Honeycomb structure, honeycomb structure of the electric heating type, catalytic converter of the electric heating type and exhaust gas purification device

A honeycomb structure with silicon-based ceramics and controlled dopant concentrations addresses excessive current issues in EHCs, ensuring effective exhaust gas purification and thermal resistance under varying voltages.

DE102020203665B4Active Publication Date: 2024-11-14NGK INSULATORS LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
DE102020203665
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-18
Filing Date
2020-03-20
Publication Date
2024-11-14
Estimated Expiration
2040-03-20

AI Technical Summary

Technical Problem

Existing honeycomb structures used in electrically heated catalysts (EHC) for exhaust gas purification face issues with excessive current generation when used under lower voltages, necessitating a solution to suppress this phenomenon effectively.

Method used

The honeycomb structure is composed of ceramics containing at least 30% silicon by mass with controlled dopant concentrations between 10^16 cm^-3 to 5 x 10^20 cm^-3, specifically using Group 13 or Group 15 elements like boron, aluminum, nitrogen, or phosphorus, to adjust volume resistivity within the range of 0.01 to 5 Ω cm, thereby preventing excessive current flow even at lower voltages.

Benefits of technology

This configuration effectively suppresses excessive current generation at lower voltages, enhances thermal shock resistance, and maintains structural integrity while ensuring rapid heating and efficient exhaust gas purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

honeycomb structure (10) which includes: an outer perimeter wall (12); and Partitions (13) arranged on an inside of the outer circumferential wall (12), wherein the partitions (13) define several cells (15), each of the several cells (15) extending from one end face to the other end face to form a flow path for a fluid, wherein the partition walls (13) and the outer circumferential wall (12) comprise ceramic containing at least silicon as a simple substance that is not a silicon compound; where the silicon content in the ceramic is 30% by mass or more; wherein a concentration of at least one dopant in the silicon of 10 16 cm -3 up to 5 · 10 20 cm -3 amounts.
Need to check novelty before this filing date? Find Prior Art

Description

AREA OF INVENTION

[0001] The present invention relates to a honeycomb structure, a honeycomb structure of the electric heating type, a support of the electric heating type, and an exhaust gas purification device. In particular, the present invention relates to a honeycomb structure, a honeycomb structure of the electric heating type, a support of the electric heating type, and an exhaust gas purification device that are capable of sufficiently preventing the generation of excessive current even when used at a lower voltage. BACKGROUND OF THE INVENTION

[0002] Traditionally, a catalyst-based system supported by a honeycomb structure made of cordierite or silicon carbide is used to treat harmful substances in exhaust gases emitted by motor vehicles. Such a honeycomb structure generally has a columnar honeycomb pattern containing partitions that define multiple cells running from one end face to the other to form flow paths for the exhaust gas.

[0003] For the exhaust gas treatment with the honeycomb-supported catalyst, it is necessary to raise the catalyst's temperature to a predetermined level. However, the catalyst temperature is lower during engine start-up, which conventionally causes problems with insufficient exhaust gas purification. Therefore, a system called an electrically heated catalyst (EHC) has been developed. In this system, electrodes are arranged on a honeycomb structure made of conductive ceramic, and the honeycomb structure itself generates heat through electrical conduction. This heat raises the temperature of the honeycomb-supported catalyst to an activation temperature before or during engine start-up.

[0004] When the EHC is used, for example, mounted on a motor vehicle or similar vehicle, it is typically powered by a power source intended for the vehicle's electrical system. Therefore, an excessive current flowing through the EHC can damage the power supply circuit. Since different voltages are used to power the EHC, it is crucial to adjust the resistance of the honeycomb structure for each voltage and control it to prevent excessive current flow.

[0005] Patent literature 1 proposes a honeycomb structure with a specific volume resistance in a certain area, which serves as a catalyst support and also functions as a heating device.

[0006] Further state of the art is also known from patent literature 2 to 5. Counter-arguments list Patent literature Patent literature 1: Japanese patent no. JP 5 735 428 B2 Patent literature 2: Chinese patent application no. CN 108 006 666 A Patent Literature 3: US Patent Application No. US 2011 / 0 250 095 A1 Patent Literature 4: US Patent Application No. US 2012 / 0 186 455 A1 Patent literature 5 German Patent No. DE 10 2017 204 329 B4 SUMMARY OF THE INVENTION

