Nickel plating solution, process for producing a wire coated with solid particles, and wire coated with solid particles
The nickel plating solution with a polyamine dispersant and surface-modified particles addresses the issue of particle aggregation, improving the cutting performance and longevity of wire saws by ensuring uniform distribution of solid particles on the wire.
Patent Information
- Application Number
- DE112015003772
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-05-29
- Filing Date
- 2015-06-08
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2035-06-08
AI Technical Summary
Conventional methods for producing wires with dispersed solid particles, such as diamond particles, result in aggregation and separation of these particles, leading to poor adhesion and cutting performance.
A nickel plating solution is developed that includes a polyamine dispersant and surface-modified solid particles with an inorganic cover layer, ensuring uniform distribution and adhesion of solid particles on the wire surface through electroplating.
The solution prevents aggregation of solid particles, enhancing the cutting behavior and service life of wire saws used for cutting materials like silicon wafers and semiconductors.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical area
[0001] The present invention relates to a nickel plating solution which is used for the production of a solid particle coated coated wire, in which solid particles of diamond or the like are deposited on the surface of the wire, a process for producing the wire containing solid particles, and a Wire containing solid particles. State of the art
[0002] Wires coated with solid particles, which adhere to the outer circumferential surfaces of the wires Solid particles of diamond or the like are suitable for cutting hard materials with high brittleness and difficult to process, such as silicon wafers for solar cells, silicon wafers for Semiconductors, sapphires for LED applications, ceramics and stones. Recently, an improvement in the Performance of cutting tools for fragile materials (wire saws), which have such Wires containing solid particles and an increase in the service life of the resulting products are required.
[0003] As regards a method for producing a wire containing solid particles, for example, Patent Literature 1 discloses a wire coated with solid particles which adheres to the outer peripheral surface of a wire solid particles. Patent Literature 1 discloses a technique in which the surface of a wire is coated with a electroplated nickel layer containing solid particles, in which surface-modified, inorganic solid particles having a covering layer are dispersed, and a plated nickel coating layer on the surface of the electroplated nickel layer containing solid particles. Literature list Patent literature
[0004] Patent Literature 1: WO 2013 / 039 097 A1 Summary of the invention Technical problem
[0005] When applying the “electroplated nickel layer containing solid particles” disclosed in Patent Literature 1, in which surface-modified solid particles having an inorganic covering layer are dispersed´´ increases However, the aggregation of the solid particles compared to those obtained by conventional techniques so that the dispersed solid particles can partially separate. However, the Market the development of techniques that allow the adhesion of solid particles with high dispersibility without ensure simultaneous aggregation of the solid particles.
[0006] The present invention has accordingly been made to solve the technical problems of the conventional Techniques, it being an object of the present invention to provide a nickel plating solution by means of which Solid particles of diamond or the like in a state of uniform distribution and without aggregation of the Solid particles can be fixed on the surface of a wire, a method for producing a wire with fixed Particle-laden wire using the nickel plating solution, as well as a solid particle-laden wire to provide. Solution to the problem
[0007] As a result of careful studies, the present inventors have, as described below, Nickel plating solution, a method for producing a wire coated with solid particles, and a Wire containing solid particles is introduced.
[0008] Nickel plating solution: The nickel plating solution of the present invention is a Nickel plating solution for forming an electroplated, dispersed solid particles nickel layer on the surface of a wire, whereby the nickel plating solution surface-modified, a inorganic covering layer containing solid particles and a polyamine acting as a dispersant.
[0009] In the nickel plating solution of the present invention, the polyamine is preferably a Polyethylenimine with a number average molecular weight of 800 to 2,000,000.
[0010] In the nickel plating solution of the present invention, the concentration of polyamine is furthermore preferably 1 mg / l to 100 mg / l.
[0011] In the nickel plating solution of the present invention, the inorganic coating layer The solid particles preferably also have a surface which is provided with a surface modifier.
[0012] In the nickel plating solution of the present invention, the surface modifier contains In addition, preferably one or more surfactants selected from amine-containing surfactants, non-ionic surfactants and cationic surfactants.
[0013] In the nickel plating solution of the present invention, the surface modifier contains preferably an amino alcohol and a non-ionic surfactant.
[0014] In the nickel plating solution of the present invention, the solid particles further preferably have a particle size of 0.01 µm to 100 µm.
[0015] In the nickel plating solution of the present invention, an inorganic covering layer having solid particles further preferably comprises one or two or more selected from Diamond particles with a palladium coating, diamond particles with a nickel coating, and diamond particles with a titanium top layer.
[0016] Method for producing a wire coated with solid particles: in the method for producing a wire coated with The present invention relates to a process for producing a wire coated with solid particles A wire containing solid particles, which comprises solid particles fixed to an outer peripheral surface of the wire, the method comprising step a and step b: Step a: a step which involves performing a composite plating by depositing nickel on the Surface of the wire by electroplating using the nickel plating solution according to the Claims 1 to 8 and the simultaneous adhesion of the inorganic covering layer Solid particles to form a plated nickel layer containing solid particles on the surface of the wire; and Step b: a step which involves forming a plated nickel coating layer on the surface of the wire formed plated nickel layer containing solid particles.
[0017] In the method for producing a particulate wire of the present invention, the Wire preferably provided with an inorganic protective layer on the surface of the wire.
[0018] In the method for producing a particulate wire of the present invention, the Wire also preferably has a diameter of 0.02 mm to 3.0 mm.
[0019] Particulate wire: The particulate wire of the present invention is obtained by the process for producing a wire containing solid particles.
