrate 108. The convex surface may be the planar front surface and the planar back surface of the first semiconductor substrate 108 so that the first semiconductor substrate 108 is free of sharp edges. In a embodiment, the first semiconductor substrate 108 may be a corresponding, commercially available, single-crystalline silicon substrate with the same diameter.

[0009] The first wafer 100 may be formed by forming semiconductor devices on the first semiconductor substrate 108 and by Forming first structures at interconnect level (Lo - L6) and a first structure at pad level LP are provided. The semiconductor devices formed on the first semiconductor substrate 108 are referred to herein as the first semiconductor devices. The first interconnect level structures (Lo - L6) can be found on the first Semiconductor substrate 108 and are incorporated into the first wafer 100. It is an embodiment with first structures at interconnect level (L0-L6). However, a person skilled in the art will know that more or less interconnect level structures are included to the extent contemplated in the disclosure The first interconnect level structures (Lo - L6) and the first pad level structure LP can be the outermost periphery of the first wafer 100 by a lateral offset distance which is in a range of 0.2 mm to 1 mm, although smaller and larger distances can also be used. The lateral offset between the first Structures at interconnect level (Lo - L6) and the outermost periphery of the first wafer 100 is referred to as Edge exclusion distance.

[0010] The first structures at the interconnect level (Lo - L6) have dielectric material layers, which are here the first dielectric layers at the interconnect level. In the first dielectric layers at the interconnect level Metal interconnect structures are formed at the second level, which are referred to here as the first metal interconnect structures. Thus, the first wafer 100 has first metal interconnect structures disposed within the first dielectric layers at the interconnect level. The first pad-level structure LP has a pad-level dielectric layer and bonding pads formed within the first dielectric layer at the pad level. The first structure on Pad level LP can be formed on top of the first wafer interconnect level structures (Lo - L6).

[0011] Fig. 1C illustrates semiconductor devices 330 and interconnect level structures (Lo - L6) formed on the first semiconductor substrate 108. In an illustrative example, the first Semiconductor substrate 108 a bulk semiconductor substrate such as a silicon substrate in which the semiconductor material layer continuously from an upper surface of the first semiconductor substrate 108 to a lower surface of the first semiconductor substrate 108, or a semiconductor-on-insulator layer comprising a semiconductor material layer as an upper semiconductor layer disposed above a buried insulator layer (such as a silicon oxide layer) and a handling semiconductor substrate.

[0012] Semiconductor devices 330, such as field effect transistors, may be formed on and / or in the first semiconductor substrate 108 For example, trench isolation structures 12 may be formed in an upper portion of the first semiconductor substrate 108 by forming trenches and then filling the trenches with a dielectric material such as silicon oxide Different doped wells (not explicitly shown) can be formed in different regions of the upper portion of the first semiconductor substrate 108 by performing masked ion implantation processes become.

[0013] Gate structures 20 may be formed over the upper surface of the first semiconductor substrate 108 by depositing and Structuring a gate dielectric layer, a gate electrode layer and a gate cap dielectric layer Each gate structure 20 may comprise a vertical stack of a gate dielectric 22, a gate electrode 24 and a dielectric gate cover 28, referred to herein as a gate stack (22, 24, 28). Ion implantation processes can be performed to form extension implant regions that can form source extension regions and drain extension regions. Dielectric gate spacers 26 may be the gate stacks (22, 24, 28). Each arrangement of a gate stack (22, 24, 28) and a dielectric gate Spacer 26 represents a gate structure 20. Additional ion implantation processes can be performed using the Gate structures 20 are carried out as self-aligned implantation masks to form deep active regions, which may have deep source regions and deep drain regions. Upper sections of the deep active regions may overlap with portions of the extension implantation regions. Any combination of a Extension implantation region and a deep active region represents an active region 14, which is a source region or a drain region, depending on the electrical bias. A semiconductor channel 15 may be located below each gate stack (22, 24, 28) between an adjacent pair of active regions 14. Metal Semiconductor alloy regions 18 may be formed on the top surface of each active region 14. Field effect transistors may be formed on the first semiconductor substrate 108. Each field effect transistor may have a gate Structure 20, a semiconductor channel 15, a pair of active regions 14 (one of which serves as a source region and the other than a drain region) and optionally metal-semiconductor alloy regions 18. A complementary Metal oxide semiconductor (CMOS) circuit may be provided on the first semiconductor substrate 108, which has a Peripheral circuitry for the array(s) of resistive memory elements that are subsequently formed. While the present disclosure only considers complementary metal oxide semiconductor (CMOS) devices as the first semiconductor devices, it is clear that any other semiconductor device (such as memory devices, radio frequency devices, image capture devices, passive devices, etc.) to the CMOS devices in the first Wafer 100 can be added or replaced.

[0014] Various interconnect level structures can then be formed. In a As an illustration, the interconnect level structures (Lo - L6) can be a contact level structure Lo, a first structure at interconnect level L1, a second structure at interconnect level L2, a third structure at Interconnect level L3, a fourth structure on Intercon nect level L4, a fifth structure at interconnect level L5 and a sixth structure at interconnect level L6 The structure at contact level L0 may include a planarization dielectric layer 31A comprising a planarizable dielectric material such as silicon oxide, and various via structures 41V, which are connected to a corresponding one of the active regions 14 or the gate electrodes 24 and within the Planarization dielectric layer 31A are formed. The first interconnect level structure L1 may include a first dielectric layer on interconnect level 31B and first metal lines 41L disposed within the first dielectric layer on interconnect level 31B. The first dielectric layer on interconnect level 31B is also referred to as a first line-level dielectric layer. The first metal lines 41L may be formed with a corresponding through-hole structures 41V are in contact. The second structure at interconnect level L2 may have a second dielectric layer on interconnect level 32. The second dielectric layer on Interconnect level 32 may include a stack of a first dielectric material layer at the via level and a second dielectric material layer at line level or a dielectric material layer at line and via level. In the second dielectric layer on interconnect level 32, the second Metal interconnect structures at interconnect level (42V, 42L) formed, the first metal via structures 42V and second metal lines 42L. Upper surfaces of the second metal lines 42L may be connected to the upper surface of the second dielectric layer at interconnect level 32.

