Anode active material, method for producing an anode active material and battery

A nonwoven-form Si fiber particle with controlled size and amorphous structure addresses the expansion issue in silicon-based anode active materials, resulting in reduced expansion and lower retention pressure, thereby improving battery stability.

DE102020208793B4Active Publication Date: 2024-12-05TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
DE102020208793
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2020-07-15
Publication Date
2024-12-05
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Existing anode active materials for batteries, particularly those based on silicon, experience significant expansion during charging, which can lead to structural instability and increased retention pressure.

Method used

The development of a nonwoven-form particle containing Si fibers with specific size and amorphous structure, produced through a method involving dispersing a LiSi precursor with a dispersant and extracting lithium using a solvent, to inhibit expansion during charging.

Benefits of technology

The proposed anode active material exhibits reduced expansion and lower retention pressure in batteries, enhancing their structural integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method for producing an anode active material, wherein the method is characterized in that it comprises: a dispersion step of adding a dispersion agent to a LiSi precursor containing a Si element and a Li element to obtain a LiSi precursor dispersion solution, wherein the LiSi precursor is obtained by mixing or milling Si particles with Li particles; and a Li extraction step for extracting the Li element from the LiSi precursor by adding a Li extraction solvent to the LiSi precursor dispersion solution to obtain a nonwoven particle containing Si fibers, wherein a relative dielectric constant of the dispersion medium is 3.08 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present disclosure relates to an anode active material, a method for producing the anode active material, and a battery. State of the art

[0002] In recent years, there has been active work on battery development. For example, the automotive industry has pushed forward the development of batteries for electric vehicles and hybrid vehicles, as well as the development of active materials for these batteries.

[0003] For example, Si-based active materials are known as one example of anode active materials used for the anode layer of an all-solid-state battery. Patent Literature 1 discloses an all-solid-state battery using a composite particle of Si and carbon as the anode active material. Patent Literature 2 and Patent Literature 3 disclose the use of porous silicon as the anode active material.

[0004] Patent Literature 4 discloses the use of carbon composite silicon materials for an anode active material, using an electrospinning method to obtain Si fibers.

[0005] The use of felt-like structures in the preparation of an anode active material is described in Patent Literature 5.

[0006] Patent Literature 6 discloses a silicon-based fibrous material and a method for producing the same by reducing SiO2-based fibers. It also describes the use of the fibrous material for producing a battery electrode. List of cited patent literature Patent literature 1: JP 2017 - 54 720 A Patent literature 2: JP 2013 - 8 487 A Patent literature 3: JP 2013 - 203 626 A Patent literature 4: JP 2016 - 28 375 A Patent literature 5: US 2013 / 0 069 601 A1 Patent literature 6: US 2019 / 0 081 316 A1 Summary of the RevelationTechnical Problem

[0007] The anode active material is required to have low expansion during charging. The present disclosure has been made in view of the above circumstances, and a primary object thereof is to provide an anode active material whose expansion during charging is low. Solution to the problem

[0008] The object is achieved by a method for producing an anode active material according to claim 1, an anode active material according to claim 6 and a battery according to claim 13.

[0009] The anode active material according to the invention is a particle in nonwoven form that contains Si fibers and is obtainable according to the inventive method for producing an anode active material described below. The anode active material has an average particle size D 50of the anode active material is 0.2 µm or more and 3.6 µm or less and is amorphous.

[0010] According to the present disclosure, the anode active material is a nonwoven particle containing Si fibers, so that the expansion of the anode active material during charging can be small.

[0011] In the disclosure, in an XRD measurement using a CuKα beam, a peak “a” originating from Si may not be observed at a position 2θ = 28.4° ± 0.5°.

[0012] In the disclosure, in an XRD measurement using a CuKα beam, a peak "a" originating from Si is observed at a position of 2θ = 28.4° ± 0.5°, a peak "b" whose half width is 3° or more is observed at a position of 2θ = 24.0° - 32.0°, and when Ia denotes an intensity of peak "a" and Ib denotes an intensity of peak "b", an XRD intensity ratio Ia / Ib may be 3.80 or less.

[0013] In the disclosure, in an XRD measurement using a CuKα beam, a peak “c” originating from SiO2 may not be observed at a position 2θ = 20.8° ± 0.5°.

[0014] In the disclosure, a peak “d” originating from lithium silicate may not be observed at a position 2θ = 20° - 30°.

[0015] In the disclosure, an average diameter of the Si fiber may be 8 nm or more and 70 nm or less.

[0016] In the disclosure, an aspect ratio, which is a ratio of average length to average diameter, may be 1 or more and 50 or less.

[0017] The method for producing an anode active material according to the present invention comprises: a dispersing step of adding a dispersant to a LiSi precursor containing a Si element and a Li element to obtain a LiSi precursor dispersion solution, wherein the LiSi precursor is obtained by mixing or grinding Si particles with Li particles; and a Li extraction step of extracting the Li element from the LiSi precursor by adding a Li extraction solvent to the LiSi precursor dispersion solution to obtain a nonwoven fabric-shaped particle containing Si fibers, wherein a relative dielectric constant of the dispersant is 3.08 or less.

[0018] According to the present disclosure, the Li extraction step is performed after the dispersion step, and thus the anode active material can be prepared, which is a particle in nonwoven form containing Si fibers.

[0019] In the disclosure, the dispersant may be at least one of n-butyl ether, 1,3,5-trimethylbenzene and n-heptane.

[0020] In the disclosure, the Li extraction solvent may be at least one of ethanol, 1-propanol, 1-butanol, 1-hexanol and acetic acid.

[0021] In the disclosure, the method may further comprise a washing step of washing the nonwoven fabric particle with an acid after the Li extraction step.

[0022] The present disclosure further provides a battery comprising a cathode active material layer, an anode active material layer, and an electrolyte layer formed between the cathode active material layer and the anode active material layer, wherein the anode active material is the anode active material described above.

[0023] According to the present disclosure, the anode active material layer contains the anode active material described above, and thus the retention pressure of the battery can be reduced. Beneficial effects of revelation

[0024] One of the effects of the anode active material in the present disclosure is that its expansion upon charging is small. Short description of the drawings Fig. 1 is a flowchart illustrating an example of the method for producing the anode active material in the present disclosure. Fig. 2 is a schematic cross-sectional view showing an example of the battery in the present disclosure. Fig. 3A and Fig. Figure 3B shows the results of XRD measurement of the anode active material in Example 1. Fig. Figure 4 is a TEM image of the active material in Examples 1, 2, and Comparative Example 1, respectively. Fig. Figure 5 is an SEM image of the anode active material in Comparative Example 1. Fig. Figure 6 is the result of an XRD measurement of the anode active materials in Examples 8 to 10. Description of the embodiments

[0025] Hereinafter, the anode active material, the method for producing the anode active material, and the battery in the present disclosure are described in detail. A. Anode active material

[0026] The anode active material in the present disclosure is an anode active material for use in a battery, wherein the anode active material is a nonwoven-form particle containing Si fibers. The average particle size D 50 of the anode active material is 0.2 µm or more and 3.6 µm or less and the anode active material is amorphous.

