Mo-doped Co2Z-type ferrite composite material, process for producing the composite material and articles operating in the high-frequency range comprising the composite material
The Mo-doped Co2Z-type hexaferrite composition addresses high-frequency application challenges by providing low losses and high permeability, enabling efficient use in miniaturized antenna elements and spintronics devices.
Patent Information
- Application Number
- DE112016000536
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-01-30
- Filing Date
- 2016-02-01
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2036-02-01
AI Technical Summary
Existing ferrite materials exhibit high magnetic and dielectric losses at high frequencies, limiting their use in ultra-high frequency and microwave applications, and there is a need for materials with high permeability and permittivity for miniaturized antenna elements in radar and wireless communication systems.
A Mo-doped Co2Z-type hexaferrite composition is developed, which includes substitutions of barium, strontium, and molybdenum in the hexaferrite structure to achieve low magnetic and dielectric losses while maintaining high permeability and permittivity, suitable for high-frequency applications.
The Mo-doped Co2Z-type hexaferrite composition achieves low magnetic and dielectric losses, high permeability, and matching impedance, making it suitable for ultra-high frequency and microwave applications, including antennas, filters, and spintronics devices, with potential for cost-effective mass production.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND
[0001] To meet the ever-increasing demand for devices used in ultra-high frequency (UHF), L-band and S-band applications, which are of particular interest to a wide range of commercial and defense industries, improved performance and miniaturization are required. Antenna elements, a critical component in radar and modern wireless communication systems, are constantly being developed with compact dimensions. However, the development of ferrite materials for use in such high-frequency applications has proven very difficult. Existing ferrite composite materials exhibit relatively high magnetic losses at high frequencies, which do not meet the requirements for constructing a practical antenna. The prior art can be found in: AOYAMA, M. [et al.]: Preparation and characterization of Z-type hexaferrites, Ba3(1−x)Sr3x Co2Fe24O41 with x = 0–0.5, via a two-step calcination with an intermediate wet milling.In: Journal of Electroceramics, Vol. 17, 2006, No. 1, S. 61-64. – ISSN 1385-3449; DE 39 07 220 A1 und US 5 494 749 A.
[0002] More generally, the need for high-performance devices with miniaturized structures in modern wireless communication systems is increasing. A material that exhibits high permeability with appropriate permittivity and low magnetic and dielectric losses is ideal as an antenna substrate material. Such materials enable miniaturization while maintaining or enhancing antenna gain and bandwidth. Spinel ferrites with high permeability values, such as NiZn ferrites, are already widely used for high-frequency applications. However, these ferrites exhibit relatively low cutoff frequencies, which prevents their use above 0.3 GHz. Some hexaferrite materials, such as cobalt-substituted barium Y-type (Co2Y) and Z-type (Co2Z) hexaferrites, exhibit much higher ferromagnetic resonance frequencies above 1.0 GHz due to their high magnetocrystalline anisotropy fields and high permeabilities.Accordingly, the use of magnetodielectric substrates with permittivity values ε' equal to the permeability µ' is common due to the ease of impedance matching between the substrate and the vacuum space, among other advantages. However, it is very difficult to achieve low magnetic and dielectric losses and high permeability for dielectric substrates. For example, it has been reported that for Co2Y, ε' is 15-20 and µ' is 2-3, while for Co2Z, ε' is 12 and µ' is 18-19. However, the magnetic loss of single-phase Y- or Z-type ferrite is still considerably high (loss tangent, tan δ). µ > ,5) at f > 0.5 GHz. SUMMARY OF THE INVENTION
[0003] The invention relates to a hexaferrite composition suitable as a magnetic material in electrical devices operating in the high-frequency range. The hexaferrite composition comprises barium and / or strontium, molybdenum, cobalt, and iron and has a Z-type hexaferrite phase. The hexaferrite can be stoichiometric or non-stoichiometric. With substitutions of barium, strontium, and molybdenum as described herein, it is possible to create magnetodielectric hexaferrite compositions with tunable permeability and permittivity and low dielectric and magnetic losses over high-frequency ranges. The hexaferrite compositions can also be cost-effective for mass production of devices such as microwave antenna substrates and in spintronic applications such as giant magnetoresistance (GMR) devices.The invention also relates to methods for producing the hexaferrite composition and to articles, devices or parts comprising the hexaferrite composition.
[0004] Further aspects of the procedure and system follow, namely: 1. A hexaferrite composition comprising iron, cobalt, one or both of barium and strontium, and molybdenum, wherein the ferrite composition comprises a Z-type hexaferrite phase having the formula (Ba z Sr (3-z) )Co (2+x) Mon x Fe (y-2x) O 41 includes, where x = 0.01 to 0.20; y = 20 to 24; and z = 0 to 3. 2. The hexaferrite composition of point 1, where x = 0.08 to 0.15. 3. The hexaferrite composition according to any of the items 1-2, where x = 0.10 to 0.12. 4. The hexaferrite composition according to any one of items 1-3, wherein the hexaferrite composition has a real permeability of at least 3.0 over a frequency range of 0.1 to 3.0 GHz, in particular from 0.1 to 1.0 GHz. 5. The hexaferrite composition according to any one of items 1-4, wherein the hexaferrite composition has a real permeability of at least 7.0 over a frequency range of 0.1 to 3.0 GHz. 6. The hexaferrite composition according to any one of items 1-5, wherein the hexaferrite composition has a real permeability in the range of 7.0 to 12.0 over a frequency range of 0.1 to 3.0 GHz. 7. The hexaferrite composition according to any one of items 1-6, wherein z = 1.2 to 3.0, and the hexaferrite composition has a real permeability in the range of 8.0 to 12.0 over a frequency range of about 0.1 GHz to at least 1.0 GHz. 8. The hexaferrite composition according to any one of items 1-7, wherein z = 0 to 0.5, and the hexaferrite composition has a real permeability in the range of 2.0 to 4.0 over a frequency range of about 0.1 GHz to about 3.0 GHz. 9. The hexaferrite composition according to any one of items 1-8, wherein the hexaferrite composition has a real permittivity of at least 6.0 over a frequency range of 0.1 to 3.0 GHz. 10. The hexaferrite composition according to any one of items 1-9, wherein the hexaferrite composition has a real permittivity of at least 8.0 over a frequency range of 0.1 to 3.0 GHz. 11. The hexaferrite composition according to any one of items 1-10, wherein the hexaferrite composition has a real permittivity in the range of 6.0 to 18.0 over a frequency range of 0.1 to 10.0 GHz. 12. The hexaferrite composition according to any one of items 1-11, wherein a real permittivity of the hexaferrite composition is equal to a real permeability of the hexaferrite composition within 10%. 13. The hexaferrite composition according to any one of items 1-12, wherein the hexaferrite composition has a characteristic impedance that matches an impedance of a vacuum within 3%. 14. The hexaferrite composition according to any one of items 1-13, wherein the hexaferrite composition has a dielectric loss tangent tanδ ε of less than 0.02 at a frequency of 0.1 to 0.8 GHz. 15. The hexaferrite composition according to any one of items 1-14, wherein the hexaferrite composition has a dielectric loss tangent tanδ ε of less than 0.16 at a frequency of 0.1 to 1.0 GHz. 16. The hexaferrite composition according to any one of items 1-15, wherein the hexaferrite composition has a magnetic loss tangent tanδ µ of approximately 0.1 at 0.4 GHz. 17. The hexaferrite composition according to any one of items 1-16, wherein the hexaferrite composition has a magnetic loss tangent tanδ µ of less than 0.3 at a frequency of 0.1 to 0.8 GHz. 18. The hexaferrite composition according to any one of items 1-17, wherein the hexaferrite composition has a magnetic loss tangent tanδ µ of less than 0.95 at a frequency of 0.1 to 3.5 GHz. 19. The hexaferrite composition according to any one of items 1-18, wherein the hexaferrite composition has a magnetic loss tangent tanδ µ in the range of 0.1 to 1.0 over a frequency range of 0.1 to 1.0 GHz. 20. The hexaferrite composition according to any one of items 1-19, wherein the hexaferrite composition has a dielectric loss factor tanδ ε / ε' of less than 0.001 at a frequency of 0.8 GHz. 21. The hexaferrite composition according to any one of items 1-20, wherein the hexaferrite composition has a magnetic loss factor tanδ µ / µ' of less than 0.03 at a frequency of 0.8 GHz. 22. An article comprising the hexaferrite composition according to any one of items 1-21, wherein the article is an antenna, a filter, a coil, a circulator, or a phase shifter. 