[0015] The third metal interconnect structures at interconnect level (43V, 43L) may be second metal via structures 43V and third metal lines 43L disposed within the third dielectric Layer at Interconnect Level 33. Additional structures at Interconnect Level (L4, L5, L6) can be formed subsequently. For example, the additional structures at the interconnect level (L4, L5, L6) can fourth structure at interconnect level L4, a fifth structure at interconnect level L5 and a sixth structure at Interconnect level L6. The fourth structure at interconnect level L4 may have a fourth dielectric layer on Interconnect level 34, in which fourth metal interconnect structures are formed at interconnect level (44V, 44L) which may include third metal via structures 44V and fourth metal lines 44L. The fifth Interconnect level structure L5 may include a fifth dielectric layer at interconnect level 35 in which fifth metal interconnect structures (45V, 45L) are formed at interconnect level, the fourth Metal via structures 45V and fifth metal lines 45L. The sixth structure on Interconnect level L6 may include a sixth dielectric layer on interconnect level 36 in which sixth metal Interconnect structures are formed at interconnect level (46V, 46L), the fifth metal via structures 46V and sixth metal lines 46L.

[0016] A pad-level structure LP, referred to herein as a second pad-level structure, can be formed via the Structures at the interconnect level (Lo - L6) are formed. The structure at the pad level LP can have a dielectric layer at pad level 37, in which final metal via structures 47V and metal bonding pads 47B The metal bonding pads 47B can be configured for metal-to-metal bonding (such as copper-to-copper bonding) be.

[0017] Each interconnect level dielectric layer may be referred to as an interconnect level dielectric layer (ILD- Layer) 30. All metal interconnect structures at the interconnect level can be described as a metal Interconnect structure 40. Any combination of a metal via structure and a overlying metal line, which is located in the same structure at interconnect level (L1 - L6), can be used in turn as two separate structures can be formed using two single damascene processes or can be simultaneously formed as a single structure using a dual damascene process. Each metal interconnect Structure 40 may have a corresponding metallic lining (such as a layer of TiN, TaN or WN with a thickness of a range of 2 nm to 20 nm) and a corresponding metallic filler material (such as W, Cu, Co, Mo, Ru, other elemental metals or an alloy or a combination thereof). Various dielectric Etch stop layers and dielectric cap layers can be placed between vertically adjacent pairs of ILD layers 30 be inserted or may be incorporated into one or more of the ILD layers 30.

[0018] While the present disclosure is described using an embodiment in which a set of seven structures at interconnect level (Lo - L6), embodiments are expressly considered here in which a different number of interconnect level structures is used in the first wafer 100. For For example, the number of interconnect level structures (Lo - L6) in the first wafer 100 can be in a range from 1 to 20, as from 2 to 10, although a smaller and larger number of Interconnect level structures can also be used. In general, the first wafer 100 can have a first two-dimensional arrangement of first semiconductor dies. The first semiconductor dies can be configured as a periodic two-dimensional arrangement and can be spaced apart from each other laterally by separation channels be.

[0019] Referring to Fig. 2A and Fig. 2B, a first pre-bonding edge trimming process may be performed to cut a front peripheral region of the first wafer 100. An edge trimming process generally refers to a process in which an edge portion of a substrate is welded along the entire circumference of the substrate is removed. The first pre-bonding edge trimming process may produce a ring-shaped peripheral Remove a portion of the first wafer 100 that is within a first edge cut width tw1 from the outermost periphery of the first wafer 100, and at a first edge cut depth td1 from a horizontal plane defining the upper surface of the first wafer 100. A commercial wafer edge cutting tool can be used to perform the first pre-bonding edge trimming process. The first pre-bonding Edge trimming process forms a ring-shaped horizontal edge cutting surface within a horizontal plane, which is located at the first edge cut depth td1 from the front surface of the first wafer 100. Furthermore, the first Pre-bonding edge trimming process, a first cylindrical sidewall on the first wafer 100 at a location that laterally offset from the outermost periphery of the first wafer 100 by the first edge cut width tw1. In a Embodiment, the first edge cutting width tw1 may be in a range of 0.1 mm to 5.0 mm, although smaller and larger first edge cutting widths can also be used. The first edge cutting width tw1 can be larger than the Edge exclusion distance and is smaller than a final edge cutting width of a post- Bonding edge trimming process. In one embodiment, the first edge cutting depth td1 may be in a range from 10 micrometers to 50 micrometers, although smaller and larger first edge cutting depths are also used The first edge cutting depth td1 is greater than a thickness to which the first wafer 100 can be cut during a post-bonding thinning process and is less than 50%, such as less than 15%, of the thickness of the first wafer 100.

[0020] Referring to Fig. 3A and Fig. 3B, a second wafer 200 having a second lateral offset according to an embodiment of the present disclosure. The second wafer 200 has a second Semiconductor substrate 208, which is a commercially available semiconductor substrate such as a single-crystalline silicon substrate with a diameter of 200 mm, 300 mm or 450 mm and with a thickness in a range of 600 micrometers to 1 mm, although smaller and larger thicknesses may also be used. The second semiconductor substrate 208 has a planar front surface and a planar back surface that are parallel to each other. The edge of the second semiconductor substrate 208 may have edge rounding. In one embodiment, the second Semiconductor substrate 208 a corresponding, commercially available, single-crystalline silicon substrate having a same diameter.