[0027] According to the present disclosure, the anode active material is a nonwoven fabric-shaped particle containing Si fibers, and therefore, the expansion of the anode active material during charging can be small. It is known, as in Patent Literatures 1-3, for example, that a high-capacity Si particle is used as the anode active material. However, if the Si particle is used as the anode active material, the expansion of the anode active material during charging would be large. In contrast, Patent Literature 1 intended to suppress the expansion by adjusting the particle size of the anode active material and allowing the anode (anode active material layer) to have a specific void. Furthermore, Patent Literatures 2 and 3 intended to suppress the expansion by allowing the anode active material to be porous. However, there is still room for further improvement in reducing the expansion.The inventors of the present disclosure subsequently conducted thorough research and found that the anode active material in a nonwoven fabric form in which Si fibers are three-dimensionally entangled is obtained by a specific method. It is believed that the porous anode active material particle described in Patent Literatures 2 and 3 has a shape as shown in the microscopic image of Comparative Example 1 described later, and the shape of the anode active material was previously unknown in the present disclosure. Furthermore, the inventors found that the expansion of the anode active material in the above-mentioned form was further reduced during charging.

[0028] Furthermore, the anode active material in the present disclosure is amorphous. It is assumed that amorphous, i.e., low-crystalline silicon, has a longer Si-Si bond distance compared to crystalline silicon; therefore, it is assumed that if the anode active material is amorphous, expansion during ion intercalation (during charging) will be further inhibited.

[0029] Furthermore, the anode active material in the present disclosure has a specific average particle size D 50When anode active materials with a large average particle size are used for an anode active material layer, it is expected that the anode active material layer would expand locally because ions are preferentially incorporated into the anode active materials with a large particle size. In contrast, with the average particle size of the present disclosure, it is expected that the ions are uniformly incorporated throughout the anode active materials, and the anode active material layer would expand uniformly. As a result, it is expected that the expansion of the anode active material layer as a whole can be inhibited.

[0030] The anode active material in the present disclosure is described in more detail below.

[0031] The anode active material in the present disclosure is a nonwoven-shaped particle containing Si fibers. In the present disclosure, the nonwoven form refers to a mesh form in which Si fibers are three-dimensionally entangled.

[0032] The Si fiber in the present disclosure may have a specific average diameter. The average diameter is, for example, 8 nm or more, may be 10 nm or more, may be 15 nm or more, and may be 20 nm or more. Meanwhile, the average diameter is, for example, 70 nm or less, may be 60 nm or less, may be 50 nm or less, may be 40 nm or less, and may be 30 nm or less. Furthermore, the Si fiber in the present disclosure may have a specific average length. The average length is, for example, 50 nm or more and 400 nm or less. The length of the Si fiber in the present disclosure is defined here as a length from a connection point (a point where a plurality of Si are connected) on one side to a connection point (a point where a plurality of Si are connected) on the other side.The average length and diameter of the Si fiber can be determined, for example, by observation with a scanning electron microscope (SEM). The number of samples is preferably very large, for example, 100 or more.

[0033] Furthermore, the Si fiber in the present disclosure may have a specific aspect ratio, which is a ratio of average length to average diameter. The aspect ratio, which is a ratio of average length to average diameter, is, for example, 1 or more, may be 5 or more, may be 15 or more, and may be 20 or more. Meanwhile, the aspect ratio, which is a ratio of average length to average diameter, is, for example, 50 or less, may be 40 or less, and may be 30 or less.

[0034] The Si fiber in the present disclosure may be a simple Si substance, or it may be an alloy containing Si elements as a main component. For example, the content of Si elements in the alloy may be 50 at% or more, may be 70 at% or more, and may be 90 at% or more. Examples of metal elements other than the Si element in the alloy may include a Li element.

[0035] The anode active material in the present disclosure has a specific average particle size D 50 The average particle size D 50 is 0.2 µm or more and may be 0.5 µm or more, may be 1.0 µm or more, and may be 1.5 µm or more. Meanwhile, the average particle size D 503.6 µm or less and may be 3.0 µm or less, may be 2.5 µm or less, and may be 2.0 µm or less. If the anode active material layer is selected from the anode active material with the average particle size D 50 used in the range described above, it is assumed that the expansion of the entire anode active material layer can be inhibited because the ions are evenly incorporated into the entire anode active material, allowing the anode active material layer to expand evenly. The average particle size D 50 can be obtained, for example, by observation with a scanning electron microscope (SEM). The number of samples is preferably very large; for example, 100 or more. The method for adjusting the average particle size D 50 is described later under “B. Process for producing an anode active material”.

[0036] Furthermore, the anode active material in the present disclosure is amorphous. The amorphous state in the present disclosure refers to a case where a halo peak (a broad peak in the halo pattern) is confirmed in an XRD measurement using a CuKα beam. In the XRD measurement using a CuKα beam, the halo peak preferably has a peak position at 2θ = 24.0° - 32.0°. Similarly, the halo peak preferably has a peak position at 2θ = 40.0° - 60.0°. Here, the half-width of the halo peak is, for example, 3° or more, may be 5° or more, and may be 10° or more. In the present disclosure, in the XRD measurement using a CuKα beam, the halo peak having a peak position at 2θ = 24.0° - 32.0° and the half-width of 3° or more (hereinafter referred to as peak “b”) is preferably observed.

[0037] Furthermore, in the anode active material in the present disclosure, in an XRD measurement using a CuKα beam, a peak "a" originating from Si and positioned at 2θ = 28.4° ± 0.5° may not be observed, or it may be observed, but it means that the former has a higher amorphous nature of the anode active material than the latter. The peak "a" is a peak originating from a Si crystal phase (Si crystal phase in a diamond shape). Furthermore, "the peak "a" is not observed" means that the intensity of the peak "a" is so low that it is difficult to distinguish from the background noise. This definition also applies to peaks other than the peak "a."

[0038] The peak position of peak "a" can be 2θ = 28.4° ± 0.4°, and can be 2θ = 28.4° ± 0.2°. Furthermore, the half-width of peak "a" is usually smaller than the half-width of peak "b"; for example, it is 3° or less, can be 1° or less, and can be 0.5° or less.

[0039] Furthermore, in the anode active material in the present disclosure, in an XRD measurement using a CuKα beam, a peak "b" positioned at 2θ = 24.0° - 32.0° is usually observed, whose half-width is 3° or more. The peak "b" is one of the halo peaks described above, which is a peak different from the peak "a". The half-width of the peak "b" may, for example, be 4° or more, may be 5° or more, and may be 10° or more. The peak intensity Ib of the peak "b" can be calculated by fitting an obtained diffraction pattern.

