CARRIER OF THE ELECTRICALLY HEATED TYPE AND EXHAUST PURIFICATION DEVICE
By forming electrode layers from a metal-ceramic mixed element and covering them with a protective layer, the issues of electrode damage and resistance increase in electrically heated catalysts are addressed, enhancing exhaust gas purification efficiency.
Patent Information
- Application Number
- DE102020203291
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-27
- Filing Date
- 2020-03-13
- Publication Date
- 2024-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing electrically heated catalysts face issues with electrode layer damage and increased resistance due to thermal stress and oxidation, particularly in plug-in hybrid vehicles and hybrid vehicles with low engine starting frequency, leading to inadequate exhaust gas purification.
The electrode layers are formed from a metal-ceramic mixed element and covered with a protective layer, with at least a portion exposed for electrical connection, to prevent damage and resistance increase during electrical heating.
This configuration effectively suppresses electrode layer damage and resistance increase, ensuring uniform heat distribution and improved exhaust gas purification performance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical field
[0001] The present invention relates to an electrically heated support and an exhaust gas purification device. In particular, the present invention relates to an electrically heated support and an exhaust gas purification device that can satisfactorily suppress an increase in resistance due to electrode layer fracture and electrode layer deterioration during electrical heating.
[0002] Traditionally, a catalyst is used that is supported on a columnar honeycomb structure with multiple partitions defining several cells that extend from one end face to another to form flow paths to remove harmful substances such as HC, CO, and NO. xto remove pollutants contained in exhaust gas emitted by a motor vehicle's engine or similar vehicle. When the exhaust gas is treated by the catalyst mounted on the honeycomb structure, it is therefore necessary to raise the catalyst's temperature to its activation temperature. However, at the moment the engine is started, the catalyst does not reach its activation temperature. Therefore, the problem arises that the exhaust gas is not adequately cleaned. In particular, in a plug-in hybrid electric vehicle (PHEV) or a hybrid vehicle (HV), driving occurs only with the engine running, resulting in a lower engine start frequency and, consequently, a lower catalyst temperature at the time of engine start, which tends to impair exhaust gas purification performance.
[0003] To solve this problem, an electrically heated catalyst (EHC) was proposed, in which a pair of terminals is connected to a columnar honeycomb structure made of conductive ceramic. The honeycomb structure itself is heated by electrical conduction, allowing the catalyst to reach its activation temperature before the engine is started. It is desirable that the EHC reduces temperature variations within the honeycomb structure, ensuring a uniform temperature distribution to achieve a sufficient catalytic effect.
[0004] To connect terminals to the honeycomb structure and generate heat within it through electrical conduction, surface electrodes must be placed on the outer perimeter of the structure. However, repeated electrical conduction can damage these surface electrodes due to thermal stress.
[0005] To solve such problems, patent document 1 discloses that ceramic surface electrodes (electrode layers) are provided on an outer circumferential surface of an EHC support and that stretchable metal elements are embedded in the surface electrodes. It also discloses that, according to such a configuration, even if the surface electrodes are damaged, the entire support can be electrically heated by the embedded stretchable metal elements.
[0006] Further prior art is also known from patent document 2. List of prior art patent documents Patent document 1: Japanese patent no. JP 5 786 961 B2 Patent document 2: German patent application no. DE 10 2017 109 206 A1 Summary of the invention
[0007] However, as a result of studies, the inventors of the present invention found that, in the configuration disclosed in patent document 1, the stretchable metal element embedded in the ceramic surface electrode is easily oxidized. It oxidizes if the surface electrode is not dense, and the function may be lost due to an increase in resistance or the like. Furthermore, the inventors of the present invention found that, since metal has a higher coefficient of thermal expansion, embedding the stretchable metal element in the ceramic surface electrode can damage the surface electrode if the metal expands thermally due to electrical heating.
[0008] The present invention was conceived in light of the above circumstances. One object of the present invention is to provide an electrically heated carrier and an exhaust gas purification device that can satisfactorily suppress damage to electrode layers during electrical heating and an increase in resistance due to deterioration of the electrode layers.
[0009] As a result of intensive studies, the inventors of the present invention have found that the above problems are solved by forming the electrode layers from a metal-ceramic composite element and covering each electrode layer with a protective layer such that at least a portion of each electrode layer is exposed. Thus, the present invention is specified as follows: (1) Carrier of an electrically heated type, comprising: - a honeycomb structure that exhibits: a columnar honeycomb structure section comprising: an outer perimeter wall; and porous partitions arranged on an inner side of the outer perimeter wall, the porous partitions defining multiple cells, each of the cells extending from one end face to the other end face to form a flow path; a pair of electrode layers arranged such that they face each other across a central axis of the columnar honeycomb structure section, each electrode layer of the pair being arranged on a surface of the outer circumferential wall; and Protective layers that cover the electrode layers in such a way that at least part of each of the pair of electrode layers is exposed; and - a pair of metal terminals provided on the pair of electrode layers, wherein each of the pair of electrode layers consists of a metal-ceramic hybrid element and wherein a section of each of the pair of electrode layers, which is exposed from the protective layer, is electrically connected to each of the pair of metal terminals. (2) Exhaust gas purification device comprising: the electrically heated carrier according to (1); and a can body for holding the electrically heated carrier. (3) Electrically heated carriers comprising: a honeycomb structure that exhibits: a columnar honeycomb structure section comprising: an outer perimeter wall; and porous partitions arranged on an inner side of the outer perimeter wall, the porous partitions defining multiple cells, each of the cells extending from one end face to the other end face to form a flow path; a pair of electrode layers arranged such that they face each other across a central axis of the columnar honeycomb structure section, each electrode layer of the pair being arranged on a surface of the outer circumferential wall; and Protective layers that cover the electrode layers in such a way that at least part of each of the pair of electrode layers is exposed, wherein each of the pair of electrode layers consists of a metal-ceramic hybrid element and wherein each of the pair of electrode layers has a section that is exposed from the protective layer and is designed to make an electrical connection with each of the metal terminals.
