Composition for brazing, heat exchanger tube and heat exchanger
A soldering composition with zinc metal powder, acrylic resin, and specific solvents addresses uneven zinc coverage and productivity issues, achieving uniform zinc diffusion and improved corrosion resistance in heat exchanger tubes.
Patent Information
- Application Number
- DE112016003080
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-07-06
- Filing Date
- 2016-03-04
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2036-03-04
AI Technical Summary
Existing soldering compositions for aluminum components in heat exchangers face issues with storage stability due to sedimentation of zinc powder, leading to uneven coverage and reduced productivity.
A soldering composition comprising zinc metal powder, a (meth)acrylic resin, and specific organic solvents with defined mass ratios, which enhances uniformity and drying speed, ensuring even zinc diffusion and improved corrosion resistance.
The composition achieves high productivity and stability by forming a uniform zinc diffusion layer, enhancing corrosion resistance and ensuring consistent application on heat exchanger tubes.
Abstract
Description
TECHNICAL FIELD
[0001] One embodiment of the present invention relates to a brazing composition having excellent productivity and deposition stability. BACKGROUND
[0002] Conventionally, components made of aluminum or aluminum alloys are used, e.g., for aluminum heat exchangers in the automotive sector, represented by an evaporator, a condenser, and the like, which are mounted in vehicles. When brazing these components, brazing fluxes or mixtures (brazing compositions) of fluxes, brazing fillers (metals), and binder resins are used. These fluxes or mixtures are applied to the areas to be brazed, and then a brazing and heating process is carried out.
[0003] A coating layer of Zn (zinc) is formed on the surface of a heat exchanger tube used in a heat exchanger to improve corrosion resistance. Such a coating layer is formed using Zn-containing fluxes or Zn powders as brazing fillers. However, Zn has a significantly high specific gravity, so the Zn powders settle while a brazing composition containing Zn powder is stored. This causes differences in concentration between the Zn powders and prevents the brazing composition from being evenly applied to the surface of the heat exchanger tube.
[0004] To solve such a problem, for example, Patent Document 1 proposes a non-aqueous zinc flux paint containing a flux comprising zinc fluoride; (meth)acrylic resin; alcoholic solvent; and at least one anti-settling agent selected from the group consisting of aliphatic polyols having 3 to 6 carbon atoms, oligomers of aliphatic polyols having 2 to 3 carbon atoms, monoesters having 3 to 7 carbon atoms comprising aliphatic polyols and aliphatic carboxylic acids, and polymers of aliphatic polyols having a weight-average molecular weight of 1,000 or less.
[0005] Because the non-aqueous zinc flux paint disclosed in Patent Document 1 is capable of inhibiting the occurrence of sediments such as fluxes or metal powders, it has excellent storage stability.
[0006] However, such a non-aqueous zinc flux paint requires the fixation of the flux and metal powders after being applied to the component surface. Therefore, the non-aqueous zinc flux paint should be kept for a certain period of time in a temperature range where the solvent evaporates, resulting in lower productivity. To improve productivity, it is necessary to improve the dryness of the brazing composition. Furthermore, to form a uniform Zn coating layer, a more uniform application of the brazing composition (application stability) is required. STATUS OF THE TECHNICAL PATENT DOCUMENT
[0007] Patent Document 1: Publication of Unexamined Japanese Patent Application No. 2013-107104 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0008] The problem according to one embodiment of the present invention is to provide a brazing composition having excellent productivity and deposition stability. MEANS TO SOLVE THE PROBLEMS
[0009] The brazing composition according to one embodiment of the present invention contains a flux, a Zn metal powder, a (meth)acrylic resin, and an organic solvent, wherein the organic solvent contains (A1) a monohydric alcohol having 5 carbon atoms; (A2) a monohydric alcohol having 6 to 8 carbon atoms; and (A3) a polyhydric alcohol having 3 or fewer carbon atoms connected by a carbon-carbon bond, wherein the mass ratio ((A1) / (A2)) of the (A1) and (A2) components is in the range of 0.25 to 4, and the mass ratio ((A1) / (A3)) of the (A1) and (A3) components is in the range of 0.2 to 4.
[0010] The heat exchanger tube according to an embodiment of the present invention includes a tube body and a coating layer formed of the above-mentioned composition for brazing on an outer surface of the tube body.