[0021] The second wafer 200 may be formed by forming semiconductor devices on the second semiconductor substrate 208 and by forming two interconnect level structures (Lo - L6) and a second pad level structure LP The semiconductor devices formed on the second semiconductor substrate 208 are referred to herein as second semiconductor devices. The second interconnect level structures (Lo - L6) can be formed on the second semiconductor substrate 208 and are incorporated into the second wafer 200. The second structures on Interconnect level (Lo - L6) and the second pad-level structure LP can be connected from the outermost periphery of the second Wafers 200 may be offset laterally by a lateral offset distance, which may be in a range of 0.2 mm to 1 mm, although a smaller or larger lateral offset distance can also be used. The lateral offset between the second interconnect level structures (Lo - L6) and the outermost periphery of the second wafer 200 is a Edge exclusion distance.

[0022] The second structures at the interconnect level (Lo - L6) have dielectric material layers, which are referred to here as second dielectric layers at interconnect level. In the second dielectric layers on Interconnect level, metal interconnect structures are formed, which are referred to here as second metal interconnect structures Thus, the second wafer 200 has second metal interconnect structures formed in the second dielectric layers at the interconnect level. The second structure at the pad level LP has a dielectric layer at the pad level and bonding pads formed in the second dielectric layer at the pad level. The second pad-level structure LP can be placed on top of the second wafer interconnect-level structures (Lo - L6) be educated.

[0023] The second wafer 200 may contain CMOS devices and / or any other semiconductor device (such as Storage devices, radio frequency devices devices, image capture devices, passive devices, etc.) as second semiconductor devices. While the present disclosure is described using an embodiment in which a set of seven Structures at interconnect level (Lo - L6) in the second wafer 200 are expressly Embodiments are contemplated in which a different number of interconnect level structures are used In one embodiment, the second wafer 200 comprises a second two-dimensional array of second semiconductor dies with the same two-dimensional periodicity as the first two-dimensional array of first semiconductor dies in the first wafer 100.

[0024] Referring to Fig. 4A and Fig. 4B, the first wafer 100 and the second wafer 200 may be bonded a front surface of the first wafer 100 to a front surface of the second wafer 200 bonded together For example, the second bonding pads formed in the second dielectric layer at the pad level of the second wafer 200 are bonded to the first bonding pads formed in the first dielectric layer on Pad level of the first wafer 100. Metal-to-metal bonding (such as copper-to-copper bonding) can be used For example, the arrangement of the first wafer 100 and the second wafer 200 at an increased Temperature in a range of 250 degrees Celsius to 450 degrees Celsius to achieve metal-to-metal bonding between the first bonding pads and the second bonding pads. In one embodiment, the the first pad-level dielectric layer and the second pad-level dielectric layer contain silicon oxide and Oxide-to-oxide bonding between the first dielectric layer at pad level and the second dielectric layer on Pad level can be prepared before metal-to-metal bonding by annealing the arrangement of the first wafer 100 and the second Wafers 200 at an elevated temperature in a range of 150 degrees Celsius to 350 degrees Celsius while the first metal pads are in contact with the second metal pads and the first dielectric layer at pad level is in contact with the second dielectric layer at pad level.

[0025] Referring to Fig. 5A and Fig. 5B, the back side of the first wafer 100 can be formed by performing at least one wafer thinning process. For example, a first wafer Thinning process may be performed to thin the first wafer 100 to a first thickness t1 which is greater than the first edge cutting depth td1. In one embodiment, the first wafer thinning process may include a wafer grinding process that grinds the back side of the first wafer 100. In a Embodiment, the first thickness t1 may be in a range from 10 micrometers to 60 micrometers, such as from 15 micrometers to 50 micrometers, although smaller and larger thicknesses can also be used. Selecting the first thickness t1, greater than the first edge cutting depth td1 provides the advantage that grinding the portion of the first wafer 100 is avoided, which has the annular horizontal surface extending vertically from the bonding interface around the first edge cutting depth td1, ie the annular horizontal surface formed by the first pre-bonding Edge trimming process is formed. This prevents fragmentation and chipping of edge sections of the first wafer 100 from the vicinity of the annular planar surface formed during the first pre-bonding edge trimming process can be avoided.

[0026] Referring to Fig. 6A and Fig. 6B, a second thinning process that further thins the first wafer 100 The second wafer thinning process thins the first wafer 100 using a thinning process, which is less susceptible to wafer chipping than a grinding process, to a second thickness t2 which is smaller than the first edge cutting depth td1. For example, the second wafer thinning process may use an isotropic etching process that removes the material from the back of the remaining portion of the first wafer 100 etching, and / or may use a chemical mechanical polishing (CMP) process. In one embodiment, the second wafer thinning process may comprise an isotropic etching process containing an ´´HNA´´ etchant that has a Mixture of hydrofluoric acid, nitric acid and acetic acid. In an illustrative example, the HNA etchant contains a 1:3:8 volume mixture of hydrofluoric acid, nitric acid, and acetic acid, which Etching rate for single crystalline silicon in a range of 1 micrometer per minute to 3 micrometers per minute, depending on the temperature of the etchant and the doping of the single-crystalline silicon. In a embodiment, the second thickness t2 may be in a range of 2 micrometers to 10 micrometers, although smaller and larger thickness can also be used.