[0010] According to the present invention, it is possible to create an electrically heated carrier and an exhaust gas purification device that can satisfactorily suppress damage to the electrode layers during electrical heating and an increase in resistance due to deterioration of the electrode layers. Brief description of the drawings Fig. Figure 1 is a schematic cross-sectional view of a carrier of the electrically heated type according to embodiment 1 of the present invention, which is perpendicular to a cell expansion direction. Fig. Figure 2 is a schematic external view of a honeycomb structure according to embodiment 1 of the present invention or of a carrier of the electrically heated type according to embodiment 2 of the present invention. Fig.Figure 3 is a schematic cross-sectional view of a column-shaped honeycomb structure section, an electrode layer and a protective layer according to embodiment 1 of the present invention, which is perpendicular to a cell expansion direction. Fig. Figure 4 is a schematic top view of an electrode layer with several linear sections extending radially from the center, in embodiment 1 of the present invention. Fig. 5 is a schematic top view of an electrode layer with the in Fig. The structure shown in Figure 4 is provided in several areas on a columnar honeycomb structure. Description of preferred embodiments
[0011] Embodiments of the present invention are described in detail below with reference to the drawings. It is understood that the present invention is not limited to the following embodiments and that various design modifications and improvements can be made based on the common knowledge of those skilled in the art without departing from the concept of the present invention. <Ausführungsform 1> (1. Carrier of the electrically heated type)
[0012] Fig. Figure 1 is a schematic cross-sectional view of a support 20 of the electrically heated type according to embodiment 1 of the present invention, perpendicular to a cell expansion direction. The electrically heated support 20 comprises a honeycomb structure 10 and a pair of metal terminals 21a, 21b. (1-1. Honeycomb structure)
[0013] Fig.Figure 2 is a schematic external view of the honeycomb structure 10 according to embodiment 1 of the present invention. The honeycomb structure 10 is provided with a columnar honeycomb structure section 11 comprising: an outer circumferential wall 12; and porous partitions 13 arranged on an inner side of the outer circumferential wall 12, defining several cells 15 extending from one end face to the other to form flow paths.
[0014] The external shape of the columnar honeycomb structure section 11 is not particularly restricted, as long as it is columnar. For example, the honeycomb structure section can have a shape such as a columnar shape with circular end faces (circular column shape) and a columnar shape with polygonal (square, pentagonal, hexagonal, heptagonal, octagonal, etc.) end faces. The columnar honeycomb structure section 11 preferably has a size of each end face of 2000 to 20000 mm². 2and preferably from 5000 to 15000 mm 2 , to improve heat resistance (suppression of cracks that penetrate circumferentially into the outer perimeter wall).
[0015] The columnar honeycomb structure section 11 consists of conductive ceramic. The electrical resistance of the ceramic is not particularly limited as long as the honeycomb structure 10 can generate heat through Joule heating when electrically conducted. The specific electrical resistance is preferably 1 to 200 Ωcm and more preferably 10 to 100 Ωcm. In the present invention, the specific electrical resistance of the columnar honeycomb structure section 11 is a value measured at 400 °C using a four-wire method.
[0016] Examples of ceramics forming the columnar honeycomb structure section 11 include, but are not limited to, oxide ceramics such as aluminum oxide, mullite, zirconium oxide, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride. Furthermore, a silicon carbide-metallic silicon composite, a silicon carbide / graphite composite, or the like may also be used. From the perspective of thermal resistance and conductivity compatibility, the material of the honeycomb structure section 11 is preferably primarily based on a silicon-silicon carbide composite or silicon carbide, and more preferably on a silicon-silicon carbide composite or silicon carbide.The phrase "the material of honeycomb section 11 is mainly based on a silicon-silicon carbide composite material" means that the columnar honeycomb section 11 contains 90% or more by mass of the silicon-silicon carbide composite material (total mass) based on the entire honeycomb structure. Here, the silicon-silicon carbide composite material contains silicon carbide particles as an aggregate and silicon as a binder to hold the silicon carbide particles together. Multiple silicon carbide particles are bound by silicon to form pores between them. The phrase "the material of honeycomb section 10 is mainly based on silicon carbide" means that honeycomb section 11 contains 90% or more by mass of silicon carbide (total mass) based on the entire honeycomb structure.
[0017] If the material of the columnar honeycomb section 11 is the silicon-silicon carbide composite material, the ratio of the mass of silicon as binder contained in the columnar honeycomb section 11 to the total mass of silicon carbide particles as aggregate contained in the columnar honeycomb section 11 and the mass of silicon as binder contained in the columnar honeycomb section 11 is preferably 10 to 40 percent by mass and more preferably 15 to 35 percent by mass. At 10 percent by mass or more, the strength of the columnar honeycomb section 11 is sufficiently maintained. At 40 percent by mass or less, the shape is easily retained during firing.
[0018] The shape of each cell in a cross-section perpendicular to an expansion direction of the cells 15 is not restricted, but is preferably a square, a hexagon, an octagon, or a combination thereof. Among these, the square and the hexagon are preferred. Such a cell shape can lead to a reduced pressure drop when exhaust gas flows through the honeycomb structure 10, resulting in an improvement in the cleaning performance of the catalyst. The rectangular shape is particularly preferred to achieve both structural strength and uniform heating.
[0019] Each of the partitions 13 forming the cells 15 preferably has a thickness of 0.1 to 0.3 mm and more preferably of 0.15 to 0.25 mm. A thickness of 0.1 mm or more for each partition 13 can suppress a decrease in the strength of the honeycomb structure. A thickness of 0.3 mm or less for each partition 13 can suppress an increase in pressure drop during the flow of exhaust gas when the honeycomb structure is used as a catalyst support and a catalyst is mounted on it. In the present invention, the thickness of the partition 13 is defined as the length of a section passing through the partition 13, along line segments connecting the centers of gravity of the adjacent cells 15, in a cross-section perpendicular to the direction of expansion of the cells 15.