[0040] When peak "a" is observed, and Ia denotes the intensity of peak "a" and Ib the intensity of peak "b", an XRD intensity ratio Ia / Ib may be within a certain range. For example, the XRD intensity ratio Ia / Ib is 3.80 or less, may be 3.50 or less, may be 3.00 or less, and may be 2.50 or less. Meanwhile, the XRD intensity ratio Ia / Ib is, for example, 0.95 or more, may be 0.99 or more, may be 1.50 or more, and may be 2.00 or more. A method for adjusting the XRD intensity ratio will be described later in "B. Method for producing an anode active material". Here, the "peak intensity" refers to a height from an X-axis (2θ) in a diffraction pattern.

[0041] Furthermore, in the anode active material in the present disclosure, in an XRD measurement using a CuKα beam, a peak "c" originating from SiO2 and positioned at 2θ = 20.8° ± 0.5° may not be observed or may be observed, but the former is preferred. This is to allow the anode active material to have fewer impurities. The peak position of peak "c" may be 2θ = 20.8° ± 0.4°, and may be 2θ = 20.8° ± 0.2°. In addition, the half-width of peak "c" is usually smaller than the half-width of peak "b"; for example, peak "c" is 3° or less, may be 1° or less, and may be 0.5° or less.

[0042] When peak "a" and peak "c" are observed, Ia denotes the intensity of peak "a" and Ic denotes the intensity of peak "c", an XRD intensity ratio Ic / Ia is preferably low. For example, the XRD intensity ratio Ic / Ia is 1.1 or less, may be 1.05 or less, and may be 1.00 or less. Meanwhile, when peak "a" is not observed but peak "c" is observed, Ia' denotes an intensity at 2θ = 28.4°. An XRD intensity ratio Ic / Ia' preferably satisfies the same relationship as the XRD intensity ratio Ic / Ia described above.

[0043] Furthermore, in the anode active material in the present disclosure, in an XRD measurement using a CuKα beam, a peak "d" derived from lithium silicate and positioned at 2θ = 20° - 30° may not be observed or may be observed, but the former is preferred. This is to allow the anode active material to have fewer impurities. The peak "d" is a peak derived from lithium silicate. Examples of the positions where the peak "d" is obtained at 2θ = 20° - 30° may be 2θ = 24.7° ± 0.5° and 2θ = 26.0° ± 0.5°. The peak "d" may be observed as a single peak and may be observed as multiple peaks. Lithium silicate is a compound containing Li, Si, and O, and typically, Li6Si2O7 falls under the compound. In addition, the half-width of peak “d” is usually smaller than the half-width of peak “b”; e.g.the peak “d” is 3° or less, may be 1° or less, and may be 0.5° or less.

[0044] When peak "a" and peak "d" are observed, Ia denotes the intensity of peak "a" and Id denotes the intensity of peak "d", an XRD intensity ratio Id / Ia is preferably low. The XRD intensity ratio Id / Ia is, for example, 0.8 or less and may be 0.6 or less. Meanwhile, when a plurality of peaks "d" are observed, Id denotes the largest intensity among the plurality of peaks "d". On the other hand, when peak "a" is not observed but peak "d" is observed, Ia' denotes an intensity at 2θ = 28.4°. An XRD intensity ratio Id / Ia' preferably satisfies the same relationship as the XRD intensity ratio Id / Ia described above.

[0045] Furthermore, the anode active material in the present disclosure may contain a specified void. The void is, for example, 5% or more, may be 10% or more, and may be 20% or more. The void is, for example, 50% or less, may be 40% or less, and may be 30% or less. The void can be obtained, for example, by observation with a scanning electron microscope (SEM). The number of samples is preferably very large; for example, it is 100 or more. The void can be an average value calculated from these samples.

[0046] Furthermore, the anode active material in the present disclosure is used for a battery. The battery is described later under "C. Battery." B. Process for producing an anode active material

[0047] Fig.1 is a flowchart illustrating an example of the method for producing the anode active material in the present disclosure. The method for producing the anode active material in the present disclosure includes: a dispersing step of adding a dispersing agent to a LiSi precursor containing a Si element and a Li element to obtain a LiSi precursor dispersion solution; and a Li extraction step of extracting the Li element from the LiSi precursor by adding a Li extraction solvent to the LiSi precursor dispersion solution to obtain a nonwoven fabric-shaped particle containing Si fibers. Furthermore, in the present disclosure, a relative dielectric constant of the dispersing agent is 3.08 or less.

[0048] With the method for producing the anode active material in the present disclosure, in which the Li extraction step is performed after the dispersing step, the anode active material, which is a nonwoven particle containing Si fibers, can be produced. This is because the dispersant used in the dispersing step has a specific relative dielectric constant, thus inhibiting the reaction of the LiSi precursor with the Li extraction solvent to limit the rate of extraction of Li elements from the LiSi precursor. It is assumed that the dispersant having a specific relative dielectric constant is used, and thus, when the Li extraction solvent is added, the solvent is immediately mixed with the dispersant to reduce the concentration of the Li extraction solvent in the surface of the LiSi precursor.As a result, it is assumed that the reaction of the LiSi precursor with the Li extraction solvent is inhibited. Furthermore, when the Li extraction reaction is inhibited as described above, it is assumed that only Li elements are extracted from the Li-Si precursor, leaving the Si skeleton behind, thus allowing the nonwoven particle to be obtained. It is assumed that if the Li extraction reaction is not inhibited, the Si skeleton is extracted simultaneously with Li elements, thus preventing the nonwoven particle from being obtained. 1. Dispersing step

[0049] The dispersing step in the present disclosure is a step of adding a dispersant to a LiSi precursor containing a Si element and a Li element to obtain a LiSi precursor dispersion solution.

[0050] The LiSi precursor is obtained by mixing or grinding Si particles with Li particles. Examples of the mixing method may include a method of mixing Si particles with Li particles using an agate mortar under an Ar atmosphere and a method of mixing Si particles with Li particles using mechanical grinding.

[0051] The LiSi precursor preferably has a (diamond-shaped) Si crystal phase. In an XRD measurement using a CuKα beam, the Si crystal phase exhibits typical peaks at the positions 2θ = 28.4°, 47.3°, 56.1°, 69.2°, and 76.4°. These peak positions can each be shifted within a range of ± 0.5° and can be shifted within a range of ± 0.3°. The Li-Si precursor can have the (diamond-shaped) Si crystal phase as its main phase. The "main phase" refers to a crystal phase to which a peak with the highest intensity in the XRD diagram belongs.