[0027] In general, the at least one wafer thinning process may be performed to obtain untrimmed to remove portions of the first wafer 100, ie the portion of the first wafer 100 which was removed during the first pre- Bonding edge trimming process is not performed laterally. In particular, the untrimmed Sections of the first wafer 100 may be sections of the first wafer 100 that are vertically from the horizontal plane forming the bonding interface between the first wafer 100 and the second wafer 200 are spaced apart by a greater vertical distance than the first edge cutting depth td1. Therefore, the at least one wafer thinning process a back surface of the first semiconductor substrate 108 within a horizontal plane extending vertically from the bonding interface between the first wafer 100 and the second wafer 200 may be offset by a vertical distance that is smaller than the first edge cutting depth td1. In other words, the second thickness t2 is smaller than the first edge cutting depth td1. As such, the annular horizontal surface of the first wafer 100, which can be formed during the first pre-bonding edge trimming process, while the second thinning process without chipping or fragmenting the portion of the first wafer 100 adjacent to the annular horizontal surface. Due to the first pre-bonding Edge trimming process, which can be performed on the first wafer 100 before bonding, the Side walls of the first wafer 100 may be offset inwards from the side walls of the second wafer 200, which the horizontal plane containing the bonding interface between the first wafer 100 and the second Wafers 200.

[0028] Referring to Figs. 7A - 7C, a final edge trimming process can be performed, which is also referred to as a post-bonding edge trimming process. The post-bonding Edge trimming process trims edges of the first wafer 100 and a front peripheral region of the second wafer 200. Portions of the first wafer 100 and the second wafer 200 that are within a final Edge cut width twt from the outermost periphery of the bonded assembly of the first wafer 100 and the second wafer 200 (which is the outermost periphery of the second wafer 200) and within a final edge cut depth tdt from the horizontal plane containing the back surface of the first wafer 100 may be formed during the Post-bonding edge trimming process.

[0029] The post-bonding edge trimming process forms a final cylindrical side wall on the first Wafer 100 and at the front peripheral region of the second wafer 200 at a location laterally from the outermost periphery of the second wafer 200 by the final edge cut width twt. The final Edge cutting width twt is greater than the first edge cutting width tw1. For example, the final Edge cutting width twt can be in a range of 1.0 mm to 10.0 mm, although a smaller and larger width is also Furthermore, the post-bonding edge trimming process can produce a ring-shaped horizontal surface on the second wafer 200. The annular horizontal surface can be within a horizontal plane which is vertically separated from the horizontal plane forming the bonding interface between the first wafer 100 and the second wafer 200, by a vertical distance in a range of 5 micrometers to 100 micrometers apart, although smaller and larger vertical spacing can also be used. In other words, the final edge cutting depth tdt may be a sum of the second thickness t2 and an additional Depth in a range of 10 micrometers to 50 micrometers, although a smaller and greater depth is also used can be.

[0030] The post-bonding edge trimming process removes only thin peripheral portions of the first wafer 100 and of the second wafer 200. As such, a very smooth profile for the trimmed side walls and the trimmed annular horizontal surface of the bonded assembly can be obtained, as shown schematically in the inset of Fig. 7C. In other words, the trimmed side walls and the trimmed annular horizontal Surface can have a very low surface roughness, such as an effective value of the surface roughness of smaller than 10 nm, such as smaller than 3 nm .

[0031] Referring to Fig. 8, an upper portion of an exemplary first wafer 100 is shown in an enlarged view. A dielectric encapsulation layer 130 can then be applied to the rear surface of the first wafer 100. The dielectric encapsulation layer 130 may contain a dielectric material, which can protect the bonded arrangement (100, 200) during a subsequent singulation process in which each bonded pair of a first semiconductor die in the first wafer 100 and a second semiconductor die in the second wafer 200 is singulated into a discrete structure. The dielectric encapsulation layer 130 may be silicon nitride or a contain high-k dielectric material with a dielectric constant greater than 7.9 (such as aluminum oxide, hafnium oxide, tantalum oxide, titanium oxide, etc.). Other suitable materials are in the The thickness of the dielectric encapsulation layer 130 may be in a range of 50 nm to 500 nm, although smaller and larger thicknesses can also be used.

[0032] A photoresist layer (not shown) may be deposited over the horizontal portion of the dielectric Encapsulation layer 130, which lies above the first semiconductor substrate 108, and can be lithographically structured to form through-holes. An anisotropic etching process can be performed to by unmasked portions of the dielectric encapsulation layer 130, the first semiconductor substrate 108 and a subset of the dielectric layers on interconnect level 30 so that a horizontal surface of a underlying metallic pad structure can be physically exposed. The metallic pad structures can one of the metal lines of the second wafer 200 (such as the first metal lines 41L, the second metal lines 42L, the third metal lines 43L, etc.). Substrate via cavities 139 may be formed by the first semiconductor substrate 108 within each die area of ​​the first wafer 100.

[0033] Referring to Fig. 9, a dielectric material such as silicon oxide can be conformally deposited and can then be anisotropically etched to form insulating spacers 146 passing through the substrate. The lateral thickness of each insulating spacer 146 passing through the substrate may be in a range of 100 nm to 500 nm, although smaller and larger thicknesses can also be used. At least one conductive Material may be deposited in the substrate via cavities 139 and over the top surface of the dielectric Encapsulation layer 130 can be deposited. For example, a metallic lining material (such as TiN, TaN and / or WN) and at least one metallic filler material (such as Cu, Mo, Ru, W, Al or a combination thereof) in remaining volumes of the substrate via cavities 139 and above the upper surface of the dielectric Encapsulation layer 130 is deposited. The at least one metallic filler material can Fill substrate via cavities 139. An underbump metallurgy (UBM) layer stack can be deposited over the at least one metallic filler material is deposited. Layer stacks used for the UBM layer stack can include, but are not limited to, stacks of f Cr / Cr-Cu / Cu / Au, Cr / Cr-Cu / Cu, TiW / Cr / Cu, Ti / Ni / Au and Cr / Cu / Au. Other suitable materials are within the contemplated scope of the disclosure.