[0020] The honeycomb structure 10 preferably has a cell density of 40 to 150 cells / cm². 2 and preferably 70 to 100 cells / cm² 2in a cross-section perpendicular to the flow direction of the cells 15. The cell density in such a region can increase the cleaning performance of the catalyst while reducing the pressure drop when an exhaust gas flows. If the cell density is less than 40 cells / cm² 2 If the cell density is higher than 150 cells / cm², the catalyst support area may decrease. 2 If the honeycomb structure 10 is used as a catalyst support and a catalyst is mounted on it, the pressure drop during the flow of exhaust gas can be increased. The cell density is a value obtained by dividing the number of cells by the area of one end face of the columnar honeycomb structure section 11, excluding the outer perimeter wall 12.
[0021] Providing the outer perimeter wall 12 of the honeycomb structure 10 is useful to ensure the structural strength of the honeycomb structure 10 and to prevent fluid flowing through the cells 15 from escaping from the outer perimeter wall 12. In particular, the thickness of the outer perimeter wall 12 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the outer perimeter wall 12 is too thick, the strength becomes too high, so that a strength equilibrium between the outer perimeter wall and the partition 13 is lost, thus reducing the thermal shock resistance. Therefore, the thickness of the outer perimeter wall 12 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less.As used herein, the thickness of the outer circumferential wall 12 is defined as a thickness of the outer circumferential wall 12 in a direction of a normal to a tangent at a measuring point when a section of the outer circumferential wall 12 is observed which is to be subjected to a thickness measurement in a cross-section perpendicular to a cell expansion direction.
[0022] The partition walls 13 can be porous. The porosity of the partition wall 13 is preferably 35 to 60% and more preferably 35 to 45%. A porosity of 35% or more can lead to easier suppression of deformation during firing. A porosity of 60% or less can allow sufficient maintenance of the strength of the honeycomb structure. The porosity is a value measured using a mercury porosimeter.
[0023] The partitions 13 of the columnar honeycomb structure section 11 preferably have an average pore diameter of 2 to 15 µm and more preferably 4 to 8 µm. An average pore diameter of 2 µm or more can prevent an excessively high electrical resistivity. An average pore diameter of 15 µm or less can prevent an excessively low electrical resistivity. The average pore diameter is a value measured using a mercury porosimeter.
[0024] The honeycomb structure 10 comprises a pair of electrode layers 14a, 14b, which are arranged on the surface of the outer circumferential wall 12 of the columnar honeycomb structure section 11 such that they face each other across a central axis of the columnar honeycomb structure section 11.
[0025] The electrode layers 14a, 14b can be formed in a non-restrictive region. To improve the uniform heat generation of the columnar honeycomb structure section 11, each of the electrode layers 14a, 14b is preferably arranged to extend in the circumferential and expansion direction of the cells 15 in the form of a belt. In particular, to facilitate current propagation in the axial direction of each of the electrode layers 14a, 14b, it is desirable that each of the electrode layers 14a, 14b extends over a length of 80% or more, and preferably 90% or more, and more preferably over the entire length between the two end faces of the columnar honeycomb structure section 11. Furthermore, the electrode layers 14a, 14b can be distributed on the outer surface of the outer circumferential wall 12.When the electrode layers 14a, 14b are dispersed, they are preferably provided at equal intervals on the outer surface of the outer circumferential wall 12 in the circumferential direction of the outer circumferential wall 12 and in the expansion direction of the cells 15, thereby improving the uniform heat generation of the columnar honeycomb structure section 11. The electrode layers 14a, 14b, which are in . Fig. 1 and Fig. The electrode layers 14a, 14b shown in Figure 2 are arranged such that each pair is distributed on the surface of the columnar honeycomb structure section 11. In particular, an example is shown in which a pair of electrode layers 14a, 14b is provided at a total of ten positions: at two positions in the circumferential direction of the columnar honeycomb structure section 11 and at five positions in the extensional direction of the cells 15.
[0026] Each of the electrode layers 14a, 14b consists of a metal-ceramic hybrid element. In such a configuration, the electrically heated support 20 according to embodiment 1 of the present invention does not require a stretchable metal element to be embedded in the ceramic electrode layer to suppress damage to the electrode layers. That is, since the electrode layers 14a, 14b are themselves formed from ceramic containing a metal, it is not necessary to form the electrode layers by separating the ceramic and the stretchable metal element, which have significantly different coefficients of thermal expansion, as described above. Therefore, fracture of the electrode layers due to a difference in thermal expansion during electrical heating can be satisfactorily suppressed.
[0027] Examples of the metal contained in the metal-ceramic hybrid element in electrode layers 14a and 14b include a single metal from Cr, Fe, Co, Ni, Si, or Ti, or an alloy containing at least one metal selected from this group. Non-restrictive examples of the ceramic contained in the metal-ceramic hybrid element in electrode layers 14a and 14b include silicon carbide (SiC), metal compounds such as metal silicides like tantalum silicide (TaSi₂) and chromium silicide (CrSi₂), and a composite material consisting of a combination of one or more of the conductive ceramics and one or more of the above metals (cermet).Specific examples of cermets include a composite material of metallic silicon and silicon carbide, a composite material of metallic silicide such as tantalum silicide and chromium silicide, metallic silicon and silicon carbide, and a composite material that, in addition to one or more of the metals listed above, contains one or more insulating ceramics such as aluminum oxide, mullite, zirconium oxide, cordierite, silicon nitride, and aluminum nitride to reduce thermal expansion. For the electrode layers 14a, 14b, a combination of a metal silicide such as tantalum silicide and chromium silicide with a composite material of metallic silicon and silicon carbide is preferable among the various metals and ceramics described above, as it can be fired simultaneously with the columnar honeycomb structure section, thus simplifying the manufacturing steps.
[0028] The electrode layers 14a, 14b preferably consist of a metal-ceramic composite with a metal content of 30 to 75 percent by volume. A metal content of 30 percent by volume or more can lead to further improved bonding properties by welding or thermal spraying to an external metal connection such as a power cable. A metal content of 75 percent by volume or less can result in a higher thermal expansion than that of the protective layer, thus suppressing cracking in the protective layer. The metal content in the electrode layers 14a, 14b is preferably 40 to 75 percent by volume and even more preferably 60 to 75 percent by volume, since the conduction resistance is reduced.