[0052] The relative dielectric constant of the dispersant in the present disclosure is 3.08 or less. The dispersant having a relative dielectric constant of 3.08 or less is usually classified as an aprotic dispersant. The relative dielectric constant is 3.08 or less; for example, it may be 3.00 or less, and it may be 2.50 or less. Meanwhile, the relative dielectric constant is, for example, 1.50 or more, it may be 1.70 or more, it may be 1.90 or more, and it may be 2.00 or more. If the relative dielectric constant is much larger than 3.08, there is a risk that the dispersant itself will react and condense with the LiSi precursor, and the LiSi precursor may not be well dispersed. The relative dielectric constant can be measured, for example, by a method described in JIS C 2565 (e.g., a method using a cavity resonator).

[0053] The dispersant may contain no benzene ring or may contain a benzene ring, but the latter is preferable. Examples of the dispersant may further include a saturated hydrocarbon such as n-heptane, n-octane, n-decane, 2-ethylhexane, and cyclohexane; an unsaturated hydrocarbon such as hexene and heptene; an aromatic hydrocarbon such as 1,3,5-trimethylbenzene, toluene, xylene, ethylbenzene, propylbenzene, cumene, 1,2,4-trimethylbenzene, and 1,2,3-trimethylbenzene; and ethers such as n-butyl ether, n-hexyl ether, isoamyl ether, diphenyl ether, methyl phenyl ether, and cyclopentyl methyl ether. Among these, n-butyl ether, 1,3,5-trimethylbenzene, and n-heptane are preferred, and 1,3,5-trimethylbenzene is particularly preferred. The relative dielectric constant of n-butyl ether is 3.08, the relative dielectric constant of 1,3,5-trimethylbenzene is 2.279 and the relative dielectric constant of n-heptane is 1.94.

[0054] Furthermore, it is preferable that the amount of moisture in the dispersant be low. This is because the moisture reacts with the LiSi precursor. For example, the amount of moisture in the dispersant is 100 ppm or less, can be 50 ppm or less, can be 30 ppm or less, and can be 10 ppm or less.

[0055] The LiSi precursor dispersion solution can be obtained by adding a dispersant to the LiSi precursor and mixing them. There are no specific restrictions on the mixing method.

[0056] The mean particle size D 50 of the anode active material in the present disclosure can be adjusted, for example, by changing the type of dispersant. The average particle size D 50 can also be adjusted by combining the type of dispersant and a Li extraction solvent described later. The average particle size D50 can also be adjusted by changing the average particle size of the LiSi precursor itself.

[0057] The main factor influencing the XRD intensity ratio of the anode active material of the present disclosure is the rate of Li extraction from the LiSi precursor (reactivity of the LiSi precursor with the Li extraction agent). If the rate of Li extraction is slow, the XRD intensity ratio would be low, and poorly crystalline silicon would be obtained. The XRD intensity ratio can be adjusted, for example, by the type of dispersant, the type of Li extraction solvent described later, and the combination of dispersant and Li extraction solvent. 2. Li extraction step

[0058] The Li extraction step in the present disclosure is a step of extracting a Li element from the LiSi precursor by adding a Li extraction solvent to the LiSi precursor dispersion solution to obtain the above-described nonwoven fabric-shaped particle.

[0059] There are no specific restrictions on the Li extraction solvent if it is a solvent that enables the extraction of a Li element from the LiSi precursor. Examples of the Li extraction solvent may include a primary alcohol such as methanol, ethanol, 1-propanol, 1-butanol, 1-pentanol, and 1-hexanol; a secondary alcohol such as 2-propanol, 2-butanol, 2-pentanol, and 2-hexanol; a tertiary alcohol such as tert-butyl alcohol; phenols such as phenol; a glycol such as 1,2-ethanediol and 1,3-butanediol; a glycol ether such as propylene glycol monomethyl ether and ethylene glycol monomethyl ether; pyranoses such as β-D-glucopyranose; furanoses such as erythrofuranose; and polysaccharides such as glucoses and fructoses. Examples of the Li extraction solvent can also be an acid solution such as acetic acid, formic acid, propionic acid and oxalic acid.Among them, the lithium extraction solvent is preferably at least one of ethanol, 1-propanol, 1-butanol, 1-hexanol, and acetic acid. As the lithium extraction solvent, only one type of the above compounds can be used, or two or more types can be used. Furthermore, the amount of moisture in the lithium extraction solvent is preferably small. For example, the amount of moisture in the lithium extraction solvent is 100 ppm or less, may be 50 ppm or less, may be 30 ppm or less, and may be 10 ppm or less. If the amount of moisture is too large, there is a risk of Si being oxidized to degrade battery performance.

[0060] The Li extraction step can be configured in one or two stages. For example, if the Li extraction step is configured in a single stage, it may be a step in which a cooled LiSi precursor dispersion solution is reacted with any Li extraction solvent other than the above-mentioned acid solution. If the Li extraction step is configured in two stages, it may be a step consisting of the first stage described above and a second stage in which the reaction solution in the first stage is reacted with the above-mentioned acid solution. If the Li extraction step is configured in two stages, a Li element can be extracted from the LiSi precursor with greater certainty. 3. Washing step

[0061] Furthermore, in the present disclosure, a washing step may be performed after the Li extraction step.

[0062] In the present disclosure, by performing the washing step, impurities can be prevented from mixing into the anode active material. Since the anode active material does not contain many impurities, condensation is also inhibited, so that an anode active material with even smaller expansion upon charging can be produced. Furthermore, the expansion and increase in retention pressure of a battery using such an anode active material can be further suppressed. Impurities include, for example, a by-product in which Li and Si contained in the solution after Li extraction are polymerized as follows.

[0063] There is a possibility that a reaction solution in which Li and Si are dissolved in the form of lithium ethoxide and tetraethoxysilane may adhere to the surface of the nonwoven particle after the Li extraction step. Lithium ethoxide and tetraethoxysilane have the properties of forming a glass through hydrolysis and dehydration synthesis (sol-gel reaction) when reacting with moisture in the atmosphere. For this reason, there is a possibility that materials such as lithium silicate, such as Li6Si2O7, and SiO2, may remain as impurities in the surface of the anode active material. The sol-gel reaction is accelerated by a base catalyst. Accordingly, by performing the washing step in the present disclosure, the reaction solution can be removed from the surface of the nonwoven particle while inhibiting the sol-gel reaction.As a result, the impurities are prevented from remaining in the surface of the anode active material and the condensation of the anode active material can be inhibited.

[0064] When the concentration of the LiSi precursor in the total amount of the LiSi precursor solution and the Li extraction solvent is high, production efficiency increases, but the formation of impurities increases. When the concentration of the LiSi precursor is 3.3 g / L or more, performing the washing step allows both to improve production efficiency and reduce the formation of impurities.

[0065] The washing step in the present disclosure is a step of washing the nonwoven-shaped particle with an acid after the Li extraction step. The washing step typically includes a collection process for collecting the nonwoven-shaped particle from the solution after the Li extraction step and a washing process for washing the collected nonwoven-shaped particle with an acid. There are no particular restrictions on the collection process if it is a method capable of collecting the nonwoven-shaped particles, and examples of the method may include filtration of the reaction solution after the Li extraction step.

