Bond wire for semiconductor device

A Cu alloy bonding wire with a Pd cap layer and specific elements addresses reliability and bondability issues in high temperature and humidity environments by reducing intermetallic compound formation and strain hardening, enhancing performance in vehicle components.

DE112016002703B4Active Publication Date: 2024-12-05NIPPON MICROMETAL CORPORATION +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
DE112016002703
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-07-22
Filing Date
2016-06-14
Publication Date
2024-12-05
Estimated Expiration
2036-06-14

AI Technical Summary

Technical Problem

The existing bonding wires for semiconductor components, particularly those using copper alloys, face challenges in maintaining bonding reliability and wedge bondability in high temperature and high humidity environments, such as those encountered in vehicle components, due to issues like oxidation, strain hardening, and intermetallic compound formation.

Method used

A bonding wire with a Cu alloy core material and a Pd cap layer, containing specific elements like Ni, Zn, Rh, In, Ir, and Pt, with a yield strength ratio of 1.1 to 1.6, and a Pd cap layer thickness of 0.015 to 0.150 µm, enhances bonding reliability and wedge bondability by reducing intermetallic compound formation and strain hardening.

Benefits of technology

The proposed bonding wire design significantly improves bonding reliability and wedge bondability in high temperature and high humidity conditions, extending the life of the ball bonding part and maintaining strong adhesion in harsh environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Bond wire for a semiconductor device, wherein the bond wire has: a copper alloy core material; and a Pd cover layer formed on a surface of the Cu alloy core material, wherein the bond wire contains an element that ensures bond reliability in a high-temperature environment and has a yield strength ratio of 1.1 to 1.6 as defined by the following equation (1): Yield strength ratio = maximum yield strength / 0.2% offset yield strength. (1)
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The invention relates to a bonding wire for a semiconductor component, which is used to connect electrodes on a semiconductor component and wiring of a printed circuit board, e.g., external terminals. Background of the technology

[0002] Currently, thin wires with a wire diameter of approximately 15 to 50 µm are mainly used as bonding wires for semiconductor devices, which connect between electrodes on a semiconductor device and external terminals (hereinafter referred to as "bonding wires"). The bonding wire bonding method is generally an ultrasonic thermocompression bonding technique using a multi-purpose bonder, a capillary wire-passing bonding tool, and the like.A bonding process of a bonding wire is performed by heating and melting a wire tip by arc heat input to form a free air ball (FAB) by surface tension; crimping the ball portion to an electrode of the semiconductor device heated in a range of 150 to 300°C (hereinafter referred to as "ball bonding"); forming a loop; and finally crimping a wire portion to an electrode of the external lead (hereinafter referred to as "wedge bonding"). As bonding counterparts of the bonding wire, an electrode structure in which an alloy mainly containing Al is formed as a film on a Si substrate is used for the electrode on the semiconductor device, whereas an Ag- or Pd-plated electrode structure is used for the electrode of the external lead.

[0003] Au, which was primarily used as a bonding wire material, has been replaced by Cu, primarily for LSI applications. Given the recent increase in the popularity of electric vehicles and hybrid vehicles, the demand for replacing Au with Cu for automotive components is also increasing.

[0004] For a Cu bonding wire, a wire using high-purity copper (at least 99.99 mass%) has been proposed (e.g., JP S61-48543 A). Cu has the disadvantage of being more susceptible to oxidation than Au and has problems such as inferior bonding reliability, balling ability, and wedge bondability. As a method for preventing surface oxidation of a Cu bonding wire, a structure in which a surface of the Cu core material is coated with a metal such as Au, Ag, Pt, Pd, Ni, Co, Cr, and Ti has been proposed (JP 2005-167020 A). A structure in which a surface of the Cu core material is coated with Pd and a surface thereof is coated with Au, Ag, Cu, or an alloy thereof has also been proposed (JP 2012-36490 A).

[0005] In addition, JP 4 904 252 B2 discloses a bonding wire for a semiconductor device, which is used for connecting an electrode on a semiconductor element and for wiring a circuit. Summary of the inventionProblem to be solved by the invention

[0006] Automotive components require bond reliability in harsher environments with high temperatures and high humidity than general electronic components. Of particular importance is the bond lifetime of a ball bond, in which the ball portion of the wire is bonded to the electrode.

[0007] A representative evaluation method for evaluating the bonding reliability of a ball bond in a high-temperature and high-humidity environment includes a highly accelerated temperature and humidity stress test (HAST). In the HAST evaluation of the bonding reliability of a ball bond, the ball bond under evaluation is subjected to a high-temperature and high-humidity environment with a temperature of 130°C and a relative humidity of 85%. Afterward, the bonding life of the ball bond is evaluated by measuring changes in the resistance value of the bond or by measuring changes in the shear strength of the ball bond.

[0008] Furthermore, a high-temperature storage test (HTS) is used to evaluate the bonding reliability of the ball bonding part in a high-temperature environment of at least 170 °C. When evaluating the bonding reliability of a ball bonding part using HTS, a sample to be evaluated is exposed to a high-temperature environment, after which the bonding life of the ball bonding part is evaluated by measuring changes in the resistance value of the bonding part over time or by measuring changes in the shear strength of the ball bonding part over time.

[0009] As a result of the investigation, the invention found that the bonding wire containing an element that provides bonding reliability in a high temperature environment, such as Ni, Zn, Rh, In, Ir and Pt, shows improved bonding reliability of the ball bonding part in a high temperature environment of at least 130 °C compared to the wire not containing such an element.

[0010] On the other hand, the bonding wire undergoes extreme deformation during wedge bonding. If the wire undergoes strain hardening during deformation, the wire hardens after bonding, resulting in a decrease in the bonding strength of the wedge bond. In cases where the bonding wire contains the aforementioned element, the wire undergoes strain hardening depending on the amount of the aforementioned element when the bonding wire undergoes extreme deformation during wedge bonding. In some cases, the wire hardens after bonding, resulting in a decrease in the bonding strength of the wedge bond.

[0011] It is an object of the invention to provide a bonding wire for a semiconductor device comprising a Cu alloy core material and a Pd cap layer formed on a surface thereof, wherein the bonding wire for a semiconductor device can improve the bonding reliability of the ball bonding part at high temperature and the wedge bondability. Problem-solving path

[0012] As a result of intensive research to solve the above-described problem, it was discovered that both the bonding reliability of the ball bonding part at high temperatures and the wedge bondability can be improved by incorporating an element that ensures bonding reliability in a high-temperature environment into the bonding wire and by setting the yield strength ratio and strength ratio defined by equation (1) to 1.1 to 1.6. The present invention is based on these new findings. Yield strength ratio (strength ratio) = maximum yield strength (breaking strength) / 0.2% offset yield strength (0.2% yield strength)

[0013] The invention can therefore be summarized as follows. [1] A bonding wire for a semiconductor device, the bonding wire comprising: a Cu alloy core material; and a Pd cap layer formed on a surface of the Cu alloy core material, the bonding wire containing an element that provides bonding reliability in a high-temperature environment, and a yield strength ratio defined by the following equation (1) is 1.1 to 1.6: Yield strength ratio=maximum yield strength / 0.2−%−offset yield strength. [2] Bonding wire for a semiconductor device according to item [1], wherein a thickness of the Pd covering layer is 0.015 to 0.150 µm. [3] Bonding wire for a semiconductor device according to item [1] or [2], which further comprises an Au and Pd-containing alloy outer layer on the Pd cover layer. [4] Bonding wire for a semiconductor component according to item [3], wherein the thickness of the Au and Pd-containing alloy outer layer is at most 0.050 µm. [5] A bonding wire for a semiconductor device according to any one of [1] to [4], wherein the bonding wire contains at least one element selected from Ni, Zn, Rh, In, Ir and Pt, and a concentration of the at least one element in total is 0.011 to 2 mass% relative to the entire wire. [6] A bonding wire for a semiconductor device according to any one of [1] to [5], wherein the bonding wire contains one or more elements selected from Ga and Ge, and a total concentration of the elements is 0.011 to 1.5 mass% relative to the entire wire. [7] A bonding wire for a semiconductor device according to any one of [1] to [6], wherein the bonding wire contains at least one or more elements selected from As, Te, Sn, Sb, Bi and Se, a concentration of the elements in total is 0.1 to 100 ppm by mass relative to the entire wire, and Sn ≤ 10 ppm by mass; Sb ≤ 10 ppm by mass; and Bi ≤ 1 ppm by mass. [8] The bonding wire for a semiconductor device according to any one of [1] to [7], wherein the bonding wire further contains at least one element selected from B, P, Mg, Ca and La, and a concentration of each of the at least one element is 1 to 200 ppm by mass relative to the entire wire. [9] Bonding wire for a semiconductor device according to any one of items [1] to [8], wherein Cu is present on an outermost surface of the bonding wire. Effect of the invention

[0014] The invention can provide a bonding wire for a semiconductor device having a Cu alloy core material and a Pd cap layer formed on a surface of the Cu alloy core material, which can improve both the bonding reliability of the ball bonding part in a high temperature environment and the wedge bondability. Embodiment of the invention

[0015] The bonding wire for a semiconductor device of the present invention comprises a Cu alloy core material and a Pd cap layer formed on a surface of the Cu alloy core material. In the invention, the bonding wire contains an element that ensures bonding reliability in a high-temperature environment, and a yield strength ratio defined by the following equation (1) is 1.1 to 1.6: Yield strength ratio = maximum yield strength / 0.2% offset yield strength. (1) A mold resin (an epoxy resin) used to package a semiconductor device contains chlorine (Cl) in its molecular framework. In a high-temperature and high-humidity environment with 130 °C and 85% relative humidity as the HAST evaluation condition, Cl in the molecular framework hydrolyzes and dissolves as chloride ion (Cl -). In a case where a Cu bonding wire without a Pd cap layer is bonded to an Al electrode, when a Cu / Al bonding interface is exposed to high temperature, Cu and Al diffuse each other, and Cu9Al4 is ultimately formed as an intermetallic compound. Cu9Al4 is susceptible to corrosion by halogen and undergoes corrosion by Cl leached from the molding resin, resulting in deterioration of bonding reliability. In a case where a Cu wire has a Pd cap layer, a bonding interface between the Pd-coated Cu wire and the Al electrode has a Cu / Pd concentrated layer / Al structure, which reduces the formation of the Cu9Al4 intermetallic compound compared to the case of the Cu wire without a Pd cap layer. However, its bonding reliability is still insufficient in the high-temperature and high-humidity environment required for automotive components.

[0016] On the other hand, it is assumed that when an element is included that ensures bonding reliability in a high-temperature environment as in the invention, formation of a Cu9Al4 intermetallic compound in the bonding part tends to be further reduced.

[0017] In view of improving the bonding reliability of the ball bonding part in a high-temperature environment (especially the HTS performance at 175°C or higher), the concentration of the element that provides bonding reliability in a high-temperature environment relative to the entire wire is preferably at least 0.011 mass%, more preferably at least 0.030 mass%, even more preferably at least 0.050 mass%, at least 0.070 mass%, at least 0.090 mass%, at least 0.10 mass%, at least 0.15 mass%, or at least 0.20 mass%. The element that provides bonding reliability in a high-temperature environment will be described in more detail later.

[0018] As described above, the bonding wire undergoes extreme deformation during wedge bonding. If the wire undergoes strain hardening during deformation, the wire hardens after bonding, resulting in a decrease in the bonding strength of the wedge bond. To maintain favorable wedge bond strength, the yield strength ratio defined by the following equation (1) is preferably 1.6 or less, more preferably 1.55 or less, and even more preferably 1.50 or less, 1.45 or less, or 1.40 or less. With a view to achieving favorable wedge bondability, the yield strength ratio is preferably 1.1 or more.

[0019] Yield strength ratio = maximum yield strength / 0.2% offset yield strength. (1) Examples of ways to maintain the yield strength ratio of equation (1) in the preferred range may include: controlling (i) an orientational fraction of a crystal orientation <100> at an angle of not more than 15 degrees to a wire longitudinal direction at crystal orientations in the wire longitudinal direction when measuring crystal orientations on a cross-section of the core material in a direction perpendicular to a wire axis of the bonding wire (hereinafter also referred to as " <100> Orientation ratio") and (ii) an average crystal grain size in the cross-section of the core material in the direction perpendicular to the wire axis of the bonding wire (hereinafter also referred to as "average crystal grain size"). It has been determined that when the bonding wire is manufactured by a normal manufacturing process, the yield strength ratio is less than 1.1 or more than 1.6.On the other hand, it was found that by designing a manufacturing process as described below, the <100> -orientation proportion at an angle of at most 15 degrees to a wire longitudinal direction of crystal orientations in the wire longitudinal direction on a cross section of the core material in the direction perpendicular to the wire axis of the bonding wire can be at least 30% and the average crystal grain size in the cross section of the core material in the direction perpendicular to the wire axis of the bonding wire can be 0.9 to 1.5 µm, whereby the yield strength ratio of equation (1) can be 1.1 to 1.6.

