Semiconductor device
By optimizing impurity concentrations and spatial arrangements of JTE regions through controlled Al ion implantation, the semiconductor devices achieve improved withstand voltage and reliability, addressing the limitations of existing designs.
Patent Information
- Application Number
- DE112013007794
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2013-03-05
- Filing Date
- 2013-12-10
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2033-12-10
AI Technical Summary
Existing semiconductor devices face issues with insufficient withstand voltage and reliability due to high impurity concentration differences between JTE regions, leading to avalanche breakthroughs and reduced performance.
The semiconductor devices are designed with a first JTE region and a second JTE region having specific impurity concentrations, with the impurity concentration difference between them minimized, and the ratio of their widths and spacings adjusted to reduce electric field concentration, using multi-stage Al ion implantation with controlled energy levels.
The solution results in semiconductor devices with high withstand voltage and reliability, exceeding 90% of ideal performance, and maintaining stability under harsh conditions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL AREA
[0001] The present invention relates to a semiconductor device. TECHNICAL BACKGROUND
[0002] Non-patent document 1 discloses a vertical pn diode in which a JTE (junction termination extension) region formed in a termination region of the diode is subdivided into two regions by the use of two implantation doses.
[0003] The vertical pn diode described in non-patent document 1 comprises a vertical pn junction structure consisting of an n + -conducting SiC substrate, a n - -leading drift area, a p + -conducting main junction, a cathode and an anode and a termination structure provided with a JTE region consisting of an annular first JTE region (high concentration implantation region) and an annular second JTE region (low concentration implantation region) on the surface of the n- exists in the leading drift area.
[0004] The first JTE region and the second JTE region, as described in Non-Patent Document 1, are formed by multi-stage ion implantation of a p-interfering substance such as A1, and the implantation dose ratio between them is 3 to 1. Although not described in Non-Patent Document 1, the maximum implantation energy in both the first and second JTE regions is 700 keV, as presented at the conference.
[0005] Non-patent document 2 discloses that an impurity concentration of a first JTE area is 2 × 10 19 cm -3 is and a fault concentration of a second JTE area 2 × 10 18 cm -3 or 2 × 10 17 cm -3 is .
[0006] Non-patent document 3 discloses that the broadening of the concentration distribution of Al ion-implanted in SiC in the depth direction depends on the implantation energy. DOCUMENTS FROM THE STATE OF THE TECHNOLOGY - PATENT DOCUMENTS Non-patent document 1: KAJI, Naoki [et al.]: Design and fabrication of 20 kV-class SiC PiN diodes with space-modulated JTE. In: Kōen yokōshū, 2012 shūki: (73.) Ōyō Butsuri Gakkai gakujutsu kōenkai ; Matsuyama, September 11-14, 2012. Tōkyō : Ōyō-Butsuri-Gakkai, 2012. Art 12p-H7-6 (1 p.) - ISBN 978-4-86348-276-0 Non-patent document 2: PÉREZ, Raúl [et al.]: Planar edge termination design and technology considerations for 1.7-kV 4H-SiC PiN diodes. In: IEEE Transactions on Electron Devices, Vol. 52, 2005, No. 10, pp. 2309-2316. ISSN 0018-9383 Non-patent document 3: MOCHIZUKI, Kazuhiro ; ONOSE, Hidekatsu: Dual-Pearson approach to model ion-implanted Al concentration profiles for high-precision design of high-voltage 4H-SiC power devices. In: Materials Science Forum, Vol. 600-603, 2008, pp. 607-610. ISSN 1662-9752 PATENT DOCUMENTS
[0007] US 2009 / 0 212 301 A1, DE 10 2006 056 139 B4, DE 10 2010 060 229 A1, US 2013 / 0 140 582 A1, US 2012 / 0 132 924 A1, DE 2006 033 506 B4 and US 2003 / 0 132 450 A1 disclose further conventional semiconductor devices. SUMMARY OF THE INVENTION; PROBLEMS TO BE SOLVED BY THE INVENTION
[0008] Because the impurity concentration could not be specified based on the description in Non-Patent Document 1 and the content of the presentation, an experimental test was performed in which the impurity concentration was varied. It was found that the withstanding stress was insufficient in some cases.