[0066] The washing method is a method in which the nonwoven particles are washed with an acid, and is not particularly limited if it is a method in which the nonwoven particles are brought into contact with the acid. Examples of such a method may include a continuous filtration method in which a solution containing the acid is poured onto the nonwoven particles collected by the above-mentioned filtration. There are no particular restrictions on the time and number of washing operations.

[0067] There are no particular restrictions on the acid used in the washing step, and the same acids as those exemplified as Li extraction solvents can be used. In this regard, the acid used in the washing process is preferably the same type of acid as that used in the Li extraction step.

[0068] The anode active material obtained through the above-described steps can be collected by any method. Examples of the method may include a method of separating a solid reactant (anode active material) from the solution after the Li extraction step or the solution after the washing step, and then drying the obtained anode active material. 4. Anode active material

[0069] The anode active material obtained by the above-described manufacturing process has the same components as those described above under "A. Anode Active Material"; therefore, descriptions thereof are omitted. C. Battery

[0070] Fig. 2 is a schematic cross-sectional view showing an example of the battery in the present disclosure. Fig.The battery 10 shown in Figure 2 comprises a cathode active material layer 1, an anode active material layer 2, an electrolyte layer 3 formed between the cathode active material layer 1 and the anode active material layer 2, a cathode current collector 4 for collecting currents from the cathode active material layer 1, and an anode current collector 5 for collecting currents from the anode active material layer 2. These elements can be housed in a general outer package. In the present disclosure, the anode active material layer 2 contains the anode active material described above.

[0071] According to the present disclosure, the anode active material layer contains the above-described anode active material, and thus the battery with reduced retention pressure can be obtained. 1. Anode active material layer

[0072] The anode active material layer is a layer containing at least the anode active material described above. The anode active material has the same components as those described above under "A. Anode Active Material"; therefore, descriptions thereof are omitted.

[0073] The anode active material layer may contain only the above-described anode active material as the anode active material, and may also contain an additional anode active material. In the latter case, the proportion of the above-described anode active material to all anode active materials may be, for example, 50 wt.% or more, 70 wt.% or more, and 90 wt.% or more.

[0074] The proportion of the anode active material in the anode active material layer is, for example, 20 wt% or more, may be 30 wt% or more, and may be 40 wt% or more. Meanwhile, the proportion of the anode active material is, for example, 80 wt% or less, may be 70 wt% or less, and may be 60 wt% or less.

[0075] In addition, the anode active material layer may further contain at least one of an electrolyte, a conductivity aid, and a binder, as needed. The type of electrolyte will be described in detail later under "3. Electrolyte Layer." The proportion of the electrolyte in the anode active material layer is, for example, 1 wt% or more, may be 10 wt% or more, and may be 20 wt% or more. Meanwhile, the proportion of the electrolyte in the anode layer is, for example, 60 wt% or less, and may be 50 wt% or less.

[0076] Examples of the conductivity aid include a carbon material and a metal particle. Specific examples of the carbon material include a particulate carbon material such as acetylene black (AB) and Ketjen black (KB), and a fibrous carbon material such as carbon fiber, carbon nanotubes (CNT), and carbon nanofiber (CNF). Examples of the metal particle include Ni, Cu, Fe, and SuS. The proportion of the conductivity aid in the anode active material layer is, for example, 1 wt% or more, and may be 5 wt% or more. Meanwhile, the proportion of the conductivity aid is, for example, 30 wt% or less, and may be 20 wt% or less.

[0077] Examples of the binder may include a rubber-based binder such as a butadiene rubber, a hydrogenated butadiene rubber, a styrene-butadiene rubber (SBR), a hydrogenated styrene-butadiene rubber, a nitrile-butadiene rubber, a hydrogenated nitrile-butadiene rubber, and an ethylene-propylene rubber; a fluoride-based binder such as polyvinylidene fluoride (PVDF), a polyvinylidene fluoride-polyhexafluoropropylene copolymer (PVDF-HFP), polytetrafluoroethylene, and a fluororubber; a polyolefin-based thermoplastic resin such as polyethylene, polypropylene, and polystyrene; an imide-based resin such as polyimide and polyamideimide; an amide-based resin such as polyamide; an acrylic resin such as polymethyl acrylate and polyethyl acrylate; and a methacrylic resin such as polymethyl methacrylate and polyethyl methacrylate. The proportion of the binder in the anode active material layer is, for example, 1 wt% or more and 30 wt% or less.

[0078] The thickness of the anode active material layer is, for example, 0.1 µm or more and 1000 µm or less. 2. Cathode active material layer

[0079] The cathode active material layer is a layer containing at least one cathode active material. Furthermore, the cathode active material layer may further contain at least one electrolyte, a conductivity aid, and a binder, as needed.

[0080] Examples of the cathode active material can be an oxide active material. Examples of the oxide active material that can be used in a lithium-ion battery can be oxide active materials such as LiCoO2, LiMnO2, Li2NiMn3O8, LiVO2, LiCrO2, LiFePO4, LiCoPO4, LiNiO2 and LiNi 1 / 3 CO 1 / 3 Mn 1 / 3 O2. In addition, a coating layer containing a Li-ion conductive oxide such as LiNbO3 can be formed on the surface of these active materials.

[0081] The proportion of the cathode active material in the cathode active material layer is, for example, 20 wt% or more, may be 30 wt% or more, and may be 40 wt% or more. Meanwhile, the proportion of the cathode active material is, for example, 80 wt% or less, may be 70 wt% or less, and may be 60 wt% or less.

[0082] The type and proportion of the solid electrolyte, the conductivity aid, and the binder used for the cathode active material layer may be in the same contents as those described for the anode active material layer described above; therefore, descriptions thereof are omitted.

[0083] The thickness of the cathode active material layer is, for example, 0.1 µm or more and 1000 µm or less. 3. Electrolyte layer

[0084] The electrolyte layer is a layer formed between the cathode active material layer and the anode active material layer. The electrolyte forming the electrolyte layer can be an electrolyte solution (liquid electrolyte) or a solid electrolyte, but the latter is preferred.

[0085] Typical examples of the solid electrolyte may include an inorganic solid electrolyte such as a sulfide solid electrolyte, a nitride solid electrolyte, and a halide solid electrolyte, and an organic polymer electrolyte such as a polymer electrolyte.

[0086] Examples of the sulfide solid electrolyte with lithium ion conductivity may be a solid electrolyte containing a Li element, an X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and an S element. In addition, the sulfide solid electrolyte may further contain at least one of an O element and a halogen element. Examples of the halogen element may include an F element, a Cl element, a Br element, and an I element.

