Semiconductor device and method for manufacturing a semiconductor device

The semiconductor device's innovative design with an overhang electrode and insulating layer structure addresses peeling and cracking issues by misaligning solder and electrode end portions, enhancing longevity and preventing stress concentration.

DE112019006936B4Active Publication Date: 2024-11-07MITSUBISHI ELECTRIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE112019006936
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-02-28
Publication Date
2024-11-07
Estimated Expiration
2039-02-28

AI Technical Summary

Technical Problem

The existing semiconductor devices face issues with peeling and cracking at the interface between metal and resin layers due to stress concentration at the end portions of the solder and nickel film, leading to a reduced lifespan.

Method used

The semiconductor device incorporates a design with a second electrode having an overhang portion and an insulating layer that covers a part of the overhang portion closer to its end than the solder, preventing alignment of the solder and electrode end portions, and includes a conductive film that restricts solder wetting and spreading, thereby minimizing crack propagation.

Benefits of technology

This design effectively prevents cracks from developing into the electrode, ensuring a longer service life and maintaining the device's integrity by avoiding stress concentration and peeling, while also ensuring the bonding area remains within the active region.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Semiconductor device (100, 200, 300), comprising: - a semiconductor substrate (10); - a first electrode (12) which is arranged on the semiconductor substrate (10); - an insulating layer (16) comprising a first part (16a) arranged on an upper surface of the first electrode (12); - a second electrode (14, 214, 314) having a main part area (14a) and an overhang part area (14b), wherein the main part area (14a) is arranged on the upper surface of the first electrode (12), wherein the overhang part area (14b) is connected to the main part area (14a) and extends over the first part (16a) of the insulating layer (16); - a solder metal (18) covering an upper surface of the main part area (14a) and part of an upper surface of the overhang part area (14b) that is connected to the upper surface of the main part area (14a) of the second electrode (14, 214, 314); and - a molding resin (20) which covers the insulating layer (16) and the solder metal (18); wherein the insulating layer (16) comprises: - a second part (16c) covering a part of the upper surface of the overhang sub-area (14b), wherein the part of the upper surface of the overhang sub-area (14b) covered by the insulating layer (16) is closer to an end sub-area (14c) of the overhang sub-area (14b) than the part covered by the solder (18); and - a third part (16b) connecting the first part (16a) and the second part (16c) and covering the end part area (14c) of the overhang sub-area (14b); wherein a length of the second part (16c) of the insulating layer (16) from the end part area (14c) of the overhang sub-area (14b) is shorter than a length of the first part (16a) of the insulating layer (16) from the end part area (14c) of the overhang sub-area (14b).
Need to check novelty before this filing date? Find Prior Art

Description

Area

[0001] The present invention relates to a semiconductor device and a method for manufacturing the semiconductor device. background

[0002] JP 2018-046151 A (PTL 1) discloses a semiconductor device comprising a semiconductor substrate, a first AlSi layer covering at least a portion of a surface of the semiconductor substrate, and a polyimide film covering a portion of a surface of the first AlSi layer. This semiconductor device further includes a second AlSi layer covering at least a portion of a surface of the polyimide film and extending from above the polyimide film to the first AlSi layer in a region not covered with the polyimide film. Furthermore, a region extending across a surface of the first AlSi layer in the region not covered with the polyimide film and a surface of the second AlSi layer is covered with a nickel layer. An upper surface of the nickel layer is bonded to a solder layer. Quotation list

[0003] JP 2017-084 911 A discloses a semiconductor module in which a second electrode layer is hardly detached from an insulating resin layer.A semiconductor module includes: a first electrode layer covering the surface of a semiconductor substrate; a first insulating resin layer covering the outer peripheral portion on the surface of the first electrode layer; a second electrode layer covering a region from the central portion on the surface of the first electrode layer to the surface of the first insulating resin layer; a second insulating resin layer covering a region spanning the surface of the first insulating resin layer in a range from the surface of the second electrode layer to a portion not covered with the second electrode layer, so as to cover the end of the second electrode layer disposed on the first insulating resin layer; and a solder layer covering the surface of the second electrode layer in a region not covered with the second insulating resin layer.In a direction from the outer peripheral side to the inner peripheral side of the first electrode layer, the end on the inner peripheral side of the second insulating resin layer is arranged at a position on an inner peripheral side than the end on the inner peripheral side of the first insulating resin layer or at the same position as the end on the inner peripheral side of the first insulating resin layer.