[0009] To understand the existing phenomenon, the inventors performed a device simulation test in which the Al ion implantation dose was up to 2 × 10 in a range disclosed in non-patent document 1. 13 cm -3 was changed. This showed that, although an avalanche breakthrough occurred near the surface, if the surface charge density described in non-patent document 2 was 7 x 10 12 cm -2 exceeded, an avalanche breakthrough at the border between the first JTE area and the second JTE area (for example, one defined by a reference number 9 in Fig. 8 specified position) in the vicinity of a region between the JTE region and the drift region (typically at a depth of about 0.7 to 0.9 µm, but depending on the standing stress) when the interfacial charge density was less than 7 × 10 12 cm -2 was.
[0010] The first JTE area and the second JTE area, as disclosed in non-patent document 2, exhibit very high fault concentrations, and the fault concentration of the first JTE area is ten times higher than that of the second JTE area. Accordingly, it is likely that an avalanche breakthrough at a boundary between a first JTE area and a second JTE area (for example, one defined by a reference number 9 in Fig. 8 specified position) occurs in a diode with a high withstand voltage such as a 3.3 kV diode, causing the reduction in withstand voltage.
[0011] One object of the present invention is to provide a semiconductor device with a high withstand voltage which exhibits high reliability. MEANS TO SOLVE THE PROBLEM
[0012] The above problem is solved by the semiconductor devices defined in claims 1 and 2. These semiconductor devices are produced, among other things, by the following manufacturing steps: forming a semiconductor device with a main transition region on a drift region with n-type conductivity and a p-type JTE region adjacent to the main transition region; providing a first JTE region and a second JTE region with an impurity concentration lower than that of the first JTE region; providing the first JTE region so that it is sandwiched between the second JTE regions; and setting the impurity concentration in the first JTE region to 4.4 x 10⁻⁴. 17 cm -3 or above and 8 × 10 17 cm -3 or below and setting the disturbance concentration in the second JTE area to 2 × 10 17 cm -3 or below in the case of a
[0013] Schottky diode and setting the impurity concentration in the first JTE area to 6 × 10 17 cm -3 or above and 8 × 10 17 cm -3 or below and setting the disturbance concentration in the second JTE area to 2 × 10 17 cm -3 or below in the case of a transition barrier Schottky diode.
[0014] It should be noted that it is desirable that the defect concentration difference between the first JTE area and the second JTE area at a pn transition depth is essentially eliminated, so that the first JTE area and the second JTE area have almost the same defect concentration.
[0015] It is also desirable that the ratio between the width and the interspace of the second JTE areas decreases in an in-plane direction according to the distance from the main transition area. EFFECTS OF THE INVENTION
[0016] According to the present invention, a semiconductor device with high withstand voltage and high reliability can be provided. BRIEF DESCRIPTION OF THE DRAWING
[0017] They show: Fig. 1 a top view of a semiconductor device according to a first embodiment, Fig. 2 a sectional view of the semiconductor device according to the first embodiment, Fig. 3 a top view of a semiconductor device according to a second embodiment, Fig. 4 a sectional view of the semiconductor device according to the second embodiment, Fig. 5 a graph of a concentration distribution of Al in the depth direction in a JTE region of the semiconductor device according to the first embodiment and the second embodiment, Fig. 6 a graph of a concentration distribution of Al in the depth direction in a JTE region of a semiconductor device according to the first embodiment and the second embodiment, Fig. 7 a graph of a concentration distribution of Al in the depth direction according to a comparative example and Fig. 8 A sectional view of a semiconductor device according to the comparative example. DETAILED DESCRIPTION OF PREFERRED EXECUTION FORMS
[0018] Embodiments of the present invention are described below. First embodiment
[0019] Fig. 1 is a top view of a semiconductor device (protective films and other components are omitted) according to the first embodiment, and Fig. Figure 2 is a sectional view of the semiconductor device.