[0007] The present invention is specified as follows: (1) Honeycomb structure comprising: an outer perimeter wall; and partitions arranged on an inner side of the outer perimeter wall, the partitions defining multiple cells, each of the multiple cells extending from one end face to the other end face to form a flow path for a fluid, wherein the partition walls and the outer perimeter wall comprise ceramic containing at least silicon as a simple substance that is not a silicon compound; wherein the silicon content in the ceramic is 30 wt% or more; wherein the concentration of at least one dopant in the silicon is 10 16 cm -3 up to 5 · 10 20 cm -3 amounts. (2) Honeycomb structure of electric heating type, comprising: the honeycomb structure according to (1); and a pair of electrode layers arranged opposite each other via a central axis of the honeycomb structure, each of the electrode layers being located on a surface of the outer circumferential wall of the honeycomb structure. (3) Carrier of the type electric heating, comprising: the honeycomb structure of the electric heating type according to (2); and a pair of metal terminals arranged opposite each other via a central axis of the honeycomb structure of the electric heating type, wherein the pair of metal terminals is arranged on the pair of electrode layers. (4) Exhaust gas purification device comprising: the electric heating type carrier according to (3); and a canister body for holding the electric heating type carrier. (5) Honeycomb structure comprising: an outer perimeter wall; and partitions arranged on an inner side of the outer perimeter wall, the partitions defining multiple cells, each of the multiple cells extending from one end face to the other end face to form a flow path for a fluid, wherein the partition walls and the outer perimeter wall comprise ceramic, wherein the ceramic contains: Silicon as a simple substance that is not a silicon compound; and at least one selected from the group consisting of aluminium oxide, mullite, zirconium dioxide, cordierite, silicon carbide, silicon nitride and aluminium nitride; wherein the silicon content in the ceramic is 30 wt% or more; wherein the silicon contains boron (B) as a dopant; and wherein the honeycomb structure has a specific volume resistivity of 0.01 Ω·cm or more and 5 Ω·cm or less. BRIEF DESCRIPTION OF THE DRAWINGS Fig. Figure 1 is a schematic external view of a honeycomb structure 10 according to an embodiment of the present invention. Fig. Figure 2 is a schematic external view of a honeycomb structure 30 of the type electric heater according to an embodiment of the present invention. Fig.Figure 3 is a schematic cross-sectional view of a carrier 20 of the type electric heating, which is perpendicular to a direction of the cells, according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0008] The honeycomb structure described in patent literature 1 is formed from a Si-SiC material. Si and SiC exhibit a slightly higher specific volume resistivity. Thus, even when the honeycomb structure, as described in patent literature 1, is used for the EHC operating at a higher voltage of 200 to 500 V, the specific volume resistivity can be adjusted within a resistance range of approximately several Ωcm to 200 Ωcm. As a result, it can prevent excessive current flow when used at a higher voltage of 200 to 500 V.

[0009] However, a very wide voltage range is used for the power supply of the EHC, depending, for example, on the types of vehicles being assembled and the like. In particular, it is necessary to adjust the specific volume resistance to a resistance range on the order of 0.1 Ωcm to prevent the generation of excessive current when the power supply for the EHC uses a lower voltage of 60 V or less, e.g., 48 V. Therefore, in the latest EHC, where a wide voltage range is used, there is a need for research and development of a technique to satisfactorily prevent the generation of excessive current, even when operating at a lower voltage.

[0010] The present invention was made in light of the problems mentioned above. One object of the present invention is to provide a honeycomb structure, an electric heating honeycomb structure, an electric heating support, and an exhaust gas purification device that can satisfactorily prevent the generation of excessive current even when used at a low voltage.

[0011] As a result of intensive investigations, the inventors have determined that the above problems can be solved by including at least silicon in the partition walls and the outer perimeter wall of the honeycomb structure and by controlling the concentration of one or more dopants in the silicon to a predetermined range.

[0012] According to the present invention, it is possible to create a honeycomb structure, an electric heating honeycomb structure, an electric heating carrier, and an exhaust gas purification device that can satisfactorily prevent the generation of excessive current even when used at a lower voltage.

[0013] The following describes embodiments of the honeycomb structure, a honeycomb structure of the electric heating type, a support of the electric heating type, and an exhaust gas purification device according to the present invention, with reference to the drawings. However, the present invention is not limited to these embodiments, and various modifications, alterations, and improvements can be added based on the knowledge of a person skilled in the art without deviating from the scope of protection of the present invention. (1. Honeycomb structure and honeycomb structure of the electric heating type)

[0014] Fig. Figure 1 is a schematic external view of a honeycomb structure 10 according to an embodiment of the present invention. The honeycomb structure 10 comprises: an outer circumferential wall 12; and partitions 13 arranged on an inner surface of the outer circumferential wall 12, defining multiple cells 15 extending from one end face to the other end face to form flow paths, wherein the honeycomb structure 10 is columnar.

[0015] The partition walls 13 and the outer circumferential wall 12 of the honeycomb structure 10 are made of ceramic containing at least silicon and have a concentration of at least one dopant in the silicon of 10 16 up to 5 · 10 20 cm -3Examples of ceramic materials other than silicon that form the partitions 13 and the outer circumferential wall 12 of the honeycomb structure 10 include, but are not limited to, oxide ceramics such as aluminum oxide, mullite, zirconium dioxide, and cordierite, as well as non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride. Since these ceramic materials function as aggregate particles for the honeycomb structure 10, the honeycomb structure 10 can be reinforced.

[0016] In the honeycomb structure 10 according to an embodiment of the present invention, the concentration of the doping agent in the silicon 10 contained in the partition walls 13 and in the outer circumferential wall 12 is 16 up to 5 · 10 20 cm -3, so that the specific volume resistivity of the honeycomb structure 10 can be reduced. The concentration of the dopant in the silicon contained in the partitions 13 and in the outer circumferential wall 12 can be adjusted as required, depending on the desired specific volume resistivity of the honeycomb structure 10. In general, the specific volume resistivity of the honeycomb structure 10 decreases as the concentration of the dopant in silicon increases, and conversely, the specific volume resistivity of the honeycomb structure 10 increases as the concentration of the dopant in silicon decreases. The inventors have determined that the specific volume resistivity of the honeycomb structure 10 can be effectively reduced by doping with silicon as a simple substance instead of a silicon compound such as silicon carbide and silicon nitride, which act as aggregate particles as described above.Preferably, the concentration of the doping agent in silicon is 5 · 10. 17 up to 5 · 10 20 cm -3 .