[0029] The honeycomb structure 10 has protective layers 17a, 17b that cover the electrode layers 14a and 14b, respectively, such that at least a portion of the electrode layers 14a, 14b is exposed. Furthermore, as described later, sections 18 of the electrode layers 14a, 14b that are exposed by the protective layers 17a, 17b are electrically connected to metal terminals 21a, 21b. This allows the electrode layers 14a, 14b to be protected by the protective layers 17a and 17b, respectively, so that an increase in resistance due to deterioration of the electrode layers 14a, 14b can be satisfactorily suppressed. The protective layers 17a, 17b have the function of protecting the electrode layers 14a, 14b from deterioration and, for example, prevent the electrode layers 14a, 14b from oxidizing.
[0030] A material that can be used for the protective layers 17a, 17b comprises ceramics, glass, or a composite material of ceramics and glass. Examples of the composite material that can be used include a material containing 50% or more by volume, preferably 60% or more by volume, and more preferably 70% or more by volume of glass. Examples of ceramics forming the protective layers 17a, 17b include ceramics such as those based on SiO2, Al2O3, SiO2, Al2O3, SiO2-ZrO2, and SiO2-Al2O3-ZrO2. Examples of the glass forming the protective layers 17a, 17b that can be used include glass such as lead-free glass based on B2O3-Bi2O3, B2O3-ZnO-Bi2O3, B2O3-ZnO, V2O5-P2O5, SnO-P2O5, SnO-ZnO-P2O5, SiO2-B2O3-Bi2O3 and SiO2-Bi2O3-Na2O.
[0031] Each of the electrode layers 14a, 14b preferably has a thickness of 0.01 to 5 mm and more preferably of 0.01 to 3 mm. Such a range can enable improved uniformity of heat generation. A thickness of 0.01 mm or more for each of the electrode layers 14a, 14b can lead to suitable control of the electrical resistance, resulting in more uniform heat generation. A thickness of 5 mm or less for each of the electrode layers 14a, 14b can reduce the risk of breakage during encapsulation. The thickness of each of the electrode layers 14a, 14b is defined as the thickness in the direction of a normal to a tangent at a measurement point on an outer surface of each of the electrode layers 14a, 14b, when the point of each electrode layer to be subjected to a thickness measurement in a cross-section is observed perpendicular to the cell expansion direction.
[0032] It is preferred that the maximum thickness of each of the protective layers 17a, 17b is 1.5 times or more the average thickness of each of the electrode layers 14a, 14b. That is, the maximum thickness of each of the protective layers 17a, 17b covering the electrode layers 14a and 14b, respectively, is preferably 1.5 times or more the average value (the average thickness of the electrode layer 14a) obtained by measuring the thicknesses at arbitrary positions of each of the electrode layers 14a, 14b. The electrode layers 14a, 14b, which consist of the metal-ceramic composite element, have a higher coefficient of thermal expansion during electrical heating than each of the protective layers 17a, 17b.The maximum thickness of each of the protective layers 17a, 17b is, however, 1.5 times or more the average thickness of each of the electrode layers 14a, 14b, thereby satisfactorily suppressing deformation of the electrode layers 14a, 14b due to thermal expansion. Accordingly, fracture of the electrode layers 14a, 14b can be satisfactorily suppressed. Since the strength of the protective layers 17a, 17b increases with increasing thickness, the maximum thickness of each of the protective layers 17a, 17b is preferably two times or more, and more preferably three times or more, the average thickness of each electrode layer 14a, 14b.
[0033] If the maximum thickness of each of the protective layers 17a, 17b is 1.5 times or more the average thickness of each of the electrode layers 14a, 14b, these layers are, for example, configured such that perhaps only a portion of the thickness of each of the electrode layers 14a, 14b is equal to the maximum thickness of each of the protective layers 17a, 17b, and a section with that portion of the thickness of each of the electrode layers 14a, 14b is section 18 of each electrode layer 14a, 14b that is exposed from each of the protective layers 17a, 17b. The electrode layers 14a, 14b can also be configured to be embedded in the protective layers 17a and 17b, respectively, and then a portion of each of the protective layers 17a, 17b can be machined and the electrode layers 14a, 14b can be excavated to form an exposed section 18.
[0034] The specific electrical resistance of each of the electrode layers 14a, 14b is lower than the electrical resistance of the columnar honeycomb section 11, causing the current to preferentially flow into the electrode layers and to propagate along the cell current path and circumferentially during electrical conduction. The specific electrical resistance of the electrode layers 14a, 14b is preferably 1 / 10 or less, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less of the specific electrical resistance of the columnar honeycomb section 11. However, if the difference in specific electrical resistance between the two becomes too large, the current concentrates between the ends of the opposite electrode layers, thus dissipating the heat generated in the columnar honeycomb section.Therefore, the specific electrical resistance of the electrode layers 14a, 14b is preferably 1 / 200 or more, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more of the specific electrical resistance of the columnar honeycomb structure section 11. In the present invention, the specific electrical resistance of the electrode layers 14a, 14b is a value measured at 400 °C using a four-wire method.
[0035] As it is in Fig. As shown in Figure 3, the electrode layers 14a, 14b can consist of a support section 22 on a surface side of the outer circumferential wall 12 of the columnar honeycomb structure section 11 and a projecting section 23 that rises from the support section 22. In the structure of Fig.3. The protective layers 17a and 17b cover the electrode layers 14a and 14b, respectively, such that at least a portion of the surface of the projecting section 23 is exposed. The support section 22 and the projecting section 23 can each be formed in any shape, including, but not limited to, for example, a flat plate shape with a plane such as a circle, an ellipse, or a polygon, or a rod shape extending to a certain length. The support section 22 and the projecting section 23 can each also be of any size. As non-restrictive examples, the thickness of the support section 22 can be 50 to 300 µm, and the thickness of the projecting section 23 can be 100 to 200 µm.