[0020] The semiconductor device according to the first embodiment is a Schottky diode with a SiC substrate. This semiconductor device comprises a drift layer 2, which is an n-type semiconductor region formed by epitaxial growth on a semiconductor substrate 1; a Schottky electrode 10 formed in a main junction region located on an upper surface of the drift layer 2; a p-type semiconductor region 3, into which a p-type impurity such as Al is implanted and which forms a guard ring around the Schottky electrode 10; and a cathode 4 formed on the back surface of the semiconductor substrate 1. Furthermore, the semiconductor device comprises a JTE (junction termination extension) region 6, which consists of an annular p-type semiconductor region surrounding the main junction region.
[0021] The semiconductor substrate 1 is an n +-conducting semiconductor substrate consisting mainly of SiC, in which an n-contaminant such as N is implanted at a high concentration.
[0022] The drift layer is a n - -conducting semiconductor layer consisting mainly of SiC, in which an n-type impurity such as N is implanted. The impurity concentration of this is lower than that of the semiconductor substrate 1.
[0023] The JTE area 6 consists of areas of high fault density (first JTE areas) 7 and areas of low fault density (second JTE areas) 8, and the ratio between the width and the spacing of the second JTE areas gradually increases in one direction outwards from the main transition 3.
[0024] According to the first embodiment, the first JTE region and the second JTE region are formed by multi-stage Al ion implantation using the following ion implantation energies.
[0025] First ion implantation energy (first JTE area): 25, 55, 95, 150, 220 and 320 keV.
[0026] Second ion implantation energy (first JTE area and second JTE area): 25, 55, 95, 150, 220, 320 and 450 keV.
[0027] The maximum Al concentration (peak concentration in the box profile) in the first JTE area is 6 × 10 17 cm -3 set, and the maximum Al concentration of the second JTE area is set to 2 × 10 17 cm -3 By setting the highest ion implantation energy for a highly doped region (first ion implantation energy) lower than the second ion implantation energy, the concentration difference between the first JTE region and the second JTE region in the horizontal direction at the depth of the pn transition becomes almost zero, as shown by the Al concentration distribution in Fig. 5 is shown.
[0028] As a comparative example, Fig. 7. An Al concentration distribution in the depth direction in the case where the first and second ion implantations are performed with the same implantation energy as in non-patent document 1. In this example, a large discontinuity in the Al concentration distribution in the horizontal direction (substrate-inside-plane direction) occurs at a depth (depth of 0.7 to 0.9 µm) of a pn junction formed between the drift layer 2 and the JTE region 6. In particular, unlike in the case where the ion implantation energy is set to a value as high as 700 keV as in non-patent document 1, the Al ion lattice guidance cannot be ignored when the ion implantation energy is less than or equal to 450 keV, as disclosed in non-patent document 3.In particular, if the Al ion implantation of the first JTE area and the second JTE area is performed with an implantation dose ratio of 3 to 1 between the first JTE area and the second JTE area as in non-patent document 1 and with the same multi-stage energy with a maximum value of 450 keV or less, the Al concentration retains even at a depth of 0.6 µm or above in a graph of the Al concentration distribution in the depth direction, as in . Fig. Figure 7 shows its state. Therefore, the diode can be described with the in Fig. The structure shown in Figure 8 can only achieve an actual withstanding voltage of at most about 70% of the ideal withstanding voltage in the case where the diode has an infinite size, namely in the case where there is no boundary region and the diode can be regarded as a one-dimensional structure in the vertical direction.
[0029] In contrast, the [document] according to the [document] Fig. In the first embodiment shown in Figure 1, the diode exhibits a withstand voltage that exceeds 90% of the ideal withstand voltage in the case where the diode is of infinite size. This is assumed to be due to the fact that the concentration values of the first and second JTE regions are matched, and that the concentration difference between the first and second JTE regions in the horizontal direction is almost zero at the depth of the pn junction, so that it is less likely that an electric field will concentrate at a boundary between the first and second JTE regions.
[0030] The field intensity of a protective insulating film (in Fig. 2 not shown) at the outermost edge position of the second JTE area at maximum Al concentration (peak concentration in the box profile) in the JTE area according to the first embodiment is not 2 MV / cm, so that the problem of a breakthrough of the insulating film when measuring the initial properties does not occur.
