Semiconductor device structure and method for forming the same
Fluorinated spacers in semiconductor devices address the challenges of dielectric constant, leakage current, and moisture absorption, improving thermal stability and device performance through controlled fluorination processes.
Patent Information
- Application Number
- DE102024100175
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-01-04
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2044-01-04
AI Technical Summary
The increasing complexity and downscaling of semiconductor integrated circuits (ICs) pose challenges in processing and manufacturing, particularly in reducing the dielectric constant (K), leakage current, and moisture absorption, while maintaining thermal stability.
The implementation of fluorinated gate spacers and dielectric spacers at various stages of semiconductor device fabrication, using controlled fluorination processes to reduce the dielectric constant, minimize leakage current, and enhance thermal stability.
The fluorinated spacers result in reduced dielectric constant, decreased leakage current, improved thermal stability, and reduced moisture absorption, thereby enhancing the performance and reliability of semiconductor devices.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND
[0001] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological advances in IC materials and design have produced generations of ICs, with each generation featuring smaller and more complex circuits than the previous generation. As ICs have evolved, functional density (i.e., the number of interconnected devices per chip area) has generally increased, while geometry size (i.e., the smallest component (or line) that can be created using a manufacturing process) has decreased. This downscaling process generally provides benefits by increasing production efficiency and reducing associated costs. Such downscaling has also increased the complexity of IC processing and manufacturing.
[0002] Therefore, there is a need to improve the processing and manufacturing of ICs.
[0003] From US 2019 / 0 006 242 A1 a method for producing a semiconductor device is known in which gate spacers are formed on a sacrificial gate electrode and, after removal of the sacrificial gate electrode, fluorine is introduced into the gate spacers.
[0004] US 2023 / 0 207 395 A1 describes a semiconductor device having a gate structure and a dielectric layer on a sidewall of the gate structure, wherein the dielectric layer contains fluorine-doped SiOCN or fluorine-doped SiOC.
[0005] From US 2022 / 0 367 670 A1 a method for producing a transistor structure is known in which dielectric spacers are formed between semiconductor layers and the dielectric spacers may contain fluorine. BRIEF DESCRIPTION OF THE DRAWINGS
[0006] Aspects of the present disclosure are best understood from the following detailed description in combination with the accompanying figures. It should be noted that, in accordance with standard industry practice, various features are not drawn to scale. Indeed, the dimensions of the various elements may be arbitrarily exaggerated or reduced for clarity of illustration. Fig. 1-5 are perspective views of various stages of fabricating a semiconductor device structure according to some embodiments. Fig. 6 is a cross-sectional side view of one of various stages of fabrication of the semiconductor device structure taken along line AA of Fig. 5 according to some embodiments. Fig. 7 illustrates the fluorination of a first gate spacer of the semiconductor device structure according to some embodiments. Fig. 8-10 are cross-sectional side views of various stages of fabrication of the semiconductor device structure along line AA of Fig. 5 according to some embodiments. Fig. 11 is a perspective view of the semiconductor device structure of Fig. 10 according to some embodiments. Fig. 12-17 are cross-sectional side views of various stages of fabrication of the semiconductor device structure along line AA of Fig. 5 according to some embodiments. Fig. 18A and Fig. 18B are diagrams illustrating a SiF concentration profile in the first and a second gate spacer according to some embodiments. Fig. 19 is a cross-sectional view of the semiconductor device structure of Fig. 16 according to alternative embodiments. Fig. 20A and Fig. 20B are various views of one of various stages of fabricating the semiconductor device structure of Fig. 19 according to some embodiments. Fig. 21 illustrates the fluorination of a dielectric spacer of the semiconductor device structure according to some embodiments. Fig. Figure 22 illustrates the fluorination of the dielectric spacer of the semiconductor device structure according to alternative embodiments. Fig. 23 is a diagram showing a SiF concentration profile in the dielectric spacer according to some embodiments. Fig. 24 illustrates a portion of the semiconductor device structure of Fig. 20B according to some embodiments. DETAILED DESCRIPTION
[0007] The present invention provides a semiconductor device structure having the features of claim 1, as well as methods having the features of claims 7 and 16, respectively. Exemplary embodiments are set forth in the dependent claims. The following disclosure provides many different embodiments or examples for implementing various features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the present disclosure. These are, of course, merely examples and are not intended to be limiting.For example, the formation of a first element over or on top of a second element in the following description may include embodiments in which the first and second elements are formed in direct contact, and may also include embodiments in which additional elements may be formed between the first and second elements such that the first and second elements may not be in direct contact. Additionally, the present disclosure may repeat reference numerals throughout the various examples. This repetition is for the purpose of simplicity and clarity and does not, in itself, prescribe any relationship between the various embodiments and / or configurations discussed.
[0008] Furthermore, spatially relative terms such as "beneath," "under," "lower," "over," "upon," "above," "above," and the like may be used herein for ease of description to describe the relationship of one component or element to one or more other components or elements, as illustrated in the figures. The spatially relative terms are intended to encompass various orientations of the device in use or operation, in addition to the orientation illustrated in the figures. The device may be oriented differently (rotated 90 degrees or in other orientations), and the spatially relative terms used herein may also be interpreted accordingly.
[0009] Embodiments of the present disclosure provide semiconductor device structures with fluorinated first and second gate spacers and fluorinated dielectric spacers. The first and second gate spacers and the fluorinated dielectric spacers are fluorinated at various stages of fabricating the semiconductor device structure. As a result, the dielectric constant (K) is reduced, leakage current is reduced, thermal stability is improved, and moisture absorption is reduced.
[0010] While the embodiments of this disclosure are discussed with respect to nanostructure channel FETs, such as gate-all-around FETs (GAA-FETs), for example, horizontal gate-all-around FETs (HGAA-FETs) or vertical gate-all-around FETs (VGAA-FETs), implementations of some aspects of the present disclosure may be used in other processes and / or in other devices, such as planar FETs, fin FETs, and other suitable devices. One of ordinary skill in the art will readily understand that other modifications that may be made are contemplated within the scope of this disclosure. In cases where gate-all-around transistor (GAA-transistor) structures are used, the GAA-transistor structures may be patterned by any suitable method.For example, the structures may be patterned using one or more photolithography processes, including double-patterning or multi-patterning processes. Generally, double-patterning or multi-patterning processes combine photolithography processes and self-aligned processes, thereby enabling structures to be created that, for example, have pitches smaller than those that can otherwise be obtained using a single, direct photolithography process. For example, in one embodiment, a sacrificial layer is formed over a substrate and patterned using a photolithography process. Spacers are formed along the patterned sacrificial layer using a self-aligned process. The sacrificial layer is then removed, and the remaining spacers can then be used to pattern the GAA structure.
[0011] Fig. 1-17 show exemplary processes for manufacturing a semiconductor device structure 100 according to embodiments of the present disclosure. It is understood that for further embodiments of the method, further steps may be performed before, during, and after the steps shown in Fig. 1-17 may be provided, and some of the steps described below may be replaced or omitted. The order of the steps / processes is not restrictive and may be interchangeable.