[0020] Is the <100> -Orientation ratio of at least 30%, the strain hardening of the wire together with the deformation during wedge bonding is small, which means that the yield strength ratio can be as low as 1.6. However, if the average crystal grain size is below 0.9 µm, the 0.2% offset yield strength is high (poor ductility), which means that the yield strength ratio is below 1.1, which is bad for wedge bondability. If the average crystal grain size is above 1.5 µm, the <100> -Orientation ratio is estimated to be below 30%, and the 0.2% offset yield strength is low, which makes the yield strength ratio exceed 1.6 and the wedge bondability is poor.

[0021] Given the reduction in wire strain hardening associated with wedge bonding deformation, the <100> -orientation proportion preferably at least 30%, more preferably at least 35%, even more preferably at least 40% or at least 45%. Although the upper limit of the <100> -orientation share is not subject to any specific restriction, it may, for example, be no more than 90%, no more than 80%, no more than 70%, no more than 60%, no more than 50% or be less than 50% (e.g. no more than 49%).

[0022] In order to suppress the increase in the yield strength ratio, the average crystal grain size in the cross section of the core material in the direction perpendicular to the wire axis of the bonding wire is preferably at least 0.9 µm and at most 1.5 µm. The lower limit of the average crystal grain size in the cross section of the core material in the direction perpendicular to the wire axis of the bonding wire may be at least 1.0 µm, at least 1.1 µm, at least 1.3 µm, or more than 1.3 µm (e.g., at least 1.35 µm).

[0023] If the wire's crystal structure conditions are met, the content of the element that ensures bonding reliability in a high-temperature environment is excessively high in the wire, the yield strength ratio may increase. Considering the goal of achieving a yield strength ratio of 1.6 or less and reducing the hardening of the bonding wire to reduce deterioration of wedge bondability, the total concentration of the element that ensures bonding reliability in a high-temperature environment relative to the entire wire is preferably 2.0 mass% or less, 1.8 mass% or less, or 1.6 mass% or less.

[0024] Regarding the addition of the element that ensures bonding reliability in a high-temperature environment into the bonding wire, the effect of the invention can be achieved by using a method of adding the element into a Cu core material or a method of depositing the element onto a Cu core material or a wire surface to add the element therein. The addition amount of these elements is infinitely small, allowing for a variety of addition methods, and the effect can be achieved by any addition method as long as the element is included.

[0025] In the bonding wire of the invention, the thickness of the Pd cap layer is preferably at least 0.015 µm, more preferably at least 0.02 µm, and even more preferably at least 0.025 µm, at least 0.03 µm, at least 0.035 µm, at least 0.04 µm, at least 0.045 µm, or at least 0.05 µm, from the viewpoint of obtaining a favorable FAB shape and from the viewpoint of further improving the bonding reliability of the ball bonding part in the high-temperature and high-humidity environment required in components in vehicles. An excessively large thickness of the Pd capping layer impairs the FAB shape, and the thickness of the Pd capping layer is preferably at most 0.150 µm, and more preferably at most 0.140 µm, at most 0.130 µm, at most 0.120 µm, at most 0.110 µm, or at most 0.100 µm.

[0026] The following describes the determination of the Cu alloy core material and the Pd cap layer of the bonding wire. A boundary between the Cu alloy core material and the Pd cap layer was determined based on a Pd concentration. The boundary was set at a position where a Pd concentration was 50 at.%, and a region where a Pd concentration was 50 at.% or more was determined as the Pd cap layer, and a region where a Pd concentration was less than 50 at.% was determined as the Cu alloy core material. This is because when the Pd concentration in the Pd cap layer is 50 at.% or more, an improvement effect of characteristics can be expected due to the structure of the Pd cap layer. The Pd cap layer may include a Pd single-layer region and a region with concentration gradients of Pd and Cu in the wire depth direction.The reason why the concentration gradient region is formed in the Pd capping layer is that Pd and Cu atoms can diffuse due to heat treatment or similar processes during the manufacturing process. In the invention, the concentration gradient refers to a degree of concentration change in the depth direction of at least 10 mol% per 0.1 µm. Furthermore, the Pd capping layer may contain unavoidable impurities.

[0027] The bonding wire of the present invention may further comprise an Au and Pd-containing alloy outer layer on the surface of the Pd cap layer. With this configuration, the bonding wire of the invention can further improve bonding reliability and wedge bondability.

[0028] The definition of the Au and Pd-containing alloy outer layer of the bonding wire is now described. A boundary between the Au and Pd-containing alloy outer layer and the Pd cap layer was defined based on the Au concentration. The boundary was defined as a position where the Au concentration was 10 at.%, and an area where the Au concentration was 10 at.% or more was defined as the Au and Pd-containing alloy outer layer. An area where the Au concentration was less than 10 at.% was defined as the Pd cap layer. Also, in an area where the Pd concentration was 50 at.% or more, an area where Au was present at 10 at.% or more was defined as the Au and Pd-containing alloy outer layer. These definitions are made because, at an Au concentration in the above-mentioned range, an improvement effect on characteristics can be expected due to the structure of the Au outer layer.The Au and Pd-containing alloy outer layer is an Au-Pd alloy and contains a region with concentration gradients of Au and Pd along the wire depth direction. The reason why the concentration gradient region is formed in the Au and Pd-containing alloy outer layer is that Au and Pd atoms diffuse through heat treatment or similar processes during the manufacturing process. Furthermore, the Au and Pd-containing alloy outer layer may contain unavoidable impurities and Cu.

[0029] In the bonding wire of the invention, the Au- and Pd-containing alloy outer layer reacts with the Pd capping layer to improve the bonding strength between the Au- and Pd-containing alloy outer layer, the Pd capping layer, and the Cu alloy core material, and to prevent the Pd capping layer and the Au- and Pd-containing alloy outer layer from peeling off during wedge bonding. Thus, the bonding wire of the invention can further improve wedge bondability. In view of obtaining favorable wedge bondability, a thickness of the Au- and Pd-containing alloy outer layer is preferably at least 0.0005 µm, and more preferably at least 0.001 µm, at least 0.002 µm, or at least 0.003 µm. In view of reducing eccentricity to obtain a favorable FAB shape, a thickness of the Au and Pd-containing alloy outer layer is preferably at most 0.050 µm, and more preferably at most 0.045 µm, at most 0.040 µm, at most 0.035 µm, or at most 0.030 µm.The Au and Pd-containing alloy outer layer can be formed by a process similar to that for the Pd top layer.

[0030] In the invention, examples of the element that ensures bonding reliability in a high-temperature environment include an element from Group 9 of the Periodic Table of Elements (Co, Rh, Ir), an element from Group 10 of the Periodic Table of Elements (Ni, Pd, Pt), an element from Group 11 of the Periodic Table of Elements (Ag, Au, etc.), an element from Group 12 of the Periodic Table of Elements (Zn, etc.), an element from Group 13 of the Periodic Table of Elements (Al, Ga, In, etc.), an element from Group 14 of the Periodic Table of Elements (Ge, Sn, etc.), an element from Group 15 of the Periodic Table of Elements (P, As, Sb, Bi, etc.), an element from Group 16 of the Periodic Table of Elements (Se, Te, etc.), etc. These elements can be contained in the bonding wire singly or in combination of two or more of them.

[0031] In the invention, it is preferred that the bonding wire contains at least one element selected from Ni, Zn, Rh, In, Ir, and Pt as the element that ensures bonding reliability in a high-temperature environment. Preferably, a total concentration of these elements is 0.011 to 2 mass% relative to the entire wire.

[0032] A mold resin (an epoxy resin) used to package a semiconductor device contains a silane coupling agent. The silane coupling agent functions to improve the adhesion between the organic material (resin) and the inorganic material (silicon or metal), thereby improving the adhesion to a silicon substrate or metal. In cases where higher adhesion is required, such as semiconductors in vehicles that require reliability at elevated temperatures, a sulfur-containing silane coupling agent is added. Sulfur contained in the mold resin is released during use under conditions of 175°C or higher, such as between 175°C and 200°C. When the sulfur released at high temperatures of 175°C or higher comes into contact with Cu, Cu corrodes severely to form a sulfide (Cu2S) or an oxide (CuO).If Cu corrosion occurs in a semiconductor device that uses Cu bonding wire, bonding reliability, especially of a ball bonding part, is affected.

[0033] Bonding reliability in a high-temperature environment (especially HTS performance at 175°C or higher) can be improved by using a configuration in which the bonding wire contains at least one element selected from Ni, Zn, Rh, In, Ir, and Pt, and a total concentration of the at least one element is 0.011 to 2 mass% relative to the entire wire. With a view to improving the bonding reliability of the ball bonding part in a high-temperature environment (especially HTS performance at 175°C or higher), the total concentration of the element relative to the entire wire is preferably at least 0.011 mass%, more preferably at least 0.050 mass%, even more preferably at least 0.070 mass%, at least 0.090 mass%, at least 0.10 mass%, at least 0.15 mass%, or at least 0.20 mass%.The at least one element selected from Ni, Zn, Rh, In, Ir and Pt may also be referred to as “Element M” in the following description. A “ be designated.

[0034] In the invention, it is preferable that the bonding wire contains one or more elements selected from Ga and Ge as the element that ensures bonding reliability in a high-temperature environment, and a total concentration of the elements is 0.011 to 1.5 mass% relative to the entire wire. The wire may contain one or more elements selected from Ga and Ge instead of the element M. A or in combination with the element M A The one or more elements selected from Ga and Ge may also be referred to as “Element M” in the following description. B “ be designated.

[0035] During FAB formation of the ball bond, Ga and Ge in the wire also diffuse to the Pd cap layer. It is assumed that Ga and Ge present in the Pd-concentrated layer at the Cu / Al interface in the ball bond enhance the reducing effect on the mutual diffusion of Cu and Al through the Pd-concentrated layer, resulting in reduced formation of Cu9Al4, which is easily corroded in high-temperature and high-humidity environments. In addition, Ga and Ge present in the wire may directly inhibit the formation of Cu9Al4.

[0036] Furthermore, when a sphere was formed using a Pd-coated Cu bonding wire containing at least one element selected from Ga and Ge in a specific amount, and the resulting FAB was observed with a scanning electron microscope (SEM), numerous precipitates with a diameter approximately in the tens of nanometers range were observed on the surface of the FAB. Analysis of the precipitates by energy-dispersive X-ray spectroscopy (EDS) revealed that Ga and / or Ge were concentrated. Although a detailed mechanism is unclear, based on this situation, it is believed that these precipitates observed on the FAB appear at the bonding interface between the sphere and the electrode, thereby significantly improving the bonding reliability of a sphere bonded part in a high-temperature and high-humidity environment of 130 °C and 85% relative humidity.

[0037] Although it is preferable that Ga and Ge be present in the Cu alloy core material, a sufficient effect can be obtained even if they are contained in the Pd overcoat layer or an Au and Pd-containing alloy outer layer as described later. A method of adding Ga and Ge to the Cu alloy core material is straightforward in terms of precise concentration control and improves wire productivity and quality stability. Furthermore, a portion of Ga and Ge is also contained in the Pd overcoat layer or the alloy outer layer due to diffusion by heat treatment or the like, which improves the adhesion of interfaces between the layers, thereby further improving wire productivity.

[0038] With a view to obtaining a favorable FAB shape and in view of reduced hardening of the bonding wire in order to obtain favorable wedge bondability, the total Ga and Ge concentration relative to the entire wire is at most 1.5 mass%, preferably at most 1.4 mass%, and more preferably at most 1.3 mass% or at most 1.2 mass%.

[0039] In the invention, it is preferable that the bonding wire contains one or more elements selected from As, Te, Sn, Sb, Bi, and Se, and a total concentration of the elements is 0.1 to 100 ppm by mass relative to the entire wire, provided that Sn ≤ 10 ppm by mass, Sb ≤ 10 ppm by mass, and Bi ≤ 1 ppm by mass. The wire may contain one or more elements selected from As, Te, Sn, Sb, Bi, and Se instead of the element M. A and / or M B or in combination with the element M A and / or M BThe one or more elements selected from As, Te, Sn, Sb, Bi and Se may also be referred to as “Element M” in the following description. C “ be designated.

[0040] The invention is based on the assumption that when the bonding wire contains at least one or more elements selected from As, Te, Sn, Sb, Bi, and Se in a certain amount as the element that ensures bonding reliability in a high-temperature environment, the formation of a Cu9Al4 intermetallic compound in the bonding part tends to be further reduced. When these elements are contained in a certain amount, the interfacial tension between Cu of the core material and Pd of the cap layer decreases upon sphere formation, and the interfacial wettability improves, allowing Pd to be significantly more concentrated in a sphere bonding interface.Therefore, it can be estimated that a reducing effect on mutual diffusion of Cu and Al by the Pd-concentrated layer is further enhanced, and as a result, a formation amount of Cu9Al4 which is easily corroded by the action of Cl is reduced, and then the bonding reliability of the ball bonding part in a high temperature and high humidity environment is significantly improved.