[0004] JP 2018-137290 A relates to a semiconductor device configured to prevent cracks in an AlSi layer. The proposed semiconductor device comprises a semiconductor substrate; an AlSi layer covering a surface of the semiconductor substrate; an insulating resin layer partially covering a surface of the AlSi layer; and a nickel layer covering a region extending from at least a partial surface of the insulating resin layer to the surface of the AlSi layer in a region not covered by the insulating resin layer, forming a flat surface on a surface of the layer. An interface between the AlSi layer and the nickel layer is bonded to the end surface of the insulating resin layer.

[0005] The publication "PVD Processing for Flip Chip: Considering Adhesion Layer Properties" by Keigler et al. describes packaging processes that use physical vapor deposition (PVD) for gold bumping, solder bumping, redistribution (RDL), and integrated passive components. A crucial element of PVD is the first layer, which attaches subsequent structures to the device elements. Titanium and titanium-tungsten are most commonly used as adhesion and barrier layers for these applications. The choice of metal to be used depends on both the material properties and reactions with neighboring metals, as well as compatibility with subsequent processing. SummaryTechnical problem

[0006] In the semiconductor device of PTL 1, when the positions of one end portion of the solder and one end portion of the Ni film coincide, a stress tends to occur at which the Ni film begins to peel off from one end. Since the adhesion between the metal and the resin is generally weak, peeling occasionally occurs at the interface between the nickel layer and the polyimide film. Furthermore, a crack may develop from the point where the aluminum film begins to peel off.

[0007] The present invention has been made to solve the above-mentioned problem, and it is an object of the present invention to provide a semiconductor device achieving a long lifetime and a manufacturing method of the semiconductor device. Solution to the problem

[0008] The object underlying the invention is achieved in semiconductor devices according to the invention with the features of claim 1 and alternatively with the features of claim 2, and in a manufacturing method for a semiconductor device according to the invention with the features of claim 11. Advantageous further developments are the subject of the respective dependent claims.

[0009] A semiconductor device according to the invention of the present application comprises a semiconductor substrate, a first electrode arranged on the semiconductor substrate, an insulating layer having a first part arranged on an upper surface of the first electrode, a second electrode having a main portion and an overhang portion, the main portion being arranged on the upper surface of the first electrode, the overhang portion being connected to the main portion and extending above the first part, a solder covering an upper surface of the main portion and a part of an upper surface of the overhang portion being connected to the upper surface of the main portion of the second electrode, and a molding resin covering the insulating layer and the solder, the insulating layer having a second part,which covers a part of the upper surface of the overhang portion, wherein the part of the upper surface of the overhang portion covered by the insulating layer is closer to an end portion of the overhang portion than the part covered by the solder, and has a third part connecting the first part and the second part and covering the end portion of the overhang portion.

[0010] A semiconductor device according to the invention of the present application comprises a semiconductor substrate, a first electrode disposed on the semiconductor substrate, an insulating layer disposed on an upper surface of the first electrode, a second electrode having a main portion and an overhang portion, the main portion being disposed on the upper surface of the first electrode, the overhang portion being connected to the main portion and extending above the insulating layer, a solder covering an upper surface of the main portion and a part of an upper surface of the overhang portion connected to the upper surface of the main portion of the second electrode, and a conductive film covering a part of the upper surface of the overhang portion.wherein the part is closer to an end portion of the overhang portion than the part covered by the solder, wherein wetting and spreading of the solder on the conductive film is more difficult than on the second electrode.,

[0011] A manufacturing method for a semiconductor device according to the invention of the present application includes a step of forming a first electrode on a semiconductor substrate, a step of forming a first insulating layer on an upper surface of the first electrode, an electrode forming step of forming a second electrode thereover from an upper surface of the first electrode to an upper surface of the first insulating layer, a step of forming a second insulating layer on the first insulating layer to cover an end portion of an overhang portion of the second electrode, the overhang portion extending over the first insulating layer, and a part of an upper surface of the overhang portion, the part being connected to the end portion, a step of forming a solder to bond an upper surface of a main portion of the second electrode,wherein the main portion is a portion located on the upper surface of the first electrode and covers a portion of the upper surface of the overhang portion, wherein the portion of the upper surface of the overhang portion covered with the insulating layer is closer to the main portion than the portion covered by the second insulating layer, and a step of sealing the semiconductor device with a molding resin after forming the solder; wherein a length of a portion of the second insulating layer from the end portion of the overhang portion, the portion covering the upper surface of the overhang portion, is shorter than a length of the first insulating layer from the end portion of the overhang portion. Advantageous effects of the invention

[0012] In the semiconductor device according to the invention, the position of the solder end portion and the position of an end portion of the second electrode do not coincide due to the second portion of the insulating layer or a conductive film. Therefore, it is difficult for a crack to develop toward the second electrode. Furthermore, even in a case where brittle fracture has occurred in the second electrode, since an insulating layer is disposed directly under the solder end portion, crack generation in the first electrode can be prevented. Thus, a long lifetime of the semiconductor device can be achieved.