23. The article of item 22, wherein the article is a filter, coil, circulator or phase shifter. 24. The article according to any of items 22-23, where the article is a microwave antenna 25. The article of item 24, wherein the article is an antenna operable at a frequency equal to or greater than 0.1 GHz. 26. The article according to any one of items 24-25, wherein the article is an antenna operable at a frequency equal to or greater than 0.3 GHz. 27. The article of item 24, wherein the article is an antenna operating at 0.1 to 1.5 GHz. 28. The article according to any one of items 24 and 27, wherein the article is an antenna operating at 0.3 to 1.0 GHz. 29. The article according to any one of items 22-28, further comprising a second hexaferrite composition comprising a Z-type hexaferrite phase having the formula (Ba z Sr (3-2) )CO (2+x) MO x Fe (y-2x) O 41 where x = 0.01 to 0.20; y = 20 to 24; and z = 0 to 3; and where the amount of Ba and the amount of Sr differ in the hexaferrite composition and the second hexaferrite composition. 30. The article of item 29, wherein a cutoff frequency of the second hexaferrite composition is higher than a cutoff frequency of the hexaferrite composition. 31. The article according to any one of items 29-30, wherein the hexaferrite composition has a real permeability in the range of 8.0 to 12.0 over a frequency range of about 0.1 GHz to at least 1.0 GHz, and the second hexaferrite composition has a real permeability in the range of 2.0 to 4.0 over a frequency range of about 0.1 GHz to about 3.0 GHz. 32. The article of item 22, wherein the article is a giant magnetoresistance device or a giant tunneling magnetoresistance device. 33. A process for producing a hexaferrite composition comprising: (a) providing hexaferrite phase precursor compounds comprising Fe, Co, Mo and Ba and / or Sr, and (b) calcining the hexaferrite phase precursor compounds in air at 1000 to 1300 °C to form a material comprising a Z-type hexaferrite phase according to any one of items 1 to 21. 34. The method of item 33, wherein the hexaferrite phase precursor compounds comprise oxides of Fe, Ba, Co, and Mo. 35. The method according to any one of items 33-34, wherein the hexaferrite phase precursor compounds comprise MoO2, BaCO3, Co3O4, and Fe2O3. 36. The process according to any one of items 33-35, wherein the hexaferrite phase precursor compounds comprise from more than 0 to 0.96 wt% MoO2, from 22.10 to 22.18 wt% BaCO3, 6.02 to 6.59 wt% Co3O4, and 70.35 to 71.8 wt% Fe2O3. 37. The procedure under any of items 33-36, further comprising the following: (c) comminuting the material formed in step (b) to form a powder mixture, and (d) Sintering the powder mixture. 38. The process of item 37, wherein the powder mixture is sintered at 1200 to 1280 °C. 39. The process according to any one of items 37-38, wherein the powder mixture is sintered for 4 to 20 hours. 40. The process according to any one of items 37-39, wherein the powder mixture is sintered in an oxygen atmosphere. 41. The method of any one of items 37-40, further comprising forming the powder mixture into a compact prior to step (d). 42. The method of any one of items 37-41, further comprising adding a binder to the powder mixture. 43. The method of item 42, wherein the binder is selected from the group consisting of a polyvinyl alcohol, methylcellulose, polyethylene glycol and poly(alkylene carbonate). 44. The method according to any one of items 42-43, wherein the binder is polyvinyl alcohol comprising 8 to 12 wt% of the powder mixture. 45. The procedure under any of items 37-44, further comprising the following: (e) comminuting the material formed in step (d) to form a powder mixture; and (f) annealing the powder mixture formed in step (e). 46. The process of item 45, wherein the powder mixture is annealed at 800 to 1000 °C. 47. The process according to any one of items 45-46, wherein the powder mixture is tempered for 9 to 20 hours. DESCRIPTION OF THE DRAWINGS
[0005] The invention will be better understood from the following detailed description taken in conjunction with the accompanying drawings, in which: Fig. Figure 1A shows a graphical representation of the frequency dependence of the real part of the permeability of Mo-Co2Z; Fig. Figure 1B shows a graphical representation of the frequency dependence of the imaginary part of the permeability of Mo-Co2Z; Fig. Figure 2A shows a graphical representation of the frequency dependence of the magnetic loss tangent of the permeability of Mo-Co2Z hexaferrites at 0 to 10 GHz; Fig. Figure 2B shows a graphical representation of the frequency dependence of the magnetic loss tangent of the permeability of Mo-Co2Z hexaferrites at 0 to 1 GHz; Fig. Figure 3A is a graphical representation of the variation of permeability and magnetic loss tangent with Mo content at f = 0.3 GHz for Mo-Co2Z hexaferrites; Fig. Figure 3B shows a graphical representation of the variation of permeability and magnetic loss tangent with Mo content at f = 0.8 GHz for Mo-Co2Z hexaferrites; Fig. 4A a graphical representation of the frequency dependence of the real permittivity for Mo-Co2Z hexaferrite at 0 to 10 GHz; Fig. 4B a graphical representation of the frequency dependence of the real permittivity for Mo-Co2Z hexaferrite at 0 to 1 GHz; Fig. Figure 5A shows a graphical representation of the frequency dependence of the dielectric loss tangent for Co2Z hexaferrite at 0 to 10 GHz; Fig. Figure 5B shows a graphical representation of the frequency dependence of the dielectric loss tangent for Mo-Co2Z hexaferrite at 0.0 to 1.0 GHz; Fig. Figure 6 is a graphical representation of the variation of permittivity and dielectric loss tangent with Mo content at 0.8 GHz for Mo-Co2Z hexaferrite; Fig. Figure 7A shows a graphical representation of the frequency dependence of permeability, permittivity, and magnetic and dielectric loss tangent for Mo-Co2Z hexaferrite ZM5, where x = 0.10; Fig. Figure 7B shows a graphical representation of the frequency dependence of permeability, permittivity, and magnetic and dielectric loss tangent for Mo-Co2Z hexaferrite ZM6, where x = 0.12; Fig. Figure 8 shows a graphical representation of the frequency dependence of permeability, permittivity and magnetic and dielectric loss tangent for the Mo-Co2Z hexaferrites ZM5, where x = 0.10, and ZM6, where x = 0.12; Fig. 9 a series of SEMs illustrating the surface morphology of Mo-Co2Z hexaferrite samples with different Mo contents; Fig. Figure 10 shows a graphical representation of the frequency dependence of the magnetic permeability for hexaferrite samples of the ZSF series; Fig. Figure 11A shows a graphical representation of the frequency dependence of the magnetic permeability and magnetic loss for sample ZSF 1; Fig. 11B an SEM image of sample ZSFI; Fig. Figure 12A is a graph showing the frequency dependence of magnetic permeability and magnetic loss for sample ZSF2; Fig. 12B an SEM image of sample ZSF2; Fig. Figure 13A is a graph showing the frequency dependence of magnetic permeability and magnetic loss for sample ZSF3; Fig. 13B an SEM image of sample ZSF3; Fig. Figure 14A is a graph showing the frequency dependence of magnetic permeability and magnetic loss for sample ZSF4; Fig. 14B an SEM of sample ZSF4; Fig. 15 a graphical representation of the dielectric spectra at 0.1 to 10.0 GHz for samples ZSF1 to ZSF4; Fig. 16 a graphical representation of the frequency dependence of the magnetic permeability for Mo-doped SrCo2Z hexaferrites; Fig. 17 a graphical representation of the frequency dependence of the magnetic loss tangent for Mo-doped SrCo2Z hexaferrites; Fig. Figure 18 shows a graphical representation of the variation of permeability and magnetic loss tangent with Mo content at f = 1.0 GHz for Mo-doped SrCo2Z hexaferrites; Fig. 19 a graphical representation of the frequency dependence of permittivity for Mo-doped SrCo2Z hexaferrites; Fig. 20 a graphical representation of the frequency dependence of the dielectric loss tangent for Mo-doped SrCo2Z hexaferrites; Fig. Figure 21 is a graphical representation of the variation of permittivity and dielectric loss tangent for Mo content at 1.0 GHz for Mo-doped SrCo2Z hexaferrites; Fig. Figure 22A is a schematic crystal structure diagram of an M-type hexaferrite; Fig. 22B is a schematic crystal structure diagram of a Z-type hexaferrite; and Fig. Figure 22C shows a schematic crystal structure diagram of a Y-type hexaferrite. DETAILED DESCRIPTION OF THE INVENTION
[0006] The present invention relates to a Co2Z-type hexaferrite composition in which the magnetic and dielectric losses can be controlled by the use of molybdenum (Mo) while maintaining high permeability and / or low permittivity. The composition comprises the substitution of iron (Fe) with Mo in Co2Z-type hexaferrites. Molybdenum can successfully reduce magnetic loss and increase permeability in both stoichiometric and non-stoichiometric strontium, barium, or strontium-barium Z-type hexaferrites. In some embodiments, MoO2 can be used to reduce magnetic losses in BasCo2Fe 24 O 41-hexaferrites (referred to herein as BaCo2Z hexaferrites) and in other embodiments in Sr3Co2Fe 24 O 41 -hexaferrites (referred to herein as SrCo2Z hexaferrites). In some embodiments, MoO2 can be used to reduce magnetic losses in Co2Z hexaferrites that include both Ba and Sr and / or non-stoichiometric amounts of Fe.