[0011] The heat exchanger according to an embodiment of the present invention comprises the above-mentioned heat exchanger tube. EFFECT OF THE INVENTION
[0012] The brazing composition according to an embodiment of the present invention possesses excellent productivity and deposition stability. Therefore, when the brazing composition according to an embodiment of the present invention is used, for example, as a starting material for the covering layer formed in a heat exchanger tube, a heat exchanger tube can be efficiently manufactured, and a uniform covering layer can be formed. PREFERRED EMBODIMENTS FOR CARRYING OUT THE INVENTION
[0013] The brazing composition according to one embodiment of the present invention contains a flux, a Zn metal powder, a (meth)acrylic resin, and an organic solvent. Each of the components will be described in detail below. As used herein, the term "(meth)acrylic" refers to "acrylic" or "methacrylic," and "(meth)acrylate" refers to "acrylate" or "methacrylate." <flussmittel>
[0014] The flux contained in the brazing composition according to one embodiment of the present invention is used to remove oxide films. Examples of the flux include potassium fluoroaluminate, potassium fluoride, aluminum fluoride, lithium fluoride, sodium fluoride, potassium fluoroaluminate-cesium complex (non-reactive cesium-type flux), cesium fluoroaluminate (non-reactive cesium-type flux), potassium fluorozincate (reactive zinc-substituted flux), and cesium fluorozincate (reactive zinc-substituted flux).
[0015] In the brazing composition, the flux is contained in a proportion preferably ranging from 5 to 32% by mass, more preferably from 10 to 30% by mass. When the flux is contained in such a proportion, the oxide films can be effectively removed. The fluxes can be used alone or in combination of two or more types. <zn-metallpulver>
[0016] The Zn metal powder contained in the brazing composition according to one embodiment of the present invention is melted by heating during brazing, so that a Zn diffusion layer is formed on the deposition surface. As a result, corrosion resistance can be improved. The Zn metal powder is not particularly limited, and, for example, a Zn metal powder with an average particle size in the range of 2 to 5 µm, preferably 3 to 4 µm, is used. The average particle size is measured, for example, using a "Laser Diffraction Scattering Type Particle Size Analyzer MT3000II" manufactured by Nikkiso Co., Ltd.
[0017] The Zn metal powder is contained in the brazing composition in a proportion of preferably 5 to 32 mass%, more preferably 10 to 30 mass%. When the Zn metal powder is contained in such a proportion, the Zn diffusion layer is easily formed with a uniform and sufficient thickness, enabling further improvement in corrosion resistance. < (Meth) acrylic resin>
[0018] The (meth)acrylic resin contained in the brazing composition according to one embodiment of the present invention serves as a binder and is used to ensure uniform adhesion of the brazing composition. The (meth)acrylic resin is a polymer produced by polymerizing (meth)acrylic compounds such as acrylic acid, methacrylic acid, and (meth)acrylate.
[0019] Examples of the (meth)acrylate include methyl (meth)acrylates, ethyl (meth)acrylates, hydroxyethyl (meth)acrylates, butyl (meth)acrylates, 2-ethylhexyl (meth)acrylates, 2,2-dimethyl lauryl (meth) acrylates, 2,3-dimethyl lauryl (meth) acrylates, 2,2-dimethyl stearyl (meth) acrylates, 2,3-Dimethylstearyl (meth)acrylates, isolauryl (meth)acrylates, isomyristyl (meth)acrylates, isostearyl (meth)acrylates and isobehenyl (meth)acrylates.
[0020] The (meth)acrylic resin may be a homopolymer of a (meth)acrylic compound or a copolymer comprising two or more types of (meth)acrylic compounds. Alternatively, it may be a copolymer comprising a (meth)acrylic compound and another monomer copolymerizable with the (meth)acrylic compound. Examples of the other monomer include acrylamide and styrene. The other monomer is adjusted to less than 50 mol% in the monomer components constituting the copolymer.
[0021] The weight-average molecular weight of the (meth)acrylic resin is not particularly limited, and is preferably in the range of 10,000 to 600,000, more preferably 50,000 to 500,000. The weight-average molecular weight is a value converted by gel permeation chromatography based on polystyrene. The weight-average molecular weight of the (meth)acrylic resin can be appropriately adjusted by adjusting the blending amount of a radical polymerization initiator or a chain transfer agent.
[0022] The (meth)acrylic resin has an acid value (measurement method: according to JIS K 2501) of preferably 0 to 65 mg KOH / g, more preferably 15 to 40 mg KOH / g, but is not limited thereto. The acid value is adjusted, for example, by the proportion of acrylic acid, methacrylic acid, or the like.