[0013] In the manufacturing method for the semiconductor device according to the invention, the position of the solder end portion and the position of the second electrode end portion do not coincide due to the second portion of the insulating layer. Therefore, it is difficult for a crack to develop toward the second electrode. Furthermore, even in a case where brittle fracture has occurred in the second electrode, since an insulating layer is disposed directly under the solder end portion, crack generation in the first electrode can be prevented. Consequently, a long lifetime of the semiconductor device can be achieved. Short description of the drawings Fig. 1 is a cross-sectional view of a semiconductor device according to a first embodiment. Fig. 2 is a view illustrating a state in which an external electrode is disposed on the semiconductor device according to the first embodiment. Fig. 3 is a view describing a structure of the second electrode according to the first embodiment. Fig. 4 is a view for describing a manufacturing method of the semiconductor device according to the first embodiment. Fig. 5 is a view for describing the structure of a semiconductor device according to a second embodiment. Fig. 6 is a view for describing a manufacturing method of the semiconductor device according to the second embodiment. Fig. 7 is a view for describing a structure of a semiconductor device according to a third embodiment. Fig. 8 is a view for describing a manufacturing method of the semiconductor device according to the third embodiment. Fig. 9 is a view for describing the structure of a semiconductor device according to a fourth embodiment. Description of embodiments

[0014] A semiconductor device and a method for manufacturing the semiconductor device according to embodiments of the present invention will be described with reference to the drawings. Identical or corresponding components are given the same reference numerals, and repeated descriptions of such components may be omitted. First embodiment

[0015] Fig. 1 is a cross-sectional view of a semiconductor device 100 according to a first embodiment. The semiconductor device 100 is used, for example, for power control. The semiconductor device 100 is a switching device such as an insulated gate bipolar transistor (IGBT). Furthermore, the semiconductor device 100 may be a metal oxide semiconductor field-effect transistor (MOSFET).

[0016] The semiconductor device 100 includes a semiconductor substrate 10. The semiconductor substrate 10 is made of, for example, Si. A first electrode 12 is arranged on the semiconductor substrate 10. The first electrode 12 is made of, for example, Al. The first electrode 12 is, for example, an emitter electrode.

[0017] A second electrode 14 and an insulating layer 16 are arranged on an upper surface of the first electrode 12. The insulating layer 16 is made of, for example, polyimide. The second electrode 14 is made of, for example, Ni. The second electrode 14 is arranged to improve bondability with a solder 18.

[0018] The insulating layer 16 has a first portion 16a disposed on an upper surface of the first electrode 12. The second electrode 14 has a main portion 14a disposed on the upper surface of the first electrode 12. Furthermore, the second electrode 14 has an eaves portion 14b connected to the main portion 14a and extending above the first portion 16a. The solder 18 is disposed on an upper surface of the second electrode 14. The solder 18 covers an upper surface of the main portion 14a of the second electrode 14 and a portion of an upper surface of the overhang portion 14b connected to the upper surface of the main portion 14a.

[0019] The insulating layer 16 has a second portion 16c covering a portion of the upper surface of the overhang portion 14b. The second portion 16c covers a portion of the upper surface of the overhang portion 14b, the portion being closer to the end portion 14c of the overhang portion 14b than the portion covered by the solder 18. An end portion of the second portion 16c and an end portion 18a of the solder 18 are in contact with each other. Furthermore, the insulating layer 16 has a third portion 16b connecting the first portion 16a and the second portion 16c. The third portion 16b covers the end portion 14c of the overhang portion 14b.

[0020] In the present embodiment, the second electrode 14 is formed in a peripheral portion of the solder 18 so as to straddle the insulating layer 16. An upper surface, a lower surface, and an end surface connecting the upper surface and the lower surface of the overhang portion 14b of the second electrode 14 are covered by the insulating layer 16. The end surface of the overhang portion 14b corresponds to the end portion 14c. A length of the second part 16c from the end portion 14c of the overhang portion 14b is shorter than a length of the first part 16a from the end portion 14c of the overhang portion 14b. In this case, the end portion 18a of the solder 18 is positioned in an area indicated by a range a. The area indicated by the area a is an area between the end portion 14c of the second electrode 14 and an end portion of the first part 16a.