[0041] The bonding reliability of the ball bonding part in a high-temperature and high-humidity environment required for in-vehicle components can be further improved when the bonding wire contains at least one element selected from As, Te, Sn, Sb, Bi, and Se, and a total concentration of the at least one element is 0.1 to 100 ppm by mass relative to the entire wire, provided that Sn ≤ 10 ppm by mass, Sb ≤ 10 ppm by mass, and Bi ≤ 1 ppm by mass. This is preferable because it can increase the bonding life of the ball bonding part in a high-temperature and high-humidity environment of 130°C and 85% relative humidity, which is required for in-vehicle components, to improve bonding reliability.The total concentration of the element relative to the entire wire is preferably at least 0.1 mass ppm, more preferably at least 0.5 mass ppm, even more preferably at least 1 mass ppm, and even more preferably at least 1.5 mass ppm, at least 2 mass ppm, at least 2.5 mass ppm, or at least 3 mass ppm. On the other hand, from the viewpoint of obtaining a favorable FAB shape, the total concentration of the element relative to the entire wire is preferably at most 100 mass ppm, and more preferably at most 95 mass ppm, at most 90 mass ppm, at most 85 mass ppm, or at most 80 mass ppm. If a Sn or Sb concentration exceeds 10 mass ppm or a Bi concentration exceeds 1 mass ppm, a FAB shape becomes defective. Therefore, to further improve a FAB shape, it is preferable that Sn ≤ 10 mass ppm; Sb ≤ 10 ppm by mass; and Bi ≤ 1 ppm by mass.

[0042] It is preferable that the bonding wire of the invention further contains at least one element selected from B, P, Mg, Ca, and La, and a concentration of each of the elements is 1 to 200 mass ppm relative to the entire wire. With this configuration, a crimp shape of a ball bonding part required for high-density mounting can be improved, that is, a shape circularity of a ball bonding part can be improved. In view of reducing ball hardening and reducing chip damage during ball bonding, the concentration of each of the elements is preferably at most 200 mass ppm, and more preferably at most 150 mass ppm, at most 120 mass ppm, at most 100 mass ppm, at most 95 mass ppm, at most 90 mass ppm, at most 85 mass ppm, or at most 80 mass ppm.

[0043] As in the invention, when the Pd-coated Cu bonding wire contains the element that ensures bonding reliability in a high-temperature environment, the formation of a Cu9Al4 intermetallic compound in the bonding part tends to be further reduced with the further presence of Cu at an outermost surface of the bonding wire. When the Pd-coated Cu bonding wire contains the element that ensures bonding reliability in a high-temperature environment, the interaction between the elements and Cu contained in the bonding wire facilitates the Pd concentration on a FAB surface during FAB formation, resulting in a more pronounced Pd concentration at a ball bonding interface.It is estimated that with this phenomenon, a reducing effect on the mutual diffusion of Cu and Al by a Pd-concentrated layer is further enhanced, a formation amount of Cu9Al4 which is easily corroded via the action of Cl is reduced, whereby the bonding reliability of the ball bonding part can be further improved in a high temperature and high humidity environment.

[0044] If Cu is present at the outermost surface of the Pd cap layer and the Cu concentration is at least 30 atomic%, the bonding wire may be unsuitable for practical use due to impaired sulfur resistance of the wire surface and reduced service life of the bonding wire. Therefore, if Cu is present at the outermost surface of the Pd cap layer, the Cu concentration is preferably below 30 atomic%.

[0045] If Cu is present at an outermost surface of the Au outer layer and the Cu concentration is at least 35 at%, the bonding wire may be unsuitable for practical use due to impaired sulfur resistance of the wire surface and reduced service life of the bonding wire. Therefore, if Cu is present at an outermost surface of the Au outer layer, the Cu concentration is preferably below 35 at%.

[0046] The outermost surface refers to a surface area of ​​the bond wire that can be measured by an Auger electron spectroscopy device without sputtering or similar.

[0047] For concentration analysis of the Pd capping layer and the Au and Pd-containing alloy outer layer, a method of performing analysis by processing the bonding wire from its surface in the depth direction by sputtering or the like, or a method of exposing a cross-section of the wire and performing line analysis, spot analysis, or the like on it, is effective. The analysis device used for such concentration analysis can include an Auger electron spectroscopy device incorporated in a scanning electron microscope or a transmission electron microscope, an energy-dispersive X-ray analyzer, and an electron probe microanalyzer, etc. Mechanical polishing, ion etching, etc., can be used as a method for exposing a cross-section of the wire.For microanalysis of Ni, Zn, Rh, In, Ir and Pt in the bond wire, a solution obtained by dissolving the bond wire with a strong acid is analyzed using an ICP emission spectrometer or an ICP mass spectrometer, which allows the concentrations of the elements contained in the entire bond wire to be detected. Manufacturing process

[0048] Next, a manufacturing method of the bonding wire according to the embodiment of the invention will be described. The bonding wire is obtained by preparing a Cu alloy used as a core material, forming it into a thin wire, forming a Pd capping layer and an Au layer, and performing heat treatment. After forming the Pd capping layer and the Au layer, further wire drawing and heat treatment may be performed. A method for manufacturing the Cu alloy core material, a method for forming the Pd capping layer and an Au- and Pd-containing alloy outer layer, and a heat treatment method will be described in detail.

[0049] The Cu core alloy used for core material is obtained by melting Cu as the raw material and additive elements together and solidifying them. An arc heating furnace, a high-frequency heating furnace, a resistance heating furnace, or similar can be used for melting. To prevent the mixing of gases, such as O2 and H2, from air, melting is preferably carried out in a vacuum atmosphere or an inert atmosphere, such as Ar or N2.

[0050] Examples of a method for forming the Pd capping layer and the Au layer on a surface of the Cu alloy core material include a plating method, a vapor deposition method, and a melting method. Both an electroplating method and an electroless plating method can be used as a plating method. Electroplating, called pre-plating or stop plating, has a high plating speed and favorable adhesion to the substrate. A solution used for electroless plating is divided into a substitution type and a reduction type. Although performing substitution type plating alone is sufficient for a smaller thickness, for a larger thickness, it is effective to perform reduction type plating step by step after substitution type plating.

[0051] For a vapor deposition process, physical adsorption, such as sputtering, ion plating, and vacuum deposition, as well as chemical adsorption, such as plasma CVD, can be used. All of these are dry processes and do not require cleaning after the formation of the Pd capping layer and the Au layer, nor do they require consideration of surface contamination and the like during cleaning.

[0052] When heat treatment is performed after the formation of the Pd capping layer and the Au layer, Pd in ​​the Pd capping layer diffuses into the Au layer to form the Au and Pd-containing alloy outer layer. Instead of forming the Au and Pd-containing alloy outer layer through heat treatment after the Au layer has been formed, the Au and Pd-containing alloy outer layer can be deposited from the beginning.

[0053] For the formation of the Pd capping layer and the Au- and Pd-containing alloy outer layer, both a method of forming them after performing wire drawing to a final wire diameter and a method of forming them on a large-diameter Cu alloy core material and then performing wire drawing several times until a target wire diameter is obtained are effective. In the former, in which the Pd capping layer and the Au- and Pd-containing alloy outer layer are formed at the final wire diameter, manufacturing and quality control, etc. are simple. In the latter, in which wire drawing is performed in combination with the formed Pd capping layer and the Au- and Pd-containing alloy outer layer, it is advantageous in that the adhesion to the Cu alloy core material is improved.Specific examples of the respective formation methods include a method of forming the Pd capping layer and the Au and Pd-containing alloy outer layer on a Cu alloy core material having a final diameter while successively passing the wire through an electroplating solution, and a method of forming the Pd capping layer and the containing alloy outer layer by immersing a Cu alloy core material having a large diameter in an electroplating or electroless plating solution and then drawing the wire to obtain a final wire diameter.

[0054] After the Pd capping layer and the Au- and Pd-containing alloy outer layer have been formed, heat treatment can be performed. Heat treatment promotes the diffusion of atoms between the Au- and Pd-containing alloy outer layer, the Pd capping layer, and the Cu alloy core material, improving the bonding strength between them and effectively preventing the Au- and Pd-containing alloy outer layer and the Pd capping layer from peeling off during machining, thus improving productivity. To prevent the mixing of O2 from air, it is preferable to perform the heat treatment in a vacuum atmosphere or an inert atmosphere, such as Ar or N2.

[0055] When a condition of the diffusion heat treatment or annealing heat treatment performed on the bonding wire is set as described above, Cu of the core material diffuses through the Pd cap layer and the Au and Pd-containing alloy outer layer through grain boundary diffusion, intragrain diffusion, or the like, whereby Cu can reach an outermost surface of the bonding wire and Cu can be present at an outermost surface. For a heat treatment to allow Cu to be present at an outermost surface, a previously described heat treatment for forming the Au and Pd-containing alloy outer layer can be used. When performing the heat treatment for forming the alloy outer layer, the temperature and time for the heat treatment can be selected so that Cu can be present at an outermost surface or so that Cu cannot be present at an outermost surface.Furthermore, the Cu concentration at an outermost surface can also be adjusted to a specific range, e.g., a range of 1 to 50 atomic %. Alternatively, Cu can diffuse to an outermost surface through heat treatment performed at a location other than the formation of the alloy outer layer.

[0056] As described above, regarding the addition of elements into the bonding wire that ensure bonding reliability in a high-temperature environment, the effect of the invention can be achieved by the method of adding these elements into the Cu core material or the method of adding these elements therein by depositing them on the Cu core material or the wire surface. The same applies to B, P, Mg, Ca, and La.

[0057] The simplest method for adding the components is a method of adding them to starting materials of the Cu alloy core material. For example, high-purity copper and raw materials of the above constituent element are weighed as starting raw materials, and then heated and melted in a high vacuum or in an inert atmosphere such as nitrogen and argon to produce an ingot in which the components are added at the concentration within the intended range, thereby obtaining the starting materials containing the constituent elements at the intended concentrations. Therefore, in a preferred embodiment, the Cu alloy core material of the bonding wire of the invention contains at least one element selected from Ni, Zn, Rh, In, Ir, and Pt such that a total concentration of the elements relative to the entire wire is 0.011 to 2 mass%.The preferred numerical range of the total concentration corresponds to the above description. In another preferred embodiment, the Cu alloy core material of the bonding wire of the invention contains one or more elements selected from Ga and Ge, such that a total concentration of the elements relative to the entire wire is 0.011 to 1.5 mass %. The preferred numerical range of the total concentration corresponds to the above description. In another preferred embodiment, the Cu alloy core material of the bonding wire of the invention contains at least one element selected from As, Te, Sn, Sb, Bi, and Se, such that a concentration of the elements is 0.1 to 100 mass ppm, and Sn ≤ 10 mass ppm; Sb ≤ 10 mass ppm; and Bi ≤ 1 mass ppm. The preferred numerical range of the concentration corresponds to the above description.In a preferred embodiment, the Cu purity of the Cu alloy core material is 3N or less (preferably 2N or less). In a conventional Pd-coated Cu bonding wire, a high-purity Cu core material (4N or less) is used for bondability, and the use of a low-purity Cu core material is tended to be avoided. The bonding wire of the invention containing the specific elements has particularly preferably achieved the bonding reliability of the ball bonding part in a high-temperature and high-humidity environment required for components in vehicles when the low-purity Cu alloy core material is used as described above.In another preferred embodiment, the Cu alloy core material of the bonding wire of the invention contains at least one element selected from B, P, Mg, Ca, and La, such that a concentration of each of the elements relative to the entire wire is 1 to 200 ppm by mass. The preferred numerical range of the concentration corresponds to the above description. In another preferred embodiment, the Cu alloy core material of the bonding wire of the invention contains a metallic element of Group 10 of the Periodic Table of Elements, such that a total concentration of the elements is 0.1 to 3.0 mass %. The preferred numerical range of the concentration corresponds to the above description.

[0058] The aforementioned components can also be incorporated by depositing them onto a wire surface during a wire manufacturing process. In this case, the deposition can be included in any part of the wire manufacturing process and can be repeated multiple times. The deposition can also be included in multiple process steps. The components can be added to a Cu surface before Pd plating, or can be added to a Pd surface after Pd plating, or they can be added to an Au surface after Au plating, or can be included in any plating process step. A deposition method can be selected from (1) applying an aqueous solution followed by drying and heat treatment, (2) plating (wet), and (3) vapor deposition (dry).

[0059] When applying an aqueous solution followed by drying and heat treatment, an aqueous solution of a suitable concentration is first prepared with a water-soluble compound containing the constituent elements. This allows the components to be incorporated into the wire material. The preparation can be incorporated into any part of the wire manufacturing process and can be repeated multiple times. The preparation can be incorporated into multiple process steps. The components can be added to a Cu surface before Pd plating, or to a Pd surface after Pd plating, or they can be added to an Au surface after Au plating, or they can be incorporated into any plating process step.

[0060] When wet plating is used, the plating can be electroplating or electroless plating. In electroplating, plating called impact plating, which has a high plating speed and advantageous adhesion to a substrate, can also be used in addition to conventional electroplating. The solution used for electroless plating is divided into substitution type and reduction type. Substitution type plating is generally used for a smaller thickness, while reduction type is used for a larger thickness. Either of these can be used and selected depending on the concentration to be added, and the concentration of the plating solution and the time can be adjusted.Both electroplating and electroless plating can be incorporated into any part of the wire manufacturing process and can be repeated multiple times. Both electroplating and electroless plating can be incorporated into multiple process steps. The components can be added to a Cu surface before Pd plating, or to a Pd surface after Pd plating, or to an Au surface after Au plating, or can be incorporated into any plating process step.