[0031] Furthermore, as a result of measurements in which the diode was held at 125 °C for 1000 hours while the reverse voltage was set to 80% of the rated withstand voltage, and then cooled to room temperature while the reverse voltage was applied, no breakdown of the Schottky diode was observed when a voltage less than or equal to the initial withstand voltage was applied. This is thought to be due to the high maximum concentration of the first JTE region, and consequently, the withstand voltage is not affected even under the harsh test conditions where the interfacial charge density is 7 × 10⁻⁶. 12 cm -2 exceeds.
[0032] The withstand voltage of the Schottky diode also exceeded 90% of the ideal withstand voltage when the maximum Al concentration in the first JTE region was set to 4 x 10 17 cm -3 was set and the maximum Al concentration in the second JTE area to 2 × 1017 cm -3 However, as a result of the measurement, in which the diode was held at 125 °C for 1000 hours while the reverse voltage was maintained at 80% of the rated withstand voltage, and then cooled to room temperature while the reverse voltage was applied, breakdown of the Schottky diode was observed when a voltage less than or equal to an initial withstand voltage was applied. The presence of a positive charge with a density of approximately 1 × 10 12 cm -2 up to 2 × 10 12 cm -2At an interface between an insulating film and the semiconductor in an initial state, it was known in the case of a semiconductor device using SiC, and it is assumed that the interface charge changes towards a larger positive value during the test, thereby reducing the withstanding voltage and causing the breakdown of the Schottky diode. If the maximum Al concentration in the first JTE region is 6 x 10 17 cm -3 was set and the maximum Al concentration in the second JTE area to 2 × 10 17 cm -3 When the parameters were set as in the first embodiment, no Schottky diode breakdown was observed. A different test was then performed in which the maximum Al concentration in the first JTE region was increased stepwise from 4.0 × 10⁻⁶. 17 cm -3 on 4 × 10 16 cm -3 was increased, while the maximum Al concentration in the second JTE area was fixed at 2 × 1017 cm -3 The test revealed that no Schottky diode breakdown occurred when the maximum Al concentration in the first JTE region was greater than or equal to 4.4 x 10⁻⁶. 17 cm -3 was. Furthermore, it was also found that the initial standing stress was reduced when the maximum Al concentration in the first JTE area was reduced to 8.4 × 10 17 cm -3 was increased. Accordingly, the range of the maximum concentration of the first JTE area is desirablely between 4.4 × 10⁻⁶. 17 cm -3 and 8 × 10 17 cm -3 , in order to achieve a Schottky diode as a semiconductor device with high reliability.
[0033] As described above, according to the first embodiment it is possible to increase the withstand voltage of a semiconductor device in the form of a Schottky diode using SiC and thus achieve a high reliability of the semiconductor device. Second embodiment
[0034] Fig. 3 is a top view of a semiconductor device according to the second embodiment, and Fig. Figure 4 is a sectional view of the semiconductor device.
[0035] The main difference compared to the first embodiment is that the first JTE regions are arranged discretely beneath the Schottky electrode 10 and in a ring around the Schottky electrode 10, instead of the p-type semiconductor region 3 which uses a guard ring, thus forming a JBS diode. The implantation energy of the first and second JTE regions is the same as in the first embodiment, and the implantation dose of the first JTE region is controlled such that the maximum Al concentration in the first JTE region has three values, such as 4.4 × 10⁻⁶. 17 cm -3 (not shown), 6 × 10 17 cm -3 ( Fig. 5) and 8 × 10 17 cm -3 ( Fig. 6), and the implantation dose of the second JTE area is controlled such that the maximum Al concentration in the second JTE area is 2 × 10 17 cm -3 becomes ( Fig. 5 and Fig. 6).