[0021] Fig. 2 is a view illustrating a state in which an external electrode 22 is disposed on the semiconductor device 100 according to the first embodiment. The solder 18 directly bonds the second electrode 14 and the external electrode 22. The external electrode 22 is made of copper, for example. Furthermore, the semiconductor device 100 is sealed by a mold resin 20. The insulating layer 16, the solder 18, and the external electrode 22 may be covered by the mold resin 20.

[0022] Fig. 3 is a view describing a structure of the second electrode 14 according to the first embodiment. In Fig. 3, the solder 18, the external electrode 22, and the mold resin 20 are omitted. The second electrode 14 includes a Ti film 15a disposed on an upper surface of the first electrode 12 and a Ni film 15b disposed on an upper surface of the Ti film 15a. The second electrode 14 is a front-side metal positioned closer to a front surface than the first electrode 12. The second electrode 14 forms a suitable composite film with the solder 18. In addition, the second electrode 14 acts as a barrier against excessive erosion by the solder 18. This excessive erosion is also referred to as Ni erosion.

[0023] The Ti film 15a improves the adhesion between the first electrode 12, which is an Al film, and the Ni film 15b. Furthermore, an Au film may be further disposed on an upper surface of the Ni film 15b. By disposing an Au film on an outermost surface of the second electrode 14, oxidation of the metal films can be prevented. Thus, wettability of the solder 18 can be ensured. Note that at the time of soldering, the Au film diffuses into the solder 18. Therefore, in many cases, the Au film does not remain at a bonding interface after soldering.

[0024] Furthermore, a back metal can be disposed on a rear surface of the semiconductor substrate 10. The back metal is formed with Ti / Ni / Au films, just like the front metal. The back metal is also designed for solder bonding. By using a Mo film instead of the Ti film 15a, the same function can be achieved.

[0025] An example of a thickness of each layer is given: 0.5 to 2.0 µm for the Ni film 15b, 0.05 to 0.2 µm for the Ti film 15a, 3.0 to 5.0 µm for the first electrode 12, which is an Al film, and 0.03 to 0.2 µm for the Au film; further, 2 to 20 µm for the insulating layer 16, which is a coating film formed of polyimide.

[0026] In the present embodiment, the Ni film 15b is formed as a single layer and has a stepped structure. Since the Ni film 15b is a single layer in the present embodiment, it is formed through a single process. Thus, film quality can be uniformly produced. Furthermore, delamination in the film due to thermal stress, for example, hardly occurs, and durability is excellent.

[0027] Next, a manufacturing method for the semiconductor device 100 will be described. Fig. 4 is a view for describing a manufacturing method for the semiconductor device according to the first embodiment. First, the first electrode 12 is formed on the semiconductor substrate 10. Next, a first insulating layer is formed on the upper surface of the first electrode 12 (step 1). Here, the first insulating layer corresponds to the first part 16a.

[0028] Next, an electrode formation step is performed. In the electrode formation step, a Ti film 15a is first formed by sputtering on the upper surface of the first electrode 12 so as to extend over the first portion 16a and the first electrode 12 (step 2). The Ti film 15a is thus formed in a stepped shape in a peripheral portion of the electrode. Next, the Ni film 15b is formed by sputtering on the upper surface of the Ti film 15a (step 3). The second electrode 14 is thus formed thereover from the upper surface of the first electrode 12 to the upper surface of the first portion 16a.

[0029] Next, polyimide is applied to a peripheral portion of the Ni film 15b (step 4). A second insulating layer is thus formed on the first insulating layer. The second insulating layer corresponds to the second portion 16c and the third portion 16b. The end portion 14c of the overhang portion 14b and a portion of the upper surface of the overhang portion 14b, the portion connected to the end portion 14c, are covered by the second insulating layer.

[0030] Next, the solder 18 is formed on the upper surface of the second electrode 14. The solder 18 is formed to cover the upper surface of the main portion 14a and a portion of the upper surface of the overhang portion 14b, the portion being closer to the main portion 14a than the portion covered by the second insulating layer. The external electrode 22 and the second electrode 14 are next formed using the solder 18. After that, the semiconductor device 100 is sealed using the molding resin 20.

[0031] In the present embodiment, the Ni film 15b is formed by sputtering once. Therefore, a reduction in man-hours during assembly can be achieved.