[0061] Dry vapor deposition includes sputtering, ion plating, vacuum deposition, plasma CVD, and the like. It has the advantage of being a dry process and eliminating pretreatment and post-treatment, thus eliminating the risk of contamination. Although vapor deposition generally has the problem of a slow addition rate of a target element, it is one of the suitable methods for the object of the invention because the addition amount of the aforementioned constituent elements is relatively low.

[0062] Evaporation can be incorporated into any part of the wire manufacturing process or can be repeated multiple times. Evaporation can be incorporated into multiple process steps. The components can be added to a Cu surface before Pd plating, or to a Pd surface after Pd plating, or to an Au surface after Au plating, or can be incorporated into any plating process step.

[0063] A method of manufacturing is now described by which a crystal orientation <100> at an angle of at most 15 degrees to a wire longitudinal direction, among crystal orientations in the wire longitudinal direction, has a proportion of at least 30% when measuring crystal orientations on a cross section of the core material in the direction perpendicular to a wire axis of the bonding wire, and an average crystal grain size in the cross section of the core material in the direction perpendicular to the wire axis of the bonding wire is 0.9 to 1.5 µm.

[0064] If the bonding wire contains the element that ensures bonding reliability in a high-temperature environment in the Cu alloy core material, the material strength (hardness) of the wire increases. Consequently, when wire drawing was performed on the bonding wire with a Cu core wire, the area reduction rate during wire drawing was low at 5 to 8%. During heat treatment after wire drawing, the hardness is still high, and the heat treatment was carried out at a temperature of at least 600°C to soften it to a degree that can be used as a bonding wire. Due to the high-temperature heat treatment, the <100> -Orientation ratio in the wire longitudinal direction was below 30%, and at the same time the average crystal grain size in the cross section of the core material was above 1.5 µm, and the yield strength ratio exceeded 1.6.When the heat treatment temperature was reduced in an effort to reduce the yield strength ratio, the average crystal grain size in the cross section of the core material was below 0.9 µm, the yield strength ratio was less than 1.1, and the wedge bondability was poor.

[0065] In contrast, the invention, when wire drawing using a tool, sets the area reduction rate to at least 10% for at least half of the tools among all the tools and sets the heat treatment temperature in the heat treatment after wire drawing to a low temperature of at most 500 °C. Consequently, when measuring crystal orientations on a cross section of the core material in the direction perpendicular to the wire axis of the bonding wire, the orientation proportion of the crystal orientation <100> at an angle of no more than 15 degrees to a wire longitudinal direction at the crystal orientations in the wire longitudinal direction, at least 30%, and the average crystal grain size in the cross section of the core material in the direction perpendicular to the wire axis of the bonding wire could be 0.9 to 1.5 µm.Due to the synergy of using the latest wire drawing technology; designing a lubricant with a higher than conventional concentration of a non-ionic surfactant contained in the lubricant; designing a tool mold with a gentler than conventional tool pressure angle; setting a lower than conventional tool cooling water temperature; and the like, wire drawing with an area reduction rate of at least 10% was achieved despite the hardening caused by the Cu alloy core material containing the components, e.g., Ni, in a total amount of at least 0.03 mass%.

[0066] When measuring crystal orientations on a wire cross-section, an electron backscatter diffraction (EBSD) method is preferably used. The EBSD method is characterized by its ability to observe crystal orientations on an observation surface and graphically display the angular difference of crystal orientations between adjacent measurement points. Furthermore, the EBSD method can relatively easily observe crystal orientations with high accuracy, even for a thin wire such as a bonding wire. Regarding grain size measurement, it can be determined using analysis software installed in a device for EBSD measurement results.The crystal grain size prescribed in the invention is obtained by determining an arithmetic mean on an equivalent diameter of crystal grains included in a measurement area (the diameter of a circle equivalent to an area of ​​a crystal grain; a circle equivalent diameter).

[0067] The invention is not limited to the above embodiments, and suitable modifications may be made within the scope and spirit of the invention. Examples

[0068] The bonding wires according to embodiments of the invention are described in more detail below using examples. <Arbeitsbeispiele 1 bis 59 und Vergleichsbeispiele 1 bis 16> (Sample preparation)

[0069] First, a method for preparing a sample is described below. For Cu as the raw material of a core material, Cu with a purity of at least 99.99 mass% was used, containing unavoidable impurities as the remainder. For Au, Pd, Ni, Zn, Rh, In, Ir, and Pt, materials with a purity of at least 99 mass% were used, containing unavoidable impurities as the remainder. Addition elements to the core material, such as Ni, Zn, Rh, In, Ir, and Pt, are mixed so that the wire or core material has a desired composition. Regarding the addition of Ni, Zn, Rh, In, Ir, and Pt, these can be mixed individually. Alternatively, they can be mixed to have a desired amount using a pre-prepared Cu master alloy containing the addition elements when the element has a high melting point as a single body or when the element is added in an infinitesimal amount.Furthermore, working examples 27 to 47 contain Ga, Ge, As, Te, Sn, Sb, Bi, Se, B, P, Mg, Ca and / or La.

[0070] The Cu alloy as the core material was manufactured to have a wire diameter of a few millimeters by continuous casting. The obtained alloy with a diameter of a few millimeters was drawn to produce a wire with a diameter of 0.3 to 1.4 mm. A commercially available lubricant was used for wire drawing, and a wire drawing speed was 20 to 150 m / min. To remove an oxide film on a wire surface, pickling treatment with hydrochloric acid or the like was performed, and a Pd overcoat layer of 1 to 15 μm was formed to cover the entire surface of the Cu alloy as the core material. Furthermore, for some wires, an Au and Pd-containing alloy outer layer of 0.05 to 1.5 μm was formed on the Pd overcoat layer. Electroplating was used to form the Pd overcoat layer and the Au and Pd-containing alloy outer layer. A commercially available semiconductor plating solution was used as the plating solution.Wire drawing was then performed, primarily using dies with an area reduction rate of 10 to 21%. Furthermore, one to three heat treatments were performed at 200 to 500°C during wire drawing to achieve a forming diameter of 20 µm. After forming, a heat treatment was performed so that the final elongation at break was approximately 5 to 15%. A heat treatment process was performed with successive wire passing and was carried out with N2 or Ar gas flowing through it. The wire feed speed was 10 to 90 m / min, the heat treatment temperature was 350 to 500°C, and the heat treatment time was 1 to 10 seconds. (Evaluation procedure)

[0071] The contents of Ni, Zn, Rh, In, Ir, Pt, Ga, Ge, As, Te, Sn, Sb, Bi, Se, B, P, Mg, Ca, and La in the wire were analyzed as the concentrations of the elements contained in the entire bonding wire using an ICP emission spectrometer.

[0072] Auger electron spectrometry was used to analyze the concentration of the Pd capping layer and the Au- and Pd-containing alloy outer layer, while the bond wire was processed from its surface in the depth direction by sputtering or similar. Based on the resulting concentration profile in the depth direction, the thickness of the Pd capping layer, the maximum Pd concentration in the Pd capping layer, and the thickness of the Au- and Pd-containing alloy outer layer were determined.

[0073] The orientation component of the crystal orientation <100> at an angle of no more than 15 degrees to the wire's longitudinal direction at the crystal orientations in the wire's longitudinal direction in the cross-section of the core material in the direction perpendicular to the wire axis of the bonding wire was calculated by observing crystal orientations on an observation surface (i.e., the cross-section of the core material in the direction perpendicular to the wire axis) by EBSD. Exclusive software (e.g., OIM Analysis, manufactured by TSL Solutions) was used to analyze EBSD measurement data. The average crystal grain size in the cross-section of the core material in the direction perpendicular to the wire axis was calculated by observing the crystal orientations on the observation surface by EBSD. Exclusive software (e.g., OIM Analysis, manufactured by TSL Solutions) was used to analyze EBSD measurement data.The crystal grain size was obtained by arithmetic averaging at an equivalent diameter of crystal grains contained in a measurement area (the diameter of a circle equivalent to an area of ​​a crystal grain; a circle equivalent diameter).

[0074] The 0.2% offset yield strength and the maximum yield strength were evaluated by conducting a tensile test with an inter-mark spacing of 100 mm. A Type 5542 multi-purpose materials testing machine manufactured by Instron was used as the tensile tester. The 0.2% offset yield strength was calculated using exclusive software installed in the machine. A load at the time of failure was determined as the maximum yield strength. The yield strength ratio was calculated using the following equation (1): Yield strength ratio = maximum yield strength / 0.2% offset yield strength. (1)

[0075] The evaluation of wedge bondability in the wire bond part was carried out by performing 1000 bonding operations on wedge bond parts of a BGA substrate and by assessing the frequency of bond part debonding. The BGA substrate used was plated with Ni and Au. In this evaluation, assuming more severe bonding conditions than normal, a chuck temperature of 150 °C was set, which was lower than a generally specified temperature range.In the evaluation, in the "wedge bondability" column in Tables 1 to 4, a case where at least 11 defects occurred was determined as problematic and marked with a "cross" symbol, a case of 6 to 10 defects was determined as practical but somewhat problematic and marked with a "triangle" symbol, a case of 1 to 5 defects was evaluated as problem-free and marked with a "circle" symbol, and a case where no defect occurred was determined as excellent and marked with a "double circle" symbol.

[0076] The bonding reliability of the ball bonded part in a high-temperature and high-humidity or high-temperature environment was determined by preparing a sample for bonding reliability evaluation, performing HTS evaluation, and evaluating the bonding life of the ball bonded part. The sample for bonding reliability evaluation was prepared by ball bonding to an electrode formed by forming an Al-1.0%Si-0.5%Cu alloy as a 0.8 μm-thick film on a Si substrate on a general metallic frame using a commercially available wire bonder and sealing with a commercially available epoxy resin. A ball was formed by flowing a gas of N2 + 5% H2 at a flow rate of 0.4 to 0.6 1 / min, and its size ranged from 33 to 34 μm in diameter.

[0077] For the HTS evaluation, the manufactured sample was exposed to a high-temperature environment of 200°C using a high-temperature thermostatic device for bond reliability evaluation. A shear test was performed on the ball bonded part every 500 hours, and the time taken to reach a shear strength value half the initial shear strength was determined as the bond life of the ball bonded part. The shear test after the high-temperature and high-humidity test was performed after removing the resin by acid treatment and exposing the ball bonded part.

[0078] A tester manufactured by DAGE was used as the shear tester for the HTS evaluation. The average of the measured values ​​from 10 randomly selected ball bonds served as the shear strength value. In this evaluation, in the "HTS" column of Tables 1 to 4, bond life of at least 500 hours and less than 1000 hours was determined as practical but requiring improvement and marked with a "triangle" symbol; at least 1000 hours and less than 3000 hours was determined as practically satisfactory and marked with a "circle" symbol; and at least 3000 hours was determined as particularly excellent and marked with a "double circle" symbol.

[0079] To evaluate the sphere formation ability (FAB shape), a sphere was sampled and observed before bonding. The presence or absence of voids on a surface of the sphere, as well as the presence or absence of deformation of the sphere, which is primarily a perfect sphere, were determined. Any of the above cases was determined as defective. The sphere was formed while blowing N2 gas at a flow rate of 0.5 l / min to reduce oxidation in a melting process. The sphere size was 34 µm. Fifty spheres were observed for one condition. An SEM was used for observation.When evaluating the ball forming ability, in the "FAB shape" column in Tables 1 to 4, a case where at least five defects occurred was determined as problematic and marked with a "cross" symbol, a case of three or four defects was determined as practicable but somewhat problematic and marked with a "triangle" symbol, a case of one or two defects was determined as problem-free and marked with a "circle" symbol, and a case where no defects occurred was determined as excellent and marked with a "double circle" symbol.

[0080] The bonding life of the ball bonding part in the high-temperature and high-humidity environment of 130°C and 85% relative humidity can be evaluated by the following HAST evaluation. For HAST evaluation, the manufactured sample for bonding reliability evaluation was exposed to a high-temperature and high-humidity environment of 130°C and 85% relative humidity using an unsaturated-type vapor pressure tester and applied with a 5V bias voltage. A shear test on the ball bonding part was performed every 48 hours, and a time until a shear strength value was half of the initial shear strength was determined as the bonding life of the ball bonding part. The shear test after the high-temperature and high-humidity test was performed after removing the resin by acid treatment and exposing the ball bonding part.

[0081] A tester manufactured by DAGE was used as the shear tester for HAST evaluation. The average of the measured values ​​of 10 randomly selected ball bonds served as the shear strength value. In this evaluation, in the "HAST" column in Tables 1 to 4, bond life of at least 144 hours and less than 288 hours was determined to be practically satisfactory and marked with a "circle" symbol; at least 288 hours and less than 384 hours was determined to be excellent and marked with a "double circle" symbol; and at least 384 hours was determined to be particularly excellent and marked with a "double circle pair" symbol.