[0034] The UBM layer stack and the at least one conductive material can then be structured. Example by applying and structuring a photoresist layer and by transferring the structure in the photoresist layer through the horizontal sections of the UBM layer stack and the at least one conductive material. Each remaining portion of the at least one conductive material which is in a corresponding one of the Substrate via cavities 139 represents a substrate via structure 148. Each remaining portion of the at least one conductive material and the UBM layer stack that is above the horizontal plane containing the distal horizontal surface of the dielectric encapsulation layer 130, has a bonding Pad 160, which can be an external bonding pad on which a solder ball for wire bonding or C4 bonding In an alternative embodiment, the UBM layer stack may be omitted and the at least A conductive material may contain copper or a copper alloy as a metallic filler. In such a In one embodiment, the bonding pads 160 may have a copper surface that is subsequently used for copper-to-copper Bonding with copper bonding pads can be used in another wafer in a subsequent wafer-to- wafer bonding process that forms a bonded assembly of three wafers.

[0035] Referring to Fig. 10A and Fig. 10B, the exemplary structure comprises a bonded arrangement (100, 200) which comprises a first wafer 100 bonded to a second wafer 200 at a bonding interface. A straight cylindrical sidewall may extend vertically from a rear surface of the first wafer 100 over a periphery of the Bonding interface to a peripheral region of the second wafer 200.

[0036] In one embodiment, the first wafer 100 may comprise a first two-dimensional array of first semiconductor dies with a two-dimensional periodicity and the second wafer 200 has a second two-dimensional Arrangement of second semiconductor dies with the same two-dimensional periodicity as the first two-dimensional Arrangement of first semiconductor dies. In this case, the bonded arrangement of the first wafer 100 and the second Wafers 200 can be separated along separation channels into several bonded semiconductor chips. For example, the bonded arrangement (100, 200) are separated with a separating saw along separating channels DC. The Separation channels DC may have first separation channels that are parallel to each other and extend laterally along a first horizontal direction, and second separation channels which are parallel to each other and extend laterally along a second horizontal direction that is perpendicular to the first horizontal direction. Each the dicing channels DC can be used between adjacent pairs of semiconductor dies in the first wafer 100 and between adjacent pairs of semiconductor dies in the second wafer.

[0037] Each semiconductor chip 300 that can be singulated by the singulation process can have a first semiconductor Die, which is a singulated portion of the first wafer 100, and a second semiconductor die, which is a singulated portion of the second wafer 200. As such, each semiconductor chip 300 may comprise a stack of a first semiconductor dies and a second semiconductor die, which are bonded by metal-to-metal bonding between first bonding Pads in a first dielectric layer at pad level of the first semiconductor die and second bonding pads in a second dielectric layer at the pad level of the second semiconductor die. In general, each of the bonded semiconductor chips formed by singulating the bonded arrangement (100, 200) has a bonded pair of a corresponding one of the first semiconductor dies and a corresponding one of the second semiconductor dies Additional bonding pads 160, which may be external bonding pads having a corresponding UBM Layer stacks may be provided on the back side of the second semiconductor die.

[0038] Referring to Fig. 11A and Fig. 11B, a second wafer 200 according to a second embodiment of the present disclosure, which is formed from the second wafer 200 of the first embodiment of Fig. 3A and Fig. 3B can be derived by performing a second pre-bonding edge trimming process. The second Pre-bonding edge trimming process trims edges of a front peripheral region of the second wafer 200. The second pre-bonding edge trimming process may include an annular peripheral portion of the second wafer 200 which is within a second edge cut width tw2 from the outermost periphery of the second wafer 200 and is within a second edge cut depth td2 of a horizontal plane defining the upper surface (ie, a bonding side surface) of the second wafer 200. It may be a commercial wafer Edge trimming tool can be used to perform the second pre-bonding edge trimming process. second pre-bonding edge trimming process forms a ring-shaped horizontal edge cut surface within a horizontal plane located at the second edge cut depth td2 from the front surface of the second wafer 200. Further, the second pre-bonding edge trimming process forms a second cylindrical side wall on the second Wafer 200 at a location that is laterally spaced from the outermost periphery of the second wafer 200 by the second Edge cutting width tw2 is offset. In one embodiment, the second edge cutting width tw2 can be in a range from 0.1 mm to 5.0 mm, although smaller and larger second edge cutting widths can also be used. second edge cut width tw2 may be greater than the edge exclusion distance of the second wafer 200 and is less than a final edge cut width from a post-bonding edge trimming process to be used. In a embodiment, the second edge cutting depth td2 may be in a range of 5 micrometers to 20 micrometers, although smaller and larger second edge cutting depths can also be used.

[0039] In the second embodiment, the first wafer 100 can be formed using the same methods as in the first Thus, a first pre-bonding edge trimming process on the first wafer 100 in the same manner as in the first embodiment. As such, the second pre-bonding Edge trimming process may be an additional pre-bonding edge trimming process performed on the second wafer 200 before bonding the front surface of the first wafer 100 to the front surface of the second wafer 200 In general, the second pre-bonding edge trimming process can be a second cylindrical sidewall on the second wafer 200 at a location extending laterally from an outermost periphery of the second wafer 200 is offset by the second edge cut width tw2.

[0040] Referring to Fig. 12A and Fig. 12B, the first wafer 100 and the second wafer 200 may be bonded a front surface of the first wafer 100 to a front surface of the second wafer 200 bonded together For example, the second bonding pads formed in the second dielectric layer at the pad level of the second wafer 200 are bonded to the first bonding pads formed in the first dielectric layer on Pad level of the first wafer 100. Metal-to-metal bonding (such as copper-to-copper bonding) can be used The same bonding process as in the first embodiment can be used.