[0020] In the wire of the present invention containing solid particles, preferably 10 to 100 of the one inorganic covering layer containing solid particles with a particle size of 0.01 µm to 100 µm per 500 µm Length of wire on the wire. Advantageous effects of the invention
[0021] The nickel plating solution of the present invention is a nickel plating solution for Forming an electroplated nickel layer containing dispersed solid particles on the surface of a wire, which surface-modified, inorganic coating layer Solid particles and a polyamine acting as a dispersant. In this way, the Nickel plating solution of the present invention can avoid aggregation of the solid particles and electroplated nickel layer in which the solid particles are distributed with greater uniformity on the surface of the wire. Accordingly, the cutting behavior of the wire used in wire saws, with Wire containing solid particles can be significantly improved. Short description of the drawings Fig. 1: Fig. 1 is a schematic representation of a cross-section of the wire covered with solid particles of the present invention. Fig. 2: Fig. 2 is a photograph showing the condition of the surface of a wire with a electroplated nickel layer containing solid particles, which was prepared in Example 1 using a 1 mg / l of nickel plating solution containing polyethyleneimine. Fig. 3: Fig. 3 is a photograph showing the condition of the surface of a wire with a electroplated nickel layer containing solid particles, which was prepared in Example 2 using a 5 mg / l of nickel plating solution containing polyethyleneimine. Fig. 4: Fig. 4 is a photograph showing the condition of the surface of a wire with a electroplated nickel layer containing solid particles, which in Example 3 using a 10 mg / l of nickel plating solution containing polyethyleneimine. Fig. 5: Fig. 5 is a photograph showing the condition of the surface of a wire with a electroplated nickel layer containing solid particles, which in the comparative example was obtained using a polyethyleneimine-free nickel plating solution. Description of embodiments
[0022] Hereinafter, preferred embodiments of the nickel plating solution of the present invention, a Process for producing a wire coated with solid particles using the plating solution, as well as a described a wire containing solid particles obtained using the manufacturing process. Embodiments of the nickel plating solution
[0023] First, embodiments of the nickel plating solution of the present invention will be described. Nickel plating solution of the present invention is a nickel plating solution for forming a electroplated nickel layer containing dispersed solid particles on the surface of a wire.
[0024] The nickel plating solution of the present invention comprises a plating solution which has a Nickel component and at least surface-modified solid particles having an inorganic covering layer and contains a polyamine acting as a dispersant.
[0025] As the nickel plating solution of the present invention, a solution can be used which is obtained by Adding a polyamine acting as a dispersant to a commercially available nickel electroplating solution, such as for example, a plating solution containing pure nickel or a nickel alloy (nickel-based alloys such as nickel-phosphorus, nickel-cobalt and nickel-zinc) containing plating solution, forming a Suspension of surface-modified solid particles having an inorganic covering layer is produced, or A solution can be used which is produced by producing a Watts- Bath or sulfamic acid bath and adding a polyamine acting as a dispersant to suspend surface-modified solid particles with an inorganic coating layer. For example, Any polyamine can be used as a dispersant for the nickel plating solution without restriction. A polyamine allows the use of a bath composition and electrolysis conditions that allow a gentle Nickel plating. Examples of nickel plating baths and plating conditions are shown below listed.
[0026] When using nickel sulfamate plating baths, for example, a Nickel plating composition containing 200 g / l to 800 g / l of nickel sulfamate tetrahydrate, 1 g / l to 10 g / l of nickel chloride hexahydrate, and 20 g / l to 50 g / l of boric acid and has a pH of 3 to 5.
[0027] When using Watts-type nickel plating baths, for example, a Nickel plating composition containing 200 g / l to 500 g / l of nickel sulfate heptahydrate, 10 g / l to Contains 100 g / l of nickel chloride heptahydrate and 20 g / l to 50 g / l of boric acid and has a pH of 3 to 5.
[0028] In the nickel plating solution of the present invention, polyethyleneimines and modified Polyethylenimines are used as the polyamine acting as a dispersant. Among these polyethyleneimines Polyethylenimines with a number-average molecular weight of 800 to 2,000,000 are preferably used. Using such a polyamine-containing dispersant in the nickel plating solution results in the Solid particles are evenly distributed without major aggregation and can be dispersed during the subsequent Electroplating of a wire coated with solid particles adhere to the surface of the wire, so that a quantity of the solid particles having an inorganic coating layer adheres to the wire containing solid particles, which is proportional to the amount of the nickel plating solution contained solid particles having an inorganic covering layer.
[0029] The concentration of the polyamine used as a dispersant in the nickel plating solution is preferably 1 mg / l to 100 mg / l. If the concentration of polyamine in the nickel plating solution is less than 1 mg / l, the effect due to the dispersant hardly occurs during electroplating, and the aggregation state of the solid particles adhering to the surface of the wire changes compared to In cases where no polyamine is added, this is not the case. If the concentration of polyamine in the nickel plating solution more than 100 mg / l, there is a possibility that the electroplated solid particles formed containing nickel layer breaks.
[0030] The surface-modified solid particles having an inorganic covering layer, which are used in the Nickel plating solution of the present invention, solid particles of cerium oxide, Silicon oxide (such as quartz and silica glass), aluminum oxide, silicon carbide, silicon nitride, zirconium oxide, Contain diamond and Teflon (registered trademark) as core material. Please note that the core material is not materials listed above and in a suitable manner according to the respective application of the of the particulate wire produced using the nickel plating solution. When using the wire containing solid particles produced using the nickel plating solution in a wire saw for cutting silicon wafers and the like, diamond particles are particularly preferred used.
[0031] The solid particles used preferably have a particle size of 0.01 µm to 100 µm. Particle size of the solid particles of less than 0.01 µm is not preferred, since the If the wire produced with nickel plating solution and containing solid particles has an excessively smooth surface, that the advantage regarding the adhesion of the solid particles to the wire is not only in applications that involve wire saws in related to, but also in other applications. For solid particles with a particle size of more than 100 µm, it is difficult to achieve adhesion to the surface of the wire and while maintaining a uniform dispersibility of the solid particles, even if the formation of the electroplated nickel layer containing solid particles using nickel plating, a wire with a diameter of 0.8 mm is used. Furthermore, there is no market demand for such In particular, if the nickel plating solution produced with solid particles wire is used to cut silicon wafers for solar cells, the use of solid particles with a particle size of 4 µm to 40 µm for a wire with a diameter of 0.08 mm to 0.2 mm is more preferred, because the resulting wire, which is loaded with solid particles, is an excellent material for applications in wire saws shows suitable cutting behavior and hardly leads to a falling off of the adhering to the surface of the wire solid particles, resulting in a longer service life for the wire saw.