[0017] The specific volume resistivity of the honeycomb structure 10 can be adjusted as required depending on an applied voltage and is not particularly limited. For example, it can be adjusted from 0.001 to 200 Ω·cm. For higher voltages above 60 V, it can range from 2 to 200 Ω·cm, and typically from 5 to 100 Ω·cm. For lower voltages of 60 V or less, such as about 48 V, the specific volume resistivity can range from 0.001 to 2 Ω·cm, and typically from 0.001 to 1 Ω·cm, and even more commonly from 0.01 to 1 Ω·cm. In particular, the concentration of the dopant in the silicon contained in the partitions 13 and in the outer circumferential wall 12 in the honeycomb structure 10 according to one embodiment of the present invention is 10 16 up to 5 · 10 20 cm-3 , so that the specific volume resistivity of the honeycomb structure 10 can be reduced in such a way that no excessive current is generated even when it is used at a lower voltage of 60 V or less than 48 V. Furthermore, the specific volume resistivity of the honeycomb structure can be 0.01 Ω·cm or more and 5 Ω·cm or less. If the specific volume resistivity is 5 Ω·cm or less, the generation of excess current can be satisfactorily suppressed even at a lower voltage of 48 V. On the other hand, the generation of excess current cannot be sufficiently suppressed at a lower voltage of 48 V if the specific volume resistivity is more than 5 Ω·cm.

[0018] The dopant in the silicon contained in the partitions 13 and in the outer circumferential wall 12 may preferably be elements of group 13 or elements of group 15. The elements of group 13 or group 15 can readily be used as dopant in the concentration range of 10 16 up to 5 · 10 20 cm -3in silicon. As used here, the elements of group 13 refer to boron (B), aluminum (Al), gallium (Ga), indium (In), and the like, and the elements of group 15 refer to nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), and the like. As long as the dopants in the silicon contained in the partitions 13 and in the outer circumferential wall 12 are elements belonging to the same group, several types of elements may be present, since they can exhibit conductivity without being affected by counter-doping. It is preferred that one or two dopants be used that are selected from the group consisting of B and Al. It is also preferred that one or two dopants be used that are selected from the group consisting of N and P. B, Al, N, and P can be more readily used as dopants in silicon in the concentration range of 10 16 up to 5 · 1020 cm -3 It should be included.

[0019] Except by increasing the concentration of the doping agent in the silicon contained in the partitions 13 and in the outer circumferential wall 12, as described above, to 10 16 up to 5 · 10 20 cm -3 The specific volume resistivity of the honeycomb structure 10 can be controlled as needed by adjusting the specific volume resistivity of the ceramic material other than silicon, which forms the partitions 13 and the outer circumferential wall 12, and by adjusting the porosity of the partitions 13. The concentration of the dopant(s) in the silicon of the honeycomb structure can be measured, for example, by the following procedure. The following describes a case in which boron is present as a dopant. However, it should be noted that dopant materials other than boron can be measured using the same procedure.

[0020] First, the honeycomb structure is cut along a surface perpendicular to a central axis to expose a cross-sectional area. Then, irregularities in a cross-section of the honeycomb structure are filled with resin, and the resin-filled surface is further polished. The polished surface of the honeycomb structure is then observed, and an elemental analysis of the material forming the honeycomb structure is performed using energy-dispersive X-ray spectroscopy (EDX analysis).

[0021] The following procedure is used to determine whether "other elements" are present in a section of the polished surface identified as "silicon." First, for sections where the silicon element has been detected, a section where elements other than silicon have been detected is identified as "other components" by imaging a cross-sectional structure photograph and an electron probe microanalyzer (EPMA analysis) of the polished surface. The "other elements" include boron and metal borides or borides present in silicon as boron sources.

[0022] In the section where the silicon element alone or silicon and boron were detected by EPMA analysis and identified as "silicon," the amount of boron in silicon is identified using the following procedure. First, the honeycomb structure containing the section identified as "silicon" is cut to a thickness of a few millimeters. The cut honeycomb structure is then subjected to cross-sectional preparation using a broad ion beam technique, thus preparing a sample for measuring the amount of boron. The broad ion beam technique is a method for preparing a sample cross-section using an argon ion beam.In particular, it relates to a method for preparing a sample cross-section along an end face of a shielding plate by positioning the shielding plate directly above the sample and etching the sample by irradiating it from the top of the shielding plate with a broad argon ion beam. The sample, after cross-sectional preparation, is then analyzed for boron in silicon by time-of-flight secondary mass spectrometry (TOF-SIMS). In TOF-SIMS, the sample is first irradiated with a primary ion beam to emit secondary ions from the sample surface. The released secondary ions are then introduced into a time-of-flight mass spectrometer to obtain a mass spectrum of the outermost surface of the sample.The sample is then analyzed based on the obtained mass spectrum, and the concentration of boron in silicon (parts / cm²) is determined by converting it based on the correlation between a spectral intensity of boron in silicon and previously measured concentration values ​​(e.g., a calibration curve). 3 ) certainly.