[0041] Referring to Fig. 13A and Fig. 13B, the back side of the first wafer 100 can be formed by performing at least one wafer thinning process. For example, a first wafer Thinning process may be performed to thin the first wafer 100 to a first thickness t1 which is greater than the first edge cut depth td1. In one embodiment, the first wafer thinning process may include a Wafer grinding process comprising and / or consisting of the back side of the first wafer 100 In one embodiment, the first thickness t1 may be in a range of 10 micrometers to 60 micrometers, as described by 15 micrometers to 50 micrometers. Select the first thickness t1 so that it is greater than the first edge cutting depth td1 offers the advantage of avoiding grinding of the portion of the first wafer 100 which forms the annular horizontal surface which is vertically offset from the bonding interface by the first edge cut depth td1, ie the annular horizontal surface formed by the first pre-bonding edge trimming process. Therefore Fragmentation and chipping of edge portions of the first wafer 100 from the vicinity of the annular planar surface formed during the first pre-bonding edge trimming process is avoided become.

[0042] Referring to Fig. 14A and Fig. 14B, a second thinning process that thins the first wafer 100 The second wafer thinning process thins the first wafer 100 to a second Thickness t2 which is smaller than the first edge cutting depth td1, using a thinning process which is suitable for wafer chipping is less prone than a grinding process. For example, the second wafer thinning process can use an isotropic etching process that removes the material from the back of the remaining portion of the first wafer 100 etched and / or may use a chemical mechanical polishing (CMP) process. In one embodiment, the second wafer thinning process may comprise an isotropic etching process using the HNA etchant described above used. In one embodiment, the second thickness t2 may be in a range of 2 micrometers to 10 micrometers.

[0043] In general, the at least one wafer thinning process may be performed to obtain untrimmed to remove portions of the first wafer 100, ie the portion of the first wafer 100 which was removed during the first pre- Bonding edge trimming process is not laterally edge trimmed. The at least one wafer Thinning process forms a back surface of the first semiconductor substrate 108 within a horizontal Plane separated from the bonding interface between the first wafer 100 and the second wafer 200 by a vertical distance which is smaller than the first edge cutting depth td1. The annular horizontal Surface of the first wafer 100 formed during the first pre-bonding edge trimming process may during the second thinning process without chipping or fragmenting the portion of the first wafer 100 which borders the annular horizontal surface.

[0044] Referring to Fig. 15A and Fig. 15B, a final edge trimming process can be performed which is also referred to as a post-bonding edge trimming process. The post-bonding Edge trimming process trims edges of the first wafer 100 and a front peripheral region of the second wafer 200. Portions of the first wafer 100 and the second wafer 200 that are within a final Edge cut width twt from the outermost periphery of the bonded assembly of the first wafer 100 and the second wafer 200 (which is the outermost periphery of the second wafer 200) and within a final edge cut depth tdt from the horizontal plane containing the back surface of the first wafer 100 are, during the Post-bonding edge trimming process removed.

[0045] The post-bonding edge trimming process forms a final cylindrical sidewall on the first wafer 100 and at the front peripheral region of the second 200 at a location laterally from the outermost Periphery of the second wafer 200 is offset by the final edge cut width twt. The final Edge cutting width twt is greater than the first edge cutting width tw1 and is greater than the second edge cutting width tw2. For example, the final edge cutting width twt can be in a range from 1.0 mm to 10.0 mm. the post-bonding edge trimming process may form a ring-shaped horizontal surface on the second wafer 200 The annular horizontal surface can be formed within a horizontal plane which is vertically the horizontal plane containing the bonding interface between the first wafer 100 and the second wafer 200, offset by a vertical distance greater than the second edge cutting depth td2. For example, the annular horizontal surface formed on the second wafer 200 by the post-bonding edge trimming process formed within a horizontal plane that is vertically separated from the horizontal plane that forms the bonding Interface between the first wafer 100 and the second wafer 200, by a vertical distance in a range of 5 micrometers to 100 micrometers. In other words, the final edge cutting depth tdt can a sum of the second thickness t2 and an additional depth in a range of 10 micrometers to 50 micrometers.

[0046] Subsequently, the processing steps of Fig. 8, Fig. 9 and Fig. 10A and Fig. 10B can be carried out, to convert the bonded arrangement of the first wafer 100 and the second wafer 200 into a plurality of bonded semiconductor chips isolate, which is a corresponding pair of a first semiconductor die and a second semiconductor die.

[0047] Referring to Fig. 16, a first flowchart illustrates steps necessary for forming one of the exemplary structures of the present disclosure. In step 1610, a front-side peripheral region of a first wafer 100 by performing a pre-bonding edge trimming process (such as first pre-bonding edge trimming process of Fig. 2A and Fig. 2B). In step 1620 a front surface of the first wafer 100 can be bonded to a front surface of a second wafer 200 Referring to step 1630, a backside of the first wafer 100 may be formed by performing at least a wafer thinning process. Referring to step 1640, the first wafer 100 and a front peripheral region of the second wafer 200 by performing a post-bonding Edge trimming process.

[0048] Referring to Fig. 17, a second flowchart illustrates steps involved in forming one of the exemplary structures of the present disclosure. In step 1710, a front-side peripheral region of a first wafer 100 by performing a first pre-bonding edge trimming process In step 1720, a front peripheral region of a second wafer 200 may be edge trimmed by Performing a second pre-bonding edge trimming process. In step 1730, a bonded assembly (100, 200) by bonding a front surface of the first wafer 100 to a front surface of the second wafer 200. In step 1740, untrimmed portions of the first wafer 100 by thinning a backside of the first wafer 100 in the bonded arrangement (100, 200) using at least one thinning process. A rear surface of the first wafer 100 is adjacent to a cylindrical sidewall formed during the first pre-bonding edge trimming process. In In step 1750, the bonded assembly (100, 200) may be bonded by performing a post-bonding edge trimming process, which trims the first wafer 100 and the front peripheral region of the second wafer 200 (without edge trimming of the rear peripheral region of the second Wafers 200).