[0032] The inorganic covering layer which is applied to the surface of the above-described core material The solid particles that function as a binder consist of a metal component. In detail, the inorganic Top layer forming component according to the respective application of the Nickel plating solution produced wire containing solid particles in suitable Examples of the compounds used in the present invention include Solid particles having an inorganic covering layer can in particular be solid particles with a Palladium cover layer, solid particles with a nickel cover layer, and solid particles with a titanium cover layer If the wire containing solid particles produced using the nickel plating solution is used as Wire saw used for cutting silicon wafers or the like, are used as an inorganic covering layer having solid particles particularly preferably one or two or more selected from diamond particles having a Palladium top layer, diamond particles with a nickel top layer, and diamond particles with a titanium top layer Solid particles having an inorganic covering layer which are coated with such an inorganic top layer, have a high wettability for the deposited, using the Nickel plating solution formed nickel component or nickel alloy component, which provides excellent Adhesion is achieved. Commercially available products that contain these solid particles with an inorganic top layer can be used in the nickel plating solution of the present invention.
[0033] Among these solid particles having an inorganic covering layer, the use of solid particles with a palladium coating layer, in which the surface of the solid particles is coated using the following process has been coated with palladium is preferred.
[0034] A first method for coating the surface of the solid particles with palladium is a ´´method, which involves the simultaneous deposition of palladium and tin on the surface of the solid particles, as well as the specific removal of tin from the surface of the solid particles by decomposition, whereby solid particles which have only palladium on the surface.´´ An example of this process is described in detail below. A solution containing a colloidal palladium-tin Containing catalyst as the main component, can be used as a solution containing tin and palladium. Solid particles are then immersed in such a solution, whereby adsorption of colloidal palladium-tin to the surface of the solid particles. The amount of palladium to be adsorbed is preferably 0.1 mg to 20 mg per gram of solid particles. An amount of palladium to be adsorbed of less than 0.1 mg per gram of Solid particles is not preferred because the amount of palladium adsorbed to the surface of the solid particles is too is low to ensure the wettability of the deposited nickel plating solution of the present invention formed nickel component or nickel alloy component, so that no excellent adhesion On the other hand, an adsorbed amount of palladium of more than 20 mg per gram of the Solid particles are not preferred because the effect achieved by the simultaneous deposition of nickel and the solid particles The effect reaches saturation and cannot be further improved. If the amount of palladium to be adsorbed is too small of more than 10 mg per gram of solid particles, the simultaneous deposition of nickel improves and the solid particles, the effect achieved is only slight. Accordingly, a more preferred amount of adsorbing palladium 0.1 mg to 10 mg per gram of solid particles.
[0035] Next, the solid particles on whose surface the colloidal palladium-tin is adsorbed are an acid such as chlorine, sulfuric acid or tetrafluoroboric acid to remove the tin component by dissolving and simultaneously depositing palladium particles on the surface of the solid particles. In In this stage, a palladium coating layer forms on the surface of the solid particles.
[0036] A second method for coating the surface of the solid particles with palladium is a ´´method, which involves immersing solid particles in a tin solution for a predetermined period of time for the purpose of deposition of tin on the surface of the solid particles, as well as immersing the solid particles in a palladium solution for a predetermined period of time for the deposition of palladium on the surface of the solid particles under using a substitution reaction between tin and palladium.
[0037] In both the first and the second method for coating the surface of the solid particles with Palladium can react with an acidic solution of chlorine, sulfuric acid, tetrafluoroboric acid, a carboxylic acid, a Oxycarboxylic acid, or an aromatic carboxylic acid can be used after carrying out the coating process to ensure removal of the tin contained in the palladium top layer.
[0038] The first and second methods for coating the surface of the solid particles with palladium are are given merely as examples. Among the substances used in the present invention, Solid particles with an inorganic covering layer are those whose surfaces are covered with a palladium coating, although this should not be interpreted as meaning that the Coating process is limited to these processes.
[0039] In the case of the inorganic top layer used in the present invention Solid particles are particles that have undergone a surface modification treatment. During the formation of the electroplated nickel layer containing solid particles on the surface of the wire Using the nickel plating solution of the present invention, an inorganic covering layer solid particles to the surface of the wire, whereby nickel ions with a positive charge at the same time a nickel component is deposited.
[0040] Accordingly, the material used in the surface modification treatment Surface modifier of the surface of the solid particles having an inorganic covering layer for the purpose of Stabilization a positive polarity. Preferred surface modifiers are those that Surfactant selected from amine-containing surfactants, nonionic surfactants and cationic surfactants. Among these Surfactants, the use of a nonionic surfactant containing an amino alcohol is preferred. Surface modifier can be applied to the surface of the solid particles having an inorganic coating layer effectively impart a positive charge by contacting the surface modifier with the solid particles and can change the state of the surface of the positive polarity As described above, the surface-modified, inorganic coating containing solid particles suspended in a nickel plating solution for use. This improves the distribution of the solid particles on the surface and the adhesion of the solid particles to the Surface of the wire during electroplating of the process described below for producing a wire containing solid particles, so that a quantity of the inorganic coating layer Solid particles adhere to the wire containing solid particles, which are proportional to the amount of Solid particles containing an inorganic covering layer contained in the plating solution.