[0023] The method for synthesizing the (meth)acrylic resin is not particularly limited, and a known method can be used. For example, the monomer component constituting the (meth)acrylic resin can be subjected to radical polymerization using a solvent, a polymerization initiator, a chain transfer agent, or the like, as required. The polymerization initiator used for radical polymerization is not particularly limited as long as it is a compound that decomposes to form radicals. Examples of the polymerization initiator include azo-type initiators and peroxide-type initiators. If a solvent is used, one of the organic solvents described below can be used, for example.The use of the organic solvent described below makes it possible to use such an organic solvent as it is without removing the solvent.
[0024] The (meth)acrylic resin is preferably contained in the brazing composition in a proportion of 0.5 to 15 mass%, more preferably 3 to 10 mass%. When the (meth)acrylic resin is contained in such a proportion, the brazing composition can adhere more uniformly. The (meth)acrylic resins can be used individually or in combination of two or more types. <Organisches Lösungsmittel>
[0025] The organic solvent contained in the brazing composition according to one embodiment of the present invention contains the following (A1), (A2) and (A3) components. (A1) Monohydric alcohol with 5 carbon atoms (A2) Monohydric alcohol with 6 to 8 carbon atoms (A3) Polyhydric alcohol having 3 or fewer carbon atoms linked by a carbon-carbon bond.
[0026] Among organic solvents, the (A1) component is used for dryness and compatibility with other components. That is, by including the (A1) component with a relatively low boiling point in the brazing composition, the organic solvent tends to evaporate, thereby improving dryness. In addition to alcohols, low-boiling-point organic solvents are available, but such organic solvents exhibit poor compatibility with other components. Furthermore, organic solvents with excessively low boiling points impair deposition stability and productivity due to an excessively high evaporation rate.
[0027] Specific examples of the (A1) component include methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, sec-butyl alcohol, tert-butyl alcohol, 3-methoxy-1-butanol, ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), diethylene glycol methyl ether (methyl carbitol), propylene glycol monomethyl ether, and propylene glycol monoethyl ether. Of these, a monohydric alcohol having 5 carbon atoms is preferred, and 3-methoxy-1-butanol is more preferred.
[0028] The (A1) component is included in the brazing composition in a proportion preferably ranging from 1 to 83.5 mass%. The (A1) components can be used individually or in combination of two or more types.
[0029] Among the organic solvents, the (A2) component is used to ensure uniformity after application. Specific examples of the (A2) component include ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol ethyl ether (ethyl carbitol), diethylene glycol butyl ether (butyl carbitol), propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and 3-methoxy-3-methyl-1-butanol. Of these, 3-methoxy-3-methyl-1-butanol is preferred.
[0030] The (A2) component is included in the brazing composition in a proportion preferably ranging from 1 to 83.5 mass%. The (A2) components can be used individually or in combination of two or more types.
[0031] Among organic solvents, the (A3) component is used to prevent settling of the Zn metal powder or the like. Compared with the case of using a polyhydric alcohol other than the (A3) component (e.g., hexylene glycol, etc.), the use of the (A3) component can more effectively prevent settling of the Zn metal powder or the like. Examples of the (A3) component include the following (A31) and (A32) components. (A31) Component: A compound having 3 or fewer carbon atoms and having at least 2 hydroxyl groups in its molecule; (A32) Component: a compound in which a hydrocarbon unit having 3 or fewer carbon atoms is bonded in plurality through a heteroatom (oxygen atom, etc.) and which has at least 2 hydroxyl groups in its molecule.
[0032] Specific examples of the (A31) component include ethylene glycol, propylene glycol, trimethylene glycol, and glycerin. Specific examples of the (A32) component include polyols where at least one of oxyethylene and oxypropylene is bonded in plural, e.g., diethylene glycol, triethylene glycol, and dipropylene glycol.
[0033] Of the (A3) components, the (A31) component is preferred, and propylene glycol is more preferred. The (A3) component is contained in the brazing composition in an amount ranging preferably from 5 to 20 mass%, more preferably from 10 to 15 mass%. The (A3) components can be used individually or in combination of two or more types.