[0049] Referring to Fig. 18, a third flowchart illustrates steps involved in forming one of the exemplary structures of the present disclosure. In step 1810, a first wafer 100 containing a first two-dimensional array of first semiconductor dies. In step 1820, a second wafer 200 comprising a second two-dimensional array of second semiconductor dies having a same two-dimensional periodicity as the first two-dimensional arrangement of first semiconductor dies. In step 1830, a front peripheral region of the first wafer may be bonded by performing a pre-bonding Edge trimming process (such as the first pre-bonding edge trimming process of Fig. 2A and Fig. 2B) In step 1840, a bonded assembly (100, 200) can be bonded by bonding a front surface of the first wafer 100 to a front surface of a second wafer 200. Each of the first Semiconductor die is bonded to a corresponding one of the second semiconductor dies. In step 1850, a backside of the first wafer 100 by performing at least one wafer thinning process. In step 1860 the first wafer 100 and a front peripheral region of the second wafer 200 may be formed by performing a post- Bonding edge trimming process. In step 1870, the bonded assembly (100, 200) into several bonded semiconductor chips. Each of the bonded semiconductor chips has a bonded Pair of a corresponding one of the first semiconductor dies and a corresponding one of the second semiconductor dies.

[0050] The various structures and methods of the present disclosure can be used to provide effective edge trimming for two wafers bonded to form a bonded assembly. The vertical extent of a first pre-bonding edge trimming process is limited to an upper peripheral region of a first wafer 100 and can have a first edge cutting depth td1 in a range of 10 micrometers to 50 micrometers and thus less than 10% of the total thickness of the first wafer. If a second pre-bonding Edge trimming process is used, a vertical extent of the second pre-bonding Edge trimming process is limited to an upper peripheral region of the second wafer 200 and may form a second Edge cutting depth td2 in a range of 5 micrometers to 20 micrometers. The vertical extent of a post- Bonding edge trimming process is limited to a final edge cutting depth tdt, which must be the same can be the sum of the second thickness t2 and a vertical depth in a range of 10 micrometers to 50 micrometers. Each edge trimming process can have a vertical extent that is significantly smaller than the thickness of a Wafers from thinning, which is in an area from 725 micrometers to 825 micrometers. Thus, the methods of the present disclosure reduce the total processing time spent on edge trimming processes reduce the total Processing costs for edge trimming processes and provide high wafer processing capacity for the Edge trimming processes with a moderate number of machining tools. Further reduce the Methods of the present disclosure effectively exfoliate interconnect level structures (Lo - L6) and structures at pad level LP in the first wafer 100 and second wafer 200 before and / or after bonding the first wafer 100 with the second wafer 200. Thus, the effectiveness of edge trimming can be increased throughout the bonding process and of the singulation process. Therefore, the methods of the present disclosure represent a cost-effective and reliable edge trimming during bonding and wafer singulation.

Claims

1. A method for forming a semiconductor structure, comprising: Edge trimming (1610) of a front peripheral region of a first wafer (100) by performing a pre- Bonding edge trimming process; Bonding (1620) a front surface of the first wafer (100) to a front surface of a second wafer (200); Thinning (1630) a back side of the first wafer (100) by performing at least one wafer Thinning process, wherein the at least one wafer thinning process comprises: a first wafer thinning process that thins the first wafer (100) to a first thickness (t1) that is greater than a first edge cutting depth (td1); and a second wafer thinning process that thins the first wafer (100) to a second thickness (t2) that is less than the first edge cutting depth (td1) and wherein the first wafer thinning process comprises a wafer grinding process and the second wafer thinning process comprises an isotropic etching process; and Edge trimming (1640) of the first wafer (100) and a front peripheral region of the second wafer (200) by performing a post-bonding edge trimming process.

2. The method of claim 1, wherein the pre-bonding edge trimming process comprises an annular horizontal Edge cutting surface within a horizontal plane which, at the first edge cutting depth (td1), is formed by the front surface of the first wafer (100).

3. The method of claim 2, wherein the at least one wafer thinning process comprises a back surface of the first wafer (100) within a horizontal plane defined by a bonding interface between the first wafer (100) and the second wafer (200) by a vertical distance (t2) which is smaller than the first Edge cutting depth (td1).

4. The method of claim 1, wherein the isotropic etching process includes an HNA etchant comprising a mixture of Hydrofluoric acid, nitric acid and acetic acid.

5. The method of claim 4, wherein the HNA etchant is a 1:3:8 volume mixture of hydrofluoric acid, Contains nitric acid and acetic acid.

6. The method according to claim 1, wherein: the first thickness (t1) is in a range of 10 micrometers to 60 micrometers; and the second thickness (t2) is in a range of 2 micrometers to 10 micrometers.

7. The method according to any one of the preceding claims, wherein the pre-bonding edge trimming process comprises a first cylindrical sidewall on the first wafer (100) at a location extending laterally from an outermost periphery of the first wafer (100) is offset by a first edge cut width (tw1).

8. The method of claim 7, wherein the post-bonding edge trimming process includes a final cylindrical sidewall on the first wafer (100) and on the front peripheral region of the second wafer (200) at a point extending laterally from an outermost periphery of the second wafer (200) by a final edge cutting width (twt) which is greater than the first edge cutting width (tw1).

9. The method according to claim 8, wherein: the first edge cutting width (tw1) is in a range of 0.1 mm to 5.0 mm; and the final edge cutting width (twt) is in a range of 1.0 mm to 10.0 mm.

10. Method according to one of the preceding claims, wherein: the post-bonding edge trimming process forms an annular horizontal surface on the second wafer (200); and the annular horizontal surface is formed within a horizontal plane which is vertically separated from a horizontal plane containing a bonding interface between the first wafer (100) and a second wafer (200), by a ver tical distance in a range of 5 micrometers to 100 micrometers.