[0087] Examples of the sulfide solid electrolyte may include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-GeS2, Li2S-P2S5-Li 2O , Li2S-P2S5-Li2O-LiI, Li2S-P2S5-LiI-LiBr, Li2S-SiS2, Li2S-SiS2-LII, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2-P2S5-Z m S n (provided that m and n are each a real number; Z is one of Ge, Zn and Ga), Li2S-GeS2, Li 25 -SiS2-Li3PO4 and Li 2S -SiS2-Li x MO y(provided that x and y are each a real number; M is one of P, Si, Ge, B, Al, Ga and In).

[0088] Examples of the oxide solid electrolyte with lithium ion conductivity may also include a solid electrolyte containing a Li element, a Y element (Y is at least one of Nb, B, Al, Si, P, Ti, Zr, Mo, W, and S), and an O element. Specific examples may include a garnet-type solid electrolyte such as Li7La3Zr2O. 12 , Li 7-x La3 (Zr 2-x Nb x ) O 12 (0 ≤ x ≤ 2), Li5La3Nb2O 12; a perovskite-type solid electrolyte such as (Li,La)TiO3, (Li,La)NbO3 and (Li,Sr)(Ta,Zr)O3; a nasicon-type solid electrolyte such as Li(Al,Ti)(PO4)3 and Li(Al,Ga)(PO4)3; a Li-PO-based solid electrolyte such as Li3PO4 and LIPON (a compound in which part of the O in Li3PO4 is substituted by N); and a Li-BO-based solid electrolyte such as Li3BO3 and a compound in which part of the O in Li3BO3 is substituted by C.

[0089] The binder has the same components as those described above under "1. Anode active material layer"; therefore, descriptions thereof are omitted.

[0090] The thickness of the electrolyte layer is, for example, 0.1 µm or more and 1000 µm or less. 4. Other configurations

[0091] The battery in the present disclosure includes at least the above-described anode active material layer, the cathode active material layer, and the electrolyte layer, and typically further includes a cathode current collector for collecting currents from the cathode active material layer and an anode current collector for collecting currents from the anode active material layer. Examples of the material for the cathode current collector may include SUS, aluminum, nickel, iron, titanium, and carbon. Meanwhile, examples of the material for the anode current collector include SUS, copper, nickel, and carbon. 5. Battery

[0092] The battery in the present disclosure is preferably a lithium-ion battery. Furthermore, the battery in the present disclosure may be a liquid-based battery or a pure solid-state battery, with the latter being preferred.

[0093] Furthermore, the battery in the present disclosure may be a primary battery or a secondary battery, but preferably a secondary battery because it can be repeatedly charged and discharged and is useful, for example, as a car battery. The secondary battery includes using the secondary battery as a primary battery (using it only for the purpose of initial charging).

[0094] Furthermore, the battery in the present disclosure may be a single cell or a stacked cell. The stacked cell may be a monopolar stacked cell (a parallel-connected stacked cell) and a bipolar stacked cell (a series-connected stacked cell). Examples of the shape of the battery may include a coin shape, a laminate shape, a cylindrical shape, and a square shape.

[0095] However, the present disclosure is not limited to the embodiments. The embodiments are for illustrative purposes, and any other variations are considered to be within the technical scope of the present disclosure as long as they have substantially the same nature as the technical idea described in the claims of the present disclosure and have a similar operation and effect. ExamplesExample 1Synthesis of anode active material

[0096] 0.65 g of Si particles (particle size: 5 µm, from Kojundo Chemical Laboratory Co., Ltd.) and 0.60 g of Li metal (from Honjo Metal Co., Ltd.) were mixed with an agate mortar under an Ar atmosphere to obtain a LiSi precursor. In a glass reactor under an argon atmosphere, 1.0 g of the LiSi precursor and 125 mL of a dispersant (1,3,5-trimethylbenzene, from NACALAI TESQUE, INC.) were mixed using an ultrasonic homogenizer (UH-50 from SMT Co., LTD.). After mixing, the resulting LiSi precursor dispersion solution was cooled to 0°C, 125 mL of ethanol (from NACALAI TESQUE, INC.) was added dropwise, and the reaction was continued for 120 minutes. After the reaction, 50 ml of acetic acid (from NACALAI TESQUE, INC.) was added dropwise, and the reaction continued for 60 minutes. After the reaction, a liquid and a solid reactant (anode active material) were separated by suction filtration.The resulting solid reactant was vacuum dried at 120°C for 2 hours, thereby collecting the anode active material. The measured mean particle size D. 50 of the obtained anode active material was 0.27 µm. Synthesis of the solid electrolyte

[0097] 0.550 g of Li2S (from Furuuchi Chemical Corporation), 0.887 g of P2S5 (from Sigma-Aldrich), 0.285 g of LiI (from NIPPOH CHEMICALS CO., LTD.), and 0.277 g of LiBr (from Kojundo Chemical Laboratory Co., Ltd.) were mixed for 5 minutes with an agate mortar. 4 g of n-heptane (dehydration grade, from KANTO CHEMICAL CO., INC.) was added to the resulting mixture and mechanically ground with a planetary ball mill for 40 hours, thereby obtaining a solid electrolyte. Production of an evaluation battery

[0098] LiNi 1 / 3 Co 1 / 3 Mn 1 / 3O2 (from NICHIA CORPORATION) was surface-treated with LiNbO3 to obtain a cathode active material. 1.5 g of this cathode active material, 0.023 g of a conductivity aid (VGCF, from Showa Denko KK), 0.239 g of the solid electrolyte, 0.011 g of a binder (PVdF, from KUREHA CORPORATION), and 0.8 g of butyl butylate (from Kishida Chemical Co., Ltd.) were mixed using an ultrasonic homogenizer (UH-50, from SMT Co., Ltd.) to obtain a cathode mixture.

[0099] 1.0 g of the synthesized anode active material, 0.04 g of a conductivity aid (VGCF, from Showa Denko KK), 0.776 g of the solid electrolyte, 0.02 g of a binder (PVdF, from KUREHA CORPORATION), and 1.7 g of butyl butylate (from Kishida Chemical Co., Ltd.) were mixed using an ultrasonic homogenizer (UH-50, from SMT Co., Ltd.), thereby obtaining an anode mixture.