[0041] The above-described surface modification treatment of an inorganic covering layer containing solid particles can be carried out using an optimal method which is suitable Way from a process which provides for the immersion of the solid particles in the surface treatment agent, a process which involves spraying the surface treatment agent onto the surface of the solid particles and the like. If the immersion method is used, the solid particles are a treatment container containing the surface modifier and stirred for a immersed in it for a predetermined period of time. After the treatment has been completed for a predetermined period of time, the solid particles are separated, removed from the treatment tank, washed with water, and dried.
[0042] Taking into account the relationship between the amount of nickel and that of the surface of the wire simultaneously deposited solid particles, the nickel plating solution of the present invention can be given any Amount of solid particles with an inorganic coating layer must be added. The content of Solid particles in the production of a wire containing solid particles for use in Wire saws, for example, prefer about 0.1 g / l to 40 g / l. If the content of solid particles is less than 0.1 g / l the resulting wire saw cannot achieve excellent cutting performance. On the other hand, a content of more than 40 g / l of solid particles is not preferred, since an excess of solid particles will adhere to the surface of the wire, which leads to problems regarding uniform adhesion of the solid particles to the surface of the wire leads.
[0043] Using the nickel plating solution which contains at least surface-modified, an inorganic Contains solid particles having a covering layer and a polyamine acting as a dispersant, as a A plating solution containing nickel component is used to form an electroplated layer on the surface of a wire, which A nickel layer containing dispersed solid particles is formed. This allows the surface of the wire to an electroplated nickel layer is formed in which the solid particles are evenly distributed, while At the same time, aggregation of the solid particles is avoided. Accordingly, the cutting behavior can be Use of the wire containing solid particles in wire saws can be significantly improved. Embodiment of a method for producing a wire containing solid particles
[0044] Next, the method for producing a particulate wire of the present invention Invention is described. First, the method for producing a wire coated with solid particles wire used in the present invention, and then the steps of the method for producing a wire of the present invention containing particulate matter.
[0045] Wire: in the process for producing a wire containing solid particles of the present The wire used in the invention can be any wire whose surface can be electroplated and which has a predetermined strength. Such a wire can be used without any restrictions and can be selected appropriately according to the respective application. Examples of a Such wire includes steel wires such as piano wires, tungsten wires, molybdenum wires, as well as wires made of stainless steel.
[0046] The wire, ie the core material of the wire containing solid particles, can be used without restriction in Essentially any diameter and can be cut to size according to the application. Considering the fact that most applications of the filter involve solid particles If the wire is to be used as a ´´wire saw´´, the diameter of the wire is preferably 0.02 mm to 3.0 mm. The wire acting as a wire saw, which is covered with solid particles, contains a Diameters of less than 0.02 mm are not preferred, as such a diameter tends to cause problems with effective adhesion of the solid particles having an inorganic coating layer to the surface of the wire On the other hand, the upper limit of the wire diameter depends on the application and is called A provisional guideline value has been determined. For example, the upper limit in a cutting machine used for cutting silicon wafers is For example, a wire with solid particles is 0.8 mm. From the point of view of cutting accuracy of objects, however, a wire diameter of more than 0.8 mm is not preferred, since for cutting objects It is not always necessary to have a wire saw made of a wire with such a diameter and therefore loses its necessity. When using the wire with solid particles for cutting Silicon wafers for solar cells require the use of a wire with a diameter of 0.06 mm to 0.23 mm at the best meets the needs of the market. The upper limit of the wire diameter for cutting components, such as reinforced concrete and steel for construction elements, used wire containing solid particles is 3.0 mm. With a wire diameter of more than 3.0 mm, the wire no longer has any flexibility and is therefore difficult to handle.
[0047] First, the surface of the wire coated with solid particles of the present invention The wire used should preferably be degreased and cleaned. Any type of wire can be used without any restrictions. Degreasing processes, such as immersion in an acid, degreasing with a solvent, Degreasing with an emulsifier and degreasing with alkali can be applied. If necessary, In addition, electrochemical degreasing can be carried out.
[0048] In addition, in the process for producing a wire coated with solid particles of the present invention In the invention, a wire is preferably used whose surface is provided with an inorganic protective layer. The inorganic protective layer present on the surface of the wire can prevent the formation of microcracks on the surface of the wire during the process and during separation, and can prevent corrosion of the wire. In addition In addition, some types of inorganic protective coatings can also affect the adhesion state of the Stabilize solid particles. For the inorganic protective layer, nickel, nickel alloys (Ni-Co, Ni-Sn, Ni-Zn), Cu, copper alloys (Cu-Zn, Cu-Sn) can be used. Taking into account the corrosion protection behavior and the The use of nickel or a nickel alloy is considered optimal for the adhesion stability of the solid particles. An inorganic protective layer consisting of nickel or a nickel alloy is preferably applied by means of a so-called ´´pre-plating process´´. This pre-plating process uses an electrolyte solution with low ion concentration to perform plating at high current density and in a short time and to produce a thin plating layer with a thickness of 1.0 µm or less. Although the plating can be carried out using a simple DC current, the power supply method used is preferably a ´´Pulse plating process´´ is used, which involves the repeated setting of an electrically conductive state and a current-free state to avoid a problem caused by the use of high current densities To avoid any reduction in quality. If pulse plating is used, the pulse can be applied without any Restriction of any waveform, such as a square wave or a triangular wave. It can be used without Any rectification system can be used without restriction, whereby a half-wave rectifier or a Full-wave rectifiers can be used. The conditions, such as a frequency of 200 Hz to 2000 2 2 Hz, a relative duty cycle (on: 20, off: 80) and a current density of 3 A / dm to 10 A / dm , can be adopted become.
[0049] Typical bath compositions used in pre-plating are as follows For safety reasons, sulfamic acid-based nickel plating can be used, for example. Nickel plating baths and Watts baths, as described below, are used. For copper cyanide pre-plating, an electrolyte solution can be used which contains 20 g / l to 35 g / l of copper cyanide, 37 g / l to 60 g / l of sodium cyanide, 3 g / l to 5 g / l of potassium hydroxide, and 10 g / l to 20 g / l of Rochelle salt. For copper pyrophosphate pre-plating, an electrolyte solution can be used which contains 16 g / l of Contains copper pyrophosphate, 120 g / l of potassium pyrophosphate, and 10 g / l of potassium oxalate.