[0034] In the organic solvent contained in the brazing composition according to one embodiment of the present invention, the (A1) and (A2) components are contained in a mass ratio ((A1) / (A2)) ranging from 0.25 to 4 to improve productivity and deposition stability. Furthermore, the (A1) and (A3) components are contained in a mass ratio ((A1 / (A3)) ranging from 0.2 to 4. <Zusammensetzung für das Hartlöten>
[0035] The brazing composition according to one embodiment of the present invention is prepared by mixing the flux, the Zn metal powder, the (meth)acrylic resin, and the organic solvent as described above, and stirring the mixture. The mixing and stirring methods are not particularly limited, and the components can be stirred by a known method to be evenly mixed.
[0036] The brazing composition according to one embodiment of the present invention may optionally contain various additives, as long as the effect of the brazing composition according to one embodiment of the present invention is not impaired. Examples of such an additive include antioxidants (dibutylhydroxytoluene, etc.), corrosion inhibitors (benzotriazole, etc.), antifoaming agents (silicone oil, etc.), thickeners (wax, hydrogenated oil, fatty acid amides, polyamides, etc.), colorants, and amino alcohols. For example, the addition of a thickener enables further improvement of the storage stability, anti-sinking properties, and brazing performance of the brazing composition.
[0037] The brazing composition according to one embodiment of the present invention is prepared to have a solid component concentration in the range of, for example, 15 to 85 mass%, preferably 30 to 70 mass%, more preferably 45 to 60 mass%. The solid component concentration can be adjusted by, for example, the amount of the organic solvent used. Furthermore, in view of processability, the brazing composition according to one embodiment of the present invention is prepared to have a viscosity (25°C) in the range of, for example, 50 to 1,000 mPa·s, preferably 100 to 60 mPa·s. The viscosity is measured using an "E-type viscometer (100 rpm / 1°34' cone)" manufactured by Toki Sangyo Co., Ltd.
[0038] The thus-obtained brazing composition according to one embodiment of the present invention exhibits excellent productivity and deposition stability. Thus, when the brazing composition is used, for example, as a raw material for the coating layer formed on a heat exchanger tube, a heat exchanger tube can be effectively manufactured, and a uniform coating layer can be formed. The heat exchanger tube may have the brazing composition according to one embodiment of the present invention coated thereon so as to form, for example, a coating layer having a thickness of 2 to 10 μm on the outer surface of the tube body. A heat exchanger comprising such a heat exchanger tube is suitably mounted, for example, in vehicles such as automobiles. EXAMPLES
[0039] One embodiment of the present invention will be specifically described below by illustrative examples and comparative examples, but it is not intended to limit one embodiment of the present invention to these examples. Example 1
[0040] The following components were mixed in the following proportions, and the mixture was sufficiently stirred to prepare a brazing composition. A resin derived from NHM-SW71-15MMB (manufactured by Harima Chemicals, Inc.) was used as the methacrylic resin. FL-7SS (manufactured by Morita Chemical Industries Co., Ltd.) was used as the flux. Methacrylic resin: 8.9% by mass Flux: 23.6 mass% Zn metal powder: 23.6 mass% 3-Methoxy-3-methyl-1-butanol: 20.3% by mass 3-Methoxy-1-butanol: 8.6% by mass Propylene glycol: 15% by mass Examples 2 to 16 and Comparative Examples 1 to 5
[0041] A brazing composition was prepared in the same manner as in Example 1, except that the components listed in Tables 1 and 2 were mixed in the proportions listed in Tables 1 and 2. <auswertung>
[0042] The brazing compositions obtained in Examples 1 to 16 and Comparative Examples 1 to 5 were evaluated for (1) deposition stability, (2) Zn diffusion, (3) productivity, and (4) brazing performance. The results are shown in Tables 1 and 2. If none of (1) to (4) was rated as (-), the brazing composition was rated as excellent. (1) Order stability
[0043] The brazing composition was applied to the outer surface of a tube body (length: approximately 10 cm) of a heat exchanger tube and then dried. After drying, the mass (W1) of the tube body on which a coating layer had been formed was weighed with a precision balance. Next, the coating layer was removed with acetone, and the mass (W0) of the tube body after removal of the coating layer was weighed. Then, the area (A1) of the coated surface of the tube body was determined, and the dried coating amount (g / m 2 ) was calculated using the following formula (I). The difference between the resulting dried application amount and the desired dried application amount (calculated dried application amount) was determined and evaluated based on the following criteria. Dried application amount (g / m2)=(W1−W0) / A1 ++ The difference between the desired dried application amount and the actual dried amount was less than ± 0.5 g / m 2 and continuous application control was possible. + The difference between the desired dried application amount and the actual dried amount was less than ± 1.0 g / m 2 and continuous application control was possible. - The difference between the desired dried application amount and the actual dried amount was ± 1.0 g / m 2 or more, and uneven application occurred. (2) Zn diffusion