[0082] The evaluation of the crimp shape of the ball bonded part was performed by observing the ball bonded part immediately after bonding from above and evaluating its circularity. An electrode in which an Al-0.5% Cu alloy was formed as a 1.0 μm thick film on a Si substrate was used as the bonding counterpart. Observation was performed using an optical microscope, and 200 locations were observed for one condition. Elliptical shapes with significant deviation from a perfect circle and anisotropic deformation were determined as defective crimp shape of the ball bonded part. In this evaluation, in the "Crimp Shape" column in Tables 1 to 4, a case of one to three defects was determined as unproblematic and marked with a "circle" symbol, and a case in which a favorable perfect circle was obtained for all was determined as particularly excellent and marked with a "double circle" symbol. [Table 1] Nr. Additive element (mass%) Top layer Thickness of the alloy outer layer (µm) MA Total staff Other Ni Pt Zn Rh In Ir Thickness (µm) Maximum Pd concentration (atomic %) Work example 1 0,7 0,7 0,015 97 -- 2 1,2 1,2 0,050 100 -- 3 1,0 1,0 0,100 100 -- 4 0,5 0,5 0,150 100 -- 5 0,1 0,1 0,015 98 -- 6 0,03 0,03 0,050 100 -- 7 1,1 0,3 1,4 0,100 100 -- 8 1,2 0,8 2,0 0,150 100 -- 9 0,1 0,7 0,8 0,015 98 -- 10 0,6 0,1 0,05 0,75 0,100 100 -- 11 0,8 0,8 0,3 1,9 0,150 100 -- 12 0,05 0,05 0,05 0,15 0,015 99 -- 13 0,3 1,0 0,1 1,4 0,015 97 - - 14 0,5 0,5 0,015 98 0,0005 15 1,2 1,2 0,050 100 0,0010 16 0,7 0,7 0,100 100 0,0100 17 0,3 0,3 0,150 100 0,0500 18 0,1 0,1 0,015 98 0,0005 19 0,05 0,05 0,050 100 0,0010 20 0,5 0,3 0,8 0,100 100 0,0100 21 1,2 0,1 1,3 0,150 100 0,0500 22 0,01 0,7 0,71 0,015 99 0,0005 23 0,6 0,1 0,05 0,75 0,050 100 0,0010 [Table 1] (continued) Nr. Crystal structure Mechanical characteristics Wire quality <100> -Proportion of wire cross-section (%) Average crystal grain size (µm) Max. yield strength ① 0.2% offset yield strength ② Yield strength ratio ① / ② Wedge bondability HTS FAB form HAVE squeezing mold (mN / µm 2 ) - Work example 1 92 1,1 0,19 0,16 1,19 ⊚ ⊚ ◯ ◯ ◯ 2 72 0,9 0,22 0,17 1,29 ⊚ ⊚ ⊚ ◯ ◯ 3 71 1,0 0,24 0,16 1,50 ◯ ⊚ ⊚ ◯ ◯ 4 72 1,1 0,29 0,24 1,21 ⊚ ⊚ ◯ ◯ ◯ 5 75 1,2 0,30 0,22 1,36 ⊚ ⊚ ◯ ◯ ◯ 6 63 1,3 0,31 0,20 1,55 ◯ ⊚ ⊚ ◯ ◯ 7 75 1,0 0,33 0,28 1,18 ⊚ ⊚ ⊚ ◯ ◯ 8 65 0,9 0,34 0,27 1,26 ⊚ ⊚ ◯ ◯ ◯ 9 51 1,2 0,35 0,22 1,59 ◯ ⊚ ◯ ◯ ◯ 10 97 1,2 0,33 0,30 1,10 ⊚ ⊚ ⊚ ◯ ◯ 11 80 1,1 0,34 0,28 1,21 ⊚ ⊚ ◯ ◯ ◯ 12 70 1,2 0,35 0,22 1,59 ◯ ⊚ ◯ ◯ ◯ 13 54 1,0 0,35 0,23 1,52 ⊚ ⊚ ◯ ◯ ◯ 14 91 1,1 0,20 0,18 1,11 ⊚ ⊚ ◯ ◯ ◯ 15 70 0,9 0,21 0,17 1,24 ◯ ⊚ ◯ ◯ ◯ 16 69 1,1 0,22 0,15 1,47 ⊚ ⊚ ⊚ ◯ ◯ 17 70 1,2 0,28 0,24 1,17 ⊚ ⊚ ◯ ◯ ◯ 18 76 1,2 0,29 0,22 1,32 ◯ ◯ ◯ ◯ ◯ 19 64 1,3 0,30 0,19 1,58 ⊚ ⊚ ⊚ ◯ ◯ 20 74 1,1 0,33 0,28 1,18 ⊚ ◯ ⊚ ◯ ◯ 21 64 1,2 0,34 0,26 1,31 ⊚ ◯ ◯ ◯ ◯ 22 50 1,1 0,35 0,23 1,52 ◯ ⊚ ◯ ◯ ◯ 23 98 1,0 0,30 0,20 1,50 ⊚ ◯ ⊚ ◯ ◯ [Table 1] (continued) Nr. Additive element (mass%) Top layer Thickness of the alloy outer layer (µm) MA Total staff Other Ni Pt Zn Rh In Ir Thickness (µm) Maximum Pd concentration (atomic %) Work example 24 0,8 0,8 0,3 1,9 0,100 100 0,0100 25 0,05 0,05 0,05 0,15 0,150 100 0,0500 26 0,3 1,0 0,1 1,4 0,015 97 0,0100 [Table 1] (continued) Nr. Crystal structure Mechanical characteristics Wire quality <100> -Proportion of wire cross-section (%) Average crystal grain size (µm) Max. yield strength ① 0.2% offset yield strength ② Yield strength ratio ① / ② Wedge bondability HTS FAB form HAVE squeezing mold (mN / µm 2 ) - Work e.g. 24 85 0,9 0,33 0,29 1,14 ⊚ ⊚ ⊚ ◯ ◯ 25 74 1,3 0,34 0,25 1,36 ⊚ ⊚ ◯ ◯ ◯ 26 51 0,9 0,35 0,25 1,40 ⊚ ⊚ ◯ ◯ ◯ [Table 2] Nr. Additive element (mass%) Top layer Thickness of the alloy outer layer (µm) MA Total staff Other Ni Pt Zn Rh In Ir Thickness (µm) Maximum Pd concentration (atomic %) Work example 27 0,7 0,7 Ga:0.007 0,100 100 - 28 1,1 1,1 Ge:0.008 0,050 100 - 29 0,7 0,7 Ace:0.003 0,050 100 - 30 1,2 1,2 Te:0.001 0,150 100 - 31 0,5 0,5 Sn: 0.0007 0,015 96 - 32 0,05 0,05 Sb:0.0008 0,050 100 - 33 1,0 1,0 Bi:0.00008 0,100 100 -- 34 0,8 0,8 Se:0.0001 0,100 100 - 35 0,05 0,05 Ga: 0.003 Te: 0.0008 0,100 100 - 36 0,08 0,08 Ge:0.003 Sb:0.0007 0,150 100 0,0050 37 0,1 0,1 As:0.001 Se:0.001 0,150 100 0,0100 38 0,08 0,08 B:0,0008 0,050 100 - 39 1,2 1,2 P:0,004 0,050 100 - 40 0,05 0,05 Mg:0.005 0,100 100 - 41 0,5 0,5 Approx.: 0.003 0,015 95 - 42 0,1 0,1 La:0.003 0,100 100 0,0100 43 0,05 0,05 P:0.006 B:0.0008 0,050 100 0,0050 44 0,6 0,6 P:0.003 Ca:0.001 0,015 100 0,0100 [Table 2] (continued) Nr. Crystal structure Mechanical characteristics Wire quality <100> -Proportion of wire cross-section (%) Average crystal grain size (µm) Max. yield strength ① 0.2% offset yield strength ② Yield strength ratio ① / ② Wedge bondability HTS FAB form HAVE squeezing mold (mN / µm 2 ) - Work example 27 88 0,9 0,22 0,18 1,22 ⊚ ⊚ ⊚ ⊚ ◯ 28 75 1,0 0,25 0,17 1,47 ⊚ ⊚ ⊚ ⊚ ◯ 29 72 1,0 0,30 0,21 1,43 ⊚ ⊚ ⊚ ⊚ ◯ 30 67 1,2 0,31 0,24 1,29 ⊚ ⊚ ◯ ⊚ ◯ 31 66 1,0 0,29 0,22 1,32 ◯ ⊚ ◯ ⊚ ◯ 32 74 1,1 0,35 0,29 1,21 ⊚ ⊚ ⊚ ⊚ ◯ 33 80 1,1 0,31 0,22 1,41 ⊚ ⊚ ⊚ ⊚ ◯ 34 92 0,9 0,27 0,19 1,42 ⊚ ⊚ ⊚ ⊚ ◯ 35 72 1,2 0,30 0,19 1,58 ◯ ⊚ ⊚ ⊚ ◯ 36 55 1,3 0,33 0,25 1,32 ⊚ ⊚ ◯ ⊚ ◯ 37 82 1,1 0,32 0,25 1,28 ⊚ ⊚ ◯ ⊚ ◯ 38 74 1,1 0,34 0,23 1,48 ⊚ ⊚ ⊚ ◯ ⊚ 39 77 1,2 0,29 0,20 1,45 ⊚ ⊚ ⊚ ◯ ⊚ 40 91 1,0 0,33 0,28 1,18 ⊚ ⊚ ⊚ ◯ ⊚ 41 68 1,0 0,23 0,19 1,21 ⊚ ⊚ ◯ ◯ ⊚ 42 91 0,9 0,26 0,21 1,24 ⊚ ⊚ ◯ ◯ ⊚ 43 68 1,1 0,29 0,19 1,53 ◯ ⊚ ⊚ ◯ ⊚ 44 57 1,3 0,33 0,24 1,38 ⊚ ⊚ ◯ ◯ ⊚ [Table 2] (continued) Nr. Additive element (mass%) Top layer Thickness of the alloy outer layer (µm) MA Total staff Other Ni Pt Zn Rh In Ir Thickness (µm) Maximum Pd concentration (atomic %) Work example 45 0,5 0,5 B:0,015 0,100 100 0,0100 46 0,5 0,5 P:0,02 0,050 100 0,0050 47 0,5 0,5 La:0.018 0,015 100 0,0100 48 0,011 0,011 0,015 98 - 49 0,011 0,011 0,050 100 - 50 0,011 0,011 0,100 100 - 51 0,011 0,011 0,150 100 - 52 0,011 0,011 0,050 100 - 53 0,011 0,011 0,100 100 - [Table 2] (continued) Crystal structure Mechanical characteristics Wire quality Nr. <100> -Proportion of wire cross-section (%) Average crystal grain size (µm) Max. yield strength ① 0.2% offset yield strength Yield strength ratio ① / ② Wedge bondability HTS FAB form HAVE squeezing mold (mN / µm 2 ) - Work example 45 90 0,9 0,25 0,21 1,19 ⊚ ⊚ ⊚ ◯ ⊚ 46 67 1,1 0,28 0,19 1,47 ⊚ ⊚ ⊚ ◯ ⊚ 47 56 1,3 0,33 0,24 1,38 ⊚ ⊚ ◯ ◯ ⊚ 48 75 1,0 0,21 0,18 1,17 ⊚ ◯ ◯ ◯ ◯ 49 72 1,0 0,19 0,16 1,19 ⊚ ◯ ⊚ ◯ ◯ 50 67 1,2 0,23 0,19 1,21 ⊚ ◯ ⊚ ◯ ◯ 51 66 1,0 0,22 0,18 1,22 ⊚ ◯ ◯ ◯ ◯ 52 74 1,1 0,21 0,18 1,17 ⊚ ◯ ◯ ◯ ◯ 53 80 0,9 0,23 0,2 1,15 ⊚ ◯ ⊚ ◯ ◯ [Table 3] Nr. Additive element (mass%) Top layer Thickness of the alloy outer layer (µm) MA Total staff Other Ni Pt Zn Rh In Ir Thickness (µm) Maximum Pd concentration (atomic percent) Work example 54 0,02 0,02 0,015 97 - 55 0,02 0,02 0,05 100 - 56 0,02 0,02 0,1 100 - 57 0,02 0,02 0,15 100 - 58 0,02 0,02 0,05 100 - 59 0,02 0,02 0,1 100 - [Table 3] (continued) Nr. Mechanical characteristics Wire quality <100> -Proportion of wire cross-section (%) Average crystal grain size (µm) Max. yield strength ① 0.2% offset yield strength ② Yield strength ratio ① / ② Wedge bondability HTS FAB form HAVE squeezing mold (mN / µm 2 ) - – Work example 54 30 1 0,31 0,24 1,29 ⊚ ◯ ◯ ◯ ◯ 55 41 1 0,33 0,22 1,50 ⊚ ◯ ⊚ ◯ ◯ 56 49 1,2 0,28 0,19 1,47 ⊚ ◯ ⊚ ◯ ◯ 57 52 1,3 0,32 0,27 1,19 ⊚ ◯ ◯ ◯ ◯ 58 60 1,4 0,22 0,18 1,22 ⊚ ◯ ⊚ ◯ ◯ 59 74 1,5 0,25 0,20 1,25 ⊚ ◯ ⊚ ◯ ◯ Evaluation results

[0083] The bonding wires according to Working Examples 1 to 59 each contain Ni, Zn, Rh, In, Ir, or Pt in an amount of 0.011 to 2 mass%, and their yield strength ratio (= maximum yield strength / 0.2% offset yield strength) is in a range of 1.1 to 1.6, and they achieved favorable results in both the reliability of the ball bonding part at high temperature in the HTS evaluation and the wedge bondability.For the bonding wire of the invention, the area decrease rate during wire drawing was at least 10%, and the heat treatment temperature after wire drawing was a low temperature of at most 500 °C, which ensured the crystal orientation <100> At an angle of no more than 15 degrees to the wire's longitudinal direction, the crystal orientations in the wire's longitudinal direction could be at least 30% when measuring crystal orientations at the cross-section of the core material perpendicular to the wire axis of the bonding wire, and the average crystal grain size in the cross-section of the core material perpendicular to the wire axis of the bonding wire could be 0.9 to 1.5 µm. Thus, it is assumed that the yield strength ratio could be within the previously described range.