[0032] Next, effects of the present embodiment will be described. Generally, in a semiconductor device, stress tends to be concentrated at an end portion of the solder due to a thermal cycle of the device itself. This occurs, for example, due to a difference in a linear expansion coefficient of each constituent. This may cause a crack to be generated on an electrode such as an emitter electrode. In particular, brittle fracture tends to occur on a Ni plating film due to thermal stress. In this case, the crack may develop into an underlying Al film.

[0033] On the other hand, in the semiconductor device 100 of the present embodiment, the position of the end portion 18a of the solder 18 on the upper surface of the second electrode 14 is determined by the second portion 16c of the insulating layer 16. In short, the second portion 16c limits the area of ​​wetting and spreading of the solder 18. Therefore, the position of the end portion 18a of the solder 18 and the position of the end portion 14c of the second electrode 14 do not coincide. Consequently, even if a crack occurs in the solder 18, the crack hardly develops to the second electrode 14.

[0034] Furthermore, the first part 16a is disposed directly below the end portion 18a of the solder 18 on the overhang portion 14b, with the second electrode 14 disposed between the first part 16a and the end portion 18a. Therefore, even if the second electrode 14 may cause brittle fracture due to variations in film quality, cracking in the first electrode 12 can be prevented. Consequently, the first electrode 12 is protected, and a long lifetime of the semiconductor device 100 can be achieved. Furthermore, in the present embodiment, a product lifetime can be appropriately designed, and uniformity of the product lifetime can be achieved.

[0035] Furthermore, when a bonding surface of a solder metal is extended to the outside of an active region, a solder bridge may occur straddling a guard ring of a peripheral portion. In this case, there is a possibility of a withstand voltage of the device dropping. On the other hand, the bonding surface remains within an active region through which a main current of the semiconductor device 100 flows by the solder 18 of the present embodiment. In short, the second electrode 14, the insulating layer 16, and the solder 18 are disposed on or above the first electrode 12, which is a main electrode of the semiconductor device 100. Thus, a drop in a withstand voltage of the device can be prevented.

[0036] Furthermore, when the positions of an end portion of the solder metal and an end portion of the Ni film coincide, a stress tends to occur at which peeling of the Ni film starts from an end portion. On the other hand, in the present embodiment, the position of the end portion 18a of the solder metal 18 and the position of the end portion 14c of the second electrode 14 do not coincide with each other. Consequently, peeling between the second electrode 14 and the insulating layer 16 can be prevented. Furthermore, development of a crack to the first electrode 12 starting from a peeling portion can be prevented. Moreover, in the insulating layer 16, the first part 16a and the second part 16c are connected by the third part 16b. Consequently, the end portion 14c of the second electrode 14 is held by the insulating layer 16.Detachment between the second electrode 14 and the insulating layer 16 can thus be further prevented.

[0037] Furthermore, the materials of the layers are not limited to those described above. For example, the second electrode 14 is not limited to Ni, and it is only required that it be made of a metal that allows for easier wetting and spreading of the solder than the first electrode 12.

[0038] The semiconductor substrate 10 can be made of a wide-bandgap semiconductor. The wide-bandgap semiconductor is silicon carbide, a gallium nitride-based material, or diamond. Thus, the heat resistance of the semiconductor substrate 10 can be improved. According to the present embodiment, the reliability of the electrodes against thermal stress can be improved. Consequently, by combining the structure of the present embodiment with a semiconductor substrate 10 made of a wide-bandgap semiconductor, the effect of improving heat resistance due to the wide-bandgap semiconductor can be effectively utilized.

[0039] These modifications can be applied to a semiconductor device and a method for manufacturing the semiconductor device according to the following embodiments, as appropriate. Note that the semiconductor device and the method for manufacturing the semiconductor device according to the following embodiments are similar to those of the first embodiment in many respects, and thus, the following primarily describes differences between the semiconductor device and the method for manufacturing the semiconductor device according to the following embodiments and those of the first embodiment. Second embodiment

[0040] Fig. 5 is a view for describing the structure of a semiconductor device 200 according to a second embodiment. In Fig. In FIG. 5, the solder 18, the external electrode 22, and the molding resin 20 are omitted. In the semiconductor device 200, the structure of the second electrode 214 is different from that of the first embodiment. The remaining configurations are the same as in the first embodiment.

[0041] The second electrode 214 includes a first Ni film 215b disposed on the upper surface of the first electrode 12, a Ti film 215 disposed on an upper surface of the first Ni film 215b, and a second Ni film 215c disposed on an upper surface of the Ti film 215a. The second electrode 214 of the present embodiment has a stepped structure formed from a double-layered Ni film.