[0012] Fig. 1-5 are perspective views of various stages of fabricating a semiconductor device structure 100 according to some embodiments. As shown in Fig. 1, a semiconductor device structure 100 includes a stack of semiconductor layers 104 formed over a front surface of a substrate 101. The substrate 101 may be a semiconductor substrate. The substrate 101 may include a crystalline semiconductor material such as, but not limited to, silicon (Si), germanium (Ge), silicon germanium (SiGe), gallium arsenide (GaAs), indium antimonide (InSb), gallium phosphide (GaP), gallium antimonide (GaSb), indium aluminum arsenide (InAlAs), indium gallium arsenide (InGaAs), gallium antimony phosphide (GaSbP), gallium arsenic antimonide (GaAsSb), and indium phosphide (InP). In some embodiments, substrate 101 is a silicon-on-insulator (SOI) substrate with an insulating layer (not shown) sandwiched between two silicon layers for enhancement. In one aspect, the insulating layer is an oxygen-containing layer.
[0013] The substrate 101 may include various regions doped with impurities (e.g., p-type or n-type dopants). Depending on the circuit design, the dopants may be, for example, phosphorus for an n-type field-effect transistor (NFET) and boron for a p-type field-effect transistor (PFET).
[0014] The stack of semiconductor layers 104 comprises alternating semiconductor layers made of different materials to enable the formation of nanostructure channels in a multi-gate device, such as nanostructure channel FETs. In some embodiments, the stack of semiconductor layers 104 comprises first semiconductor layers 106 and second semiconductor layers 108. In some embodiments, the stack of semiconductor layers 104 comprises alternating first and second semiconductor layers 106, 108. The first semiconductor layers 106 and the second semiconductor layers 108 are made of semiconductor materials with different etch selectivity and / or different oxidation rates. For example, the first semiconductor layers 106 may be made of Si and the second semiconductor layers 108 may be made of SiGe.In some examples, the first semiconductor layers 106 may be made of SiGe and the second semiconductor layers 108 may be made of Si. Alternatively, in some embodiments, each of the semiconductor layers 106, 108 may be or comprise other materials, such as Ge, SiC, GeAs, GaP, InP, InAs, InSb, GaAsP, AlInAs, AlGaAs, InGaAs, GaInP, GaInAsP, or any combination thereof.
[0015] The first and second semiconductor layers 106, 108 are formed by any suitable deposition process, such as epitaxy. For example, the epitaxial growth of the layers of the stack of semiconductor layers 104 can be performed by a molecular beam epitaxy (MBE) process, a metalorganic chemical vapor deposition (MOCVD) process, and / or other suitable epitaxial growth processes.
[0016] The first semiconductor layers 106 or portions thereof may form nanostructure channels of the semiconductor device structure 100 in later manufacturing stages. The term "nanostructure" is used here to refer to any material portion with nanoscale or even microscale dimensions and with an elongated shape, regardless of the cross-sectional shape of this portion. Thus, this term refers to both elongated material portions with a circular or substantially circular cross-section, as well as bar- or rod-shaped material portions, for example, having a cylindrical or substantially rectangular cross-section. The nanostructure channel(s) of the semiconductor device structure 100 may be surrounded by a gate electrode. The semiconductor device structure 100 may comprise a nanostructure transistor.The nanostructure transistors may be referred to as nanosheet transistors, nanowire transistors, gate-all-around (GAA) transistors, multibridge channel (MBC) transistors, or any transistor with the gate electrode surrounding the channels. The use of the first semiconductor layers 106 to define a channel or channels of the semiconductor device structure 100 is discussed further below.
[0017] Each first semiconductor layer 106 may have a thickness in a range between about 5 nm and about 30 nm. Each second semiconductor layer 108 may have a thickness that is equal to, less than, or greater than the thickness of the first semiconductor layer 106. In some embodiments, each second semiconductor layer 108 has a thickness in a range between about 2 nm and about 50 nm. Three first semiconductor layers 106 and three second semiconductor layers 108 are arranged alternately, as shown in Fig. 1, which is for illustrative purposes and is not intended to be limiting beyond what is expressly stated in the claims. It should be understood that any number of first and second semiconductor layers 106, 108 may be formed in the stack of semiconductor layers 104, and the number of layers depends on the predetermined number of channels for the semiconductor device structure 100.
[0018] As in Fig. 2, fin structures 112 are formed from the stack of semiconductor layers 104. Each fin structure 112 has a top portion comprising the semiconductor layers 106, 108, and a well portion 116 formed from the substrate 101. The fin structures 112 may be formed by patterning a hard mask layer (not shown) formed on the stack of semiconductor layers 104 using multiple patterning steps, including photolithography and etching processes. The etching process may include dry etching, wet etching, reactive ion etching (RIE), and / or other suitable processes. The photolithography process may include forming a photoresist layer (not shown) over the hard mask layer, exposing the photoresist layer to a pattern, performing post-exposure annealing processes, and developing the photoresist layer to form a masking element comprising the photoresist layer.In some embodiments, patterning the photoresist layer to form the masking element may be performed using an electron beam (e-beam) lithography process. The etching process forms trenches 114 in unprotected regions through the hard mask layer, through the stack of semiconductor layers 104, and into the substrate 101, leaving the plurality of extending fin structures 112. The trenches 114 extend along the X-direction. The trenches 114 may be etched using a dry etch (e.g., RIE), a wet etch, and / or a combination thereof.
[0019] As in Fig. As shown in Figure 3, after the fin structures 112 are formed, an insulating material 118 is formed on the substrate 101. The insulating material 118 fills the trenches 114 between adjacent fin structures 112 until the fin structures 112 are embedded in the insulating material 118. Then, a planarization step, such as a chemical mechanical polishing (CMP) process and / or an etch-back process, is performed so that the top surface of the fin structures 112 is exposed. The insulating material 118 may be made of silicon oxide, silicon nitride, silicon oxynitride (SiON), SiOCN, SiCN, fluorine-doped silicate glass (FSG), a low-K dielectric material, or any suitable dielectric material.The insulating material 118 may be formed by any suitable process, such as low-pressure chemical vapor deposition (LPCVD), plasma enhanced CVD (PECVD), or flowable CVD (FCVD).
[0020] As in Fig. As shown in Figure 4, the insulating material 118 is recessed to form isolation regions 120. The recess of the insulating material 118 exposes portions of the fin structures 112, such as the stack of semiconductor layers 104. The recess of the insulating material 118 exposes the trenches 114 between the adjacent fin structures 112. The isolation regions 120 may be formed using a suitable process, such as a dry etching process, a wet etching process, or a combination thereof. A top surface of the insulating material 118 may be flush with or below a surface of the second semiconductor layers 108 in contact with the well portion 116 formed from the substrate 101.
[0021] As in Fig. 5, one or more sacrificial gate structures 130 (only one is shown) are formed over the semiconductor device structure 100. The sacrificial gate structures 130 are formed over a portion of the fin structures 112. Each sacrificial gate structure 130 may include a sacrificial gate dielectric layer 132, a sacrificial gate electrode layer 134, and a mask layer 136. The sacrificial gate dielectric layer 132, the sacrificial gate electrode layer 134, and the mask layer 136 may be formed by sequentially depositing cap layers of the sacrificial gate dielectric layer 132, the sacrificial gate electrode layer 134, and the mask layer 136 and then patterning these layers into the sacrificial gate structures 130. While one sacrificial gate structure 130 is shown, in some embodiments, two or more sacrificial gate structures 130 may be arranged along the X-direction.