[0084] The bonding wires according to the working examples each comprise a Cu alloy core material and a Pd cap layer formed on a surface of the Cu alloy core material, and the thickness of the Pd cap layer is in the preferred range of 0.015 to 0.150 µm. They all exhibited a favorable FAB shape.

[0085] On the other hand, in Comparative Examples 1, 3, 10, and 11 with yield strength ratios below 1.1, the wedge bondability was defective in all cases. In Comparative Examples 2, 4 to 9, and 12 to 16 with yield strength ratios above 1.6, the wedge bondability was defective or problematic. In particular, in Comparative Examples 15 and 16, the HST and HAST were also defective because the element that ensures bonding reliability in a high-temperature environment was not contained in the wire. It is believed that the reason for the low yield strength ratio in Comparative Examples 1, 3, 10, and 11 was partly due to the average crystal grain size in the cross section of the core material being below 0.9 μm, because the area decrease rate was less than 10%.In addition, it is assumed that the reason for the increased yield strength ratio in Comparative Examples 2, 4 to 9, 12 to 14 was partly that the <100> The orientation ratio in the wire's longitudinal direction was below 30% due to the high heat treatment temperature of at least 600 °C. In particular, it is believed that in Comparative Examples 2, 6, 8, 9, and 14, the reason for this was partly that the average crystal grain size in the cross-section of the core material exceeded 1.5 µm because the heat treatment temperature was at least 620 °C. <Arbeitsbeispiele 2-1 bis 2-40> (Sample)

[0086] First, a method for preparing a sample is described below. For Cu as the raw material of the core material, Cu with a purity of at least 99.99 mass% was used, containing unavoidable impurities as the remainder. For Ga, Ge, Ni, Ir, Pt, Pd, B, P, and Mg, materials with a purity of at least 99 mass% were used, containing unavoidable impurities as the remainder. Ga, Ge, Ni, Ir, Pt, Pd, B, P, and Mg as additive elements to the core material are mixed so that the wire or core material has a desired composition. Regarding the addition of Ga, Ge, Ni, Ir, Pt, Pd, B, P, and Mg, they can be mixed individually. Alternatively, they can be mixed to have a desired amount using a pre-prepared Cu master alloy containing the additive elements when the element has a high melting point as a single body or when the element is added in an infinitesimal amount.

[0087] The Cu alloy as the core material was prepared by loading raw materials into a carbon crucible formed into a 3 to 6 mm diameter cylinder, heating and melting the raw materials at 1090 to 1300 °C in vacuum or in an inert atmosphere such as N2 or Ar gas using a high-frequency furnace, and performing furnace cooling. The obtained alloy with a diameter of 3 to 6 mm was drawn to form a diameter of 0.9 to 1.2 mm, and a wire with a diameter of 300 to 600 μm was prepared by successive wire drawing using dies. A commercially available lubricant was used for wire drawing, and a wire drawing speed was 20 to 150 m / min. To remove an oxide film on a wire surface, a pickling treatment with sulfuric acid was performed, and a Pd capping layer of 1 to 15 µm was formed to cover the entire surface of the Cu alloy as the core material.Furthermore, for some wires, a 0.05 to 1.5 µm Au and Pd-containing alloy outer layer was formed on the Pd top layer. Electroplating was used to form the Pd top layer and the Au and Pd-containing alloy outer layer. A commercially available semiconductor plating solution was used as the plating solution. This was followed by repeated heat treatment at 200 to 500 °C and wire drawing to form it to a diameter of 20 µm. After forming, heat treatment was performed under N2 or Ar gas flow, so that the final elongation at break was approximately 5 to 15%. A heat treatment process was carried out with successive wire passage and was carried out with N2 or Ar gas flowing through it. A wire feeding speed was 20 to 200 m / min, a heat treatment temperature was 200 to 600 °C, and a heat treatment time was 0.2 to 1.0 second.

[0088] For the concentration analysis of the Pd capping layer and the Au- and Pd-containing alloy outer layer, the analysis was performed using an Auger electron spectroscopy device while sputtering the bonding wire from its surface with Ar ions in the depth direction. The thicknesses of the capping layer and the alloy outer layer were determined from an obtained concentration profile (the unit of depth was related to SiO2) in the depth direction. A region where a Pd concentration was at least 50 atomic % and an Au concentration was below 10 atomic % was determined as the Pd capping layer, and a region where an Au concentration was in a range of at least 10 atomic % on a surface of the Pd capping layer was determined as the alloy outer layer. The thicknesses of the capping layer and the alloy outer layer and a maximum Pd concentration are listed in Tables 5 and 6.The Pd concentration in the Cu alloy core material was measured by a method that exposes a wire cross-section and performs line analysis, spot analysis, or the like on the exposed wire cross-section using an electron probe microanalyzer built into a scanning electron microscope. Mechanical polishing, ion etching, or the like were used for the wire cross-section exposure method. For the concentrations of Ga, Ge, Ni, Ir, Pt, B, P, and Mg in the bonding wire, a solution obtained by dissolving the bonding wire with a strong acid was analyzed using an ICP emission spectrometer or an ICP mass spectrometer, and they were detected as the concentrations of the elements contained in the entire bonding wire.

[0089] The configurations of the respective samples prepared according to the above procedure are listed in Tables 5 and 6 below. [Table 5] Nr. Addition element Top layer Thickness of the alloy outer layer (µm) M B In total M A Other Ga Ge Ni Pd Pt Ir B P Mg Thickness (µm) Maximum Pd concentration (atomic %) (Mass-%) (Mass-%) (mass ppm) Work example 2-1 0,025 0,025 0,015 98 0,0005 2-2 0,500 0,500 0,1 100 0,0005 2-3 1,500 1,500 0,05 100 0,001 2-4 0,011 0,011 0,1 100 0,001 2-5 0,025 0,025 0,05 100 0,08 2-6 0,300 0,300 0,05 100 0,01 2-7 1,500 1,500 0,1 100 0,01 2-8 0,015 0,011 0,026 0,05 100 0,001 2-9 0,050 0,600 0,650 0,05 100 0,01 2-10 0,600 0,850 1,450 0,05 100 0,003 2-11 0,002 0,800 0,802 0,05 100 0,003 2-12 0,030 0,030 0,50 0,15 100 0,001 2-13 0,030 0,030 0,50 0,05 100 - 2-14 0,030 0,030 1,20 0,1 100 0,01 2-15 0,030 0,030 0,50 0,05 100 0,01 2-16 0,030 0,030 1,20 0,1 100 0,01 2-17 0,030 0,030 0,50 0,015 96 0,0005 2-18 0,030 0,030 1,20 0,1 100 0,01 2-19 0,030 0,030 0,80 0,15 100 0,01 2-20 0,030 0,030 1,20 0,05 100 0,003 [Table 5] (continued) Nr. Crystal structure Mechanical characteristics Wire quality <100> -Proportion of wire cross-section (%) Average crystal grain size (µm) Max. yield strength ① 0.2% offset yield strength ② Yield strength ratio ① / ② Wedge bondability HTS FAB form HAVE squeezing mold Skew (mN / µm 2 ) - Work e.g. 2-1 71 1,2 0,23 0,17 1,35 ⊚ △ ◯ ◯ ◯ ⊚ 2-2 70 0,9 0,25 0,18 1,39 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-3 71 1,0 0,30 0,23 1,30 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-4 74 1,1 0,31 0,23 1,35 ⊚ △ ⊚ △ ◯ ⊚ 2-5 62 1,1 0,32 0,25 1,28 ⊚ △ △ ◯ ◯ ⊚ 2-6 74 1,3 0,34 0,26 1,31 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-7 64 1,0 0,35 0,30 1,17 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-8 50 1,2 0,34 0,22 1,55 ⊚ △ ⊚ △ ◯ ⊚ 2-9 96 0,9 0,21 0,19 1,11 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-10 79 1,0 0,22 0,16 1,38 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-11 69 1,0 0,23 0,19 1,21 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-12 53 1,1 0,30 0,19 1,58 ⊚ ◯ ⊚ ◯ ◯ ⊚ 2-13 70 1,2 0,28 0,21 1,33 ⊚ ◯ ⊚ ◯ ◯ ⊚ 2-14 68 1,0 0,29 0,25 1,16 ⊚ ⊚ ⊚ ◯ ◯ ⊚ 2-15 69 1,1 0,32 0,26 1,23 ⊚ ◯ ⊚ ◯ ◯ ⊚ 2-16 75 1,3 0,33 0,25 1,32 ⊚ ⊚ ⊚ ◯ ◯ ⊚ 2-17 63 1,2 0,34 0,28 1,21 ⊚ ◯ ⊚ ◯ ◯ ⊚ 2-18 73 1,0 0,31 0,23 1,35 ⊚ ⊚ ⊚ ◯ ◯ ⊚ 2-19 63 1,0 0,34 0,29 1,17 ⊚ ◯ ⊚ ◯ ◯ ⊚ 2-20 51 1,0 0,21 0,14 1,50 ⊚ ⊚ ⊚ ◯ ◯ ⊚ [Table 6] Nr. Addition element Top layer Thickness of the alloy outer layer (µm) M B M B Total M A Other Ga Ge Ni Pd Pt Ir B P Mg Thickness (µm) Maximum Pd concentration (atomic %) (Mass-%) (Mass-%) (mass ppm) Work example 2-21 0,030 0,030 1,20 0,15 100 0,001 2-22 0,030 0,030 0,80 0,15 100 0,08 2-23 0,030 0,030 1,20 0,15 100 0,001 2-24 0,030 0,030 0,80 0,015 97 0,003 2-25 0,030 0,030 1,20 0,1 100 0,003 2-26 0,500 0,500 0,90 30 0,05 100 0,003 2-27 0,500 0,500 0,90 30 0,05 100 -- 2-28 0,500 0,500 0,90 50 0,05 100 0,003 2-29 0,500 0,500 0,90 50 0,15 100 0,01 2-30 0,500 0,500 0,90 10 0,15 100 0,001 2-31 0,500 0,500 0,90 10 0,15 100 0,01 2-32 0,800 0,500 1,300 0,50 15 0,015 99 0,003 2-33 0,080 1,200 1,280 0,50 15 0,15 100 0,01 2-34 0,300 0,500 0,800 0,50 100 0,015 96 0,003 2-35 0,080 0,040 0,120 0,50 30 0,015 98 0,001 2-36 1,000 0,100 1,100 0,50 30 0,15 100 0,05 2-37 0,050 0,015 98 -- 2-38 0,050 0,015 96 -- 2-39 1,000 0,1 100 -- 2-40 1,000 0,1 100 -- [Table 6] (continued) Nr. Crystal structure Mechanical characteristics Wire quality <100> -Proportion of wire cross-section (%) Average crystal grain size (µm) Max. yield strength ① 0.2% offset yield strength ② Yield strength ratio ① / ② Wedge bondability HTS FAB form HAVE squeezing mold Skew (mN / µm 2 ) - Work e.g. 2-21 84 0,9 0,29 0,20 1,45 ⊚ ⊚ ⊚ ◯ ◯ ⊚ 2-22 73 1,0 0,30 0,23 1,30 ⊚ ◯ △ ◯ ◯ ⊚ 2-23 50 1,1 0,28 0,18 1,56 ⊚ ⊚ ⊚ ◯ ◯ ⊚ 2-24 87 1,3 0,34 0,23 1,48 ⊚ ◯ ⊚ ◯ ◯ ⊚ 2-25 76 1,1 0,30 0,22 1,36 ⊚ ⊚ ⊚ ◯ ◯ ⊚ 2-26 66 0,9 0,26 0,21 1,24 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-27 65 1,2 0,29 0,24 1,21 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-28 92 1,2 0,32 0,29 1,10 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-29 72 1,2 0,33 0,25 1,32 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-30 54 1,1 0,31 0,2 1,55 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-31 81 1,0 0,25 0,17 1,47 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-32 73 1,2 0,33 0,25 1,32 ⊚ ◯ ◯ ⊚ ⊚ ⊚ 2-33 76 1,3 0,29 0,22 1,32 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-34 67 1,0 0,23 0,2 1,15 ⊚ ◯ ◯ ⊚ ⊚ ⊚ 2-35 91 1,1 0,33 0,3 1,10 ⊚ ◯ ◯ ⊚ ⊚ ⊚ 2-36 67 1,2 0,29 0,25 1,16 ⊚ ◯ ⊚ ⊚ ⊚ ⊚ 2-37 57 1,1 0,29 0,19 1,53 ⊚ △ ◯ ⊚ ◯ ⊚ 2-38 98 1,0 0,26 0,23 1,13 ⊚ △ ◯ ⊚ ◯ ⊚ 2-39 75 1,0 0,35 0,26 1,35 ⊚ △ ⊚ ⊚ ◯ ⊚ 2-40 69 1,2 0,21 0,18 1,17 ⊚ △ ⊚ ⊚ ◯ ⊚ (Evaluation procedure)

[0090] A crystal structure on a wire surface was evaluated as the observation surface. An electron backscatter diffraction (EBSD) method was used as the evaluation method. The EBSD method is characterized by its ability to observe crystal orientations on an observation surface and graphically display the angular difference in crystal orientations between adjacent measurement points. Furthermore, the EBSD method can observe crystal orientations relatively easily with high accuracy, even for a thin wire such as the bond wire.