[0023] For every 100 parts by mass of the partitions 13 and the outer perimeter wall 12, the ceramic forming the partitions 13 and the outer perimeter wall 12 contains 30% or more silicon by mass. Such a configuration can enable a structure in which the doped silicon-containing materials with lower resistivity are arranged microscopically in series for easy absorption. As a result, the specific volume resistivity of the honeycomb structure 10 can be reduced, and excess current generation can be satisfactorily suppressed even when used for a lower voltage of 60 V or less, such as 48 V. Furthermore, such a configuration can provide a higher strength-modulus ratio for the honeycomb structure 10, thus improving its thermal shock resistance.Preferably, the ceramic forming the partition walls 13 and the outer circumferential wall 12 may contain silicon in an amount of 30 wt% or more and less than 100 wt% and preferably 40 wt% or more and less than 100 wt%.

[0024] One method for calculating the silicon content in the partitions and the outer perimeter wall is, for example, the following procedure. The following procedure describes a calculation method when silicon and silicon carbide are used as ceramic starting materials. When silicon and silicon carbide are used as ceramic starting materials, the composition of each partition and the outer perimeter wall, after the formation of the honeycomb structure, consists of silicon (Si), silicon carbide (SiC), and silicon dioxide (SiO2). The amounts of silicon and oxygen elements in the partitions and the outer perimeter wall can be measured using a fluorescence X-ray method, and the amounts of carbon elements can be measured using an infrared absorption method of the resistance heating type.The amount of SiC is calculated by molecular weight calculation, assuming that all carbon elements are based on SiC, and the amount of SiC in the partitions and the outer perimeter wall is calculated by molecular weight calculation. Similarly, the amount of SiO2 in the partitions and the outer perimeter wall is calculated by molecular weight calculation, assuming that all oxygen elements are based on SiO2. The amount of Si can be calculated from the amounts of silicon elements using the X-ray fluorescence method by subtracting the amount of Si obtained by summing the amounts of Si in the SiC and SiO2 calculated above from the total amount of silicon elements.If a material other than silicon carbide is used as the ceramic starting material, the compositions of the partitions and the outer perimeter wall can be confirmed after the formation of the honeycomb structure, and the quantities of the elements can then be measured and calculated using a fluorescence x-ray method or an infrared absorption method of the resistance heating type.

[0025] As described above, the porosity of the partitions 13 can be adjusted as required, depending on the desired specific volume resistance of the honeycomb structure 10. It can, for example, preferably be from 35% to 60% and more preferably from 35% to 45%. A porosity of 35% or more of the partitions 13 can provide a lower heat capacity for the honeycomb structure 10, allowing it to heat up quickly. A porosity of 60% or less of the partitions 13 can ensure that the strength of the honeycomb structure 10 is adequately maintained. The porosity of the partitions 13 is a value measured by a mercury porosimeter.

[0026] The external shape of the honeycomb structure 10 is not particularly restricted, as long as it is columnar, and can be, for example, a columnar shape with circular end faces (circular column shape), a columnar shape with oval end faces, and a columnar shape with polygonal (square, pentagonal, hexagonal, heptagonal, octagonal, and the like) end faces, and so on. Furthermore, the honeycomb structure 10 has an end face area of ​​2000 to 20000 mm². 2 and preferably from 5000 to 15000 mm 2 to increase thermal resistance (to suppress cracks generated in a perimeter wall of the outer perimeter side wall).

[0027] The shape of each cell 15 of the honeycomb structure 10 in a cross-section perpendicular to a flow path direction of the cell is not restricted, but can preferably be a square, a hexagon, an octagon, or a combination thereof. Among these, the square and the hexagonal shapes are preferred. Such a square or hexagonal cell shape leads to a reduced pressure drop when exhaust gas flows through the honeycomb structure 10 and to an improved cleaning performance of the catalyst. The rectangular shape is particularly preferred with regard to the ease of achieving both structural strength and uniformity of heating.

[0028] The provision of the outer circumferential wall 12 is useful for ensuring the structural strength of the honeycomb structure 10 and for preventing fluid flowing through the cells 15 from escaping from the outer circumferential wall 12. In particular, the thickness of the outer circumferential wall 12 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the outer circumferential wall 12 is too thick, the strength becomes too high, so that a strength equilibrium between the outer circumferential wall and the partition 13 is lost, which reduces the thermal shock resistance. Therefore, the thickness of the outer circumferential wall 12 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less.As used here, the thickness of the outer circumferential wall 12 is defined as a thickness of the outer circumferential wall 12 in a direction of a normal to a tangential at a measuring point when a section of the outer circumferential wall 12 is observed which is to be subjected to a thickness measurement in a cross-section perpendicular to a flow path direction of the cells.

[0029] Preferably, the partitions 13 have an average pore diameter of 2 to 15 µm, and more preferably of 4 to 8 µm. An average pore diameter of 2 µm or more of the partitions 13 allows the specific volume resistivity to be controlled within the above range. An average pore diameter of 15 µm or less of the partitions 13 also allows the specific volume resistivity to be controlled within the above range. The average pore diameter is a value measured by a mercury porosimeter.