[0007] More generally, hexagonal ferrites, or hexaferrites, are a type of iron oxide ceramic compound that has a hexagonal crystal structure and exhibits magnetic properties. Several types or families of hexaferrites are known, including the Z-type ferrites Ba3Me2Fe 24 O 41 , where Me can be a small 2+ cation, such as Co, Ni, or Zn. Ba can be substituted by Sr. Other hexaferrite types include M-type hexaferrites ((Ba,Sr)Fe 12 O 19 ), W-type hexaferrites ((Ba,Sr)Me2Fe 16 O 27), Y-type hexaferrite ((Ba,Sr)2Me2Fe 12 O 22 ), X-type hexaferrite ((Ba,Sr)2Me2Fe 28 O 46 ) and V-type hexaferrites ((Ba,Sr)4Me2Fe 36 O 60 )).
[0008] Cobalt-substituted barium (Co2Z) hexaferrites of the Z-type can exhibit high ferromagnetic resonance frequencies and permeabilities, although the construction of high-frequency devices requiring a relative permeability µ and relative permittivity ε with an equal or substantially equal value as well as low magnetic and dielectric loss tangents (tanδ µ , tanδ ε ) and loss factors (tanδ / µ , tanδ ε / ε) has been very difficult to obtain. (As used herein, the permeability and permittivity values are the relative permeability and the relative permittivity, respectively.) Schematic crystal structure diagrams of M-type phase, Y-type phase, and Z-type phase hexaferrites are shown in Fig. 16A-16C. The hexaferrite compounds are made from R-, S-, and T-layers or from minor modifications of these layers. Some properties of the Y-type and Z-type hexaferrites are shown in Table 1. Table 1: Some properties of Y-type and Z-type hexaferrites Co2Y Co2Z Formel Ba2Co2Fe 12 O 22 Ba3Co2Fe 24 O 41 Stapelordnung (TS)3 RSTSR*S*T*S* C(Å) 43,56 52,30 4πM s ·G 2300 3360 µ i 3-4 17 H A (no) 28 13 K1+K2 -2,6 -1,8 f r ·(GHz) 3 1-2 T c 340 410 ρ(g / cm 3 ) 5,4 5,35
[0009] The present hexaferrite composition is suitable for use in high-frequency applications, particularly ultra-high frequency (UHF) and microwave applications and devices, such as antennas, filters, coils, and circulators operating in the ultra-high and microwave frequency ranges. The ultra-high frequency (UHF) range is 0.3 GHz to 3 GHz. The microwave frequency range is 0.3 GHz to 300 GHz. The hexaferrite composition is also suitable for use in spintronic applications, such as giant magnetoresistance (GMR) devices. The present hexaferrite composition contains Fe, Co, Mo, and one or both of Ba and Sr, and has a Z-type hexaferrite phase. The hexaferrite composition has the formula (Ba z Sr (3-z) )Co (2+x) Mon x Fe (y-2x) O 41 on, where x = 0.01 to 0.20; y = 20 to 24; and z = 0 to 3.
[0010] In some embodiments, x = 0.08 to 0.15. In other embodiments, x = 0.10 to 0.12.
[0011] In some embodiments, the composition exhibits high real permeability µ' at high frequencies: Permeability at f = 0.1 to 1 GHz: µ' > 8; Permeability at f = 0.1 to 0.8 GHz: µ' > 10.
[0012] In addition, in some embodiments, the composition exhibits high, equal, or substantially equal values of ε' and µ' (from approximately 8 to 9) at f = 0.1 to 1 GHz. The composition exhibits low magnetic and dielectric losses and loss factors: Loss at f = 0.1 to 0.8 GHz: tan δµ < 0.3 and tan δ ε < 0.01; Loss factor at f = 0.8 GHz: tan δµ / µ' < 0.03 and tan ε / ε' < 0.001.
[0013] In some embodiments, a hexaferrite composition is a Mo-doped BaCo2Z hexaferrite, with 1.2 < z < 3. In some embodiments, a hexaferrite composition is a Mo-doped BaCo2Z hexaferrite, with z = 3. In some embodiments, Mo-doped BaCo2Z hexaferrites can have a real permeability in the range of 8.0 to 12.0 at frequencies from about 0.1 GHz to about 1.0 GHz. In some embodiments, the material can have a magnetic loss tangent in the range of 0.08 to 0.15 at f = 0.3 GHz and a magnetic loss tangent in the range of 0.3 to 0.75 at f = 0.8 GHz with a Mo content of 0.08 < x < 0.15. In some embodiments, the material may have a real permittivity in the range of 8 to 13 over a range of f = 0.1 to 10.0 GHz at a Mo content of 0.01 < x < 0.20.In some embodiments, the dielectric loss tangent for a Mo content of 0.01 < x < 0.12 may be less than 0.02 at f = 0.1 to 10.0 GHz.
[0014] A Mo-doped BaCo2Z hexaferrite can be used for applications such as microwave antennas. The material can be used in conjunction with a second hexaferrite that operates over a different frequency range, for example, a higher frequency range, to provide a single device with a wider operating frequency range. In some embodiments, the second hexaferrite can be a Mo-doped SrCo2Z hexaferrite.
[0015] In some embodiments, a hexaferrite composition is a Mo-doped SrCo2Z hexaferrite, where 0.0 < z < 0.5. In some embodiments, a hexaferrite composition is a Mo-doped SrCo2Z hexaferrite, where z = 0.0. In some embodiments, Mo-doped SrCo2Z hexaferrites can have a real permeability in the range of 2.0 to 4.0 over a frequency range of about 0.1 GHz to about 3.0 GHz. In some embodiments, Mo-doped SrCo2Z hexaferrites can have a real permeability in the range of 2.7 to 4.1, at f = 0.1 to 1.0 GHz. In some embodiments, the real permeability is greater than 3.6 at f = 1.0 GHz and a Mo content of 0.08 < x < 0.12. In some embodiments, the material may have a magnetic loss tangent in the range of 0.08 to 0.3 at f = 0.1 to 1.0 GHz. In some embodiments, the magnetic loss tangent is less than 0.25 at f = 1.0 GHz and a Mo content of 0.08. <x<0,12.In some embodiments, the material may have a real permittivity in the range of 12 to 18 over a range of f = 0.1 to 10.0 GHz at a Mo content of 0.01 <x<0,20 aufweisen. In einigen Ausführungsformen kann die dielektrische Verlusttangente geringer sein als 0,03, bei f = 1,0 GHz, für einen Mo-Gehalt von 0,08 < x < 0,12.