[0091] When performing EBSD with a curved surface such as the wire surface as the object of observation, care should be taken. If a region with a large curvature is measured, measurement with high accuracy is difficult. However, by fixing a bonding wire to be measured to a line on a plane and measuring a flat part near the center of the bonding wire, measurement with high accuracy can be performed. In particular, the measurement region shown below works well. The circumferential size is at most 50% of the wire diameter with the center in the wire longitudinal direction as the axis, while the size in the wire longitudinal direction is at most 100 μm. Preferably, the circumferential size is at most 40% of the wire diameter, while the size in the wire longitudinal direction is at most 40 μm, which can improve measurement efficiency by shortening measurement time.To further increase accuracy, it is desirable to measure three or more points to obtain mean information while taking deviations into account. The measurement points can be spaced at least 1 mm apart to avoid excessive proximity.

[0092] Regarding the orientation component of the crystal orientation <100> at an angle of at most 15 degrees to the wire longitudinal direction at the crystal orientations in the wire longitudinal direction in the cross section of the core material in the direction perpendicular to the wire axis of the bonding wire, and the average crystal grain size (µm) in the cross section of the core material in the direction perpendicular to the wire axis, were obtained by the same method as in Working Examples 1 to 59. Regarding the 0.2% offset yield strength and maximum yield strength, these were evaluated by the same method as in Working Examples 1 to 59, and a yield strength ratio was calculated by the above equation (1).

[0093] The bonding reliability of the ball bonded part was determined in a high-temperature and high-humidity or high-temperature environment by preparing a bonding reliability evaluation sample, performing HAST and HTS evaluation, and evaluating the bonding life of the ball bonded part in each test. The bonding reliability evaluation sample was prepared by performing ball bonding on an electrode formed by forming an Al-1.0% Si-0.5% Cu alloy film with a thickness of 0.8 μm on a Si substrate on a general metallic frame using a commercially available wire bonder and sealing it with a commercially available epoxy resin. A ball was formed by flowing a gas of N2 + 5% H2 at a flow rate of 0.4 to 0.6 l / min, and its size ranged from 33 to 34 μm in diameter.

[0094] For the HAST evaluation, the manufactured sample for bond reliability evaluation was exposed to a high-temperature and high-humidity environment of 130°C and 85% relative humidity using an unsaturated-type vapor pressure tester and applied with a 7V bias voltage. A shear test was performed on the ball bonded part every 48 hours, and the time taken to reach a shear strength value half the initial shear strength was determined as the bond life of the ball bonded part. The shear test after the high-temperature and high-humidity test was performed after removing the resin by acid treatment and exposing the ball bonded part.

[0095] A tester manufactured by DAGE was used as the shear tester for the HAST evaluation. The average of the measured values ​​of 10 randomly selected ball bonds served as the shear strength value. In this evaluation, in the "HAST" column in Tables 5 and 6, bond life under 96 hours was determined to be practically problematic and marked with a "cross" symbol; at least 96 hours and under 144 hours were determined to be practical but somewhat problematic and marked with a "triangle" symbol; at least 144 hours and under 288 hours were determined to be practically problem-free and marked with a "circle" symbol; and at least 288 hours was determined to be excellent and marked with a "double circle" symbol.

[0096] For the HTS evaluation, the manufactured sample was exposed to a high-temperature environment of 200°C using a high-temperature thermostatic device for bond reliability evaluation. A shear test was performed on the ball bonded part every 500 hours, and the time until a shear strength value was half the initial shear strength was determined as the bond life of the ball bonded part. The shear test after the high-temperature and high-humidity test was performed after removing the resin by acid treatment and exposing the ball bonded part.

[0097] A tester manufactured by DAGE was used as the shear tester for the HTS evaluation. The average of the measured values ​​from 10 randomly selected ball bonds served as the shear strength value. In this evaluation, bond life of at least 500 hours and less than 1000 hours was determined to be practical but requiring improvement and marked with a "triangle" symbol; at least 1000 hours to less than 3000 hours was rated as practically satisfactory and marked with a "circle" symbol; and at least 3000 hours was determined to be particularly excellent and marked with a "double circle" symbol.

[0098] To evaluate the sphere formation ability (FAB shape), a sphere was sampled and observed prior to bonding. The presence or absence of voids on the sphere surface and the presence or absence of deformation of the sphere, which is primarily a perfect sphere, were determined. Any of the above-mentioned cases was considered defective. The sphere was formed while bubbling with N2 gas at a flow rate of 0.5 l / min to reduce oxidation in a melting process. The sphere size was 34 µm. 50 spheres were examined for one condition. An SEM was used for observation.When evaluating the spherical forming ability, in the "FAB shape" column in Tables 5 and 6, a case where at least five defects occurred was determined as problematic and marked with a "cross" symbol, a case of three or four defects was determined as practical but somewhat problematic and marked with a "triangle" symbol, a case of one or two defects was determined as problem-free and marked with a "circle" symbol, and a case where no defects occurred was determined as excellent and marked with a "double circle" symbol.

[0099] The wedge bondability of the wire bonding part was evaluated by performing 1,000 bonding operations on the leads of a lead frame and by the frequency with which the bonding part debonded. A lead frame made of an Fe-42 at.% Ni alloy plated with 1 to 3 µm Ag was used as the lead frame. In this evaluation, assuming more severe bonding conditions than normal, a step temperature was set at 150 °C, which was lower than a generally specified temperature range.In the evaluation, in the “Wedge Bondability” column in Tables 5 and 6, a case where at least 11 defects occurred was determined as problematic and marked with a “cross” symbol, a case of 6 to 10 defects was determined as practical but somewhat problematic and marked with a “triangle” symbol, a case of 1 to 5 defects was evaluated as problem-free and marked with a “circle” symbol, and a case where no defect occurred was determined as excellent and marked with a “double circle” symbol.

[0100] The evaluation of the crimp shape of the ball bonded part was carried out by observing the ball bonded part immediately after bonding and evaluating its circularity. An electrode in which an Al-0.5% Cu alloy film with a thickness of 1.0 µm was formed on a Si substrate was used as the bonding counterpart. Observation was carried out using an optical microscope, and 200 locations were observed for one condition. Elliptical shapes with a significant deviation from a perfect circle, as well as anisotropic deformation, were determined as defective crimp shapes of the ball bonded part.In this evaluation, in the “squeeze shape” column in Tables 5 and 6, a case of at least six defects occurring was determined as problematic and marked with a “cross” symbol, a case of four or five defects was determined as feasible but somewhat problematic and marked with a “triangle” symbol, one to three were determined as problem-free and marked with a “circle” symbol, and a case in which a favorable perfect circle was obtained for all was determined as particularly excellent and marked with a “double circle” symbol. [Skewed]

[0101] For evaluation, 100 bonding operations with a loop length of 5 mm and a loop height of 0.5 mm were performed on a lead frame. As an evaluation method, an upright wire portion was observed from a horizontal chip direction, and the evaluation was performed based on a distance when the distance between a perpendicular passing through the center of the ball bond portion and the upright wire portion was maximized (skew distance). If the skew distance was smaller than the wire diameter, the skew was determined to be favorable; whereas, if the skew distance was larger, the upright portion exhibited skew, and the skew was determined to be defective. One hundred bonding wires were observed with an optical microscope, and the number of skew defects was counted.In the “Skewedness” column in Tables 5 and 6, a case in which at least seven errors occurred was determined as problematic and marked with a “cross” symbol, a case of four to six errors was determined as feasible but somewhat problematic and marked with a “triangle” symbol, a case of one to three errors was determined as problem-free and marked with a “circle” symbol, and a case in which no errors occurred was determined as excellent and marked with a “double circle” symbol. (Evaluation results)

[0102] According to Tables 5 and 6, the bonding wires of Working Examples 2-1 to 2-40 each comprise a Cu alloy core material and a Pd cap layer formed on the surface of the Cu alloy core material. The bonding wire contains one or more elements selected from Ga and Ge, and the total element concentration is 0.011 to 1.5 mass% relative to the entire wire. It was found that with this configuration, the bonding wires of Working Examples 2-1 to 2-40 can achieve ball bonding reliability in the HAST test in a high-temperature and high-humidity environment of 130°C and 85% relative humidity.

[0103] In addition, it was demonstrated that the bonding wires of Working Examples 2-1 to 2-40 can obtain excellent wedge bondability since their yield strength ratio was 1.1 to 1.6.

[0104] In the working examples where the bonding wires further contain at least one element selected from Ni, Ir, Pt and Pd, it was found that the high-temperature reliability of the ball bonding part is even more advantageous in the HTS evaluation.

[0105] In the working examples in which the bonding wires further contain at least one element selected from B, P, and Mg, the crimp shape of the ball bonding part was advantageous when a concentration of each of the elements was 1 to 200 ppm by mass relative to the entire wire. <Arbeitsbeispiele 3-1 bis 3-56> (Sample)

[0106] First, a method for preparing a sample is described. For Cu as the raw material of a core material, Cu with a purity of at least 99.99 mass% was used, containing unavoidable impurities as the residue. For As, Te, Sn, Sb, Bi, Se, Ni, Zn, Rh, In, Ir, Pt, Ga, Ge, Pd, B, P, Mg, Ca, and La, materials with a purity of at least 99 mass% were used, containing unavoidable impurities as the residue. As, Te, Sn, Sb, Bi, Se, Ni, Zn, Rh, In, Ir, Pt, Ga, Ge, Pd, B, P, Mg, Ca, and La as additive elements to the core material are mixed so that the wire or core material has a desired composition. Regarding the addition of As, Te, Sn, Sb, Bi, Se, Ni, Zn, Rh, In, Ir, Pt, Ga, Ge, Pd, B, P, Mg, Ca and La, these can be mixed individually.Alternatively, they may be mixed to have a desired amount using a pre-prepared Cu master alloy containing the addition elements when the element has a high melting point as a single body or when the element is added in an infinitesimal amount.

[0107] The Cu alloy for the core material was prepared by loading raw materials into a carbon crucible formed into a cylindrical shape with a diameter of 3 to 6 mm, heating and melting the raw materials at 1090 to 1300 °C in a vacuum or in an inert atmosphere such as N2 or Ar gas using a high-frequency furnace, and performing furnace cooling. The resulting alloy with a diameter of 3 to 6 mm was drawn to produce a wire with a diameter of 0.9 to 1.2 mm. Subsequently, a wire with a diameter of 300 to 600 µm was produced by successive wire drawing and the like using a die. A commercially available lubricant was used for wire drawing, and the wire drawing speed was 20 to 150 m / min.To remove an oxide film on a wire surface, a pickling treatment with hydrochloric acid was performed, and a Pd capping layer of 1 to 15 μm was formed to cover the entire surface of the Cu alloy as the core material. Furthermore, for some wires, an Au and Pd-containing alloy outer layer of 0.05 to 1.5 μm was formed on the Pd capping layer. Electroplating was used to form the Pd capping layer and the Au and Pd-containing alloy outer layer. A commercially available semiconductor plating solution was used as the plating solution. Heat treatment at 200 to 500 °C and wire drawing were then repeatedly performed to form the wire to a diameter of 20 μm. After forming, heat treatment was performed under flow of N2 or Ar gas, so that the final elongation at break was approximately 5 to 15%.A heat treatment process was carried out with successive wire passage and was carried out with a flowing N2 or Ar gas. The wire feed speed was 20 to 200 m / min, the heat treatment temperature was 200 to 600 °C, and the heat treatment time was 0.2 to 1.0 second.

[0108] To analyze the concentration of the Pd cap layer and the Au- and Pd-containing alloy outer layer, Auger electron spectrometry was performed by sputtering or similarly processing the bond wire from its surface in the depth direction. Based on the resulting concentration profile in the depth direction, the thickness of the Pd cap layer, the thickness of the Au- and Pd-containing alloy outer layer, and the maximum Pd concentration were determined.

[0109] In Working Examples 3-1 to 3-50, an element selected from As, Te, Sn, Sb, Bi, and Se is contained in the core material. In Working Examples 3-51 to 3-56, Cu with 99.99 mass% purity was used for the core material, and As, Te, Sn, Sb, Bi, or Se were deposited on the wire surface (cover layer) by electroplating during the wire manufacturing process.