11. A method according to any one of the preceding claims, further comprising edge trimming of the front peripheral region of the second wafer (200) by performing an additional pre-bonding Edge trimming process before bonding the front surface of the first wafer (100) to the front surface of the second wafer (200).

12. Method according to one of the preceding claims, wherein: the first wafer (100) comprises a first two-dimensional array of first semiconductor dies; the second wafer (200) comprises a second two-dimensional array of second semiconductor dies having the same two-dimensional Periodicity such as the first two-dimensional array of first semiconductor dies; and the method of separating a bonded arrangement of the first wafer (100) and the second wafer (200) along Separation channels included.

13. A method of forming a semiconductor structure, comprising: Edge trimming (1710) of a front peripheral region of a first wafer (100) by performing a first pre-bonding edge trimming process; Edge trimming (1720) of a front peripheral region of a second wafer (200) by performing a second pre-bonding edge trimming process; Forming (1730) a bonded assembly by bonding a front surface of the first wafer (100) to a front surface of the second wafer (200); Removing (1740) uncut portions of the first wafer (100) by thinning a backside of the first wafer (100) in the bonded arrangement using at least one thinning process, wherein a rear Surface of the first wafer (100) is adjacent to a cylindrical side wall which, during the first pre-bonding edge trimming process, wherein the back side of the first wafer (100) in the bonded arrangement is thinned out by performing: a first wafer thinning process that thins the first wafer (100) to a first thickness (t1) that is greater than a first edge cutting depth (td1); and a second wafer thinning process that thins the first wafer (100) to a second thickness (t2) that is smaller as the first edge cutting depth (td1), and wherein the first wafer thinning process comprises a wafer grinding process and the second wafer thinning process comprises an isotropic etching process; and Edge trimming (1750) of the bonded assembly by performing a post-bonding Edge trimming process comprising the first wafer (100) and the front peripheral region of the second wafer (200) circumcised.

14. The method according to claim 13, wherein: the pre-bonding edge trimming process creates a ring-shaped horizontal edge cut surface within a horizontal plane located at the first edge cut depth (td1) from the front surface of the first wafer (100); and the annular horizontal edge cut surface is removed during thinning of the back side of the first wafer (100).

15. The method of claim 13, wherein the isotropic etching process includes an HNA etchant comprising a mixture of Hydrofluoric acid, nitric acid and acetic acid.

16. The method of claim 15, wherein the HNA etchant is a 1:3:8 volume mixture of hydrofluoric acid, Contains nitric acid and acetic acid.

17. A method according to any one of the preceding claims 13 to 16, wherein: the first pre-bonding edge trimming process forms a first cylindrical sidewall on the first wafer (100) a location laterally spaced from an outermost periphery of the first wafer (100) by a first edge cut width (tw1) is offset; the second pre-bonding edge trimming process forms a second cylindrical sidewall on the second wafer (200) a location laterally spaced from an outermost periphery of the second wafer (200) by a second edge cut width (tw2) is offset; and the post-bonding edge trimming process forms a final cylindrical sidewall on the first wafer (100) and on the front peripheral region of the second wafer (200) at a location laterally separated from a outermost periphery of the second wafer (200) by a final edge cut width (twt) which is greater than the first edge cutting width (tw1) and greater than the second edge cutting width (tw2).

18. A method according to any one of the preceding claims 13 to 17, wherein: the post-bonding edge trimming process forms an annular horizontal surface on the second wafer (200); and the annular horizontal surface within a horizontal plane vertically separated from a horizontal plane forming a bonding interface between the first wafer (100) and the second wafer (200), by a vertical distance in a range of 5 micrometers to 100 micrometers apart.

19. A method for forming bonded semiconductor chips, comprising: Providing (1810) a first wafer (100) having a first two-dimensional array of first semiconductor dies; Providing (1820) a second wafer (200) comprising a second two-dimensional array of second semiconductor dies with has the same two-dimensional periodicity as the first two-dimensional arrangement of first semiconductor dies; Edge trimming (1830) of a front peripheral region of the first wafer (100) by performing a pre- Bonding edge trimming process; Forming (1840) a bonded assembly by bonding a front surface of the first wafer (100) to a front surface of a second wafer (200), wherein each of the first semiconductor dies is bonded to a corresponding one of the second semiconductor dies are bonded; Thinning (1850) a back side of the first wafer (100) by performing at least one wafer Thinning process, wherein the at least one wafer thinning process comprises: a first wafer thinning process that thins the first wafer (100) to a first thickness (t1) that is greater than a first edge cutting depth (td1); and a second wafer thinning process that thins the first wafer (100) to a second thickness (t2) that is smaller as the first edge cutting depth (td1), and wherein the first wafer thinning process comprises a wafer grinding process and the second wafer thinning process comprises an isotropic etching process; Edge trimming (1860) of the first wafer (100) and a front peripheral region of the second wafer (200) by performing a post-bonding edge trimming process; Separating (1870) the bonded arrangement into a plurality of bonded semiconductor chips, each of the bonded Semiconductor chips a bonded pair of a corresponding one of the first semiconductor dies and a corresponding one of the second semiconductor dies.

20. The method of claim 19, further comprising edge trimming (1720) of the front peripheral region of the second wafer (200) by performing an additional pre-bonding edge trimming process before bonding the front surface of the first wafer (100) to the front surface of the second wafer (200).

Citation Information

Patent Citations

  • Bonded wafer processing method

    US20050215056A1

  • Methods of avoiding wafer breakage during manufacture of backside illuminated image sensors

    US20080044984A1

  • Methods for Minimizing Edge Peeling in the Manufacturing of BSI Chips