[0036] Each of the electrode layers 14a, 14b can have the shape shown in the schematic top view of Fig.Figure 4 shows that each of the electrode layers 14a, 14b can be formed from several linear sections 24, in which the support section 22 extends radially from a central point directly below the projecting section 23 along the surface of the outer circumferential wall 12 of the columnar honeycomb structure section 11. In such a structure, the projecting section 23 can be in a columnar shape, an elliptical columnar shape, a prismatic shape, or the like. Fig.The multiple linear sections 24, extending radially from the central point directly below the projecting section 23, each have an angle θ formed by the other linear section (an angle formed by the center lines 29 of two adjacent linear sections 24) of approximately 60°, and all six linear sections are shown. It is not necessary for the multiple linear sections 24 to have the same angle θ, and the angles may differ from one another. The number of linear sections 24 is not particularly restricted and may be three, four, five, or more.The length L1 and width d of each linear section 24 are not particularly restricted and can be suitably designed based on the relationships and adhesion with the number of electrode layers 14a, 14b provided in the columnar honeycomb structure section 11, the size of the projecting section 23, and the like. For example, in the case where the electrode layers 14a, 14b each have the shape as shown in . Fig. Figure 4 shows a cross-section perpendicular to the direction in which the projecting sections 23 of the electrode layers 14a, 14b project, a circle with a diameter of 0.5 to 2 µm, a length L1 of 5 to 30 µm, and a width d of 0.5 to 2 µm. Furthermore, the support section 22 of the electrode layers 14a, 14b can have at least one branching section that branches from the several radially extending linear sections 24.
[0037] Each of the electrode layers 14a, 14b, which are in Fig. The structure shown in section 4 is preferably provided in several areas on the columnar honeycomb structure section 11 at a respective distance L2, as shown in Fig. Figure 5 shows that this can further improve the uniform heat generation of the columnar honeycomb structure section 11. The spacing L2 is not particularly limited and can be suitably designed based on the number, size, and other characteristics of the electrode layers 14a, 14b provided on the columnar honeycomb structure section 11. For example, if the length L1 of each linear section 24 of each of the electrode layers 14a, 14b is 5 to 30 µm, then each spacing L2 can be 15 to 60 mm. (1-2. Metal connection)
[0038] The pair of metal terminals 21a, 21b are arranged such that one metal terminal from the pair faces the other metal terminal from the pair across the central axis of the columnar honeycomb section 11 of the honeycomb structure 10, and are each provided on the pair of electrode layers 14a and 14b, respectively. The metal terminals 21a, 21b are electrically connected to the electrode layers 14a and 14b at sections 18 of the electrode layers 14a and 14b that are exposed by the protective layers 17a and 17b, respectively. When a voltage is applied to the metal terminals 21a, 21b through the electrode layers 14a, 14b, a corresponding current is conducted through the metal terminals 21a, 21b, enabling the honeycomb structure 10 to generate heat through Joule heating. Therefore, the honeycomb structure 10 can also be used as a suitable heater.The applied voltage is preferably 12 to 900 V and more preferably 64 to 600 V, although the applied voltage can be changed as required. The sections 18 of the electrode layers 14a, 14b, which are exposed by the protective layers 17a and 17b respectively, can be sections to be joined to the metal terminals 21a, 21b. The metal terminals 21a, 21b can be electrically connected to the electrode layers 14a, 14b via other conductive materials at the sections 18 exposed by the protective layers 17a, 17b.
[0039] The material of the metal terminals 21a, 21b is not particularly restricted, as long as it is a metal, and a single metal, an alloy, or the like may be used. With regard to corrosion resistance, electrical resistance, and coefficient of linear expansion, the material is, for example, preferably an alloy containing at least one element selected from the group consisting of Cr, Fe, Co, Ni, and Ti, and preferably stainless steel and Fe-Ni alloys. The shape and size of each of the metal terminals 21a, 21b are not particularly restricted, and they may be designed according to the size of the electrically heated support 20, the electrical conductivity, and the like.
[0040] By carrying the catalyst on the electrically heated support 20, the electrically heated support 20 can be used as a catalyst. For example, a fluid such as exhaust gas from a motor vehicle can flow through the flow paths of the multiple cells 15. Examples of the catalyst include precious metal catalysts or catalysts other than these. Illustrative examples of precious metal catalysts include a three-way catalyst and an oxidation catalyst obtained by carrying a precious metal such as platinum (Pt), palladium (Pd), and rhodium (Rh) on the surfaces of pores made of aluminum oxide and containing a co-catalyst such as cerium oxide and zirconium oxide, or a lean nitrogen oxide trap catalyst (LNT catalyst) that uses an alkaline earth metal and platinum as storage components for nitrogen oxides (NOx). x). Illustrative examples of a catalyst that does not use a precious metal include a catalyst with NO. x -selective catalytic reduction (SCR catalyst) containing a copper-substituted or iron-substituted zeolite and the like. Furthermore, two or more catalysts selected from the group consisting of these catalysts may be used. The method for carrying the catalyst is not particularly restricted and can be carried out according to a conventional method for carrying the catalyst onto the honeycomb structure. (2. Method for manufacturing a carrier of the electrically heated type)
[0041] A method for manufacturing the electrically heated carrier 20 according to the present invention will now be described by way of illustration. In one embodiment, the method for manufacturing the electrically heated carrier 20 according to the present invention comprises: a step A1 of obtaining an unfired honeycomb structure section with an electrode coating paste; a step A2 of firing the unfired honeycomb structure section with the electrode coating paste to form a fired honeycomb body; a step A3 of providing the honeycomb-shaped body with protective layers to obtain a honeycomb structure; and a step A4 of welding metal connections to the honeycomb structure.
[0042] Step A1 consists of producing a honeycomb-shaped body, which is a precursor to the honeycomb structure section, and applying an electrode layer formation paste to a side face of the honeycomb-shaped body to obtain an unfired honeycomb structure section with the electrode layer formation paste. The production of the honeycomb-shaped body can be carried out according to a known method for producing a honeycomb structure. For example, a forming material is first prepared by adding metallic silicon powder (metallic silicon), a binder, surfactant(s), a pore-forming agent, water, and the like to silicon carbide powder (silicon carbide). It is preferred that the mass of metallic silicon is 10 to 40 percent by mass, based on the total mass of silicon carbide powder and the mass of metallic silicon.The average particle diameter of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 µm and more preferably 3 to 40 µm. The average particle diameter of the metallic silicon (in the metallic silicon powder) is preferably 2 to 35 µm. The average particle diameter of both the silicon carbide particles and the metallic silicon (in the metallic silicon particles) refers to an arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction. The silicon carbide particles are fine silicon carbide particles that constitute the silicon carbide powder, and the metallic silicon particles are fine particles of metallic silicon that constitute the metallic silicon powder.It should be noted that this formula is for forming raw materials in the case where the material of the honeycomb structure section is the silicon-silicon carbide composite material. In the case where the material of the honeycomb structure section is silicon carbide, no metallic silicon is added.