[0110] In Working Examples 3-34 to 3-44, Cu is caused to be present at an outermost surface of the bonding wire. In this regard, a column "Cu Concentration at Wire Surface" is provided in Table 8, and results obtained by measuring a surface of the bonding wire by an Auger electron spectroscopy device were entered therein. By selecting a temperature and time for heat-treating the bonding wire, Cu was caused to be present at an outermost surface at a specific concentration. In Working Examples 3-1 to 3-33 and 3-45 to 3-56, heat treatment conditions were applied that caused Cu to be absent at an outermost surface, and therefore, Cu was not detected by the Auger electron spectroscopy device.

[0111] The configurations of the samples prepared according to this procedure are listed in Tables 7 and 8. (Evaluation procedure)

[0112] A crystal structure was evaluated using a wire surface as the observation surface. An electron backscatter diffraction (EBSD) method was used as the evaluation method. The EBSD method is characterized by observing crystal orientations on an observation surface and graphically displaying the angular difference in crystal orientations between adjacent measurement points. The EBSD method can relatively easily observe crystal orientations with high accuracy, even for a thin wire such as the bond wire.

[0113] When performing the EBSD method with a curved surface such as the wire surface as the subject, care should be taken. If a region with a large curvature is measured, measurement with high accuracy is difficult. However, by fixing a bonding wire to be measured on a line on a plane, and measuring a flat part near the center of the bonding wire, measurement with high accuracy can be achieved. In particular, the measurement region shown below works well. The circumferential size is at most 50% of the wire diameter with the center in the wire longitudinal direction as the axis, and the wire longitudinal size is at most 100 μm. Preferably, the circumferential size is at most 40% of the wire diameter, and the wire longitudinal size is at most 40 μm, which can improve measurement efficiency by shortening measurement time.To further improve accuracy, it is desirable to measure at least three points to obtain mean information, taking deviations into account. The measurement points can be spaced at least 1 mm apart to avoid excessive proximity.

[0114] Regarding the orientation component of the crystal orientation <100> at an angle of at most 15 degrees to the wire longitudinal direction at the crystal orientations in the wire longitudinal direction in the cross section of the core material in the direction perpendicular to the wire axis of the bonding wire, and the average crystal grain size (µm) in the cross section of the core material in the direction perpendicular to the wire axis, were obtained by the same method as in Working Examples 1 to 59. Regarding the 0.2% offset yield strength and maximum yield strength, these were evaluated by the same method as in Working Examples 1 to 59, and a yield strength ratio was calculated by the above equation (1).

[0115] The bonding reliability of the ball bonded part was determined in a high-temperature and high-humidity or high-temperature environment by preparing a bonding reliability evaluation sample, performing HAST and HTS evaluation, and evaluating the bonding life of the ball bonded part in each test. The bonding reliability evaluation sample was prepared by performing ball bonding on an electrode formed by forming an Al-1.0%Si-0.5%Cu alloy film with a thickness of 0.8 μm on a Si substrate on a general metallic frame using a commercially available wire bonder and sealing it with a commercially available epoxy resin. A ball was formed by flowing an N2 + 5% H2 gas at a flow rate of 0.4 to 0.6 l / min, and its size ranged from 33 to 34 μm in diameter.

[0116] For the HAST evaluation, the manufactured sample for bond reliability evaluation was exposed to a high-temperature and high-humidity environment of 130°C and 85% relative humidity using an unsaturated-type vapor pressure tester and applied with a 5V bias voltage. A shear test was performed on the ball bonded part every 48 hours, and the time taken to reach a shear strength value of half the initial shear strength was determined as the bond life of the ball bonded part. The shear test after the high-temperature and high-humidity test was performed after removing a resin by acid treatment and exposing the ball bonded part.

[0117] A tester manufactured by DAGE was used as the shear tester for HAST evaluation. The average of measured values ​​from 10 randomly selected ball bonds served as the shear strength value. In this evaluation, in the "HAST" column in Tables 7 and 8, bond life under 96 hours was determined to be practically problematic and marked with a "cross" symbol; at least 96 hours and under 144 hours were determined to be practical but somewhat problematic and marked with a "triangle" symbol; at least 144 hours and under 288 hours were determined to be practically problem-free and marked with a "circle" symbol; at least 288 hours and under 384 hours were determined to be excellent and marked with a "double circle" symbol; and at least 384 hours were determined to be particularly excellent and marked with a "double circle pair" symbol.

[0118] For the HTS evaluation, the manufactured sample was exposed to a high-temperature environment of 200°C using a high-temperature thermostatic device for bond reliability evaluation. A shear test was performed on the ball bonded part every 500 hours, and the time taken to reach a shear strength value half the initial shear strength was determined as the bond life of the ball bonded part. The shear test after the high-temperature and high-humidity test was performed after removing the resin by acid treatment and exposing the ball bonded part.

[0119] A tester manufactured by DAGE was used as the shear tester for HTS evaluation. An average of the measured values ​​of 10 randomly selected ball bond pieces served as the shear strength value. In this evaluation, in the "HTS" column of Tables 7 and 8, bond life from at least 500 hours to less than 1000 hours was determined as practical but requiring improvement and marked with a "triangle" symbol; at least 1000 hours to less than 3000 hours was determined as practically satisfactory and marked with a "circle" symbol; and at least 3000 hours was determined as particularly excellent and marked with a "double circle" symbol.

[0120] To evaluate the sphere formation ability (FAB shape), a sphere was sampled and observed before bonding, and the presence or absence of voids on a surface of the sphere, as well as the presence or absence of deformation of the sphere, which is primarily a perfect sphere, were determined. The occurrence of any of the above cases was considered defective. The sphere was formed while bubbling with N2 gas at a flow rate of 0.5 l / min to reduce oxidation in a melting process. The sphere size was 34 µm. 50 spheres were observed for one condition. An SEM was used for observation.When evaluating the spherical forming ability, in the "FAB shape" column in Tables 7 and 8, a case where at least five defects occurred was determined as problematic and marked with a "cross" symbol, a case of three or four defects was determined as practical but somewhat problematic and marked with a "triangle" symbol, a case of one or two defects was determined as problem-free and marked with a "circle" symbol, and a case where no defects occurred was determined as excellent and marked with a "double circle" symbol.

[0121] The wedge bondability evaluation of the wire bonding part was performed by performing 1,000 bonding operations on the leads of a lead frame and assessing the frequency of bonding part debonding. A lead frame made of an Fe-42 at.% Ni alloy plated with 1 to 3 µm Ag was used for the lead frame. For this evaluation, assuming more severe bonding conditions than normal, a jig temperature was set to 150 °C, which was lower than a generally established temperature range.In this evaluation, in the “Wedge Bondability” column in Tables 7 and 8, a case where at least 11 defects occurred was determined as problematic and marked with a “cross” symbol, a case of 6 to 10 defects was determined as practical but somewhat problematic and marked with a “triangle” symbol, a case of 1 to 5 defects was evaluated as problem-free and marked with a “circle” symbol, and a case where no defect occurred was determined as excellent and marked with a “double circle” symbol.

[0122] The evaluation of the crimp shape of the ball bonded part was carried out by observing the ball bonded part from above immediately after bonding and evaluating its circularity. An electrode in which an Al-0.5% Cu alloy film with a thickness of 1.0 µm was formed on a Si substrate was used as the object to be bonded with the bonding wire. Observation was carried out using an optical microscope, and 200 locations were observed for one condition. Elliptical shapes with a significant deviation from a perfect circle and anisotropic deformation were determined as defective crimp shapes of the ball bonded part.In this evaluation, in the “squeeze shape” column in Tables 7 and 8, a case of at least six defects occurring was determined as problematic and marked with a “cross” symbol, a case of four or five defects was determined as feasible but somewhat problematic and marked with a “triangle” symbol, one to three were determined as problem-free and marked with a “circle” symbol, and a case in which a favorable perfect circle was obtained for all was determined as particularly excellent and marked with a “double circle” symbol. [Skewed]

[0123] 100 bonding operations with a 5 mm loop length and a 0.5 mm loop height were performed on a lead frame for evaluation. As an evaluation method, an upright wire portion was observed from the horizontal chip direction, and evaluation was performed based on a distance when the distance between a perpendicular passing through the center of the ball bond portion and the upright wire portion was maximized (skew distance). If the skew distance was smaller than the wire diameter, the skew was determined to be favorable. Whereas if the skew distance was larger, the upright portion exhibited skew, and the skew was determined to be defective. One hundred bond wires were observed with an optical microscope, and the number of skew defects was counted.In the “Skewedness” column in Tables 7 and 8, a case in which at least seven errors occurred was determined as problematic and marked with a “cross” symbol, a case of four to six errors was determined as feasible but somewhat problematic and marked with a “triangle” symbol, a case of one to three errors was determined as problem-free and marked with a “circle” symbol, and a case in which no errors occurred was determined as excellent and marked with a “double circle” symbol. (Evaluation results)

[0124] The bonding wires according to Working Examples 3-1 to 3-56 each comprise a Cu alloy core material and a Pd cap layer formed on the surface of the Cu alloy core material. The bonding wire contains at least one or more elements selected from As, Te, Sn, Sb, Bi, and Se, with a total element concentration of 0.1 to 100 ppm by mass relative to the entire wire. It was found that with this configuration, the bonding wires according to Working Examples 3-1 to 3-50 can achieve ball bonding reliability in the HAST test in a high-temperature and high-humidity environment of 130°C and 85% relative humidity.

[0125] In the working examples, which further comprise an Au and Pd-containing alloy outer layer on the Pd cap layer, it was found that excellent wedge bondability can be obtained when a thickness of the Au and Pd-containing alloy outer layer is 0.0005 to 0.050 µm.

[0126] In Working Examples 3-21 to 3-33, 3-35, 3-37, and 3-39 to 3-44, it was found that the high-temperature reliability of the ball bonding part is favorable by the HTS evaluation because the bonding wire further contains at least one or more elements selected from Ni, Zn, Rh, In, Ir, Pt, Ga, and Ge, and a concentration of each of the elements except Pd is 0.011 to 1.2 mass% relative to the entire wire, and a concentration of Pd contained in the Cu alloy core material is 0.05 to 1.2 mass%.

[0127] In Working Examples 3-22 to 3-26 and 3-29 to 3-32, the FAB shape was favorable and the wedge bondability was advantageous when the bonding wire further contains at least one or more elements selected from B, P, Mg, Ca, and La, and a concentration of each of the elements is 1 to 100 ppm by mass relative to the entire wire.

[0128] In Working Examples 3-34 to 3-44, the wire contains As, Te, Sn, Sb, Bi, and Se, and Cu was present at an outermost surface of the wire. With this configuration, Working Examples 3-34 to 3-44 had a "double circle pair" symbol or a "double circle" symbol in the HAST evaluation results, indicating the effect of causing Cu to be present at an outermost surface.

Claims

[1] Bonding wire for a semiconductor device, the bonding wire comprising: a Cu alloy core material; and a Pd cap layer formed on a surface of the Cu alloy core material, wherein the bonding wire contains an element that ensures bonding reliability in a high temperature environment, and a yield strength ratio defined by the following equation (1) is 1.1 to 1.6: Yield strength ratio = maximum yield strength / 0.2% offset yield strength. (1) [2] The bonding wire for a semiconductor device according to claim 1, wherein a thickness of the Pd cap layer is 0.015 to 0.150 µm. [3] A bonding wire for a semiconductor device according to claim 1 or 2, further comprising an Au and Pd-containing alloy outer layer on the Pd cap layer. [4] A bonding wire for a semiconductor device according to claim 3, wherein a thickness of the Au and Pd-containing alloy outer layer is at most 0.050 µm. [5] A bonding wire for a semiconductor device according to any one of claims 1 to 4, wherein the bonding wire contains at least one element selected from Ni, Zn, Rh, In, Ir and Pt, and a concentration of the at least one element in total is 0.011 to 2 mass% relative to the entire wire. [6] A bonding wire for a semiconductor device according to any one of claims 1 to 5, wherein the bonding wire contains one or more elements selected from Ga and Ge, and a concentration of the elements in total is 0.011 to 1.5 mass% relative to the entire wire. [7] A bonding wire for a semiconductor device according to any one of claims 1 to 6, wherein the bonding wire contains at least one or more elements selected from As, Te, Sn, Sb, Bi and Se, a total concentration of the elements is 0.1 to 100 ppm by mass relative to the entire wire and Sn ≤ 10 ppm by mass; Sb ≤ 10 ppm by mass; and Bi ≤ 1 ppm by mass. [8] A bonding wire for a semiconductor device according to any one of claims 1 to 7, wherein the bonding wire further contains at least one element selected from B, P, Mg, Ca and La, and a concentration of each of the at least one element is 1 to 200 ppm by mass relative to the entire wire. [9] A bonding wire for a semiconductor device according to any one of claims 1 to 8, wherein Cu is present at an outermost surface of the bonding wire.

Citation Information

Patent Citations

  • Copper alloy wire for connecting semiconductor element

    JP1986048543A

  • Bonding wire and integrated circuit device using the same

    JP2005167020A

  • Gold-coated copper wire for ball bonding

    JP2012036490A

  • Bonding wires for semiconductor devices

    JP4904252B2

  • JP000004904252B2