[0022] The sacrificial gate dielectric layer 132 may comprise one or more layers of dielectric material, such as a silicon oxide-based material. The sacrificial gate electrode layer 134 may include silicon, such as polycrystalline silicon or amorphous silicon. The mask layer 136 may comprise more than one layer, such as an oxide layer and a nitride layer. The portions of the fin structures 112 covered by the sacrificial gate electrode layer 134 of the sacrificial gate structure 130 serve as channel regions for the semiconductor device structure 100.
[0023] Fig. 6 is a cross-sectional side view of one of various stages of fabrication of the semiconductor device structure 100 taken along line AA of Fig. 5 according to some embodiments. As in Fig. 6, a first gate spacer 138 is deposited on the exposed surfaces of the semiconductor device structure 100. For example, the first gate spacer 138 is deposited on the fin structures 112, the isolation regions 120, and the sacrificial gate structure 130. The first gate spacer 138 may be made of a dielectric material, such as silicon oxide, silicon nitride, silicon carbide, silicon oxynitride, SiCN, silicon oxycarbide, SiCON, and / or combinations thereof. The first gate spacer 138 may be formed by any suitable process. In some embodiments, the first gate spacer 138 is a conformal layer formed by a conformal process, such as an atomic layer deposition (ALD) process.
[0024] After deposition of the first gate spacer 138, one or more processes are performed to introduce fluorine into the first gate spacer 138. Fig. Figure 7 illustrates the fluorination of the first gate spacer 138 of the semiconductor device structure 100 according to some embodiments. In some embodiments, the first gate spacer 138 includes as-deposited SiOCN and may have a chemical structure A, as shown in Fig. 7. In some embodiments, a plasma treatment process may be performed on the first gate spacer 138 as deposited, and the chemical structure of the first gate spacer 138 changes from chemical structure A to chemical structure B, as shown in Fig. 7. The plasma treatment process includes exposing the first gate spacer 138 to a hydrogen-containing plasma. The hydrogen-containing plasma may be formed by activating a hydrogen-containing gas by a low-power plasma source or a remote plasma source. The hydrogen-containing gas may be any suitable hydrogen-containing gas. In some embodiments, the hydrogen-containing gas is hydrogen gas (H2). In some embodiments, the low-power plasma source is a capacitively coupled plasma source, and the plasma power ranges from about 10 W to about 250 W. The plasma generated by the capacitively coupled plasma source or the remote plasma source contains more hydrogen radicals than ions. Additionally, the processing temperature of the plasma treatment process is relatively low, such as from about 20 degrees Celsius to about 100 degrees Celsius.As a result, the hydrogen radicals replace the methyl end groups or are bonded to the unoccupied Si bonds to form SiH bonds, as in chemical structure B in . Fig. 7 shown.
[0025] Next, a fluorination process is performed on the treated first gate spacer 138. The fluorination process may be any suitable fluorination process. In some embodiments, the fluorination process is a fluorine impregnation process. The fluorine impregnation process may include exposing the treated first gate spacer 138 to a fluorine-containing precursor at a processing temperature of less than about 100 degrees Celsius. In some embodiments, the fluorine-containing precursor includes HF, CF4, F2, C2F6, a combination of HF and F2, or another suitable fluorine-containing precursor. The processing temperature may range from about 20 degrees Celsius to about 99 degrees Celsius, and a processing pressure may range from about 13 Pa (0.1 Torr) to about 1.3 kPa (10 Torr).The treated first gate spacer 138 may be exposed to the fluorine-containing precursor for a duration ranging from about 1 minute to about 30 minutes. In some embodiments, the fluorine-containing precursor is F2, and the treated first gate spacer 138 may be exposed to the F2 for a duration ranging from about 5 minutes to about 5 hours. The fluorine in the fluorine-containing precursor has a higher probability of breaking the SiH bonds than SiO bonds under the aforementioned process conditions. As a result, the chemical structure of the first gate spacer 138 changes from chemical structure B to chemical structure C, as shown in FIG. Fig. 7. The hydrogen atoms bonded to Si are replaced by fluorine atoms. Due to the increased SiH bonds created by the plasma treatment process, the fluorination process can be carried out with relatively low energy, such as at a low temperature without plasma. A low-energy fluorination process can prevent the fluorine-containing precursor from becoming an etchant.
[0026] In some embodiments, the plasma treatment process is not performed, and the fluorination process is performed with higher energy, such as at a higher temperature, for example, greater than about 200 degrees Celsius. The SiCH3 bonds and / or SiO bonds may be broken by the fluorination process, and the CH3 and / or O are replaced by F to form SiF bonds. In some embodiments, the SiF bonds formed from SiH are more thermally stable than the SiF bonds formed from SiCH3 or SiO. One reason is that the Si in the SiF bond formed from SiH may additionally be bonded to two or more oxygen atoms, as in Fig. 7, while the Si in the SiF bond formed from SiCH3 or SiO may additionally be bonded to an oxygen atom and / or one or more methyl groups. The two or more oxygen atoms bonded to the Si of the SiF bond formed from SiH may result in a more stable SiF bond. For example, when exposed to a temperature greater than or equal to 600 degrees, the SiF bonds formed from SiCH3 or SiO may decompose, while the SiF bonds formed from SiH may still be stable. In some embodiments, the SiF bonds formed from SiH are stable when exposed to a temperature greater than about 750 degrees Celsius for a duration ranging from about 30 minutes to about 12 hours.
[0027] After the fluorination process, the first gate spacer 138 may contain about one atomic percent to about five atomic percent fluorine. As shown in Fig. As shown in Figure 6, the first gate spacer 138 has an outer surface 1380 and an inner surface 138i. The concentration of fluorine decreases from the outer surface 1380 to the inner surface 138i because the outer surface 1380 is exposed to the fluorine-containing precursors. The K value of the first gate spacer 138 may have decreased by about 0.1 to about 0.5. The density of the first gate spacer 138 may be in the range of about 2 g / cm 3 up to about 3.2 g / cm 3In some embodiments, the first gate spacer 138 may include about five atomic percent to about 20 atomic percent carbon and about zero atomic percent to about 10 atomic percent nitrogen. In some embodiments, the as-deposited first gate spacer 138 has an average surface charge Vcpd in the range of about 0.245 V to about 0.351 V. The fluorinated first gate spacer 138 has an average surface charge Vcpd in the range of -0.083 to about 0.127. Thus, the fluorinated first gate spacer 138 may have a negative surface charge.