[0043] Examples of binders include methylcellulose, hydroxypropylmethylcellulose, hydroxypropoxylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyvinyl alcohol, and the like. Among these, the use of methylcellulose in combination with hydroxypropoxylcellulose is preferred. The binder content is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.
[0044] The water content is preferably 20 to 60 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.
[0045] The surfactant that can be used includes ethylene glycol, dextrin, fatty acid soaps, polyalcohols, and the like. These can be used alone or in combination with two or more. The surfactant content is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.
[0046] The pore-forming agent is not particularly restricted, as long as it forms pores itself after firing, and includes, for example, graphite, starch, foamed resins, water-absorbing resins, silica gel, and the like. The pore-forming agent content is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass. The average particle diameter of the pore-forming agent is preferably 10 to 30 µm. If the average particle diameter is less than 10 µm, the pores may not form sufficiently. If the average particle diameter is more than 30 µm, a nozzle may become clogged during formation.The average particle diameter of the pore-forming agent refers to an arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction. If the pore-forming agent is the water-absorbing resin, the average particle diameter of the pore-forming agent is the average particle diameter after water absorption.
[0047] The resulting raw materials are then kneaded to form a green body, which is then extruded to produce a honeycomb structure. During extrusion, a die with a desired overall shape, cell shape, diaphragm thickness, cell density, and the like can be used. Preferably, the resulting honeycomb structure is then dried. If the length along the central axis of the honeycomb structure is not the desired length, both end faces of the honeycomb structure can be trimmed to the required length. The honeycomb structure after drying is referred to as a dried honeycomb body.
[0048] The electrode layer formation paste for forming electrode layers is then produced. This paste can be formed by appropriately adding and kneading various additives into raw material powder (metal powder, ceramic powder, and the like), which is formulated according to the required properties of the electrode layers. When each electrode layer is formed as a laminated structure, the bond strength between each metal terminal and each electrode layer tends to be improved by increasing the average particle diameter of the metal powder in the paste for the second electrode layer compared to the average particle diameter of the metal powder in the paste for the first electrode layer.The average particle diameter of the metal powder refers to an arithmetic mean diameter on a volume basis when the frequency distribution of the particle diameter is measured by laser diffraction methods.
[0049] The resulting electrode layer formation paste is applied to the side surface of the honeycomb-shaped body (typically the dried honeycomb body) to create an unfired honeycomb structure section with an electrode layer formation paste. The process for producing the electrode layer formation paste and the process for applying the electrode layer formation paste to the honeycomb-shaped body can be carried out according to a known method for producing a honeycomb structure. However, to achieve a lower specific electrical resistance, it is possible to increase the metal content or to decrease the particle diameter of the metal particles compared to the honeycomb structure section.
[0050] As a variation of the process for producing the honeycomb structure, in step A1 the honeycomb-shaped body can be temporarily baked before the electrode layer formation paste is applied. That is, in this variation, the honeycomb-shaped body is baked to create a baked honeycomb structure, and the baked electrode paste is applied to the baked honeycomb structure.
[0051] In step A2, the unfired honeycomb structure section is fired with the electrode layer formation paste to obtain a honeycomb structure. Prior to firing, the unfired honeycomb structure can be dried with the electrode layer formation paste. Degreasing can also be performed prior to firing to remove the binder and similar substances. For firing conditions, the unfired honeycomb structure is preferably heated to 1400 to 1500 °C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon. After firing, an oxidation treatment is preferably carried out for 1 to 10 hours at 1200 to 1350 °C to improve durability. The degreasing and firing methods are not particularly restricted and can be carried out using an electric furnace, a gas furnace, or the like.
[0052] In step A3, each protective layer is provided to cover the respective electrode layers of the fired honeycomb body, forming a honeycomb structure. At this stage, each protective layer may be provided such that at least a portion of each electrode layer is exposed. Alternatively, a portion of each electrode layer may be exposed by forming each protective layer to cover the entire electrode layer and then removing a portion of each protective layer. A method for forming each protective layer may be performed using a sputtering process or by depositing or spraying a material and subsequently heating it, although this depends on the material. Furthermore, the electrode layer and the protective layer may not be formed in separate steps, and the electrode layer and the protective layer may be formed simultaneously by firing.In particular, a honeycomb structure provided with electrode layers and protective layers can be produced by further providing protective layers on the unfired honeycomb structure section with the electrode layer formation paste and then firing it.