[0050] In the process for producing a wire coated with solid particles of the present invention, the following steps a and b are carried out to form an electroplated nickel layer containing solid particles on the surface of a wire or to create a plated nickel coating layer. These steps of the Described in order.
[0051] Step a: as described in detail above, in this step the wire is prepared by depositing Nickel on the surface of the wire by electroplating using a polyamine as a dispersant and surface-modified solid particles containing an inorganic covering layer Nickel plating solution undergoes a composite plating, and at the same time an inorganic top layer containing solid particles are fixed to the wire to form an electroplated nickel layer containing solid particles on the surface of the wire.
[0052] The process for producing a particulate wire of the present invention can simultaneously deposit nickel and solid particles on the surface of the wire by applying a plating solution under typical plating conditions, whereby the plating solution is prepared by suspending the surface-modified solid particles with an inorganic covering layer in which a polyamine is used as Nickel plating solution containing dispersant is prepared. Preferably, 10 to 100, more Preferably, 20 to 50 solid particles per 500 µm length of wire are deposited on the wire. Less than 10 Solid particles per 500 µm length of wire are not preferred, as this will affect the cutting behavior of the wire On the other hand, more than 100 solid particles are not preferred, since the distance between adhering Solid particles even in cases where the uniformly dispersed solid particles on the surface of the wire can be separated is so small that the solid particles are easily removed during the handling of the wire saw. drop off, which means that objects to be cut tend to develop rough cutting surfaces. In this way, a electroplated nickel layer containing solid particles, in which the inorganic Solid particles with a covering layer are dispersed on the surface of the wire with only slight aggregation are.
[0053] Step b: in this step, on the surface of the electroplated solid particles obtained in step a containing nickel layer, a plated nickel coating layer is further formed on the surface of the wire formed electroplated nickel layer containing solid particles. From the point of view of Production rate, a preferred nickel plating process used here is Electroplating. The plating solution used in step b preferably consists of a pure nickel-containing plating solution or a nickel alloy (nickel-based alloy such as nickel-phosphorus, nickel- Cobalt, or nickel-zinc) containing plating solution. However, the plating solution used in step b is not limited to the latter. As described in detail in ´´Nickel Plating Solution´´, a commercially available Nickel plating bath can be used, or a Watts bath or sulfamic acid bath prepared by a specialist be used.
[0054] The wire on which the electroplated nickel layer containing solid particles is formed is heated at a solution temperature of 30°C to 60°C immersed in the nickel plating solution to form the wire a cathode and to form a plated layer on the electroplated nickel layer containing solid particles. Nickel plating layer with desired thickness. Note that a solution temperature of Nickel plating solution of less than 30°C not preferred is because the amount of saturated nickel contained in the plating solution tends to decrease, thereby reducing the Plating rate and thus industrial productivity decreases, and since the smoothness of the surface of the formed plated nickel coating layer tends to be reduced. On the other hand, a solution temperature of the Nickel plating solution of more than 60°C is not preferred, since in this case the use of vinyl chloride pipes problematic, which leads to a significant limitation regarding the components for the production plant used materials. In addition, the evaporation rate of the moist components in the plating solution, increasing fluctuations in the composition of the plating solution, leading to problems during the plating process. There are no restrictions on the other Plating conditions, especially as long as gentle nickel plating is possible.
[0055] The plated nickel coating layer formed in step b is on the outer surface of the electroplated, nickel layer containing solid particles, whereby they are located on the outermost layer of the Accordingly, the plated nickel coating layer can prevent the effectively prevent the solid particles contained in the electroplated nickel layer containing solid particles. The plated nickel coating layer preferably has a thickness of 0.1 µm to 40 µm. A plated Nickel plating layer with a thickness of less than 0.1 µm may cause a drop in the electroplated, Solid particles containing nickel layer, which during handling of the wire contaminated with solid particles or during a cutting process. plated nickel coating layer with a thickness of more than 40 µm is formed by electroplating, concentrated the current at the tips of those diamond particles on which nickel has been deposited unevenly, so that the thickness of the plating at the tips of the diamond particles increases. Assuming that the surface covered with solid particles When the wire is used as a wire saw, the tips of the increased thickness of the plating containing diamond particles immediately after starting to use the wire saw containing these diamond particles barely free, which impairs the initial cutting behavior. This case is not preferred.
[0056] Furthermore, the plated nickel coating layer more preferably has a thickness of 2 µm to 4 µm. The plated nickel coating layer preferably has a thickness of 0.1 µm to 40 µm. A plated nickel coating layer with a thickness of 2 µm, a fall in the nickel layer containing solid particles in the electroplated contained solid particles during handling of the wire containing solid particles or during a This effect of preventing the cutting process from falling off can be almost completely prevented. The electroplated nickel layer containing solid particles is already undergoing a plated nickel coating layer with a thickness of more than 4 µm, there is a tendency for the Current is simply concentrated at the tips of the diamond particles, which makes the process difficult to handle.
[0057] The method for determining the thickness of the plated nickel coating layer will now be described. shown schematically in Fig. 1, by directly observing the cross-section of a solid particle-filled coated wire 1 with a metallograph clearly a wire 2, an inorganic protective layer (pre-plating layer) 3, an electroplated nickel layer 5 containing solid particles 4, and a plated Nickel coating layer 6 can be observed. Here, the thickness of the plated nickel coating layer 6 is measured at locations of plated nickel coating layer 6 on which no solid particles 4 are present.