[0100] The solid electrolyte of 0.065 g was placed in a large ceramic mold with 1 cm 2 given, with 1 t / cm 2 pressed, thereby creating a separating layer (solid electrolyte layer). 0.018 g of the cathode mixture was added to one side of the separating layer, with 1 t / cm 2 pressed, thereby creating a cathode active material layer. 0.0054 g of the anode mixture was added to the other side of the cathode active material layer, with 4 t / cm 2 pressed, thereby creating an anode active material layer. Additionally, an aluminum foil was used as the cathode current collector and a copper foil as the anode current collector. In this way, an evaluation battery (solid-state battery) was manufactured. Examples 2 to 7

[0101] In the same manner as in Example 1, an anode active material was synthesized and an evaluation battery was prepared, except that the dispersant and the Li extraction solvent were changed as shown in Table 1. In addition, the average particle size D of each of the obtained anode active materials was measured. 50 measured. The results are shown in Table 2. Comparison example 1

[0102] An anode active material was synthesized and an evaluation battery was prepared in the same manner as in Example 1, except that the dispersant was not used and ethanol cooled to 0°C was used as the Li extraction solvent during the synthesis of the anode active material. In addition, the average particle size D 50 of the resulting anode active material. The results are shown in Table 2. Comparative examples 2 to 4

[0103] An anode active material was synthesized and an evaluation battery was prepared in the same manner as in Comparative Example 1, except that the Li extraction solvent was changed as shown in Table 1. In addition, the average particle size D 50 of the resulting anode active material. The results are shown in Table 2. Evaluation of 1XRD measurement

[0104] X-ray diffraction (XRD) measurements using a CuKα beam were performed on the anode active materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4. The XRD data obtained for Example 1 are shown in Fig. 3A and Fig. 3B. Fig. Figure 3B is an enlarged view of a portion of Fig. 3A. As in Fig. 3A, halo peaks were confirmed near 2θ = 25° to 30° and 2θ = 50° to 60°. The former corresponds to peak “b”. As shown in Fig. 3B, a peak “a” at the position 2θ = 28.4° was also confirmed to be extremely low. Fig. 3B at a level that can be assessed as "peak "a" was not confirmed". In addition, the Fig. 3A and Fig. 3B, the peak position of peak "a" almost coincides with the peak position of peak "b." From these data, the XRD intensity ratio Ia / Ib was determined: Ia / Ib = 0.99; thus, Ia and Ib had almost the same intensity. The XRD intensity ratios for Examples 2 to 7 and Comparative Examples 1 to 4 were obtained in the same way. The results are shown in Table 2.

[0105] As shown in Table 2, the XRD intensity ratios of Examples 1 to 7 were smaller than those of Comparative Examples 1 to 4, and it was confirmed that the crystallinity of the anode active material was lower and more amorphous. Microscopic observation

[0106] The shapes of the anode active materials obtained in Examples 1 to 2 and Comparative Example 1 were observed using a transmission electron microscope (TEM). The results are shown in Fig. 4. In addition, the shape of the anode active material obtained in Comparative Example 1 was observed with a scanning electron microscope (SEM). The result is shown in Fig. 5 shown.

[0107] As in Fig. As shown in Figure 4, it was confirmed that in the anode active material in the examples where the LiSi precursor was dispersed in the dispersant and then Li was extracted, the Si fibers were three-dimensionally entangled. In contrast, the shape of the anode active material in Comparative Example 1, where the LiSi precursor was not dispersed in the dispersant and Li was extracted, was completely different from that in the examples. As can be seen from the Fig.As can be seen from the SEM image shown, this is because the shape of the anode active material in Comparative Example 1 was not a nonwoven fabric, but a shape in which the particles were merely porous. The reason why the fibrous shape was not confirmed in Comparative Example 1 was presumably because the Li extraction reaction was not inhibited, and thus not only Li elements but also the Si skeleton were extracted from the LiSi precursor at the same time. Cavity, mean diameter and aspect ratio

[0108] The cross-sectional images of the anode active materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4 were taken with a scanning electron microscope (SEM), and their voids were measured. In addition, the average diameter and aspect ratio of the Si fiber were calculated for the examples. The results are shown in Table 2.

[0109] As shown in Table 2, the voids of Examples 1 to 4 were larger than those of Comparative Examples 1 to 4, but the voids of Examples 5 to 7 were smaller than those of Comparative Example 1 (void: 12%). Generally, the expansion (amount of retention pressure increase) tends to be small when the void is large because the void can absorb the expansion. However, as described later, the amounts of retention pressure increase in Examples 5 to 7, in which the voids were smaller than those of Comparative Example 1, were remarkably small. It was also confirmed that the aspect ratio of each of the examples was 1 or more, and thus, it was a fibrous form. Amount of retention pressure increase

[0110] The evaluation batteries obtained in Examples 1 to 7 and Comparative Examples 1 to 4 were CC / CV charged at 0.245 mA to 4.55 V and then discharged at 0.245 mA to 3.0 V CC / CV. During the initial charge, the retention pressure of each battery was monitored, and the retention pressure at 4.55 V was measured. Relative evaluation was performed using the retention pressure of Comparative Example 1 as 1.00. The results are shown in Table 2. As can be seen from Table 2, the retention pressure increase amounts in Examples 1 to 7 were remarkably smaller than those in Comparative Examples 1 to 4. Table 1 Dispersant (relative dielectric constant) Li extraction agent Example 1 1,3,5-Trimethylbenzene (2,279) Ethanol acetic acid Example 2 n-Butyl ether (3.08) Ethanol acetic acid Example 3 n-Heptane (1.94) Ethanol acetic acid Example 4 1,3,5-Trimethylbenzene (2,279) 1-Propanol acetic acid Example 5 n-Butyl ether (3.08) 1-Propanol acetic acid Example 6 1,3,5-Trimethylbenzene (2,279) 1-Butanol acetic acid Example 7 1,3,5-Trimethylbenzene (2,279) 1-Hexanol acetic acid Comparison example 1 - Ethanol acetic acid Comparison example 2 - 1-Propanol acetic acid Comparison example 3 - 1-Butanol acetic acid Comparison example 4 - 1-Hexanol acetic acid Table 2 Average particle size [D 50 µm] XRD intensity ratio (Ia / Ib) Average diameter (nm) Aspect ratio Cavity [%] Amount of retention pressure increase Example 1 0,27 0,99 14 30 14 0,51 Example 2 0,42 1,06 28 20 15 0,52 Example 3 1,40 1,20 26 20 14 0,60 Example 4 0,92 1,70 29 20 13 0,57 Example 5 2,03 1,65 34 10 11 0,62 Example 6 2,60 2,15 46 25 11 0,68 Example 7 3,58 3,80 68 5 10 0, 69 Comparison example 1 15,96 5,80 - - 12 1,00 Comparison example 2 16,31 6,83 - - 10 1,09 Comparison example 3 16,52 13,67 - - 9 1,07 Comparison example 4 19,23 20, 50 - - 8 1,05

[0111] As described above, with the method for producing the anode active material in the present disclosure, it was confirmed that the anode active material was obtained in a nonwoven fabric form with a small average particle size and low crystallinity. It was also confirmed that the amount of retention pressure increase of a battery was remarkably inhibited when the anode active material obtained as described above was used for an all-solid-state battery. Example 8

[0112] In the same manner as in Example 1, an anode active material was synthesized and an evaluation battery was manufactured. Example 9