[0028] Fig. 8-10 are cross-sectional side views of various stages of fabrication of the semiconductor device structure 100 along line AA of Fig. 5 according to some embodiments. As in Fig. 8, a second gate spacer 139 is deposited on the first gate spacer 138. The second gate spacer 139 may include any suitable dielectric material, such as SiO x, SiON, SiN, SiCON, or SiCO. The second gate spacer 139 may have a thickness ranging from about 0.5 nm to about 5 nm. The second gate spacer 139 may also function as a capping layer for the fluorinated first gate spacer 138. Subsequent processes, such as etching or epitaxial growth processes, may cause the fluorine in the first gate spacer 138 to be released, which may damage the exposed surfaces of the semiconductor device structure 100. The second gate spacer 139 may be formed by any suitable process. In some embodiments, the second gate spacer 139 is deposited by CVD, PECVD, or electron cyclotron resonance CVD (ECR-CVD). The plasma source may be an inductively coupled plasma source or a capacitively coupled plasma source.The plasma power may range from about 100 W to about 500 W, and the processing temperature may range from about 100 degrees Celsius to about 600 degrees Celsius. In some embodiments, a layer is deposited and a treatment process is performed to form the second gate spacer 139. For example, the layer, such as an amorphous silicon layer, a silicon carbide layer, a SiCN layer, or a SiCON layer, is first deposited on the first gate spacer 138, and the layer is then exposed to a treatment gas to form the second gate spacer 139. The treatment gas may be an oxygen-containing gas, a nitrogen-containing gas, or a combination thereof. In some embodiments, the treatment gas includes N2O, NH3, O2, or a combination of N2 and O2.
[0029] At this stage, the second gate spacer 139 is not fluorinated. If the second gate spacer 139 is fluorinated immediately after deposition, subsequent processes, such as etching or epitaxial growth processes, may cause the fluorine in the second gate spacer 139 to be released.
[0030] As in Fig. As shown in Figure 9, horizontal portions of the first and second gate spacers 138, 139 are removed. In some embodiments, the horizontal portions of the first and second gate spacers 138, 139 are removed by an anisotropic etching process. The anisotropic etching process may be a selective etching process that does not significantly affect the mask layer 136, the stack of semiconductor layers 104, and the isolation regions 120.
[0031] As in Fig. As shown in Figure 10, the portions of the fin structures 112 not covered by the sacrificial gate structure 130 and the first and second gate spacers 138, 139 are recessed to a level above, at, or below the upper surfaces of the isolation regions 120. The recessing of the portions of the fin structures 112 may be performed by an etching process. The etching process may be a dry etch, such as an RIE, NBE, or the like, or a wet etch, such as using tetramethylammonium hydroxide (TMAH), ammonium hydroxide (NH4OH), or any suitable etchant.
[0032] Fig. 11 is a perspective view of the semiconductor device structure 100 of Fig. 10 according to some embodiments. Fig. 12-18 are cross-sectional side views of various stages of fabrication of the semiconductor device structure along line AA of Fig. 5 according to some embodiments. As in Fig. As shown in Figure 12, edge portions of each second semiconductor layer 108 of the stack of semiconductor layers 104 are removed horizontally along the X-direction. Removing the edge portions of the second semiconductor layers 108 forms recesses. In some embodiments, the portions of the second semiconductor layers 108 are removed by a selective wet etching process. In cases where the second semiconductor layers 108 are made of SiGe and the first semiconductor layers 106 are made of silicon, the second semiconductor layer 108 may be selectively etched using a wet etchant, such as, but not limited to, ammonium hydroxide (NH4OH), tetramethylammonium hydroxide (TMAH), ethylenediamine pyrocatechol (EDP), or potassium hydroxide (KOH).
[0033] After removing edge portions of every second semiconductor layer 108, a dielectric layer is deposited in the recesses to form dielectric spacers 144. The dielectric spacers 144 may be made of a low-k dielectric material, such as SiON, SiCN, SiOC, SiOCN, or SiN. The dielectric spacers 144 may be formed by first forming a conformal dielectric layer using a conformal deposition process, such as ALD, followed by an anisotropic etch to remove portions of the conformal dielectric layer other than the dielectric spacers 144. The dielectric spacers 144 are protected by the first semiconductor layers 106 during the anisotropic etch process.The remaining second semiconductor layers 108 are covered between the dielectric spacers 144 along the X-direction.
[0034] As in Fig. 13, source / drain (S / D) regions 146 are formed from the well portion 116. The S / D regions 146 may grow both vertically and horizontally to form facets that may correspond to crystalline planes of the material used for the well portion 116. In this disclosure, a source region and a drain region are used interchangeably, and their structures are substantially the same. Further, the source / drain region(s) may refer to a source or a drain, individually or collectively, depending on the context. The S / D regions 146 may be made of one or more layers of Si, SiP, SiC, and SiCP for n-channel FETs, or Si, SiGe, Ge for p-channel FETs. For p-channel FETs, p-type dopants, such as boron (B), may also be included in the S / D regions 146. The S / D regions 146 may be formed by an epitaxial growth process using CVD, ALD, or MBE.
[0035] As in Fig. As shown in Figure 14, exposed portions of the S / D regions 146 are oxidized to form oxide layers 147. The oxide layers 147 may be formed by any suitable process. In some embodiments, the oxide layers 147 are formed as a result of a cleaning process. The cleaning process may be performed after the formation of the S / D regions 146. The cleaning process may use solutions such as HF, a high-temperature sulfuric peroxide mixture (HTSPM), or ammonia plus hydrogen peroxide. The oxide layer 147 may have a thickness in the range of about 0.5 nm to about 3 nm.
[0036] Next, one or more processes are performed to introduce fluorine into the second gate spacer 139. The one or more processes for introducing fluorine into the second gate spacer 139 may be the same as or different from the one or more processes for introducing fluorine into the first gate spacer 138. In some embodiments, the one or more processes for introducing fluorine into the second gate spacer 139 may be the same as or different from the one or more processes for introducing fluorine into the first gate spacer 138. Fig. 7 is performed to fluorinate the second gate spacer 139. In some embodiments, the higher energy fluorination process is performed to fluorinate the second gate spacer 139 without the plasma treatment process. In some embodiments, the first gate spacer 138 is fluorinated by the higher energy fluorination process without the plasma treatment process, and the second gate spacer 139 is fluorinated by the higher energy fluorination process described in Fig. 7. The entire semiconductor device structure 100 is covered with the first gate spacer 138 during the higher energy fluorination process. A small portion of the first gate spacer 138 can be removed by the fluorine during the higher energy fluorination process, and the other components of the semiconductor device structure 100 are protected by the first gate spacer 138. Components of the semiconductor device structure 100 are exposed during the fluorination of the second gate spacer 139. Thus, the low energy plasma treatment process and fluorination are performed to fluorinate the second gate spacer 139, thereby protecting other components of the semiconductor device structure 100.In other words, in some embodiments, the first and second gate spacers 138, 139 are fluorinated using different processes so as to protect other components of the semiconductor device structure 100.
[0037] As in Fig. As shown in Figure 14, the second gate spacer 139 has an outer surface 1390 and an inner surface 139i. The concentration of fluorine decreases from the outer surface 1390 to the inner surface 139i because the outer surface 1390 is exposed to the fluorine-containing precursors. At this stage, both the first and second gate spacers 138, 139 are fluorinated. As a result, the K value of the first and second gate spacers 138, 139 is reduced. Furthermore, leakage current is reduced, thermal stability is improved, and moisture absorption is reduced. In some embodiments, the combined thickness of the first and second gate spacers 138, 139 is less than about 20 nm, such as from about 5 nm to about 18 nm.