[0058] Embodiment of a wire coated with solid particles Next, an embodiment of the The wire coated with solid particles of the present invention is described. In the wire coated with solid particles The present invention is a wire containing solid particles, which is formed by means of the above described method for producing a wire of the present invention containing solid particles, Using the nickel plating solution of the present invention. In detail, the solid particles wire of the present invention having an ´´electroplated, solid particle-containing nickel layer´´, in which has ´´surface-modified solid particles with an inorganic covering layer´´ on the outer peripheral surface of the wire, as well as a ´´plated nickel coating layer´´ on the surface of the electroplated nickel layer containing solid particles. particulate nickel layer'' and the ''plated nickel coating layer'' are described.
[0059] Electroplated nickel layer containing solid particles: the electroplated nickel layer containing solid particles Nickel layer is in direct contact with the surface of the wire and thus covers it, wherein the solid particles having an inorganic covering layer are dispersed in the electroplated nickel layer and are contained in their interior. The nickel component plays a role as a binding agent to fix the inorganic coating layer on the surface of the wire. The electroplated, The nickel component contained in the nickel layer containing solid particles not only acts as a simple surface coating, but also shows excellent wettability and chemical affinity for the wire. For this reason, the electroplated nickel layer formed on the surface of the wire by electrolysis has excellent adhesion.
[0060] As described in detail in ´´Embodiment of a nickel plating solution´´, the core material the inorganic top layer contained in the electroplated nickel layer containing solid particles containing solid particles, for example particles of cerium oxide, silicon oxide (such as quartz and silica glass), Aluminum oxide, silicon carbide, silicon nitride, zirconium oxide, diamond and Teflon (registered trademark) can be used. In addition, the inorganic covering layer formed on the surface of the solid particles consists of a Metal component, which is selected according to the respective application of the nickel plating solution manufactured wire containing solid particles can be selected in a suitable manner. In detail, as solid particles having an inorganic covering layer, which in the electroplated, solid particles containing nickel layer of the particulate wire of the present invention, preferably one or two or more selected from diamond particles with a palladium coating, diamond particles with a nickel top layer, and diamond particles with a titanium top layer.
[0061] As described in detail above, the “electroplated, solid particle-containing Nickel layer'' of the particulate wire of the present invention by electroplating under Using the nickel plating solution, which contains surface-modified, inorganic top layer Solid particles and a polyamine acting as a dispersant. For this reason, the particles deposited on the The solid particles on the surface of the wire hardly come together and are in a state in which the Solid particles are dispersed with higher uniformity than conventional solid particles, to the electroplated Accordingly, the cutting behavior of a wire saw, which consists of the solid particles wire has been produced, can be significantly improved.
[0062] In particular, in the electroplated nickel layer containing solid particles, preferably 10 to 100 of solid particles with an inorganic covering layer (particle size: 0.01 µm to 100 µm) per 500 µm length of the wire on the wire. When using such an electroplated nickel layer containing solid particles, in which contains 10 to 100 of the solid particles having an inorganic covering layer per 500 µm length of the wire adhere to the wire, an electroplated nickel layer containing solid particles can be formed in which Solid particles are dispersed properly and without aggregation. Accordingly, the solid particles from a wire saw which comprises such an electroplated nickel layer containing solid particles, which allows good cutting performance to be maintained.
[0063] Plated nickel plating layer: the plated nickel plating layer is formed on the surface of the above described electroplated nickel layer containing solid particles and forms the outermost layer of the wire containing solid particles. For this reason, the plated nickel coating layer has the function of preventing the solid particles contained in the electroplated To avoid solid particles contained in the nickel layer.
[0064] The ´´plated nickel coating layer´´ is preferably produced by processing a pure nickel containing plating solution or a nickel alloy (nickel-based alloy such as nickel- phosphorus, nickel-cobalt, or nickel-zinc) containing plating solution as in ´´embodiment of a Process for producing a wire coated with solid particles'' as described above. The The nickel component contained in the ´´plated nickel coating layer´´ not only functions as a simple surface coating, but also shows excellent wettability for the ´´electroplated, nickel layer containing solid particles'', and even then easily forms a thin, even Coating film, if the underlying layer has depressions and projections due to the solid particles has.
[0065] By using the wire coated with solid particles, which is connected to the electroplated, Nickel layer containing solid particles, in which the solids containing an inorganic covering layer particles distributed on the surface of the wire, as well as the plated nickel coating layer on its surface The solid particles adhering to the wire can be effectively prevented from falling off. In this way a wire coated with solid particles can be obtained which has a high degree of reliability and is suitable for can be used for a long time.
[0066] The present invention will now be described in detail by way of examples. This should not be interpreted that the present invention is limited to the following examples. Example 1
[0067] Wire: In Example 1, the wire used was a steel wire manufactured by Japan Fine Steel Co., Ltd. having a diameter of 0.35 mm. Before the formation of the electroplated nickel layer containing solid particles In step c described below, the wire was subjected to a degreasing pretreatment, followed by a Immersion in 10% sulfuric acid. The surface of the wire was then treated with a nickel Pre-plating treatment to form an inorganic protective layer with a thickness of 0.5 µm. The Nickel pre-plating treatment was carried out using an electrolyte solution containing 240 g / l of nickel chloride and 125 g / l of hydrochloric acid, a pulse current with a short waveform, pulse electrolysis conditions at a 2 Frequency of 1000 Hz, a duty cycle (on: 20, off: 80), and a current density of 2.5 A / dm. The wire was also used in the other examples and in the comparison example.
[0068] Solid particles having an inorganic covering layer: in Example 1, the solid particles Diamond particles with a particle size in the range of 30 µm to 40 µm (average particle size: 35 µm) are used. An inorganic coating layer was formed on the surfaces of the diamond particles. In Example 1, the inorganic Cover layer formed by a process which involves the deposition of palladium and tin on the surfaces of the Diamond particles using a colloidal palladium-tin catalyst as the main component In particular, in Example 1, a solution of 0.1 g / l palladium and 2 g / l tin was used containing solution. The diamond particles were immersed in this solution for 10 minutes and were then removed from the solution. The diamond particles were then washed with water. Diamond particles were immersed in 50 g / l sulfuric acid for 10 minutes. In this way, the surfaces of the Diamond particles formed a palladium coating layer, wherein ´´diamond particles having a palladium coating layer´´ The ´´diamond particles with a palladium coating´´ had a particle size in the range from 30 um to 40 µm (average particle size: 35 µm).