[0036] If, in the JBS diode manufactured according to the second embodiment, the maximum Al concentration in the first JTE region is 4.4 × 10 17 cm -3 When the voltage drop was high, the withstanding voltage was reduced to 60% of the ideal withstanding voltage in the case where the diode was infinitely large. This is assumed to be due to the fact that the maximum Al concentration in the first JTE region was 4.4 × 10⁻⁶. 17 cm -3 for replacing the p-type semiconductor region 3 according to the first embodiment was too low. However, if the maximum Al concentration in the first JTE region was 6 × 10 17 cm -3 and 8 × 10 17 cm -3 The withstand voltage exceeded 90% of the ideal withstand voltage in the case where the diode was of infinite size. If then the maximum Al concentration in the first JTE region was 6 × 10 17 cm -3 and 8 × 10 17 cm -3In a measurement where the diode was held at 125 °C for 1000 hours with the reverse voltage applied to 80% of its rated withstand voltage, and then cooled to room temperature while the reverse voltage was applied, no breakdown of the JBS diode was observed when a voltage less than or equal to the initial withstand voltage was applied. Accordingly, the range of maximum concentration of the first JTE region is desirablely between 6 × 10 17 cm -3 and 8 × 10 17 cm -3 , in order to achieve a JBS diode as a semiconductor device with high reliability.
[0037] According to the second embodiment, it is possible to achieve a semiconductor device in the form of a JBS diode using SiC with high reliability and also to avoid a process in which the p-type semiconductor region 3 is formed as a guard ring according to the first embodiment, thereby reducing the manufacturing costs of the semiconductor device.
[0038] The present invention has been described above in detail based on specific embodiments. It goes without saying, however, that the present invention is not limited to the aforementioned embodiments and that various modifications and alterations can be made within the scope of protection of the present invention. Reference symbol list 1 Semiconductor substrate 2 Drift area 3 p-type semiconductor region 4 Cathode 6 JTE area 7 First JTE area with high implantation dose 8 Second JTE area with small implantation dose 9. Example of the position of an avalanche breakthrough 10 Schottky electrode
Claims
[1] A semiconductor device which is a Schottky diode and comprises: a main junction region at a drift region (2) with an n-conductivity and a p-conducting JTE region (6) formed adjacent to the main junction region, wherein the JTE region (6) comprises a first JTE region (7) and a second JTE region (8) whose impurity concentration is lower than that of the first JTE region (7), the first JTE region (7) is arranged so that it is sandwiched between the second JTE regions (8), the impurity concentration in the first JTE region (7) to 4.4 × 10 17 cm -3 or above and 8 × 10 17 cm -3 or below and the impurity concentration in the second JTE region (8) is set to 2 × 10 17 cm -3 or below, and the first JTE region (7) and the second JTE region (8) are formed by a multi-stage ion implantation with first ion implantation energies for the first JTE region (7) and second ion implantation energies for the first and second JTE regions (7, 8), wherein the highest ion implantation energy of the first ion implantation energies is made lower than the second ion implantation energies. [2] A semiconductor device which is a junction barrier Schottky diode and comprises: a main junction region at a drift region (2) with an n-conductivity and a p-conducting JTE region (6) formed adjacent to the main junction region, wherein the JTE region (6) comprises a first JTE region (7) and a second JTE region (8) whose impurity concentration is lower than that of the first JTE region (7), the first JTE region (7) is arranged so that it is sandwiched between the second JTE regions (8), the impurity concentration in the first JTE region (7) to 6 × 10 17 cm -3 or above and 8 × 10 17 cm -3 or below and the impurity concentration in the second JTE region (8) is set to 2 × 10 17 cm -3 or below, and the first JTE region (7) and the second JTE region (8) are formed by a multi-stage ion implantation with first ion implantation energies for the first JTE region (7) and second ion implantation energies for the first and second JTE regions (7, 8), wherein the highest ion implantation energy of the first ion implantation energies is made lower than the second ion implantation energies. [3] A semiconductor device according to claim 1 or 2, wherein the ratio between the width and the pitch of the second JTE regions (8) decreases according to the distance from the main junction region.
Citation Information
Patent Citations
schottky contact component and its use
DE102006033506B4
semiconductor device with an improved structure for high withstand voltage
DE102006056139B4
Semiconductor device with semiconductor zones, manufacturing process for this and integrated circuit
DE102010060229A1
Semiconductor device and method of manufacturing the same
US20030132450A1
Double Guard Ring Edge Termination for Silicon Carbide Devices and Methods of Fabricating Silicon Carbide Devices Incorporating Same
US20090212301A1