[0030] Preferably, each partition 13 has a thickness of 50 to 200 µm and a cell density of 50 to 150 cells / cm². 2 By controlling the thickness and cell density of the partitions 13 in these areas, the specific volume resistance of the honeycomb structure 10 can be easily reduced. Furthermore, a thickness of 50 µm or more for each partition 13 can prevent a reduction in the strength of the honeycomb structure 10. A thickness of 200 µm or less for each partition 13 can prevent an increase in pressure drop when exhaust gas flows through it, if the honeycomb structure 10 is used as a catalyst support and a catalyst is supported on it. Furthermore, the cell density of the partitions 13 can be reduced to 50 cells / cm². 2 or more, enabling an increased catalyst support area and enhanced catalyst cleaning performance. The cell density of the partition walls is 13 out of 150 cells / cm². 2or less can prevent an increase in pressure loss during the flow of exhaust gas when the honeycomb structure 10 is used as a catalyst support and a catalyst is supported thereon. Preferably, the thickness of the partition 13 is from 50 to 150 µm and the cell density is from 75 to 150 cells / cm³. 2 In the present invention, the thickness of the partition wall 13 is defined as the length of a section passing through the partition wall 13, along the segments connecting the centroids of adjacent cells 15 in a cross-section perpendicular to the orientation of the cells 15. Furthermore, the cell density in the present invention is a value obtained by dividing the number of cells by the area of ​​an end face of the honeycomb structure 10, excluding the outer perimeter wall 12.

[0031] Fig.Figure 2 is a schematic external view of a honeycomb structure 30 of the type of electric heater according to an embodiment of the present invention. The honeycomb structure 30 of the type of electric heater according to the embodiment of the present invention comprises: the honeycomb structure 10 shown above; and a pair of electrode layers 14a, 14b, which are arranged opposite each other on the surface of the outer circumferential wall 12 of the honeycomb structure 10 via a central axis of the honeycomb structure 10. Each of the electrode layers 14a, 14b is electrically connected to the honeycomb structure 10. This structure enables the honeycomb structure 30 of the type of electric heater to prevent a systematic deviation of a current flowing through the honeycomb structure 10 when a voltage is applied, thereby preventing a systematic deviation of a temperature distribution in the honeycomb structure 10.The shape and size of each of the electrode layers 14a, 14b are not particularly restricted and can be designed as required, depending on the size of the honeycomb structure 30, the type of electric heating, and / or the electrical conductivity. For example, each of the electrode layers 14a, 14b can be provided in a strip shape running in the direction of the cells 15 of the honeycomb structure 10.

[0032] The electrode layers 14a, 14b are formed from a conductive material. Preferably, the electrode layers 14a, 14b are made of an oxide ceramic or of a mixture of a metal or metal compound with an oxide ceramic. The metal can be either a single metal or an alloy, wherein, for example, silicon, aluminum, iron, stainless steel, titanium, tungsten, a Ni-Cr alloy, or the like may be suitable. Examples of the metal compound include compounds other than oxide ceramics, such as metal oxides, metal nitrides, metal carbides, metal silicides, metal borides, and composite oxides. For example, FeSi₂, CrSi₂, aluminum oxide, silicon dioxide, titanium oxide, or the like may be suitable. Both the metal and the metal compound can be used alone or in pairs or groups. Specific examples of the oxide ceramic include glass, cordierite, and mullite.The glass may further contain an oxide composed of at least one component selected from the group consisting of B, Mg, Al, Si, P, Ti and Zr. In order to further improve the strength of the electrode layers 14a, 14b, it is preferred that they also contain at least one component selected from the above group.

[0033] The honeycomb structure 10 can be produced according to a known method for producing a honeycomb structure. For example, a binder, a surfactant, a pore-forming agent, water, and the like are first added to silicon powder containing one or more added dopants, or to silicon powder obtained by mixing another ceramic material with this silicon powder containing the added dopants, to form a starting material. The silicon to be contained in the starting material is preferably mixed such that it amounts to 30 parts by mass, or more and less than 100 parts by mass, per 100 parts by mass of the partitions 13 and the outer circumferential wall 12 of the honeycomb structure 10 produced by the firing step and the like.Furthermore, the amount of dopant is adjusted appropriately depending on the dopant elements in such a way that the concentration of the dopant in silicon in the honeycomb structure produced by the firing step and the like is 10 10. 16 up to 5 · 10 20 cm -3 The silicon powder preferably has an average particle diameter of 3 to 50 µm and more preferably of 3 to 40 µm. The average particle diameter of the silicon powder refers to an arithmetically averaged diameter on a volume basis when the particle diameter frequency distribution is measured by a laser diffraction method.

[0034] Examples of the binder include methylcellulose, hydroxypropylmethylcellulose, hydroxypropylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyvinyl alcohol, and the like. Among these, it is preferred to use methylcellulose together with hydroxypropylcellulose. The binder content is preferably 2.0 to 10.0 parts by mass per 100 parts by mass of the silicon powder containing the added dopant(s), or of the powder obtained by mixing another ceramic material with the silicon powder containing the added dopant(s).

[0035] The water content is preferably 20 to 60 parts by mass per 100 parts by mass of the silicon powder containing the added dopant(s), or of the powder obtained by mixing another ceramic material with the silicon powder containing the added dopant(s).

[0036] The surfactant that can be used contains ethylene glycol, dextrin, fatty acid soaps, polyalcohol, and the like. These can be used alone or in combination. The surfactant content is preferably 0.1 to 2.0 parts by mass per 100 parts by mass of the silicon powder containing the added dopant(s), or of the silicon powder obtained by mixing another ceramic material with the silicon powder containing the added dopant(s).