[0016] A Mo-doped SrCo2Z hexaferrite can be used for applications such as microwave antennas. The material can be used in conjunction with a second hexaferrite that operates over a different frequency range, for example, a lower frequency range to provide a single device with a wider operating frequency range. In some embodiments, the second hexaferrite can be Mo-doped BaCo2Z.
[0017] In some embodiments, a hexaferrite composition is a Mo-doped Co2Z hexaferrite with Sr and Ba, with z = 1.5. In some embodiments, a Mo-doped hexaferrite composition with Sr and Ba may have a real permeability in the range of 7.5 to 9.0 at f = 0.8 to 1.0 GHz. In some embodiments, a Mo-doped hexaferrite composition with Sr and Ba may have a magnetic loss tangent in the range of 0.7 to 0.2 at f = 0.8 to 1.0 GHz.
[0018] In some embodiments, a Mo-doped hexaferrite composition with Sr and Ba may have a real permittivity in the range of 6.6 to 8.7 at f = 0.8 to 1.0 GHz. In some embodiments, a Mo-doped hexaferrite composition with Sr and Ba may have a dielectric loss tangent in the range of 0.0019 to 0.0028 at f = 0.8 to 1.0 GHz.
[0019] In some embodiments, the Mo-doped hexaferrite composition has a real permeability µ' in the range of about 2.0 to about 12.0 at frequencies of about 0.1 GHz to about 3 GHz or greater. In some embodiments, at frequencies in the range of 0.1 GHz to at least 3.0 GHz, and in some embodiments at higher frequencies, the real permeability is at least 3.0, at least 5.0, at least 7.0, at least 8.0, at least 9.0, at least 10.0, at least 11.0, or at least 12.0.
[0020] In some embodiments, the hexaferrite composition has a real permittivity ε' in the range of about 6.0 to about 18.0 at frequencies from about 0.1 GHz to about 10 GHz. In some embodiments, at frequencies in the range of 0.1 GHz to at least 3.0 GHz, and in some embodiments at higher frequencies, the real permittivity is at least 6.0, at least 7.0, at least 8.0, at least 9.0, at least 10.0, at least 11.0, at least 12.0, at least 13.0, at least 14.0, at least 15.0, at least 16.0, or at least 17.0.
[0021] In some embodiments, the real permittivity ε' is equal to a real permeability µ' of the hexaferrite composition within 10%. In other embodiments, the real permittivity and the real permeability may be equal to within 15%, within 5%, within 2%, or within 1%. The hexaferrite composition may have a characteristic impedance that matches a vacuum impedance within 3%. In other embodiments, the characteristic impedance may match the vacuum impedance within 5%, within 2%, or within 1%.
[0022] In some embodiments, the magnetic loss tangent tan δµ ranges from less than 0.1 to about 1.0 at frequencies less than about 3.0 GHz. In some embodiments, the magnetic loss tangent is less than 0.3 or less than 0.1 at frequencies less than about 0.4 GHz. In some embodiments, the magnetic loss tangent is less than 0.75, less than 0.5, or less than 0.3 at frequencies less than about 0.8 GHz. In some embodiments, the magnetic loss tangent is less than 0.95, less than 0.6, or less than 0.3 at frequencies less than about 1.0 GHz. In some embodiments, the magnetic loss tangent is less than 2.4 or less than 0.9 at frequencies less than about 3.0 GHz.
[0023] In some embodiments, the hexaferrite composition has a magnetic loss tangent tanδ µof approximately 0.1 at 0.4 GHz. In some embodiments, the hexaferrite composition has a magnetic loss tangent tanδ µ of less than 0.3 at a frequency of 0.1 to 0.8 GHz. In some embodiments, the hexaferrite composition has a magnetic loss tangent tanδ µ of less than 0.95 at a frequency of 0.1 to 3.5 GHz. In some embodiments, the hexaferrite composition has a magnetic loss tangent tanδ µ in the range of 0.1 to 1.0 over a frequency range of 0.1 to 1.0 GHz.
[0024] In some embodiments, the dielectric loss tangent tan δ εfrom less than 0.01 to 0.16, at frequencies less than about 1.0 GHz, and in other embodiments, at frequencies less than about 10.0 GHz. At frequencies less than about 0.4 GHz, the dielectric loss tangent is less than 0.09 in some embodiments, less than 0.12 in other embodiments, or less than 0.02 in still other embodiments. At frequencies less than about 1.0 GHz, the dielectric loss tangent is less than 0.10 in some embodiments, less than 0.08 in other embodiments, or less than 0.02 in still other embodiments. At frequencies less than about 3.0 GHz, the dielectric loss tangent is less than 0.07 in some embodiments.
[0025] In some embodiments, the hexaferrite composition has a dielectric loss tangent tanδ εof less than 0.02 at a frequency of 0.1 to 0.8 GHz. In some embodiments, the hexaferrite composition has a dielectric loss tangent tanδ ε of less than 0.16 at a frequency of 0.1 to 1.0 GHz.
[0026] The hexaferrite composition exhibits a low dielectric loss factor and magnetic loss factor within the high frequency range. In some embodiments, the hexaferrite composition exhibits a dielectric loss factor tan δ at a frequency of 0.8 GHz. ε / ε' of less than 0.001 and a magnetic loss factor tan δ µ / µ' of less than 0.03.
[0027] The hexaferrite composition can be prepared in any suitable manner. In one embodiment, the hexaferrite composition can be prepared by providing hexaferrite phase precursor compounds. Suitable precursor compounds can be, for example, oxides or carbonates of Mo, Ba and / or Sr, Co, and Fe. The precursor compounds are ground and blended to small particle sizes and then calcined in air to form a material comprising a Z-type hexaferrite phase. Milling the materials to a small size and long-term mixing results in smaller particle sizes, which can assist in lowering the temperatures and energies required to form the hexaferrite phases. The particle sizes can be reduced by successive rounds of milling, blending, and sintering, with screening after each step to ensure particle size reduction.The time required to reduce the particle size to a suitable range is a function of the powder-to-sphere mass ratio, the sphere and cylinder material, and the solvent used (if any). Suitable particle sizes range from 0.1 µm to 100 µm, with tens of micrometers being typical for the effective diameter. The resulting material after calcination can be milled to form a powder mixture, which can be pressed and sintered to form a dense solid body. The resulting material can be milled and annealed in a stream of oxygen gas to improve the phase oxygen stoichiometry, which would also improve the magnetic properties.
[0028] In some embodiments, a mixture of MoO2, BaCO3, SrCO3, Co3O4, and Fe2O3 is provided. The amounts can be mixed proportionally, determined by the desired nominal stoichiometry. In some embodiments, the amounts can be 0 to 0.96 wt% MoO2, 22.10 to 22.18 wt% BaCO3, 6.02 to 6.59 wt% Co3O4, and 70.35 to 71.8 wt% Fe2O3.
[0029] The materials can be mixed with a solvent and milled in a ball mill or other suitable mixing device, such as, without limitation, a roller blender, a vibratory mill, or a planetary mill, using a variety of spherical and cylindrical materials. In one embodiment, the materials are mixed in an agate jar at 400 rpm for 3 hours using a 4-station planetary ball mill. The materials are mixed in nominal ratios of oxides and carbonates to mixed balls to solvent: 1:(1-2):(1-2) wt%. The solvent can be, for example, and without limitation, water, including distilled water or deionized water, toluene, or an alcohol, including, for example, and without limitation, ethyl alcohol or a reagent-grade alcohol (which in some embodiments is 90% ethyl alcohol, 5% methyl alcohol, and 5% isopropyl alcohol).In some embodiments, no solvent needs to be used.