[0053] In step A4, each metal connection is welded to the exposed surface of the respective electrode layers of the honeycomb structure. Laser welding from the metal connection side may be a preferred welding method with regard to control of the welding area and production efficiency. <Ausführungsform 2>
[0054] An electrically heated support 30 according to embodiment 2 of the present invention has the same configuration as the electrically heated support 20 according to embodiment 1, except that the former does not have a metal connection. That is, the electrically heated support 30 according to embodiment 2 has the same configuration as the honeycomb structure 10 of the electrically heated support 20 according to embodiment 1, as shown in Fig. 2 is shown. The carrier 30 of the electrically heated type can be used as in embodiment 1 as a carrier of the electrically heated type by providing metal terminals to sections of the electrode layers exposed by the protective layers in order to connect them electrically. (3. Exhaust gas purification device)
[0055] The electrically heated support according to the embodiment of the present invention can be used for an exhaust gas purification device. The exhaust gas purification device comprises the electrically heated support and a housing for holding the electrically heated support. In the exhaust gas purification device, the electrically heated support can be installed in an exhaust gas flow path through which exhaust gas from a power engine can flow. A metal tube element or the like can be used as the housing for receiving the electrically heated support. Examples
[0056] Examples are given below to better understand the present invention and its advantages, but the present invention is not limited to these examples. <Beispiel 1> (1. Production of a circular column-shaped green body)
[0057] Silicon carbide powder (SiC powder) and metallic silicon powder (Si powder) were mixed in a mass ratio of 80:20 to produce a ceramic raw material. Hydroxypropyl methylcellulose was added to the ceramic raw material as a binder, a water-absorbing resin as a pore-forming agent, and water to form a molding raw material. The molding raw material was then kneaded using a vacuum green body kneader to produce a circular column-shaped green body. The binder content was 7 parts by mass when the total amount of silicon carbide powder (SiC powder) and metallic silicon powder (Si powder) was 100 parts by mass. The pore-forming agent content was 3 parts by mass when the total amount of silicon carbide powder (SiC powder) and metallic silicon powder (Si powder) was 100 parts by mass.The water content was 42 parts by mass when the total amount of silicon carbide powder (SiC powder) and metallic silicon powder (Si powder) was 100 parts by mass. The average particle diameter of the silicon carbide powder was 20 µm, and the average particle diameter of the metallic silicon powder was 6 µm. The average particle diameter of the pore-forming agent was also 20 µm. The average particle diameters of the silicon carbide powder, the metallic silicon powder, and the pore-forming agent, respectively, are calculated as a volume-based arithmetic mean diameters when the particle size frequency distribution is measured by laser diffraction. (2. Production of the dried honeycomb body)
[0058] The resulting columnar green body was formed using an extruder with a grid-patterned die structure to obtain a circular columnar honeycomb body in which, in a cross-section perpendicular to the flow path of the cells, each cell had a square shape. The honeycomb body was subjected to dielectric high-frequency heating and drying, and then dried for 2 hours at 120 °C using a hot air dryer. A predetermined amount was then trimmed from both end faces to produce a dried honeycomb body. (3. Preparation of the electrode layer formation paste)
[0059] Tantalum silicide powder (TaSi₂ powder), metallic silicon powder (Si powder), silicon carbide powder (SiC powder), methylcellulose, glycerin, and water were mixed using a planetary centrifugal mixer to produce an electrodeposition paste. The TaSi₂ powder, Si powder, and SiC powder were mixed in a volume ratio of 50:30:20. With a total mass of 100 parts by mass of TaSi₂ powder, Si powder, and SiC powder, methylcellulose comprised 0.5 parts by mass, glycerin 10 parts by mass, and water 38 parts by mass. The average particle diameter of the tantalum silicide powder was 7 µm. The average particle diameter of the metallic silicon powder was 6 µm. The average particle diameter of the silicon carbide powder was 35 µm.These average particle diameters each refer to an arithmetic mean diameter on a volume basis when the frequency distribution of the particle diameter is measured by laser diffraction methods. (4. Applying the paste)
[0060] The electrode layer formation pastes were applied as described above at the ten positions in total (five positions × two rows for one side), as shown in the electrode layer arrangement of Fig. Figure 2 shows the electrodes being applied so that they face each other across the central axis. After the application of the electrode layer formation paste, the dried honeycomb structure was then dried at 120 °C to obtain an unfired honeycomb structure section containing the electrode layer formation paste. (5. Burning)
[0061] The unfired honeycomb structure section with the electrode-forming paste was then degreased in an air atmosphere at 550 °C for 3 hours. The degreased, unfired honeycomb structure section with the electrode-forming paste was then fired and subjected to an oxidation treatment to produce a fired honeycomb body. The firing was carried out in an argon atmosphere at 1450 °C for 2 hours. The oxidation treatment was carried out for one hour in the atmosphere at 1300 °C.
[0062] The fired honeycomb structure had circular end faces, each with a diameter of 100 mm and a height (length in the direction of cell flow) of 100 mm. The cell density was 93 cells / cm³. 2The partition wall thickness was 101.6 µm, the partition wall porosity was 45%, and the average pore diameter of the partition walls was 8.6 µm. The thickness of each electrode layer was 0.2 mm. The specific electrical resistivity at 400 °C was measured using a four-wire method with samples made of the same materials as the honeycomb structure and the electrode layer, yielding values of 5 Ωcm, 0.01 Ωcm, and 0.001 Ωcm, respectively. (6. Formation of the protective layer)
[0063] Glass was then applied to cover each electrode layer of the fired honeycomb structure, and the structure was subsequently fired in an air atmosphere at 1000 °C for 6 hours to form each protective layer with the thickness shown in Table 1. A portion of each protective layer was then removed from each electrode layer using a milling cutter, leaving a surface area of 3.14 mm² for each electrode layer. 2was exposed. Thus, the honeycomb structures were created according to examples 1 to 4.
[0064] Furthermore, as a comparative example 1, a honeycomb structure was produced using the same method as in example 1, except that each electrode layer consisted of SUS430 and no protective layer was provided. (7. Welding of metal connections)
[0065] Plate-shaped SUS metal connectors (each dimension: 30 mm × 50 mm × 0.5 mm) were brought into contact with the exposed sections of the respective electrode layers of the honeycomb structure, which were obtained under the manufacturing conditions described above. Subsequently, each plate-shaped metal connector was irradiated with a laser at a power of 180 W / mm². 2Each electrode layer was welded from the metal connection side using a fiber laser welding machine. The thickness of each plate-shaped metal connection was 0.4 mm. Thus, each sample of each type of electrically heated support was produced. (8. Electric heating test)
[0066] An external power supply was connected to the metal terminals of each sample, and electrical heating was performed for 30 seconds at an applied voltage of 300 V. The electrical heating test was then repeated 50 times. Subsequently, for each sample, after repeated electrical heating tests, the presence or absence of electrode layer fractures was checked, depending on whether electrical conductivity was possible or not. A sample in which electrical conductivity was possible was defined as "OK," indicating that a honeycomb structure exhibiting the effects of the present invention was obtained. Conversely, a sample in which electrical conductivity was not possible was defined as "NG," indicating that it exhibited a honeycomb structure that did not possess the effects of the present invention.Furthermore, the specific electrical resistance at 400 °C was measured for each sample after 50 electrical heating cycles using a four-terminal method, and an increase rate (resistance increase rate) was measured compared to that before electrical heating.