[0037] As long as the pore-forming agent itself forms pores after firing, the pore-forming agent, including, for example, graphite, starch, foamed resins, water-absorbing resins, silica gel, and the like, is not particularly limited. The pore-forming agent content is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the silicon powder containing the added dopant(s), or of the powder obtained by mixing another ceramic material with the silicon powder containing the added dopant(s). An average particle diameter of the pore-forming agent is preferably 10 to 30 µm. If it is greater than 10 µm, sufficient pores can preferably be formed. If it is less than 30 µm, it is difficult to infuse a mold with the pore-forming agent during the formation process, which is preferred.The average particle size of the pore-forming agent refers to an arithmetically averaged diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction. If the pore-forming agent is the water-absorbing resin, the average particle diameter of the pore-forming agent is the mean particle diameter after water absorption.

[0038] The resulting starting materials are then kneaded to form a blank, which is subsequently extruded to create a raw (unfired) columnar honeycomb structure. During extrusion, a die with a desired overall shape, cell shape, septum thickness, cell thickness, and the like can be used. Preferably, the resulting unfired columnar honeycomb structure is dried. If the length of the columnar honeycomb structure along its central axis is not the desired length, both end faces of the columnar honeycomb structure can be trimmed to the required length.

[0039] The unfired columnar honeycomb structure is then fired to prepare a honeycomb structure 10. Prior to firing, calcination can preferably be carried out to remove the binder and the like. The calcination is preferably carried out for 0.5 to 20 hours in an air atmosphere at a temperature of 400 to 500 °C. The calcination and firing processes are not limited and can be carried out using an electric furnace, a gas furnace, or the like. The firing can preferably be carried out for 1 to 20 hours in an inert atmosphere such as nitrogen and argon at a temperature of 1300 to 1500 °C. After firing, an oxidation treatment of 1 to 10 hours at a temperature of 1200 to 1350 °C is preferably carried out to improve durability. Thus, the honeycomb structure 10 can be produced according to the embodiment of the present invention.

[0040] The honeycomb structure 30 of the electric heating type according to the embodiment of the present invention can be produced by arranging the pair of electrode layers 14a, 14b opposite each other on the honeycomb structure 10 via the central axis of the honeycomb structure 10. (2nd carrier of the electric heating type)

[0041] Fig.Figure 3 is a schematic cross-sectional view of a carrier 20 of the type electric heater according to an embodiment of the present invention, perpendicular to the orientation of the cells. The carrier 20 of the type electric heater contains the honeycomb structure 30 of the type electric heater and a pair of metal terminals 21a, 21b. The pair of metal terminals 21a, 21b are arranged opposite each other along the central axis of the columnar honeycomb structure 10 and are provided on the pair of electrode layers 14a and 14b, respectively, and are electrically connected. Accordingly, electricity is then conducted through the metal terminals 21a, 21b to enable the honeycomb structure 30 of the type electric heater to generate Joule heating, while a voltage is applied to the metal terminals 21a, 21b through the electrode layers 14a, 14b.Therefore, the honeycomb structure 30 of the electric heating type can also be used as a heating device.

[0042] The material of the metal terminals 21a, 21b is not particularly restricted, as long as it is a metal, and a single metal, an alloy, or the like may be used. With regard to corrosion resistance, specific electrical resistance, and coefficient of linear expansion, the material is, for example, preferably an alloy containing at least one element selected from the group consisting of Cr, Fe, Co, Ni, and Ti, and preferably stainless steel and Fe-Ni alloys. The shape and size of each of the metal terminals 21a, 21b are not particularly restricted and may be suitably designed in accordance with the size of the electric heating element 20, the electrical conductivity, and the like.

[0043] Because the catalyst is supported on the electric heating support 20, the electric heating support 20 can be used as a catalyst. For example, a fluid such as exhaust gas from a motor vehicle can flow through the flow paths of the multiple cells 15. Examples of the catalyst include precious metal catalysts or catalysts other than these. Illustrative examples of precious metal catalysts include a three-way catalyst and an oxidation catalyst obtained by supporting a precious metal such as platinum (Pt), palladium (Pd), and rhodium (Rh) on the surface of pores of aluminum oxide, and which contains a cocatalyst such as cerium dioxide and zirconium dioxide, or a lean nitrogen oxide trap catalyst (LNT capacitor) which uses an alkaline earth metal and platinum as storage components for nitrogen oxides (NOx). x). Illustrative examples of a catalyst that does not use the precious metal include a selective catalytic NOx reduction (SCR) catalyst containing a copper-substituted or iron-substituted zeolite, and the like. Furthermore, two or more catalysts selected from the group consisting of these catalysts may be used. A method for supporting the catalyst is not particularly restricted and may be carried out in accordance with a conventional method for supporting the catalyst on the honeycomb structure. (3. Exhaust gas purification device)

[0044] The electric heating element 20 according to the above embodiment of the present invention can be used for an exhaust gas purification device. The exhaust gas purification device includes the electric heating element 20 and a canister body to hold the electric heating element 20. The electric heating element 20 in the exhaust gas purification device can be installed in an exhaust gas flow path to allow exhaust gas from a power engine to flow. A metal pipe section or the like can be used as the canister body to receive the electric heating element 20. EXAMPLES

[0045] The following are examples to better understand the present invention and its advantages, although the present invention is not limited to these examples. (1. Production of the honeycomb structure)