[0030] The resulting mixture can be dried at 200 to 300 °C for 3 to 10 hours in a forced-air oven and then pressed into a suitable shape to increase its density. In one embodiment, the material can be uniaxially compressed into a 1-in. disk at 0.1 to 0.3 t / cm 2 pressed in a set of dies. Higher pressures can be used depending on the press used. The pressure can be adjusted to achieve a suitable densification after sintering. Typically, a densification of over 90% after sintering is suitable.
[0031] The materials can be calcined in air to form the Z-type hexaferrite phase at 1000 to 1300 °C. In some embodiments, the following calcination temperature profile can be used: 1) Start at an ambient temperature (e.g. ~20°C), ramp up to 1200 °C ± 100 °C over a period of 240 minutes ± 60 minutes; 2) Remaining at 1200 °C ± 100 °C for a period of 300 minutes ± 60 minutes; 3) Allow the furnace to cool down to ambient temperature, for example over a period of 240 minutes ± 60 minutes.
[0032] The resulting calcined ferrites can be crushed and sieved through a No. 40 screen to separate the particles by size. The smaller particles and a solvent (e.g., alcohol or water, as previously described) can be milled, for example, in a ball mill, and dried. The resulting powder mixture can be compressed into a compact with the addition of a binder to help maintain the compact shape. In some embodiments, polyvinyl alcohol can be used as a binder in the range of 8 to 12 wt.% of the powder mixture. Other suitable binders include methylcellulose, polyethylene glycol, or poly(alkylene carbonate). The binder leaches off during subsequent sintering.
[0033] The compact may be sintered in a furnace, such as a tube furnace, for a suitable time at a suitable temperature. In some embodiments, the compact may be sintered at 1200 to 1280°C. In some embodiments, the compact may be sintered for 4 to 20 hours. The compact may be sintered in an oxygen atmosphere in a tube furnace to assist in reducing dielectric loss. For example, O2 gas may flow throughout the process at a rate of 0.5 to 2.0 l / min. In some embodiments, the following sintering temperature profile may be employed: 1) Start at an ambient temperature (e.g. -20 °C), ramp up to 800 °C ± 100 °C over a period of 180 minutes ± 60 minutes; 2) Ramp-up to 1200 °C ± 100 °C over a period of 180 minutes ± 60 minutes; 3) Remain at 1200 °C ± 100 °C for a period of 240 minutes ± 60 minutes; 4) Allow the furnace to cool down to ambient temperature, for example over a period of 480 minutes ± 60 minutes.
[0034] The sintered hexaferrites can be crushed, sieved through a No. 100 sieve, ground with a solvent (as described above), and dried. The resulting powder can be annealed in an O2 gas stream. In some embodiments, the resulting powder can be annealed at 800 to 1000°C. In some embodiments, the following annealing temperature profile can be used with an O2 gas flow at 0.2 to 2.0 l / min throughout the annealing process: 1) Start at an ambient temperature (e.g. -20 °C), ramp up to 400 °C ± 100 °C over a period of 80 minutes ± 10 minutes; 2) Ramp-up to 900 °C ± 100 °C over a period of 200 minutes ± 100 minutes; 3) Remain at 900 °C ± 100 °C for a period of 240 minutes ± 100 minutes; 4) Allow the furnace to cool down to ambient temperature, for example over a period of 360 minutes ± 100 minutes.
[0035] In other embodiments, the powder mixture may be formed prior to the sintering steps described herein by mechanisms such as tape casting or additive manufacturing.
[0036] The permeability, permittivity, and resonant frequency of the Co2Z hexaferrites described herein can be adjusted by substitution with Mo, Sr, and Ba ions. These Mo-doped Co2Z hexaferrites are therefore desirable candidates for magnetodielectric microwave substrate materials operating at 0.3–10 GHz. The compositions can exhibit high permeability (μ' > 8) over a high operating frequency (0.1 to 1 GHz and greater). Equal or substantially equal values of permeability and permittivity can be achieved, for both μ' and ε', of greater than 7 or, in some embodiments, greater than 8 at f = 0.8 GHz, resulting in matching impedance. The compositions can exhibit low magnetic and dielectric loss factors, for example, of tanδ µ / µ' = 0.03 and tanδ ε / ε' = 0.001, at f = 0.8 GHz. The material costs are low compared to, for example, Ir-doped hexaferrites.
[0037] The hexaferrite composition can be used for a variety of devices that operate within the radio frequency range, such as an ultra-high frequency or microwave antenna, a filter, a coil, a circulator, or a phase shifter. In some embodiments, the device can operate at frequencies greater than 0.1 GHz, in some embodiments at frequencies greater than 0.3 GHz, and in some embodiments at frequencies greater than 0.5 GHz. In some embodiments, the device can operate at frequencies up to 1.0 GHz, up to 1.5 GHz, up to 3.0 GHz, or up to 10.0 GHz. For example, in some embodiments, the device can operate over a frequency range of 0.1 to 1.5 GHz. In some embodiments, the device can operate over a frequency range of 0.3 to 1.0 GHz. In some embodiments, the device may be operable over a frequency range of 0.3 to 0.5 GHz.In some embodiments, the device may be operable over a frequency range of 0.5 to 1.0 GHz.
[0038] In some devices, two or more hexaferrite compositions may be used, with the hexaferrite compositions having different cutoff frequencies to provide operation over a wider frequency range. For example, an antenna device may use a Mo-doped BaCo2Z hexaferrite that is functional over a lower frequency range, such as 0.1 to 0.5 GHz, and a Mo-doped SrCo2Z hexaferrite that is functional over a higher frequency range, such as greater than 0.5 to 1.5 GHz.
[0039] Such devices can be used in commercial and military applications, weather radar, scientific communications, mobile and wireless communications, vehicles, aircraft communications, space communications, satellite communications, and surveillance.
[0040] The hexaferrite composition can be used in spintronic applications, such as giant magnetoresistance (GMR) devices and giant tunneling magnetoresistance (TMR) devices, which are used in disk drive read heads and other data storage and memory devices, as well as in magnetic sensors. Other spintronic applications include semiconductor devices, such as spin transistors and spin light-emitting diodes. Example 1:
[0041] Polycrystalline Co2Z hexaferrites with the composition Ba3Co 2+x Mon x Fe 24-2x O 41, where x = 0, 0.01, 0.02, 0.05, 0.08, 0.10, 0.12, 0.15, and 0.20, were prepared using a two-step ceramic process. Starting materials of BaCO3, MoO2, Co3O4, and Fe2O3 were calcined in air at 1000 °C for 6 hours and then crushed and ball-milled. The mixture, comprising 90 vol.% fine ferrite powder and 10 vol.% polyvinyl alcohol (PVA) binder, was pressed into a toroid with an outer diameter of 7 mm, an inner diameter of 3 mm, and a width of approximately 2 mm. This sample size is well suited for microwave measurements. Since an oxygen atmosphere can help reduce dielectric loss, the hexaferrite samples were sintered in oxygen at 1200 to 1280 °C for 4 to 20 hours as the final process step. (An annealing step, typically used to develop oxygen stoichiometry, was not used due to the long 20-hour heat treatment step.)) Eight samples, listed with a corresponding identification code ZM0 to ZM8, correspond to the inclusion of Mo in the Co2Z hexaferrites, as listed below. Table 2: Sample codes of Ba3Co2+xMoxFe24-2xO41 hexaferrites Mo(x) 0 0,01 0,02 0,05 0,08 0,10 0,12 0,15 0,20 Code ZM0 ZM1 ZM2 ZM3 ZM4 ZM5 ZM6 ZM7 ZM8
[0042] The crystallographic structure was determined by X-ray diffraction (XRD, Philips X'pert PRO) measurements at room temperature in a θ-2θ geometry using CuKα radiation. The complex permittivity and permeability spectra were measured over a frequency range of 0.3–10 GHz using an Agilent E864A 45 MHz–50 GHz PNA series vector network analyzer (VNA) with a 7 mm HP-85050C precision air line and an Agilent impedance analyzer (IA) for a toroidal sample at f = 0.05–1.0 GHz. The morphology was observed by scanning electron microscopy (SEM). Results 1. Mo dependence of the permeability spectra for Co2Z hexaferrites
[0043] Changes in real permeability with varying Mo (Mo 4 + -ion) content (x) of Co2Z hexaferrite are in Fig. 1A. This figure shows that with increasing molybdenum content (x > 0.10), the permeability decreases at low frequencies. The cutoff frequency (resonance frequency) increases above 1.0 GHz when x increases above 0.10, as shown in Fig. 1B shown.