[0038] After introducing fluorine into the second gate spacer 139, the oxide layers 147 may be removed. The removal of the oxide layers 147 may be performed by any suitable process. In some embodiments, a selective etch process is performed to remove the oxide layers 147. Because the oxide layers 147 are substantially thin, the selective etch process does not significantly affect the second gate spacer 139 and the S / D regions 146.
[0039] As in Fig. As shown in Figure 15, a contact etch stop layer (CESL) 162 is conformally formed on the exposed surfaces of the semiconductor device structure 100. The CESL 162 covers the second gate spacer 139, the isolation regions 120, and the S / D regions 146. The CESL 162 may also function as a capping layer for the fluorinated second gate spacer 139. Subsequent processes, such as etching and thermal processes, may cause the fluorine in the second gate spacer 139 to be released, which may damage the exposed surfaces of the semiconductor device structure 100. The CESL 162 may include an oxygen-containing material or a nitrogen-containing material, such as silicon nitride, silicon carbon nitride, silicon oxynitride, carbon nitride, silicon oxide, silicon carbon oxide, or the like, or a combination thereof, and may be formed by CVD, PECVD, ALD, or any suitable deposition technique.In some embodiments, the CESL 162 is a single layer, as shown in FIG. Fig. 15. In some embodiments, the CESL 162 comprises two or more layers. Next, an interlayer dielectric (ILD) layer 164 is formed on the CESL 162. The materials for the ILD layer 164 may include compounds containing Si, O, C, and / or H, such as silicon oxide, SiCOH, or SiOC. Organic materials, such as polymers, may also be used for the ILD layer 164. The ILD layer 164 may be deposited by a PECVD process or other suitable deposition technique. In some embodiments, after the formation of the ILD layer 164, the semiconductor device structure 100 may be subjected to a thermal process to anneal the ILD layer 164.
[0040] After the ILD layer 164 is formed, a planarization step, such as CMP, is performed on the semiconductor device structure 100 until the sacrificial gate electrode layer 134 is exposed, as shown in Fig. 15 shown.
[0041] As in Fig. 16, the sacrificial gate structure 130 and the second semiconductor layers 108 are removed. The removal of the sacrificial gate structure 130 and the semiconductor layers 108 forms an opening between the first gate spacers 138 and between the first semiconductor layers 106. The ILD layer 164 protects the S / D regions 146 during the removal processes. The sacrificial gate structure 130 may be removed using plasma dry etching and / or wet etching. The sacrificial gate electrode layer 134 may first be removed by any suitable process, such as dry etching, wet etching, or a combination thereof, followed by the removal of the sacrificial gate dielectric layer 132, which may also be performed by any suitable process, such as dry etching, wet etching, or a combination thereof.In some embodiments, a wet etchant, such as a tetramethylammonium hydroxide (TMAH) solution, may be used to selectively remove the sacrificial gate electrode layer 134, but not the first gate spacers 138, the ILD layer 164, and the CESL 162.
[0042] The second semiconductor layers 108 may be removed using a selective wet etching process. In cases where the second semiconductor layers 108 are made of SiGe and the first semiconductor layers 106 are made of Si, the chemicals used in the selective wet etching process remove the SiGe while leaving Si, the dielectric materials of the first gate spacers 138, and the dielectric spacers 144 unaffected. In one embodiment, the second semiconductor layers 108 may be removed using a wet etchant, such as, but not limited to, hydrogen fluoride (HF), nitric acid (HNO3), hydrochloric acid (HCl), or phosphoric acid (H3PO4).
[0043] In some embodiments, after removing the sacrificial gate structure 130, but before removing the second semiconductor layers 108, one or more processes are performed to introduce additional fluorine into the first gate spacer 138. The one or more processes for introducing additional fluorine into the first gate spacer 138 may be the same as or different from the one or more processes for introducing initial fluorine into the first gate spacer 138 or the one or more processes for introducing fluorine into the second gate spacer 139. In some embodiments, the one or more processes for introducing additional fluorine into the first gate spacer 138 may be the same as or different from the one or more processes for introducing initial fluorine into the first gate spacer 138 or the one or more processes for introducing fluorine into the second gate spacer 139. Fig. 7 are performed to further fluorinate the first gate spacer 138. In some embodiments, the higher energy fluorination process is performed to further fluorinate the first gate spacer 138 without the plasma treatment process. In some embodiments, the first gate spacer 138 is initially fluorinated by the higher energy fluorination process without the plasma treatment process prior to the formation of the second gate spacer 139, the second gate spacer 139 is formed by the Fig. 7 described plasma treatment process and fluorination process before the formation of the CESL 162 and the first gate spacer 138 is fluorinated by the in Fig. 7, the first gate spacers 138 are further fluorinated after removing the sacrificial gate structure 130 because the first semiconductor layers 106 are exposed. In other words, in some embodiments, the first gate spacers 138 are fluorinated more than once using different processes so as to protect other components of the semiconductor device structure 100. The first gate spacer 138 is fluorinated more than once. As a result, the K value of the first gate spacer 138 is further reduced. Furthermore, the leakage current is further reduced, the thermal stability is further improved, and the moisture absorption is further reduced.
[0044] Fig. 18A and Fig. 18B are diagrams illustrating a SiF concentration profile in the first and second gate spacers 138, 139, respectively, according to some embodiments. As shown in Fig. 18A illustrates the fluorine concentration profile (measured as SiF concentration) in the first gate spacer 138. The minimum value on the X-axis represents the position of the inner surface 138i, and the maximum value on the X-axis represents the position of the outer surface 1380. The fluorine concentration is highest at the inner surface 138i and the outer surface 1380, and the fluorine concentration gradually decreases toward the center of the first gate spacer 138.
[0045] As in Fig. 18B illustrates the fluorine concentration profile (measured as SiF concentration) in the second gate spacer 139. The minimum value on the X-axis represents the position of the inner surface 139i, and the maximum value on the X-axis represents the position of the outer surface 1390. The fluorine concentration is lowest at the inner surface 139i and highest at the outer surface 1390. Thus, the fluorine concentration profiles of the first and second gate spacers 138, 139 are different as a result of the fluorination processes described above.
[0046] As in Fig. As shown in Figure 17, after the formation of the nanostructure channels (i.e., the exposed portions of the first semiconductor layers 106), a gate dielectric layer 170 is formed to surround the exposed portions of the first semiconductor layers 106, and a gate electrode layer 172 is formed on the gate dielectric layer 170. The gate dielectric layer 170 and the gate electrode layer 172 may collectively be referred to as a gate structure 174. In some embodiments, an interfacial layer (IL) (not shown) is formed between the gate dielectric layer 170 and the exposed surfaces of the first semiconductor layers 106.In some embodiments, the gate dielectric layer 170 includes one or more layers of a dielectric material, such as silicon oxide, silicon nitride, or a high-K dielectric material, another suitable dielectric material, and / or combinations thereof. Examples of a high-K dielectric material include HfO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO, zirconium oxide, alumina, titanium oxide, hafnium dioxide-alumina alloy (HfO2-Al2O3 alloy), other suitable high-K dielectric materials, and / or combinations thereof. The gate dielectric layer 170 may be formed by CVD, ALD, or any suitable deposition technique.The gate electrode layer 172 may include one or more layers of conductive material, such as polysilicon, aluminum, copper, titanium, tantalum, tungsten, cobalt, molybdenum, tantalum nitride, nickel silicide, cobalt silicide, TiN, WN, TiAl, TiAlN, TaCN, TaC, TaSiN, metal alloys, other suitable materials, and / or any combination thereof. The gate electrode layer 172 may be formed by CVD, ALD, electroplating, or another suitable deposition technique. The gate electrode layer 172 may also be deposited over the top surface of the ILD layer 164. The gate dielectric layer 170 and the gate electrode layer 172 formed over the ILD layer 164 are then removed, for example, using CMP, until the top surface of the ILD layer 164 is exposed.