[0069] The resulting ´´diamond particles having a palladium coating´´ were prepared using a Surface modifier or a solution containing a nonionic surfactant containing an amino alcohol The surface modifier used was a Solution containing 5 mass% of 2-aminoethanol (primary amine) and 1 mass% of a non-ionic surfactant and had a pH of 10. As part of the surface modification treatment, the ´´a palladium top layer containing diamond particles'' into the solution at a temperature of about 30°C surface modifier and immersed in it for 10 minutes. After that, the ´´one diamond particles with a palladium coating are washed with water, whereby ´´surface-modified, Diamond particles with a palladium coating" were obtained. A palladium coating Diamond particles that had undergone the same modification treatment were also used in the following described Example 2, Example 3, and in the Comparative Example.
[0070] Step a: In step a, the diamond particles having a palladium coating were introduced into the Nickel electroplating solution is introduced, whereby a ´´nickel electroplating solution containing diamond particles´´ in which 0.2 g / l of diamond particles with a palladium coating were suspended. The nickel electroplating solution containing diamond particles used was a nickel sulfamate Plating solution containing 400 g / l of nickel sulfamate tetrahydrate, 2 g / l of nickel chloride heptahydrate, 1 mg / l of Polyethylenimine (number average molecular weight: 70,000), and 35 g / l of boric acid and had a pH of 4.0.
[0071] The electrolysis was carried out for 30 minutes at a solution temperature of the diamond particles containing 2 Nickel electroplating solution of 65°C and a current density of 7.8 A / dm, whereby the surface of the degreased wire and the inorganic protective layer of a composite plating formed on it were subjected to an electroplated nickel layer containing diamond particles, in which the diamond particles dispersed in a palladium-coated layer. The electroplated diamond particles containing nickel layer'' had an equivalent thickness of 6.2 µm.
[0072] Step b: In step b, a nickel sulfamate plating bath containing 450 g / l of Nickel sulfamate tetrahydrate, 3 g / l of nickel chloride heptahydrate, and 40 g / l of boric acid and a pH of 4.0 The electrolysis was carried out for 15 minutes at a solution temperature of the nickel plating solution of 65°C and a 2 current density of 8.7 A / dm, whereby a ´´plated nickel coating layer´´ with a converted Thickness of 10.5 µm on the surface of the electroplated layer arranged on the surface of the wire according to step a, nickel layer containing diamond particles and thereby creating a ´´wire coated with diamond particles´´ became.
[0073] A 200-fold magnified photograph of the wire coated with diamond particles produced in Example 1 is shown in Fig. 2. In the wire coated with diamond particles according to Example 1, the final value of the outer diameter after plating and the wire diameter indicating the aggregation state of diamond. Monitoring value 446.9 µm. In addition, an average of 32.5 of the palladium-coated Diamond particles per 500 µm length of wire on the wire coated with diamond particles. Example 2
[0074] In Example 2, using the same conditions as in Example 1, a diamond particle coated wire, except that the concentration of polyethyleneimine (number average Molecular weight: 70,000) in step a differed from that of Example 1. In the following, only those Conditions of step a are described, which differ from those of Example 1.
[0075] In Example 2, the concentration of polyethyleneimine (number average molecular weight: 70,000) in the solution prepared in step a used nickel sulfamate plating solution to adjust the nickel electroplating solution 5 mg / l. The Conditions such as the temperature of the other plating solution, the current density and the electrolysis time, were the same as in Example 1.
[0076] A 200-fold magnified photograph of the wire coated with diamond particles produced in Example 2 is shown in Fig. 3. The wire coated with diamond particles according to Example 2 had a wire diameter monitoring value of 435.3 µm. In addition, an average of 32.1 of the palladium-coated Diamond particles per 500 µm length of wire on the wire coated with diamond particles. Example 3
[0077] In Example 3, using the same conditions as in Example 1, a diamond particle coated wire, except that the concentration of polyethyleneimine (number average molecular weight 70,000) in step a differed from that of Example 1. In the following, only those Conditions of step a are described, which differ from those of Example 1.
[0078] In Example 3, the concentration of polyethyleneimine (number average molecular weight: 70,000) in the solution prepared in step a used nickel sulfamate plating solution to adjust the nickel electroplating solution 10 mg / l. The Conditions such as the temperature of the other plating solution, the current density and the electrolysis time, were the same as in Example 1.
[0079] A 200-fold magnified photograph of the wire coated with diamond particles produced in Example 3 is shown in Fig. 4. The wire coated with diamond particles according to Example 3 had a wire diameter monitoring value of 415.6 µm. In addition, an average of 27.15 of the palladium-coated Diamond particles per 500 µm length of wire on the wire coated with diamond particles. Comparison example
[0080] In the comparative example, using the same conditions as in Examples 1 to 3, a Diamond particles coated wire is manufactured, except that only the wire used in step a Nickel sulfamate plating solution differed from that of Examples 1 to 3. In the following, only those Conditions of step a were described, which differed from those of Examples 1 to 3.
[0081] In the comparative example, the nickel sulfamate plating solution used in step a did not contain polyethyleneimine. The conditions such as the temperature of the other plating solution, the current density and the Electrolysis time was the same as in Example 1.
[0082] A 200-fold magnified photograph of the diamond-particle-coated wire is shown in Fig. 5. The wire coated with diamond particles according to the comparative example had a Wire diameter monitoring value of 455.5 µm. In addition, an average of 34 of the one Palladium-coated diamond particles per 500 µm length of wire on the diamond-coated tainted wire.