[0044] The magnetic loss tangent is less than 0.1 at f < 0.4 GHz and is equal to 0.5 at f = 1.0 GHz for x = 0.12, as in Fig. 2A and Fig. 2B. In particular, tan δµ is less than 0.3 at f = 0.8 GHz for x = 0.12. The results show a high permeability of 8.5 to 10.
[0045] Fig. 3A and Fig. Figure 3B plots the permeability and magnetic loss tangent as a function of molybdenum content at a low frequency (0.3 GHz) and a higher frequency (0.8 GHz). Note that the real permeability at the lower frequency of f = 0.3 GHz shows a dip when the molybdenum content ranges from x = 0.08 to 0.15, corresponding to a minimum in magnetic loss. In contrast, for x = 0.08 to 0.15, the real permeability increases to a peak at f = 0.8 GHz. This increase in permeability also leads to a significant decrease in magnetic loss, corresponding to that observed at the lower frequency f = 0.3 GHz. Thus, the magnetic loss shows extremely low values when x ranges from 0.08 to 0.15, both at the lower and higher frequencies. 2. Mo dependence of permittivity spectra on frequency for Co2Z hexaferrites
[0046] The real permittivity can be tuned with molybdenum content over a frequency range of 0.1 to 10.0 GHz to range from ε' = -7.5 to > 12, as shown in Fig. 4A. Sample ZM6, with the lowest magnetic loss, shows a small permittivity of ~8, as shown in Fig. 4B shown.
[0047] For samples ZM5 (x = 0.10) and ZM6 (x = 0.12), the dielectric loss tangent remained very low, <0.02, over a wide frequency range from f = 0.1 to 10.0 GHz, as shown in Fig. 5A. In particular, the dielectric loss tangent for samples ZM5 and ZM6 was below 0.01 for frequencies below 1.0 GHz, as shown in Fig. 5B shown.
[0048] For x > 0.05, the dielectric loss tangent decreases with the molybdenum content at f = 0.8 GHz, as shown in Fig. 6. At x = 0.10 to 0.12 the lowest dielectric loss was measured, tanδ ε : < 0.01 at f = 0.8. 3. Samples with high permeability and low magnetic and dielectric losses at f = 0.1-1 GHz
[0049] The frequency dependence of the permeability, permittivity and magnetic and dielectric loss tangent of samples ZM5 and ZM6 is shown in Fig. 7A and Fig. 7B. At f < 0.5 GHz, the magnetic loss tangent is less than 0.15, while the permeability is as high as 10 to 11. The lowest magnetic loss tangent is less than 0.27, at f = 0.8 GHz, for sample ZM6.
[0050] Matching impedances can be obtained with respect to equal or substantially equal permeability and permittivity (ε' = 9 (or 8), µ' = 10). 4. Measurement of magnetic spectra by impedance analyzer
[0051] The magnetic spectra of samples ZM5 and ZM6 were measured by the impedance analyzer over a frequency range of 0.1 to 1 GHz, as shown in Fig. 8. The results are in good agreement with those measured by the VNA, which indicates a permeability of 8 to 11 and a magnetic loss tangent of less than 0.3 at 0.8 GHz.
[0052] Table 3 lists the main parameters measured by VNA and IA and indicates a measurement error of less than 1% at 0.8 GHz. Table 3: µ' and tan δµ of samples ZM5 and ZM6 at different frequencies Probe Messung µ' tan δ µ ZM5 IA 10,2 0,37 VNA 10,3 0,36 ZM6 IA 8,8 0,30 VNA 9,2 0,29 5. SEM morphology
[0053] Fig. Figure 9 shows the SEM morphology of the Mo-doped Co2Z hexaferrite, indicating an isotropic grain orientation and a uniform distribution of grains that appear to be platelets with a high aspect ratio of 8-5:1. The average grain size is estimated to be around 60 to 80 µm along the long axes. 6. Comparison of permeability, permittivity, loss tangent and grain size with existing magnetodielectric materials
[0054] Table 4 shows a comparison of ε', µ', tan δ ε and tan δ µ for Mo-doped and Ir-doped Co2Z hexaferrites at 0.8 GHz with existing Ir-doped Co2Z hexaferrites. The Mo-doped Co2Z hexaferrites are samples ZM5 and ZM6.
[0055] The Mo-doped Co2Z hexaferrites exhibit a 25 to 37% improved permeability compared to that of Ir-doped Co2Z hexaferrites. The Mo-doped Co2Z hexaferrites also exhibit a much lower dielectric loss tangent (<0.01), whereas Ir-doped Co2Z hexaferrite exhibits a dielectric loss tangent of 0.07 at 0.8 GHz. The Mo-doped Co2Z hexaferrites exhibit a magnetic loss tangent of 0.36, which is close to that of Ir-doped Co2Z hexaferrite, 0.25 to 0.30 at 0.8 GHz. Table 4: Comparison of ε', µ', tan δε and tan δµ for Mo-doped and Ir-doped Co2Z hexaferrites at 0.8 GHz 0.8 GHz µ' tan δ µ ε' tan δ ε Korngröße (µm) Mo_Zm5 10,3 0,36 9,36 0,007-0,01 60-80 Mo_Zm6 9,2-10,2 0,27-0,29 8,64 0,04 60-80 It_Co2Z 7,44 0,25-0,30 8,14 0,07 200
[0056] In brief, polycrystalline hexaferrite compositions of nominal composition Ba3Co 2+x Mon x Fe 24-2x O 41 , where x = 0 to 0.20, produced by ceramic processes. The results show that Mo-doped Co2Z polycrystalline hexaferrites exhibit permeabilities, permittivities, and magnetic and dielectric losses that are better than those of existing Ir-doped Co2Z hexaferrites over a wide frequency range of 0.1 to 5.0 GHz. The measured dielectric and magnetic microwave properties showed that the loss tan δ ε and loss tan δ µWith the addition of molybdenum, with x = 0.10 to 0.15, the permeability was reduced by 75% and 60% at 0.8 GHz, respectively, whereas the permeability at 0.8 GHz was increased to 10.1, an increase of 25% compared to the Ir-doped Co2Z hexaferrites. In addition, the Mo-doped Co2Z hexaferrites also show essentially the same value of real permittivity and permeability (8 to 9) over the frequency range from 0.1 to 1.0 GHz, in order to match the characteristic impedance to the vacuum impedance. Among the above-mentioned materials, the Mo-doped Co2Z hexaferrites not only lead to the lowest loss factors (tan δ ε / ε' < 0.00075 and tan δ µ / µ' < 0.029), but also have low material costs. The material costs of Mo-doped Co2Z hexaferrite can be one-third of those of Ir-doped Co2Z hexaferrite. These properties make these hexaferrites suitable for applications in ultra-high frequency (UHF) microwave devices, such as miniature antennas. Example 2
[0057] Polycrystalline hexaferrites with a non-stoichiometric composition with the formula (Ba z Sr (3-z) )CO (2+x) Mon x Fe (y-2x) O 41 were prepared. Table 5 lists the non-stoichiometric formulas for several samples that were prepared and tested. Table 5: Formula structure (non-stoichiometric formula) Code Formel Mo-Gehalt, x ZSF1 Ba3CO (2+x) Want (21.6-2x) Know x SHE 41 x = 0,12 ZSF2 Ba3CO (2+x) Want (22.4-2x) Know x SHE 41 x=0,12 ZSF3 Ba 1.5 3Sr 1.53 Co (2+x) Feb (21.6-2x) Mo x O 41 x = 0,12 ZSF4 Ba 1.5 Sr 1.5 Co (2+x) Feb (22.4-2x) Mo x O 41 x = 0,12
[0058] The manufacturing process begins with the following raw materials and their purities: BaCO3 (99.95%), SrCO3 (99.95%), Co3O4 (99.7%), MoO2 (99%), and Fe2O3 (99.95%). The ratios were chosen to correspond to the desired nominal compositions. For example, the hexaferrite phase precursor compounds can include 0 to 0.96 wt% MoO2, 22.10–22.18 wt% BaCO3, 6.02–6.59 wt% Co3O4, and 70.35–71.8 wt% Fe2O3. The materials were mixed with analytical grade alcohol as a solvent and milled in an agate jar and ball blender at 400 rpm for 3 to 10 hours using a 4-station planetary ball mill. The mixture was dried at 200 to 300 °C for 3 to 10 hours in a circulating air oven and formed into a 1-in. disk in a die set at 0.1 to 0.3 T / cm 2The disc was calcined in air to form the Z-type hexaferrite phase according to the following temperature profile: 1) heating to 1200 °C for 240 minutes; 2) holding at 1200 °C for 300 minutes; 3) cooling to 20 °C for 240 minutes.