[0068] [Table 1] Electrode layer material Electrode layer thickness [mm] Thickness of protective layer [mm] Possibility of electrical conduction Resistance increase rate [factor] Comparison 1 SUS430 0,2 - NG - Example 1 50TaSi / 30Si / 20S iC 0,2 0,3 OK 1,7 Example 2 50TaSi / 30Si / 20S iC 0,2 0,4 OK 1,4 Example 3 50TaSi / 30Si / 20S iC 0,2 0,6 OK 1,2 Comparison 2 50TaSi / 30Si / 20S iC 0,2 1,0 OK 1,2
[0069] (9. Discussion)
[0067] In examples 1 to 4, each electrode layer consisted of the metal-ceramic hybrid element, exhibited a reduced difference in thermal expansion compared to the columnar honeycomb structure, and showed no damage even after repeated 50 electrical heating cycles. Furthermore, it is believed that each protective layer suppresses oxidation, even when the temperature of each electrode layer is increased, and that deterioration of each electrode layer can be successfully prevented. This would be evident from the favorable results of resistance increase rates of 1.7-fold or less.
[0068] In Examples 2 to 4, because each protective layer was designed to have an increased thickness compared to Example 1, the strength of each protective layer was increased and the fracture of each protective layer due to the difference in thermal expansion was more satisfactorily suppressed. Consequently, it is believed that the oxidation of each electrode layer was suppressed and an increase in resistance was more satisfactorily suppressed.
[0069] On the other hand, in comparative example 1, every electrode layer was destroyed as a result of embedding a metal as the electrode layer material. In comparative example 1, no protective layer was provided, and every electrode layer would degrade after 50 repetitions of electrical heating.
[0070] List of reference symbols 10 honeycomb structure 11 columnar honeycomb structure section 12 Outer perimeter wall 13 Partition wall 14a, 14b Electrode layer 15 cells 17a, 17b Protective layer 21a, 21b Metal connection 22 Carrier section 23 Highlighted section 24 Linear section 29 Center line of the linear section 20, 30 carriers of the electrically heated type
Claims
[1] Carrier (20, 30) of the electrically heated type, comprising: - a honeycomb structure (10) comprising: a columnar honeycomb structure portion (11) comprising: an outer peripheral wall (12); and porous partition walls (13) disposed on an inner side of the outer peripheral wall (12), the porous partition walls (13) defining a plurality of cells (15), each of the cells (15) extending from one end face to the other end face to form a flow path; a pair of electrode layers (14a, 14b) arranged to face each other across a central axis of the columnar honeycomb structure portion (11), each of the pair of electrode layers (14a, 14b) being arranged on a surface of the outer peripheral wall (12); and protective layers (17a, 17b) each covering the electrode layers (14a, 14b) such that at least a part of each of the pair of electrode layers (14a, 14b) is exposed; and - a pair of metal terminals (21a, 21b) provided on the pair of electrode layers (14a, 14b), wherein each of the pair of electrode layers (14a, 14b) consists of a metal-ceramic mixing element and wherein a portion of each of the pair of electrode layers (14a, 14b) exposed from the protective layer (17a, 17b) is electrically connected to each of the pair of metal terminals (21a, 21b). [2] The electrically heated type carrier (20, 30) according to claim 1, wherein each of said pair of electrode layers (14a, 14b) is made of a metal-ceramic mixed element having a metal content of 30 to 75 volume percent. [3] The electrically heated type carrier (20, 30) according to claim 1 or 2, wherein a maximum thickness of each of the pair of protective layers (17a, 17b) is 1.5 times or more of an average thickness of each of the pair of electrode layers (14a, 14b). [4] Carrier (20, 30) of the electrically heated type according to one of claims 1 to 3, wherein each of the pair of electrode layers (14a, 14b) comprises: a support portion (22) on a surface side of the outer peripheral wall (12); and a protruding portion (23) rising from the support portion (22), and wherein each of the pair of protective layers (17a, 17b) is provided such that at least a part of a surface of the protruding portion (23) is exposed. [5] The electrically heated type support (20, 30) according to claim 4, wherein the support portion (22) is formed of a plurality of linear portions (24) extending radially from a center directly below the protruding portion (23) along the surface of the outer peripheral wall (12). [6] The electrically heated type carrier (20, 30) according to claim 5, wherein the carrier portion (22) further comprises at least one branch portion branched from the plurality of linear portions (24) extending radially. [7] The electrically heated type substrate (20, 30) according to any one of claims 1 to 6, wherein each of the pair of electrode layers (14a, 14b) is divided into a plurality of regions. [8] The electrically heated type substrate (20, 30) according to any one of claims 1 to 7, wherein the portion of each of the pair of electrode layers (14a, 14b) exposed from each of the pair of protective layers (17a, 17b) is a portion to be connected to each of the metal terminals (21a, 21b). [9] Exhaust gas purification device comprising: the carrier (20, 30) of the electrically heated type according to any one of claims 1 to 8; and a can body for holding the electrically heated type carrier (20, 30). [10] Carrier (20, 30) of the electrically heated type, comprising: a honeycomb structure (10) comprising: a columnar honeycomb structure portion (11) comprising: an outer peripheral wall (12); and porous partition walls (13) disposed on an inner side of the outer peripheral wall (12), the porous partition walls (13) defining a plurality of cells (15), each of the cells (15) extending from one end face to the other end face to form a flow path; a pair of electrode layers (14a, 14b) arranged to face each other across a central axis of the columnar honeycomb structure portion (11), each of the pair of electrode layers (14a, 14b) being arranged on a surface of the outer peripheral wall (12); and Protective layers (17a, 17b) each covering the electrode layers (14a, 14b) such that at least a part of each of the pair of electrode layers (14a, 14b) is exposed, wherein each of the pair of electrode layers (14a, 14b) consists of a metal-ceramic mixing element and wherein each of the pair of electrode layers (14a, 14b) has a portion exposed from the protective layer (17a, 17b) and is adapted for electrical connection to each of the metal terminals (21a, 21b).
Citation Information
Patent Citations
Electric heater for a catalytic converter and method for its production
DE102017109206A1
Electrically heated catalyst device and method for manufacturing the same
JP5786961B2
JP000005786961B2