[0046] Examples 2 to 14, 17 to 21, and for comparison, 1, 15, 16, and 22, consisted of silicon powder, silicon carbide powder, and boron nitride mixed to the proportions shown in the "Recipe" column of Table 1 to prepare a ceramic starting material. Hydroxypropyl methylcellulose (as a binder), a water-absorbing resin (as a pore-forming agent), and water were added to this ceramic starting material to form a forming starter. This forming starter was then kneaded using a vacuum kneader to produce a circular column-shaped blank. The binder content was 7 parts by mass per 100 parts by mass of the combined silicon powder and silicon carbide powder. The pore-forming agent content was 3 parts by mass per 100 parts by mass of the combined silicon powder and silicon carbide powder.The water content was 42 parts by mass per 100 parts by mass of the sum of the silicon powder and silicon carbide powder. The average particle diameter of the silicon particles was 6 µm. The average particle diameter of the pore-forming agent was 20 µm. The average particle diameter of both the silicon particles and the pore-forming agent refers to an arithmetically averaged diameter based on volume when the particle size frequency distribution is measured by laser diffraction.

[0047] The resulting columnar blank was formed using an extruder to obtain a columnar honeycomb structure section in which each cell had a square cross-sectional shape. The resulting unfired columnar honeycomb structure section was subjected to high-frequency dielectric heating and dried, then dried for 2 hours using a hot air dryer at 120 °C, and a predetermined amount was trimmed from both end faces to prepare a honeycomb structure.

[0048] The dried honeycomb structure was degreased (calcined), fired, and further oxidized to obtain a fired honeycomb body. Degreasing was carried out for 3 hours at 500 °C. Firing was carried out for 2 hours at 1400 °C in an argon atmosphere. Oxidation was carried out for 1 hour at 1300 °C. (2. Formation of the electrode layer)

[0049] A pair of electrode layers was positioned opposite each other along the central axis of the honeycomb structure. The conditions for forming the electrode layers were as follows: First, a stainless steel powder (SUS430) and a glass powder were mixed in a volume ratio of 40% stainless steel powder and 60% glass powder to prepare a ceramic starting material. The average particle diameter was 10 µm for the stainless steel powder and 2 µm for the glass powder. The average particle diameter refers to an arithmetically averaged diameter on a volume basis when the frequency distribution of particle diameters is measured by the laser diffraction method.

[0050] Subsequently, 1 wt% of a binder, 1 wt% of a surfactant, and 30 wt% water were added to the above ceramic starting material to prepare a mixture. This mixture was then applied to the honeycomb structure using screen printing. The applied mixture was dried for 30 minutes in a hot air dryer at 120 °C and then fired for 30 minutes at 1100 °C, together with the honeycomb structure, under vacuum to form electrode layers. This resulted in the production of an electrically heated honeycomb structure. (3rd evaluation test)

[0051] The concentration of the dopant (boron concentration) in silicon of the resulting honeycomb structure of the electric heating type was measured by the method described above, indicating that it was 6 · 10 15 cm -3 fraud.

[0052] The composition of each of Si, SiC, and SiO2 in the partitions and outer perimeter walls of the resulting honeycomb structure of the electric heating type was measured using the above method. Table 1 shows the measurement results.

[0053] The resulting honeycomb structure of the electric heating type had a thickness of 125 µm per partition and a cell density of 90 cells / cm². 2 The cell density was calculated by dividing the number of cells by the area of ​​an end face section of the honeycomb structure, excluding the outer perimeter wall section.

[0054] The porosity of the partition walls of the resulting honeycomb structure of the electric heating type was measured using a mercury porosimeter.

[0055] Furthermore, a pair of metal terminals was electrically connected to the pair of electrode layers of the resulting honeycomb structure of the electric heating type. A voltage of 48 V was then applied to the honeycomb structure of the electric heating type through the metal terminals, and a current value was measured. The specific volume resistance of the honeycomb structure of the electric heating type was calculated from the voltage and current values. The evaluation results are shown in Table 1.

[0055] [Table 1] Recipe Content in partition walls and in the outer perimeter wall B in Si porosity specific volume resistance Si SiC BN Si SiC SiO2 Nr. wt. % % of weight wt. % % of weight % of weight wt. % Pieces / cm 3 % Ω · cm Comparison 1 50 50 0,00003 46 42 12 6 · 10 15 44 12,92 Example 2 50 50 0,0001 46 42 12 2 · 10 16 44 4,90 Example 3 50 50 0,0003 46 42 12 6 · 10 16 44 2,62 Example 4 50 50 0,003 46 42 12 6 · 10 17 44 0,94 Example 5 50 50 0,03 46 42 12 6 · 10 18 44 0,24 Example 6 50 50 0,01 46 42 12 2 · 10 18 44 0,42 Example 7 50 50 0,3 46 42 12 6 · 10 19 45 0,05 Example 8 50 50 0,1 46 42 12 2 · 10 19 44 0,12 Example 9 50 50 1 46 42 12 2 · 10 20 44 0,03 Example 10 50 50 3 46 42 12 5 · 10 20 44 0,02 Example 11 100 0 0,03 92 0 8 1 · 10 19 40 0,08 Example 12 80 20 0,03 73 17 10 9 · 10 18 42 0,11 Example 13 60 40 0,03 55 34 11 7 · 10 18 43 0,18 Example 14 40 60 0,03 37 51 13 5 · 10 18 45 0,38 Comparison 15 30 70 0,03 27 59 13 4 · 10 18 46 7,30 Comparison 16 25 75 0,03 23 63 14 3 · 10 18 46 30,41 Example 17 100 0 0,3 92 0 8 1 · 10 20 40 0,02 Example 18 80 20 0,3 73 17 10 9 · 10 19 42 0,03 Example 19 60 40 0,3 55 34 11 7 · 10 19 43 0,05 Example 20 40 60 0,3 37 51 13 5 · 10 19 44 0,14 Example 21 35 65 0,3 32 55 13 4 · 10 19 44 0,20 Comparison 22 25 75 0,3 23 63 14 3 · 10 19 46 5,42