[0059] The material was then crushed and sieved through a #40 sieve. The smaller particles that passed through the sieve were milled with an analytical grade alcohol solvent for 4 to 20 hours at 400 rpm in an agate jar using a 4-station planetary ball mill. The mixture was dried at 200 to 300 °C for 3 to 10 hours in a forced-air oven and dried at 0.5 to 2.0 t / cm 2pressed into a 1-inch disk. The disk was sintered according to the following temperature profile: 1) Heating for 180 minutes to 800 °C with O2 gas at a flow rate of 0.7 l / min; 2) Heating for 180 minutes to 1200 °C; 3) Holding for 240 minutes at 1200 °C; 4) Cooling for 480 minutes to 20 °C in the O2 gas flow.
[0060] The sintered material was then crushed and sieved through a #100 sieve. The crushed material that passed the sieve was milled with a reagent-grade alcohol solvent for 4 to 20 hours at 400 rpm in an agate jar using a 4-station planetary ball mill. The resulting powder was dried for 3 to 10 hours at 200 to 300 °C in a forced-air oven. The powder was annealed according to the following temperature profile, with O2 gas flowing the entire time: 1) Heating to 400 °C for 80 minutes; 2) Heating to 900 °C for 200 minutes; 3) Holding at 900 °C for 240 minutes; 4) Cooling to 20 °C for 360 minutes.
[0061] Fig. Figure 10 illustrates the magnetic permeability vs. frequency for this ZSF series of hexaferrite samples. The permeability µ' was around 8 for SrBa-Co2Z hexaferrite (samples ZSF3 and ZSF4) and around 7 for Ba-Co2Z hexaferrite (samples ZSF1 and ZSF2), respectively, at frequencies below 1.0 GHz. The inclusion of Sr significantly improved the permeability. The magnetic loss tangent remained low, ranging from 0.03 to 0.1, over a frequency range of 0.1 to 1.0 GHz. The Mo-SrBa hexaferrites (ZSF3 and ZSF4) had a high cutoff frequency (fr) and permeability.
[0062] Fig. Figure 11A illustrates the magnetic permeability and loss vs. frequency for sample ZSF1. Fig. Figure 11B is an SEM image of sample ZSF1. The permeability was around 7, while the magnetic loss tangent remained low at a value of 0.01 to 0.10 up to a frequency of 1.0 GHz.
[0063] Fig. Figure 12A illustrates the magnetic permeability and loss vs. frequency for sample ZSF2. Fig. Figure 12B is an SEM image of sample ZSF2. The permeability was around 7.5, while the magnetic loss tangent remained low at a value of 0.01 to 0.09 up to a frequency of 1.0 GHz.
[0064] Fig. Figure 13A illustrates the magnetic permeability and loss vs. frequency for sample ZSF3. Fig. Figure 13B is an SEM image of sample ZSF3. The permeability was around 8, while the magnetic loss tangent remained low at a value of 0.03 to 0.09 up to a frequency of 1.0 GHz.
[0065] Fig. Figure 14A illustrates the magnetic permeability and loss vs. frequency for sample ZSF4. The permeability was around 8, while the magnetic loss tangent remained low, ranging from 0.03 to 0.09, up to a frequency of 1.0 GHz.
[0066] Fig. Figure 15 illustrates the dielectric spectra at 0.1 to 10.0 GHz for samples ZSF1 to ZSF4. The dielectric constant range was 6.5 to 9.0, while the dielectric loss tangent was 0.001 to 0.01 over a frequency range of 0.1 to 10.0 GHz for all samples in the ZSF series.
[0067] Table 6 presents a summary of the results of real permittivity, real permeability, loss tangent, tan δ ε , and loss tangent, tan δµ for the four samples at two different frequencies, 0.8 GHz and 1.0 GHz. Table 6: Summary of the samples of the ZSF series f (GHz) ε' tan δ ε µ' tan δµ f r (GHz) D (µm) ZSF1 0,8 7,24 0,0019 7,63 0,0795 2,10 3-5 (großkörnig: 15-20) 1,0 7,24 0,0025 8,10 0,11 ZSF2 0,8 6,60 0,0020 7,85 0,080 2,05 4-6 (großkörnig: 15-20) 1,0 6,60 0,00247 8,37 0,118 ZSF3 0,8 8,25 0,0021 8,61 0,069 2,37 6-8 (großkörnig: 15+) 1,0 8,25 0,0027 9,00 0,091 ZSF4 0,8 8,67 0,0023 8,51 0,071 2,40 6 (großkörnig: 15-20), einheitlich 1,0 8,67 0,0028 8,88 0,091
[0068] The best sample was ZSF4. It showed high permeability, ε'= 8.67, and low loss tangent, tan δ µ = 0.091, at 1.0 GHz, and a high cutoff frequency, fr = 2.40 GHz. Example 3
[0069] Polycrystalline Co2Z hexaferrites with the composition Sr3Co 2+xMon x Fe 24-2x O 41 , where x=0, 0.02, 0.05, 0.08, 0.10, 0.12, 0.15 and 0.20, were prepared by the two-step ceramic process described in Example 1 above using SrCO3, MoO2, Co3O4, and Fe2O3 as starting materials. Results 1. Magnetic permeability spectra and magnetic loss
[0070] The permeability spectra were measured at frequencies from 0.1 to 10.0 GHz. The permeability shows a decrease of 3.8 to 3.3 with a Mo content at low frequency (0.1 GHz), except for a Mo content of x = 0.10, as shown in Fig. 16. The Mo content reveals a shift of the loss tangent peak to higher frequencies above 5.0 GHz, as shown in Fig. 17. The Mo content x = 0.10 results in a minimal loss tangent in the frequency range from 0.4 to 1.5 GHz, also in Fig. 17. This means that the loss tangent for x = 0.20 is ~0.1 at 0.4 GHz and 0.4 at 1.5 GHz, which is the lowest loss among the Mo-doped SrCo2Z ferrites.
[0071] Fig. Figure 18 illustrates the permeability and magnetic loss tangent results for the Mo-doped SrCo2Z hexaferrites measured at 1.0 GHz. It can be seen that the sample with a Mo content of x = 0.10 exhibits a 15% increase in permeability and a 15% decrease in magnetic loss. These results are consistent with those measured for BaCo2Z hexaferrites. It is found that an optimized Mo concentration in SrCo2Z hexaferrite is comparable to that of BaCo2Z hexaferrites. 2. Permittivity spectra and dielectric loss
[0072] Basically, the permittivity of SrCo2Z hexaferrites is proportional to the Mo content and decreases slightly for x = 0.02, as shown in Fig. 19. The dielectric loss tangent increases with increasing Mo content (x = 0 to 0.20) from 0.03 to 0.08, as shown in Fig. 20 can be seen.
[0073] Fig. Figure 21 describes the permittivity and dielectric loss measured at 1.0 GHz and shows a dielectric loss dip at x = 0.10. 3. Magnetic and dielectric loss
[0074] The lowest magnetic and dielectric loss in Mo-doped SrCo2Z hexaferrites was observed at a Mo content of x = 0.10. At this Mo content, at f = 1.0 GHz, the following applies: μ'=3.7 tanδμ=0.24 ε'=14.2; and tanδε=0.03.