[0042] Fig. 6 is a view for describing a manufacturing method of the semiconductor device 200 according to the second embodiment. The manufacturing method of the semiconductor device 200 is the same as that of the first embodiment for and before step 1. Next, an electrode formation step of the present embodiment will be described. First, the first Ni film 215b is formed on an upper surface of the first electrode 12 by plating (step S202). The thickness of the first Ni film 215b formed by plating is, for example, 2.0 to 6.0 μm. The first Ni film 215b is formed, for example, to the same height as the first part 16a. Next, the Ti film 215a is formed on the upper surface of the first Ni film 215b by sputtering so as to extend over the first part 16a and the first Ni film 215b (step S202).

[0043] Next, the second Ni film 215c is formed by sputtering on the upper surface of the Ti film 215a (step 203). The second Ni film 215c is formed thereover from the first Ni film 215b to the first part 16a so as to have a larger area than the first Ni film 215b. The thickness of the second Ni film 215c formed by sputtering is, for example, 0.5 to 2.0 μm. The second electrode 214 is thus formed thereover from an upper surface of the first electrode 12 to the upper surface of the first part 16a. The subsequent steps are the same as those of the first embodiment.

[0044] In general, if the thickness of a Ni film is made 2 μm or more by sputtering, productivity may decrease. On the other hand, in the present embodiment, the thick first Ni film 215b is previously formed by plating on an upper surface of the Al film. Furthermore, a Ti / Ni film is formed thereon by sputtering. Thus, the thickness of the Ni film can be secured while ensuring productivity. By making the Ni film thick, stress on the Al film due to thermal stress can be reduced. Third embodiment

[0045] Fig. 7 is a view for describing a structure of a semiconductor device 300 according to a third embodiment. In Fig. In FIG. 7, the solder 18, the external electrode 22, and the molding resin 20 are omitted. In the semiconductor device 300, the structure of the second electrode 314 is different from that of the first embodiment. The remaining configurations are the same as in the first embodiment.

[0046] The second electrode 314 includes a Ti film 315a disposed on the upper surface of the first electrode 12, a first Ni film 315b disposed on an upper surface of the Ti film 315a, and a second Ni film 315c disposed on an upper surface of the first Ni film 315b. The second electrode 314 of the present embodiment has a stepped structure formed from a double-layered Ni film.

[0047] Fig. 8 is a view for describing a manufacturing method of the semiconductor device 300 according to the third embodiment. The manufacturing method of the semiconductor device 300 is the same as that of the first embodiment for and before step 1. Next, an electrode formation process of the present embodiment will be described. First, the Ti film 315a is formed on the upper surface of the first electrode 12 by sputtering so as to extend over the first part 16a and the first electrode 12 (step 302). Thus, a step difference is formed on the Ti film 315a in a peripheral portion of the electrode. Next, the first Ni film 315b is formed on an upper surface of the Ti film 315a by sputtering (step 302). Thus, a step difference is formed on the first Ni film 315b in the peripheral portion of an electrode.

[0048] Next, the second Ni film 315c is formed by plating on the upper surface of the first Ni film 315b (step 303). In this way, the second electrode 314 is formed thereover from the upper surface of the first electrode 12 to the upper surface of the first part 16a. The subsequent steps are the same as those of the first embodiment.

[0049] In general, sputtering makes it easier to unify the thickness and physical property values ​​of the Ni film than plating. Therefore, film quality can be improved. In the present embodiment, sputtering forms a high-quality Ni film directly on the upper surface of the Al film, thereby improving the protective effect of the Al film. Thus, brittle fracture of the Ni film due to stress concentration caused by thermal stress can be prevented, and a long product life can be achieved.

[0050] Furthermore, if a Ti / Ni film is formed by sputtering, the Ti / Ni film can be formed on the same production line after an Al film, which is the first electrode 12, is formed by sputtering. Alternatively, Al / Ti / Ni films can be formed continuously. Therefore, a manufacturing process can be simplified. Furthermore, the subsequent plating process can ensure the thickness of Ni with good productivity. Fourth embodiment

[0051] Fig.9 is a view for describing the structure of a semiconductor device 400 according to a fourth embodiment. In this embodiment, the structure of an insulating layer 416 is different from that of the first embodiment. The insulating layer 416 does not include the second portion 16c and the third portion 16b. Furthermore, a conductive film 424 is disposed on the upper surface of the overhang portion 14b. The conductive film 424 covers a portion of the upper surface of the overhang portion 14b, the portion being closer to the end portion 14c of the overhang portion 14b than the portion covered by the solder 18.