[0047] It is understood that the semiconductor device structure 100 may undergo further processes to form conductive contacts for electrical connection to the S / D regions 164 in the ILD layer 164 and to form conductive contacts for electrical connection to the gate electrode layer 172. An interconnect structure may be formed over the semiconductor device structure 100 to provide electrical paths to the devices formed on the substrate 101.
[0048] Fig. 19 is a cross-sectional view of the semiconductor device structure 100 of Fig. 16 according to alternative embodiments. In some embodiments, the Fig. 19, the semiconductor device structure 100 is at the same stage of manufacture as that shown in Fig. 16 shown semiconductor device structure 100. Alternatively, the semiconductor device structure 100 shown in Fig. 19 shown semiconductor device structure 100 in a different stage than that in Fig. 16. For example, after removing the sacrificial gate structure 130, the one or more processes for introducing fluorine into the first gate spacer 138 are not performed and the second semiconductor layers 108 are removed. In other words, the Fig. 19, the first gate spacer 138 is not fluorinated for the second time.
[0049] Fig. 20A and Fig. 20B are various views of one of various stages of fabrication of the semiconductor device structure 100 of Fig. 19 according to some embodiments. As in Fig. 20A and Fig. As shown in Figure 20B, the IL 165 is formed on the exposed surfaces of the first semiconductor layers 106. In some embodiments, the IL 165 is comprised of a chemically formed silicon oxide. After the formation of the IL 165, one or more processes are performed to fluorinate both the exposed first gate spacer 138 and the exposed dielectric spacers 144.
[0050] Fig. Figure 21 illustrates the fluorination of the dielectric spacer 144 of the semiconductor device structure 100 according to some embodiments. In some embodiments, the dielectric spacer 144 includes SiONC and may have a chemical structure A, as shown in Fig. 21. In some embodiments, the SiONC of the dielectric spacers 144 is formed by thermal ALD at a temperature in the range of about 200 degrees Celsius to about 650 degrees Celsius. The carbon concentration of the SiONC may range from about 1 atomic percent to about 10 atomic percent, and the nitrogen concentration of the SiONC may range from about 15 atomic percent to about 40 atomic percent. The dielectric spacer 144 may have a density in the range of about 2 g / cm 3 up to about 3 g / cm 3 In some embodiments, a first plasma treatment process may be performed on the as-deposited dielectric spacers 144, and the chemical structure of the dielectric spacers 144 changes from chemical structure A to chemical structure B, as shown in Fig. 21. The plasma treatment process includes exposing the dielectric spacers 144 to a nitrogen-containing plasma. The nitrogen-containing plasma may be formed by activating a nitrogen-containing gas through a low-power plasma source or a remote plasma source. The nitrogen-containing gas may be any suitable nitrogen-containing gas. In some embodiments, the nitrogen-containing gas is nitrogen gas (N2). Treatment with the nitrogen-containing plasma removes the NH2 end groups shown in chemical structure A and leaves the unoccupied Si bonds shown in chemical structure B.
[0051] Next, a second plasma treatment process may be performed on the treated dielectric spacers 144, and the chemical structure of the dielectric spacers 144 changes from chemical structure B to chemical structure C, as shown in Fig. 21. The second plasma treatment process can be the same as that shown in Fig. 7. In some embodiments, the second plasma treatment process includes exposing the dielectric spacers 144 to a hydrogen-containing plasma. The hydrogen-containing plasma may be formed by activating a hydrogen-containing gas by a low-power plasma source or a remote plasma source. The hydrogen-containing gas may be any suitable hydrogen-containing gas. In some embodiments, the hydrogen-containing gas is hydrogen gas (H2). In some embodiments, the low-power plasma source is a capacitively coupled plasma source, and the plasma power ranges from about 10 W to about 250 W. The plasma generated by the capacitively coupled plasma source or the remote plasma source contains more hydrogen radicals than ions.Additionally, the processing temperature of the plasma treatment process is relatively low, such as from about 20 degrees Celsius to about 100 degrees Celsius. As a result, the hydrogen radicals bind to the unoccupied Si bonds to form SiH bonds, as shown in chemical structure C in . Fig. 21 shown.
[0052] Next, a fluorination process is performed on the treated dielectric spacers 144. The fluorination process may be any suitable fluorination process. In some embodiments, the fluorination process is a fluorine impregnation process. The fluorine impregnation process may include exposing the treated dielectric spacers 144 to a fluorine-containing precursor at a processing temperature of less than about 100 degrees Celsius. In some embodiments, the fluorine-containing precursor includes HF, CF4, F2, C2F6, a combination of HF and F2, or another suitable fluorine-containing precursor. The processing temperature may range from about 20 degrees Celsius to about 99 degrees Celsius, such as from about 40 degrees Celsius to about 80 degrees Celsius, and a processing pressure may range from about 13 Pa (0.1 Torr) to about 1.3 kPa (10 Torr).The treated dielectric spacers 144 can be exposed to the fluorine-containing precursor for a duration ranging from about 30 seconds to about 3600 seconds. The fluorine in the fluorine-containing precursor has a higher probability of breaking the SiH bonds than SiO, SiN, or SiC bonds under the aforementioned process conditions. Furthermore, SiNSi and SiCSi bridges remain in the dielectric spacers 144. As a result, the chemical structure of the dielectric spacers 144 changes from chemical structure C to chemical structure D, as shown in FIG. Fig. 21. The hydrogen atoms bonded to Si are replaced by fluorine atoms. The SiF bonds exhibit lower polarization, which can reduce K values. Additionally, SiNSi and SiCSi bridges remaining in the dielectric spacers 144 can maintain high etch resistance. Due to the SiH bonds created by the plasma treatment processes, the fluorination process can be performed with relatively low energy, such as at a low temperature without plasma. A low-energy fluorination process can prevent the fluorine-containing precursor from becoming an etchant.
[0053] Fig. Figure 22 illustrates the fluorination of the dielectric spacer 144 of the semiconductor device structure 100 according to alternative embodiments. In some embodiments, the first and second plasma treatments are not performed, and the fluorination process is performed for a longer period of time and / or with higher energy and temperature. As a result, the chemical structure of the dielectric spacers 144 changes from chemical structure A to chemical structure B, as shown in Fig. 22. In some embodiments, the fluorination process without the first and second plasma treatments is the same as the fluorination process performed with the first and second plasma treatments, except that the duration of the fluorination process without the first and second plasma treatments is much longer, such as about two times to about 10 times longer, than the duration of the fluorination process with the first and second plasma treatments. In some embodiments, the fluorination process without the first and second plasma treatments is the same as the duration of the fluorination process performed with the first and second plasma treatments. Fig. 7 described fluorination process with higher energy and temperature.