[0075] In short, MoO2 can be usefully used to reduce the magnetic loss in SrCo2Z hexaferrites.
[0076] As used herein, "consisting essentially of" permits the inclusion of materials or steps that do not materially affect the basic and novel features of the claim. Any rendering herein of the term "comprising" may be replaced, particularly in a description of the components of a composition or in a description of elements of a device, with "consisting essentially of" or "consisting of."
[0077] It will be appreciated that the various features of the embodiments described herein may be combined in a variety of ways. For example, a feature described in connection with one embodiment may be included in another embodiment even if it is not explicitly described in that embodiment.
Claims
[1] A hexaferrite composition comprising iron, cobalt, one or both of barium and strontium, and molybdenum, wherein the ferrite composition is a Z-type hexaferrite phase having the formula (Ba z Sr (3-z) )Co (2+x) Mon x Fe (y-2x) O 41 includes where x = 0.01 to 0.20; y = 20 to 24; and z = 0 to 3. [2] The hexaferrite composition according to claim 1, wherein x = 0.08 to 0.
15. [3] The hexaferrite composition according to claim 1, wherein x = 0.10 to 0.
12. [4] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a real permeability of at least 3.0 over a frequency range of 0.1 to 3.0 GHz, in particular 0.1 to 1.0 GHz. [5] The hexaferrite composition of claim 1, wherein the hexaferrite composition has a real permeability of at least 7.0 over a frequency range of 0.1 to 3.0 GHz. [6] The hexaferrite composition of claim 1, wherein the hexaferrite composition has a real permeability in the range of 7.0 to 12.0 over a frequency range of 0.1 to 3.0 GHz. [7] The hexaferrite composition of claim 1, wherein z = 1.2 to 3.0, and the hexaferrite composition has a real permeability in the range of 8.0 to 12.0 over a frequency range of 0.1 GHz to at least 1.0 GHz. [8] The hexaferrite composition of claim 1, wherein z = 0 to 0.5, and the hexaferrite composition has a real permeability in the range of 2.0 to 4.0 over a frequency range of 0.1 GHz to about 3.0 GHz. [9] The hexaferrite composition of claim 1, wherein the hexaferrite composition has a real permittivity of at least 6.0 over a frequency range of 0.1 to 3.0 GHz. [10] The hexaferrite composition of claim 1, wherein the hexaferrite composition has a real permittivity of at least 8.0 over a frequency range of 0.1 to 3.0 GHz. [11] The hexaferrite composition of claim 1, wherein the hexaferrite composition has a real permittivity in the range of 6.0 to 18.0 over a frequency range of 0.1 to 10.0 GHz. [12] The hexaferrite composition according to claim 1, wherein a real permittivity of the hexaferrite composition is equal to a real permeability of the hexaferrite composition within 10%. [13] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a characteristic impedance that matches an impedance of the vacuum within 3%. [14] The hexaferrite composition of claim 1, wherein the hexaferrite composition has a dielectric loss tangent, tanδ εof less than 0.02 at a frequency of 0.1 to 0.8 GHz. [15] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a dielectric loss tangent, tanδ ε , of less than 0.16 at a frequency of 0.1 to 1.0 GHz. [16] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a magnetic loss tangent tanδ µ of 0.1 at 0.4 GHz. [17] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a magnetic loss tangent tanδ µ of less than 0.3 at a frequency of 0.1 to 0.8 GHz. [18] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a magnetic loss tangent tanδ µ of less than 0.95 at a frequency of 0.1 to 3.5 GHz. [19] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a magnetic loss tangent, tanδ µ , in the range of 0.1 to 1.0 over a frequency range of 0.1 to 1.0 GHz. [20] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a dielectric loss factor tanδ ε / ε' of less than 0.001 at a frequency of 0.8 GHz. [21] The hexaferrite composition according to claim 1, wherein the hexaferrite composition has a magnetic loss factor tanδ µ / µ' of less than 0.03 at a frequency of 0.8 GHz. [22] An article comprising the hexaferrite composition of claim 1, wherein the article is an antenna, a filter, a coil, a circulator, or a phase shifter. [23] The article of claim 22, wherein the article is a filter, a coil, a circulator or a phase shifter. [24] The article of claim 22, wherein the article is a microwave antenna. [25] The article of claim 24, wherein the article is an antenna operable at a frequency equal to or greater than 0.1 GHz. [26] The article of claim 24, wherein the article is an antenna operable at a frequency equal to or greater than 0.3 GHz. [27] The article of claim 24, wherein the article is an antenna operable at 0.1 to 1.5 GHz. [28] The article of claim 24, wherein the article is an antenna operable at 0.3 to 1.0 GHz. [29] The article of claim 22, further comprising a second hexaferrite composition comprising a Z-type hexaferrite phase having the formula (Ba z Sr (3-z) )Co (2+x) Mon x Fe (y-2x) O 41 where x = 0.01 to 0.20; y = 20 to 24; and z = 0 to 3; and where the amount of Ba and the amount of Sr differ in the hexaferrite composition and the second hexaferrite composition. [30] The article of claim 29, wherein a cutoff frequency of the second hexaferrite composition is higher than a cutoff frequency of the hexaferrite composition. [31] The article of claim 29, wherein the hexaferrite composition has a real permeability in the range of 8.0 to 12.0 over a frequency range of 0.1 GHz to at least 1.0 GHz, and the second hexaferrite composition has a real permeability in the range of 2.0 to 4.0 over a frequency range of 0.1 GHz to about 3.0 GHz. [32] The article of claim 22, wherein the article is a giant magnetoresistance device or a giant tunneling magnetoresistance device. [33] A process for producing a hexaferrite composition comprising: (a) providing hexaferrite phase precursor compounds comprising Fe, Co, Mo and Ba and / or Sr, and (b) calcining the hexaferrite phase precursor compounds in air at 1000 to 1300 °C to form a material comprising a Z-type hexaferrite phase according to any one of claims 1-21. [34] The method of claim 33, wherein the hexaferrite phase precursor compounds comprise oxides of Fe, Ba, Co, and Mo. [35] The method of claim 33, wherein the hexaferrite phase precursor compounds comprise MoO2, BaCO3, Co3O4, and Fe2O3. [36] The method of claim 33, wherein the hexaferrite phase precursor compounds comprise from more than 0 to 0.96 wt% MoO2, from 22.10 to 22.18 wt% BaCO3, 6.02 to 6.59 wt% Co3O4, and 70.35 to 71.8 wt% Fe2O3. [37] The method of claim 33, further comprising: (c) comminuting the material formed in step (b) to form a powder mixture, and (d) Sintering the powder mixture. [38] A process according to claim 37, wherein the powder mixture is sintered at 1200 to 1280 °C. [39] A process according to claim 37, wherein the powder mixture is sintered for 4 to 20 hours. [40] A method according to claim 37, wherein the powder mixture is sintered in an oxygen atmosphere. [41] The method of claim 37, further comprising forming the powder mixture into a compact prior to step (d). [42] The method of claim 37, further comprising adding a binder to the powder mixture. [43] The method of claim 42, wherein the binder is selected from the group consisting of a polyvinyl alcohol, methylcellulose, polyethylene glycol, and poly(alkylene carbonate). [44] The method of claim 42, wherein the binder is polyvinyl alcohol comprising 8% to 12% by weight of the powder mixture. [45] The method of claim 37, further comprising: (e) comminuting the material formed in step (d) to form a powder mixture; and (f) annealing the powder mixture formed in step (e). [46] The method according to claim 45, wherein the powder mixture is tempered at 800 to 1000 °C. [47] The process according to claim 45, wherein the powder mixture is annealed for 9 to 20 hours.
Citation Information
Patent Citations
Finely divided magnetic hexaferrites with negative temperature-dependent coercivity and their use
DE3907220A1
Magnetic powder for magnetic recording and magnetic recording medium containing the same
US5494749A