[0052] For the solder 18, wetting and spreading on the conductive film 424 is more difficult than on the second electrode 14. The conductive film 424 is made of, for example, Al. An end portion of the conductive film 424 on a side of the main portion 14a is arranged closer to the end portion 14c of the overhang portion 14b than an end portion of the insulating layer 416, and the end portion faces the main portion 14a. The end portion of the conductive film 424 on the side of the main portion 14a faces the solder 18 and is in contact with the end portion of the solder 18.

[0053] The conductive film 424 has a film quality that hardly causes solder to adhere thereto. Therefore, the conductive film 424 can prevent the solder 18 from wetting and spreading to the end portion 14c of the overhang portion 14b. The position of the end portion of the solder 18 on the upper surface of the second electrode 14 is thus determined by the conductive film 424. Therefore, in the present embodiment, the position of the end portion of the solder 18 and the position of the end portion 14c of the second electrode 14 do not coincide with each other. Consequently, even if a crack occurs in the solder 18, the crack hardly develops to the second electrode.

[0054] Furthermore, the insulating layer 416 is disposed directly below the end portion of the solder 18 on the overhang portion 14b, with the second electrode 14 being disposed between the insulating layer 416 and the end portion. This can prevent a crack in the second electrode 14 from propagating to the first electrode 12 disposed below the insulating layer 416. Consequently, the first electrode 12 is protected, and a long lifetime of the semiconductor device can be achieved.

[0055] In the present embodiment, ensuring a solder bonding surface and preventing solder flow can be controlled without polyimide. Therefore, a manufacturing process can be simplified.

[0056] Note that the technical features described in the above embodiments can be combined as applicable. List of reference symbols

[0057] 100, 200, 300, 400 semiconductor device, 10 semiconductor substrate, 12 first electrode, 14, 214, 314 second electrode, 14a main part region, 14b overhang part region, 14c end part region, 15a, 215a, 315a Ti film, 15b Ni film, 16, 416 insulating layer, 16a first part, 16c second part, 16b third part, 18 solder, 215b, 315b first Ni film, 215c, 315c second Ni film, 424 conductive film