[0113] As shown in Table 3, 12 g of the LiSi precursor, 400 ml of 1,3,5-trimethylbenzene, 400 ml of ethanol, and 600 ml of acetic acid were used in the synthesis of the anode active material. In the same manner as in Example 1, except for the above, an anode active material was synthesized and an evaluation battery was manufactured. The average particle size D of the obtained anode active material was also measured. 50 measured, and the result was 1.34 µm. Example 10

[0114] As shown in Table 3, 12 g of the LiSi precursor, 400 ml of 1,3,5-trimethylbenzene, 400 ml of ethanol, and 600 ml of acetic acid were used to synthesize the anode active material. Furthermore, after reacting the LiSi precursor dispersion solution with acetic acid, a liquid and solid reactant were separated by suction filtration using a filter. Then, for continuous suction filtration, 100 ml of acetic acid was added to the solid reactant, which settled on the filter, and the solid reactant was washed with acetic acid. The washed solid reactant was vacuum-dried at 120°C for 2 hours, thereby synthesizing an anode active material. An evaluation battery was prepared in the same manner as in Example 1, except for the above. Furthermore, the average particle size D 50 of the obtained anode active material was measured and the result was 0.61 µm. Evaluation of 2XRD measurement

[0115] In the same manner as in Evaluation 1, X-ray diffraction (XRD) measurements using a CuKα beam were performed on the anode active materials obtained in Examples 8 to 10. The XRD data obtained are shown in Fig. 6. As shown in Fig. As shown in Figure 6, peak "c" originating from SiO2 and peak "d" originating from lithium silicate were confirmed in Example 9. However, peak "c" originating from SiO2 and peak "d" originating from lithium silicate were not confirmed in Examples 8 and 10. Fig. 6 • the peak “c” and ▲ the peak “d”. Amount of retention pressure increase

[0116] The retention pressures of the evaluation batteries obtained in Examples 8 to 10 were measured in the same manner as in Evaluation 1. A relative evaluation was performed using the retention pressure from Example 8 as 1.00. The results are shown in Table 4. Table 3 Materials for the Li extraction step Washing step LiSi (g) 1,3,5-Trimethylbenzene (ml) Ethanol (ml) Acetic acid (ml) Example 8 1 125 125 50 Not carried out Example 9 12 400 400 600 Not carried out Example 10 12 400 400 600 Carried out Table 4 Average particle size [D 50 µm] Amount of retention pressure increase Example 8 0,27 1,00 Example 9 1,34 1,23 Example 10 0,61 0, 95

[0117] As shown in Table 4, in Example 9, in which the produced size of the anode active material was increased and the washing step was not performed, the average particle size and the amount of retention pressure increase of the anode active material were larger than in Example 8. On the other hand, in Example 10, in which the washing step was performed, the average particle size of the anode active material was smaller than in Example 8 and Example 9, and the amount of retention pressure increase was further inhibited. This is presumably due to the fact that impurities such as SiO2 and lithium silicate were removed in the washing step. Thus, it was confirmed that the condensation of the anode active material due to remaining impurities was inhibited, and the amount of retention pressure increase was also further inhibited when the washing step was performed in the process for producing the anode active material in the present disclosure. List of reference symbols 1 cathode active material layer 2 Anode active material layer 3 Electrolyte layer 4 Cathode current collector 5 Anode current collector 10 Battery

Claims

[1] A process for producing an anode active material, the process characterized by is that it includes: a dispersing step of adding a dispersant to a LiSi precursor containing a Si element and a Li element to obtain a LiSi precursor dispersion solution, wherein the LiSi precursor is obtained by mixing or grinding Si particles with Li particles; and a Li extraction step for extracting the Li element from the LiSi precursor by adding a Li extraction solvent to the LiSi precursor dispersion solution to obtain a nonwoven fabric-form particle containing Si fibers, wherein a relative dielectric constant of the dispersant is 3.08 or less. [2] A method for producing an anode active material according to claim 1, wherein the mixing or grinding of the Si particles with Li particles is carried out using an agate mortar under an Ar atmosphere or using mechanical grinding. [3] A process for producing an anode active material according to claim 1 or 2, characterized by that the dispersant is at least one of n-butyl ether, 1,3,5-trimethylbenzene and n-heptane. [4] A process for producing an anode active material according to any one of claims 1 to 3, characterized by that the Li extraction solvent is at least one of ethanol, 1-propanol, 1-butanol, 1-hexanol and acetic acid. [5] A method for producing an anode active material according to any one of claims 1 to 4, further comprising a washing step of washing the nonwoven fabric-shaped particle with an acid after the Li extraction step. [6] Anode active material obtainable by a process according to any one of claims 1 to 5, wherein an average particle size D 50 of the anode active material is 0.2 µm or more and 3.6 µm or less and the anode active material is amorphous. [7] Anode active material according to claim 6, characterized by that in an XRD measurement of the anode active material using a CuKα beam, a peak “a” originating from Si and positioned at 2θ = 28.4° ± 0.5° is not observed. [8] Anode active material according to claim 6 or 7, characterized by that in an XRD measurement of the anode active material using a CuKα beam, a peak “a” originating from Si is observed, positioned at 2θ = 28.4° ± 0.5°, a peak ‘b’ positioned at 2θ = 24.0° - 32.0° is observed, the half-width of which is 3° or more, and where Ia denotes an intensity of peak “a” and Ib denotes an intensity of peak “b”, an XRD intensity ratio Ia / Ib is 3.80 or less. [9] Anode active material according to one of claims 6 to 8, characterized by that in an XRD measurement of the anode active material using a CuKα beam, a peak “c” originating from SiO2, positioned at 2θ = 20.8° ± 0.5°, is not observed. [10] Anode active material according to one of claims 6 to 9, characterized by that in an XRD measurement of the anode active material using a CuKα beam, a peak “d” originating from lithium silicate, positioned at 2θ = 20° - 30°, is not observed. [11] Anode active material according to one of claims 6 to 10, characterized by that an average diameter of the Si fiber is 8 nm or more and 70 nm or less. [12] Anode active material according to one of claims 6 to 11, characterized bythat an aspect ratio of the Si fiber, which is a ratio of average length / average diameter, is 1 or more and 50 or less. [13] Battery (10) with a cathode active material layer (1), an anode active material layer (2), an electrolyte layer (3) formed between the cathode active material layer (1) and the anode active material layer (2), characterized by that the anode active material layer (2) contains the anode active material according to one of claims 6 to 12.

Citation Information

Patent Citations

  • Lock for double sliding door

    JP2008138487A

  • Porous silicon particle and method for producing the same

    JP2013203626A

  • Negative electrode for all-solid battery

    JP2017054720A

  • Carbon composite silicon material and manufacturing method therefor, and negative electrode material for lithium secondary batteries

    JP2016028375A

  • Additive for lithium ion rechageable battery cells

    US20130069601A1