[0054] After the fluorination process, the dielectric spacer 144 can contain about one atomic percent to about six atomic percent fluorine. The fluorine diffusion depth can range from the surface to about 10 nanometers. Fig. 23 is a diagram illustrating a SiF concentration profile in the dielectric spacer 144 according to some embodiments. As shown in Fig. 23, the fluorine concentration profile (measured as SiF concentration) in the dielectric spacer 144 is illustrated. The minimum value on the X-axis represents the position of an outer surface 1440 ( Fig. 20B) of the dielectric spacer 144 and the maximum value on the X-axis represents the position of the inner surface 144i ( Fig. 20B) of the dielectric spacer 144. The fluorine concentration is lowest at the outer surface 1440 and highest at the inner surface 144i.
[0055] In some embodiments, the fluorinated dielectric spacer 144 has an outgassing temperature of about 400 degrees Celsius and thermal stability at about 600 degrees Celsius to about 750 degrees Celsius with N2 and H2. Unstable fluorine bonds in the fluorinated dielectric spacers 144 are expelled (outgassed) at an outgassing temperature in the range of about 20 degrees Celsius to about 400 degrees Celsius, and the remaining fluorine bonds in the fluorinated dielectric spacers 144 are stable at a temperature up to about 750 degrees Celsius, such as from about 600 degrees Celsius to about 750 degrees Celsius. In some embodiments, as described above, the NH2 end groups of the as-deposited dielectric spacers 144 are removed by the first plasma treatment process.In some embodiments, the first plasma treatment process is not performed, and the NH2 end groups of the as-deposited dielectric spacers 144 are not removed. Next, a fluorination process is performed with a shorter duration than the fluorination process without the first and second plasma treatment processes, and the Si-NH2 bonds are converted to Si-NHF bonds. The resulting fluorinated dielectric spacers 144 exhibit poorer thermal stability compared to the dielectric spacers 144 formed by the process shown in FIG. Fig. 21 and Fig. 22. The dielectric spacers 144 with the SiF bonds exhibit improved thermal stability compared to the dielectric spacers 144 with Si-NHF bonds. In some embodiments, the K value of the dielectric spacer 144 is from 1 atomic percent to about 5 atomic percent fluorine, which is determined by the processes described in Fig. 21 and Fig. 22 described processes, is reduced by about 0.1 to about 0.5.
[0056] Fig. 24 illustrates a portion 200 of the semiconductor device structure 100 of Fig. 20B according to some embodiments. As in Fig. 24, the IL 165 can also be used in some embodiments by the Fig. 21 and Fig. 22, and the fluorine can diffuse to the interface between the IL 165 and the first semiconductor layer 106. Fluorine can repair defects at the interface between the IL 165 and the first semiconductor layer 106. In some embodiments, the fluorine replaces oxygen vacancies at the interface between the IL 165 and the first semiconductor layer 106, which in turn improves the interface density of states (Dit).
[0057] In some embodiments, the first gate spacer 138 is first formed by the Fig. 21 and Fig. 22 described processes. In other words, one or more of the Fig. 7 and Fig. 16 are not performed to introduce fluorine into the first gate spacer 138. In some embodiments, the first gate spacer 138 includes SiOCN with less than 5 atomic percent nitrogen, and the dielectric spacers 144 include SiONC with more than about 20 atomic percent nitrogen. After performing the processes described in Fig. 21 and Fig. 22, the first gate spacer 138, having a lower nitrogen concentration, has a lower fluorine concentration than the dielectric spacer 144, which has a higher nitrogen concentration. Thus, in some embodiments, a dielectric layer having a higher nitrogen concentration has a higher fluorine concentration compared to a dielectric layer having a lower nitrogen concentration when the same fluorination process is performed on both dielectric layers. In some embodiments, the fluorine concentration of the dielectric spacer 144 is about 35 percent to about 80 percent higher than the fluorine concentration of the first gate spacer 138.
[0058] In some embodiments, the first gate spacer 138 is formed for the second time by the Fig. 21 and Fig. 22 described processes. In other words, one or more of the Fig. 16 are not performed to introduce additional fluorine into the first gate spacer 138. As a result, the fluorine concentration of the first gate spacer 138 is significantly greater than the fluorine concentration of the dielectric spacers 144.
[0059] In some embodiments, the first gate spacer 138 is formed for the third time by the Fig. 21 and Fig. 22 described processes. In other words, one or more of the Fig. 7 and Fig. 16 are performed to introduce fluorine into the first gate spacer 138. As a result, the fluorine concentration of the first gate spacer 138 is significantly greater than the fluorine concentration of the dielectric spacers 144.
[0060] In some embodiments, the fluorination of the first gate spacer 138, the second gate spacer 139 and / or the dielectric spacers 144 shown in Fig. 7, Fig. 14, Fig. 16, Fig. 21 and Fig. 22, can be improved by keeping the fluorinated layers in a nitrogen environment immediately after the fluorination process, exposing the fluorinated layers to a water-free environment immediately after the fluorination process, and forming a capping layer on the fluorinated layers immediately after the fluorination process. For example, according to the process described in Fig. 21 and Fig. 22, the semiconductor device structure 100 is transferred in a container charged with nitrogen to another chamber / system for subsequent processes (e.g., forming the gate dielectric layer 170). The subsequent process is water-free. In other words, no wet etching process can be performed immediately after the fluorination process. Immediately after the Fig. 21 and Fig. 22, the gate dielectric layer 170, which acts as a capping layer for the fluorinated first gate spacer 138 and the dielectric spacers 144, is formed on the fluorinated first gate spacer 138 and the dielectric spacers 144. With these improvements, the fluorine concentration in the fluorinated layers is significantly higher compared to fluorinated layers without the improvements.
[0061] After performing the Fig. 21 and Fig. 22 described processes for fluorinating the dielectric spacers 144, the processes described in Fig. 17 described processes are performed to complete the semiconductor device structure 100.
[0062] Embodiments of the present disclosure provide a semiconductor device structure including a first gate spacer 138, a second gate spacer 139, and dielectric spacers 144. The first gate spacer 138, the second gate spacer 139, and the dielectric spacers 144 are fluorinated at various stages of fabrication of the semiconductor device structure 100. Some embodiments may achieve advantages. For example, by performing the fluorination processes at various stages of fabrication of the semiconductor device structure 100, other components of the semiconductor device structures 100 are protected.Additionally, the fluorinated first and second gate spacers 138, 139 and the fluorinated dielectric spacers 144 may result in reduced K, reduced leakage current, improved Dit, improved thermal stability, and reduced moisture absorption.