[0056] (4. Discussion)

[0056] As shown in Table 1, the partitions and the outer circumferential wall of the honeycomb structure in Examples 2 to 14 and in Examples 17 to 21 according to the present invention were made of ceramic containing at least silicon, and had a silicon content of 30 wt% or more and a silicon dopant concentration of 10 16 up to 5 · 10 20 cm -3 , so that the specific volume resistance could be lower and the generation of excess current could be satisfactorily prevented even at a lower voltage of 48 V.

[0057] In comparative example 1, the specific volume resistance was greater because the concentration of the dopant in silicon at the partitions and on the outer circumferential wall of the honeycomb structure was less than 10 16 cm -3 was.

[0058] In comparative examples 15, 16 and 22, the ceramic forming the partitions and outer perimeter wall of the honeycomb structure had a silicon content of less than 30 mass-%, so that the specific volume resistance was greater. Description of reference symbols 10 honeycomb structure 12 Outer perimeter wall 13 Partition wall 14a, 14b Electrode layer 15 cells 20 electric heating carriers 21a, 21b Metal connection 30 honeycomb structure of the electric heating type

Claims

[1] Honeycomb structure (10) comprising: an outer peripheral wall (12); and Partition walls (13) arranged on an inner side of the outer peripheral wall (12), the partition walls (13) defining a plurality of cells (15), each of the plurality of cells (15) extending from one end face to the other end face to form a flow path for a fluid, wherein the partition walls (13) and the outer peripheral wall (12) comprise ceramics containing at least silicon as a simple substance which is not a silicon compound; wherein a content of silicon in the ceramic is 30 mass% or more; wherein a concentration of at least one dopant in the silicon of 10 16 cm -3 up to 5 · 10 20 cm -3 amounts. [2] The honeycomb structure (10) of claim 1, wherein the at least one dopant is a group 13 element or a group 15 element. [3] The honeycomb structure (10) according to claim 2, wherein the at least one dopant is one or two selected from the group consisting of boron (B) and aluminum (Al). [4] The honeycomb structure (10) of claim 2, wherein the at least one dopant is one or two selected from the group consisting of nitrogen (N) and phosphorus (P). [5] The honeycomb structure (10) according to any one of claims 1 to 4, wherein the ceramic constituting the partition walls (13) and the outer peripheral wall (12) contains the silicon in an amount of 30 mass% or more and less than 100 mass%. [6] Honeycomb structure (10) according to one of claims 1 to 5, wherein the honeycomb structure (10) has a thickness of each of the partition walls (13) of 50 µm to 200 µm and a cell density of 50 cells / cm 2 up to 150 cells / cm 2 has. [7] The honeycomb structure (10) according to any one of claims 1 to 6, wherein the partition walls (13) and the outer peripheral wall (12) further contain at least one selected from the group consisting of alumina, mullite, zirconia, cordierite, silicon carbide, silicon nitride, and aluminum nitride. [8] Honeycomb structure (30) of the electric heating type, comprising: the honeycomb structure (10) according to one of claims 1 to 7; and a pair of electrode layers (14a, 14b) arranged opposite each other across a central axis of the honeycomb structure (10), each of the electrode layers (14a, 14b) being arranged on a surface of the outer peripheral wall (12) of the honeycomb structure (10). [9] Support (20) of the electric heating type, comprising: the electric heating type honeycomb structure (30) according to claim 8; and a pair of metal terminals (21a, 21b) arranged opposite to each other across a central axis of the electric heating type honeycomb structure (30), the pair of metal terminals (21a, 21b) being arranged on the pair of electrode layers (14a, 14b). [10] Exhaust gas purification device comprising: the electric heating type support (20) according to claim 9; and a canister body for holding the electric heating type carrier (20). [11] A honeycomb structure (10) comprising: an outer peripheral wall (12); and partition walls (13) disposed on an inner side of the outer peripheral wall (12), the partition walls (13) defining a plurality of cells (15), each of the plurality of cells (15) extending from one end face to the other end face to form a flow path for a fluid, the partition walls (13) and the outer peripheral wall (12) comprising ceramic, the ceramic including: Silicon as a simple substance that is not a silicon compound; and at least one selected from the group consisting of alumina, mullite, zirconia, cordierite, silicon carbide, silicon nitride and aluminum nitride; wherein a content of silicon in the ceramic is 30 mass% or more; wherein the silicon contains boron (B) as a dopant; and wherein the honeycomb structure (10) has a volume resistivity of 0.01 Ω · cm or more and 5 Ω · cm or less.

Citation Information

Patent Citations

  • Organic waste gas treatment method

    CN108006666A

  • honeycomb structure and manufacturing process thereof

    DE102017204329B4

  • Honeycomb structure

    JP5735428B2

  • Honeycomb structural body and exhaust gas conversion apparatus

    US20110250095A1

  • Method of manufacturing exhaust gas purifying apparatus and exhaust gas purifying apparatus