[0083] Considerations based on a comparison between the examples and the comparative example
[0084] To simplify the comparison between the examples and the comparative example, the Observation results for the obtained wires coated with diamond particles in the following table shown in Table 1 Concentration of wire diameter- average number of sample Polyethylenimine (mg / l) Monitoring value (µm) Diamond particles Example 1 1 446.9 32.5 Example 2 5 435.3 32.1 Example 3 10 415.6 27.15 Comparison example 0 455.5 34
[0085] Comparing Examples 1 to 3, in which the nickel electroplating solution in step a polyethyleneimine was added, with the comparative example in which no polyethyleneimine was added, the one without Addition of polyethyleneimine in the comparative example produced wire after plating a lower, the Wire diameter monitoring value indicating the aggregation state of the diamond particles, namely a lower outer wire diameter than those of Examples 1 to 3, while the average number of a palladium coating layer diamond particles adhering to the surface of the wire in the examples and in the comparative example almost This indicates that the aggregation of the palladium-coated Diamond particles on the wire coated with diamond particles is reduced and the dispersibility is increased. This This fact can be verified by looking at Fig. 2 to 5, which photographs of the examples and the Show comparison example.
[0086] Furthermore, it is evident from the results of Examples 1 to 3 that the wire diameter Monitoring value with increasing concentration of polyethyleneimine in the solution used in step a nickel electroplating solution. From this it can be concluded that the effect of polyethyleneimine as Dispersant increases with increasing concentration.
[0087] When using the wires coated with solid particles according to the examples and the Wire containing solid particles according to the comparative example as a wire saw, it turns out that the Cutting behavior of the wire covered with solid particles according to the examples, which was measured using a polyethyleneimine-containing nickel electroplating solution prepared in step a, compared to that of the Wire containing solid particles according to the comparative example due to an increase in the dispersibility of the Solid particles are significantly better. Industrial applicability
[0088] As described above, the nickel plating solution of the present invention can be used to form a electroplated nickel layer containing dispersed solid particles on the surface of a wire forming an electroplated nickel layer in which the solid particles with higher are dispersed evenly and aggregation of the solid particles adhering to the wire is avoided. In this way, wire saws can be provided cost-effectively, which are loaded with solid particles and have a have excellent cutting properties. The wire, which is contaminated with solid particles, can easily break fragile Materials such as blocks of silicon single crystals can be cut with high precision and is therefore suitable for Suitable for use in manufacturing processes for solar cells and silicon wafers for semiconductors. In addition, the The particulate wire of the present invention is suitable for a A variety of applications, such as files and knife sharpeners, and can be used in a variety of ways and Can be used for cutting or polishing. List of reference symbols 1 wire containing solid particles 2 wire 3 inorganic protective layer (pre-plating layer) 4 solid particles 5 electroplated nickel layer containing solid particles 6 plated nickel plating layer
Claims
1. Nickel plating solution for forming an electroplated nickel layer containing dispersed solid particles on the surface of a wire, whereby the nickel plating solution surface-modified, an inorganic covering layer comprising solid particles and a polyethyleneimine acting as a dispersant.
2. Nickel plating solution according to claim 1, wherein the polyethyleneimine is a polyethyleneimine having a number average molecular weight of 800 to 2,000,000.
3. Nickel plating solution according to claim 1 or 2, wherein the concentration of polyethyleneimine is 1 mg / l to 100 mg / l.
4. Nickel plating solution according to one of claims 1 to 3, wherein the inorganic coating layer Solid particles have a surface which is modified with a surface modifier for charging purposes has been.
5. Nickel plating solution according to claim 4, wherein the surface modifier comprises one or more surfactants selected from amine-containing surfactants, non-ionic surfactants and cationic surfactants.
6. Nickel plating solution according to claim 4 or 5, wherein the surface modifier comprises an amino alcohol and a contains non-ionic surfactant.
7. Nickel plating solution according to one of claims 1 to 6, wherein the solid particles have a particle size of 0.01 µm up to 100 µm.
8. Nickel plating solution according to one of claims 1 to 7, wherein the inorganic covering layer having solid particles by one or two or more selected from diamond particles having a Palladium top layer, diamond particles with a nickel top layer, and diamond particles with a titanium top layer is.
9. A method for producing a wire coated with solid particles which is bonded to an outer peripheral surface of the Wire comprises fixed solid particles, wherein the process steps a and b includes: Step a: a step which involves performing a composite plating by depositing nickel on the surface of the wire by electroplating using the nickel plating solution according to claims 1 to 8 and the simultaneous adhesion of the solid particles having an inorganic covering layer to form a plated, to form a nickel layer containing solid particles on the surface of the wire; and Step b: a step which involves forming a plated nickel coating layer on the surface of the wire formed plated nickel layer containing solid particles.
10. A method for producing a wire coated with solid particles according to claim 9, wherein the wire is coated with a inorganic protective layer on the surface of the wire.
11. A method for producing a wire coated with solid particles according to claim 9 or 10, wherein the wire has a Diameters from 0.02 mm to 3.0 mm.
12. A wire coated with solid particles, which is produced by the process for producing a wire coated with solid particles coated wire according to any one of claims 9 to 11, wherein 10 to 100 of the inorganic Cover layer containing solid particles with a particle size of 0.01 µm to 100 µm per 500 µm length of the wire adhere to the wire, with the proviso that a wire coated with solid particles on which 10 to 60 of the one inorganic covering layer containing solid particles with a particle size of 0.01 µm to 100 µm per 500 µm Length of the wire is excluded from protection.
Citation Information
Patent Citations
CURRENT TRANSFER BRUSHES FOR ELECTRICAL HIGH CURRENT MACHINES
DE3006225A1
Wire coated with solid microparticles, and method for producing wire coated with solid microparticles
WO2013039097A1