Claims

[1] A semiconductor device (100, 200, 300), comprising: - a semiconductor substrate (10); - a first electrode (12) arranged on the semiconductor substrate (10); - an insulating layer (16) having a first part (16a) arranged on an upper surface of the first electrode (12); - a second electrode (14, 214, 314) having a main portion (14a) and an overhang portion (14b), the main portion (14a) being disposed on the upper surface of the first electrode (12), the overhang portion (14b) being connected to the main portion (14a) and extending over the first portion (16a) of the insulating layer (16); - a solder (18) covering an upper surface of the main portion (14a) and a part of an upper surface of the overhang portion (14b) connected to the upper surface of the main portion (14a) of the second electrode (14, 214, 314); and - a molding resin (20) covering the insulating layer (16) and the solder (18); wherein the insulating layer (16) comprises: - a second part (16c) covering a part of the upper surface of the overhang portion (14b), wherein the part of the upper surface of the overhang portion (14b) covered by the insulating layer (16) is closer to an end portion (14c) of the overhang portion (14b) than the part covered by the solder metal (18); and - a third part (16b) connecting the first part (16a) and the second part (16c) and covering the end portion (14c) of the overhang portion (14b); wherein a length of the second part (16c) of the insulating layer (16) from the end portion (14c) of the overhang portion (14b) is shorter than a length of the first part (16a) of the insulating layer (16) from the end portion (14c) of the overhang portion (14b). [2] A semiconductor device (400) comprising: - a semiconductor substrate (10); - a first electrode (12) arranged on the semiconductor substrate (10); - an insulating layer (416) disposed on an upper surface of the first electrode (12); - a second electrode (14, 214, 314) having a main portion (14a) and an overhang portion (14b), the main portion (14a) being disposed on the upper surface of the first electrode (12), the overhang portion (14b) being connected to the main portion (14a) and extending over the insulating layer (416); - a solder (18) covering an upper surface of the main portion (14a) and a part of an upper surface of the overhang portion (14b) connected to the upper surface of the main portion (14a) of the second electrode (14, 214, 314); and - a conductive film (424) covering a part of the upper surface of the overhang portion (14b), the part being closer to an end portion (14c) of the overhang portion (14b) than the part covered by the solder (18), wherein wetting and spreading of the solder (18) is more difficult on the conductive film (424) than on the second electrode (14, 214, 314). [3] The semiconductor device (400) according to claim 2, wherein an end portion of the conductive film (424) on a side of the main portion (14a) is arranged closer to the end portion (14c) of the overhang portion (14b) than an end portion of the insulating layer (416), the end portion of the insulating layer (416) facing the main portion (14a). [4] The semiconductor device (400) according to claim 2 or 3, wherein the conductive film (424) is made with Al. [5] The semiconductor device (100, 200, 300, 400) according to any one of claims 1 to 4, wherein the second electrode (14, 214, 314) is made of Ni. [6] The semiconductor device (100, 200, 300, 400) according to any one of claims 1 to 4, wherein the second electrode (14, 214, 314) comprises a Ti film (15a, 215a, 315a) disposed on the upper surface of the first electrode (12) and a Ni film (15b) disposed on an upper surface of the Ti film (15a, 215a, 315a). [7] The semiconductor device (100, 200, 300, 400) according to any one of claims 1 to 4, wherein the second electrode (14, 214, 314) comprises a first Ni film (215b, 315b) disposed on the upper surface of the first electrode (12), a Ti film (15a, 215a, 315a) disposed on an upper surface of the first Ni film (215b, 315b), and a second Ni film (215c, 315c) disposed on an upper surface of the Ti film (15a, 215a, 315a). [8] A semiconductor device (100, 200, 300, 400) according to any one of claims 1 to 7, wherein the first electrode (12) is made of Al. [9] A semiconductor device (100, 200, 300, 400) according to any one of claims 1 to 8, wherein the semiconductor substrate (10) is made with a wide band gap semiconductor. [10] The semiconductor device (100, 200, 30, 400) according to claim 9, wherein the wide band gap semiconductor is silicon carbide, a gallium nitride-based material, or diamond. [11] A manufacturing method for a semiconductor device (100, 200, 300), comprising: - a step of forming a first electrode (12) on a semiconductor substrate (10); - a step of forming a first insulating layer (16a) on an upper surface of the first electrode (12); - an electrode forming step of forming a second electrode (14, 214, 314) thereover from an upper surface of the first electrode (12) to an upper surface of the first insulating layer (16a); - a step of forming a second insulating layer (16b, 16c) on the first insulating layer (16a) to cover an end portion (14c) of an overhang portion (14b) of the second electrode (14, 214, 314), the overhang portion (14b) extending over the first insulating layer, and a part of an upper surface of the overhang portion (14b), the part being connected to the end portion (14c); - a step of forming a solder (18) to cover an upper surface of a main portion (14a) of the second electrode (14, 214, 314), the main portion (14a) being a part disposed on the upper surface of the first electrode (12), and a part of the upper surface of the overhang portion (14b), the part of the upper surface of the overhang portion (14b) covered by the second insulating layer (16b, 16c) being closer to an end portion (14c) of the overhang portion (14b) than the part covered by the solder (18); and - a step of sealing the semiconductor device (100, 200, 300) by a molding resin (20) after forming the solder (18); wherein a length of a part (16c) of the second insulating layer (16b, 16c) from the end portion (14c) of the overhang portion (14b), the part (16c) covering the upper surface of the overhang portion (14b), is shorter than a length of the first insulating layer (16a) from the end portion (14c) of the overhang portion (14b). [12] The manufacturing method according to claim 11, wherein the electrode forming step comprises: - a step of forming a Ti film (15a, 215a, 315a) on the upper surface of the first electrode (12) by sputtering; and - a step of forming a Ni film (15b) on an upper surface of the Ti film (15a, 215a, 315a) by sputtering. [13] The manufacturing method according to claim 11, wherein the electrode forming step comprises: - a step of forming a first Ni film (215b, 315b) on the upper surface of the first electrode (12) by plating; - a step of forming a Ti film (15a, 215a, 315a) on an upper surface of the first Ni film (215b, 315b) by sputtering; and - a step of forming a second Ni film (215c, 315c) on an upper surface of the Ti film (15a, 215a, 315a) by sputtering. [14] The manufacturing method according to claim 11, wherein the electrode forming step comprises: - a step of forming a Ti film (15a, 215a, 315a) on the upper surface of the first electrode (12) by sputtering; - a step of forming a first Ni film (215b, 315b) on an upper surface of the Ti film (15a, 215a, 315a) by sputtering; and - a step of forming a second Ni film (215c, 315c) on an upper surface of the first Ni film (215b, 315b) by plating.

Citation Information

Patent Citations

  • Semiconductor module

    JP2017084911A

  • 5α-reductase inhibitor and composition for treating / preventing urinary system disease, and method for producing the same

    JP2017137290A

  • Semiconductor device

    JP2018046151A

  • JP002017084911A

  • JP002018137290A