[0063] One embodiment is a semiconductor device structure. The structure includes a gate dielectric layer disposed over a substrate, a gate electrode layer disposed over the gate dielectric layer, and a first gate spacer disposed adjacent to the gate dielectric layer. The first gate spacer has an inner surface facing the gate dielectric layer and an outer surface opposite the inner surface, and the first gate spacer has a fluorine concentration that decreases from the inner surface and the outer surface toward a center of the first gate spacer.The structure further comprises a second gate spacer disposed on the outer surface of the first gate spacer, the second gate spacer having an inner surface in contact with the outer surface of the first gate spacer and an outer surface opposite the inner surface, and the second gate spacer having a fluorine concentration that decreases from the outer surface to the inner surface.
[0064] Another embodiment is a method. The method includes forming a fin structure from a substrate, forming a sacrificial gate stack over the fin structure, depositing a first gate spacer on the sacrificial gate stack, introducing fluorine into the first gate spacer, depositing a second gate spacer on the first gate spacer, removing portions of the fin structure to expose a portion of the substrate, forming a source / drain region from the portion of the substrate, introducing fluorine into the second gate spacer, removing the sacrificial gate stack, and introducing additional fluorine into the first gate spacer.
[0065] Another embodiment is a method. The method includes forming a fin structure from a substrate, and the fin structure includes a first plurality of semiconductor layers and a second plurality of semiconductor layers. The method further includes forming a sacrificial gate stack over the fin structure, depositing a gate spacer on the sacrificial gate stack, removing portions of the fin structure to expose a portion of the substrate, recessing the second plurality of semiconductor layers to form recesses, forming dielectric spacers in the recesses, forming a source / drain region from the portion of the substrate, removing the sacrificial gate stack and the second plurality of semiconductor layers, forming an interface layer on a portion of each of the first plurality of semiconductor layers, and introducing fluorine into the dielectric spacers.
Claims
[1] A semiconductor device structure (100) comprising: a gate dielectric layer (170) disposed over a substrate (101); a gate electrode layer (172) disposed over the gate dielectric layer (170); a first gate spacer (138) disposed adjacent to the gate dielectric layer (170), the first gate spacer (138) having an inner surface (138i) facing the gate dielectric layer (170) and an outer surface (1380) opposite the inner surface (138i), and the first gate spacer (138) having a fluorine concentration that decreases from the inner surface (138i) and the outer surface (1380) toward a center of the first gate spacer (138); and a second gate spacer (139) disposed on the outer surface (1380) of the first gate spacer (138), the second gate spacer (139) having an inner surface (139i) in contact with the outer surface (1380) of the first gate spacer (138) and an outer surface (1390) opposite the inner surface (139i), and the second gate spacer (139) having a fluorine concentration that decreases from the outer surface (1390) to the inner surface (139i). [2] The semiconductor device structure (100) of claim 1, wherein the first and second gate spacers (138, 139) each comprise SiCON. [3] The semiconductor device structure (100) of claim 1 or 2, further comprising a plurality of semiconductor layers (106, 108) disposed over the substrate (101), wherein the gate electrode layer (172) surrounds a portion of each of the semiconductor layers (106, 108). [4] The semiconductor device structure (100) of claim 3, further comprising an interface layer (165) in contact with each semiconductor layer (106, 108) of the plurality of semiconductor layers (106, 108), wherein an interface between the interface layer (165) and each semiconductor layer (106, 108) of the plurality of semiconductor layers (106, 108) contains fluorine. [5] The semiconductor device structure (100) of claim 3 or 4, further comprising dielectric spacers (144) disposed between adjacent semiconductor layers (106, 108) of the plurality of semiconductor layers (106, 108). [6] The semiconductor device structure (100) of claim 5, wherein the dielectric spacers (144) have a fluorine concentration that is substantially less than the fluorine concentration of the first gate spacer (138). [7] Method comprising: Forming a fin structure (112) from a substrate (101); Forming a sacrificial gate stack (130) over the fin structure (112); depositing a first gate spacer (138) on the sacrificial gate stack (130); introducing fluorine into the first gate spacer (138); depositing a second gate spacer (139) on the first gate spacer (138) after introducing fluorine into the first gate spacer (138); Removing portions of the fin structure (112) to expose a portion of the substrate (101); Forming a source / drain region (146) from the portion of the substrate (101); introducing fluorine into the second gate spacer (139); Removing the sacrificial gate stack (130) after introducing fluorine into the second gate spacer (139); and Introducing additional fluorine into the first gate spacer (138) after removing the sacrificial gate stack (130). [8] The method of claim 7, wherein introducing fluorine into the first gate spacer (138) comprises performing a plasma treatment process on the first gate spacer (138) followed by a fluorine impregnation process on the first gate spacer (138). [9] The method of claim 8, wherein the plasma treatment process comprises activating a hydrogen-containing gas to form a hydrogen-containing plasma by a plasma source. [10] The method of claim 9, wherein the plasma source is a remote plasma source or a capacitively coupled plasma source. [11] A method according to claim 8 or 9, wherein the hydrogen-containing gas comprises hydrogen gas. [12] A method according to any one of claims 8 to 11, wherein the fluorine impregnation process is carried out at a processing temperature of less than about 100 degrees Celsius. [13] The method of any one of claims 8 to 12, wherein the fluorine impregnation process comprises exposing the first gate spacer (138) to fluorine gas (F2). [14] The method of any one of claims 7 to 13, further comprising forming an oxide layer (147) covering the source / drain region (146) prior to introducing fluorine into the second gate spacer (139). [15] The method of any one of claims 7 to 14, further comprising removing portions of the first and second gate spacers (138, 139) after introducing fluorine into the first gate spacer (138) and before introducing fluorine into the second gate spacer (139). [16] A method comprising: Forming a fin structure (112) from a substrate (101), the fin structure (112) comprising a first plurality of semiconductor layers (106) and a second plurality of semiconductor layers (108); Forming a sacrificial gate stack (130) over the fin structure (112); Depositing a gate spacer (138, 139) on the sacrificial gate stack (130); Removing portions of the fin structure (112) to expose a portion of the substrate (101); recessing the second plurality of semiconductor layers (108) to form recesses; Forming dielectric spacers (144) in the recesses; Forming a source / drain region (146) from the portion of the substrate (101); Removing the sacrificial gate stack (130) and the second plurality of semiconductor layers (108) to expose a portion of each of the first plurality of semiconductor layers (106) and the dielectric spacers (144); Forming an interface layer (165) on the exposed portion of each of the first plurality of semiconductor layers (106); and Introducing fluorine into the exposed dielectric spacers (144). [17] The method of claim 16, wherein introducing fluorine into the dielectric spacers (144) comprises; performing a first plasma treatment process on the dielectric spacers (144); performing a second plasma treatment process on the dielectric spacers (144); and Performing a fluorine impregnation process on the dielectric spacers (144). [18] The method of claim 17, wherein the first plasma treatment process comprises exposing the dielectric spacers (144) to a nitrogen-containing plasma. [19] The method of claim 17 or 18, wherein the first plasma treatment process comprises exposing the dielectric spacers (144) to a hydrogen-containing plasma. [20] The method of any one of claims 16 to 19, further comprising introducing fluorine into the gate spacer (138, 139) during the introduction of fluorine into the dielectric spacers (144).
Citation Information
Patent Citations
Method for fabricating a semiconductor device
US20190006242A1
Semiconductor device having strained channels