[0044] The Zn diffusion layer in the cross-sectional direction of the tube body, where the coating layer was formed, was observed using an electron probe microanalyzer (EPMA). The Zn diffusion depth was determined, and Zn diffusion was evaluated based on the following criteria. The deeper the Zn diffusion depth, the more favorable the Zn diffusion layer was formed, resulting in outstanding corrosion resistance. ++ The Zn diffusion depth was 100 µm or more. + The Zn diffusion depth was 50 µm or more and less than 100 µm. - The Zn diffusion depth was less than 50 µm. (3) Productivity
[0045] The brazing composition was applied to the outer surface of the tube body (length: about 10 cm) of a heat exchanger tube in an amount of 5 g / m 2 and held at 150°C for 15 seconds. The applied surface was then visually observed and evaluated based on the following criteria. ++ Completely dried and solidified. + There were some undried areas, but it was almost solidified. - Undried, not solidified and peeling of the coating occurred. (4) Brazing properties
[0046] An aluminum component to which the brazing composition had been applied (JIS-A1050, 60 mm × 25 mm × 1.0 mm) was used as the horizontal component. On the other hand, a brazing sheet on which a silicon-aluminum alloy (brazing filler) was plated on an aluminum alloy containing 1.2 mass% manganese and 2.5 mass% zinc was used as the vertical component (55 mm × 25 mm × 0.2 mm). Next, the vertical component was aligned in an inverted T-shape using the brazing composition and then fixed to the horizontal component using a stainless steel wire to obtain a test piece for evaluating brazing properties. Then, brazing was carried out using an atmospheric box-type electric furnace (A(V)-BC-M, manufactured by NORITAKE TCF Co., Ltd.).) The thus obtained test piece was heated at 605°C under a nitrogen atmosphere (oxygen concentration: 100 ppm or less) to perform brazing. The brazed areas were visually observed, thereby evaluating them based on the following criteria. In Comparative Examples 1, 2, and 5, the deposition stability was poor, so the brazing properties were not evaluated. ++ A complete fillet weld with a height of 20 mm or more on one side was formed, and sufficient joint strength was obtained. + A fillet weld with a height of 10 mm or more and less than 20 mm on one side was formed, and overall joint strength was obtained. - The evaluation of the brazing properties was not carried out.
[0047] From Table 1, it can be concluded that the brazing compositions obtained in Examples 1 to 16 generally exhibit the required brazing properties and have excellent effects on deposition stability, Zn diffusion, and productivity. On the other hand, it can be concluded from Table 2 that the brazing compositions obtained in Comparative Examples 1 to 5 are rated as (-) in at least one of deposition stability, Zn diffusion, and productivity and have poor effects.< / auswertung> < / flussmittel>
Claims
[1] A brazing composition comprising a flux, a Zn metal powder, a (meth)acrylic resin and an organic solvent, wherein the organic solvent comprises the following (A1), (A2) and (A3) components: (A1) monohydric alcohol with 5 carbon atoms (A2) monohydric alcohol with 6 to 8 carbon atoms (A3) polyhydric alcohol having 3 or fewer carbon atoms bonded by a carbon-carbon bond, wherein the mass ratio ((A1) / (A2)) of the (A1) and (A2) components is in the range of 0.25 to 4, and the mass ratio ((A1) / (A3)) of the (A1) and (A3) components is in the range of 0.2 to 4. [2] The brazing composition according to claim 1, wherein the (A1) component comprises 3-methoxy-1-butanol. [3] A brazing composition according to claim 1 or 2, wherein the (A2) component comprises 3-methoxy-3-methyl-1-butanol. [4] A brazing composition according to any one of claims 1 to 3, wherein the (A3) component comprises propylene glycol. [5] A heat exchanger tube comprising a tube body and a coating layer formed from the brazing composition according to any one of claims 1 to 4 on an outer surface of the tube body. [6] A heat exchanger comprising the heat exchanger tube defined in claim 5.
Citation Information
Patent Citations
Manufacturing method for aluminum brazing composition and brazing method for inner fin tube
JP2012024788A
Nonaqueous zinc flux paint
JP2013107104A
Brazing composition, tube for heat exchanger and heat exchanger
JP2014083570A
JP002012024788A
JP002013107104A