BATTERY
The battery design addresses the issue of maintaining an airtight condition by incorporating a housing with non-contact portions and strategic design elements to manage internal pressure, ensuring long-term reliability and reduced deterioration.
Patent Information
- Application Number
- DE112022006396
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-01-14
- Filing Date
- 2022-12-19
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional batteries face issues with maintaining an airtight condition over time due to internal pressure increases caused by expansion of the electrical storage element, leading to potential gasket deterioration and loss of sealing ability.
A battery design featuring a housing with a first part having a bottom and tube-like portion, a second part with a lid-like portion, and a gasket that includes non-contact portions to alleviate pressure on the seal, maintaining an airtight state through strategic design elements like step portions and non-contact areas.
The battery maintains an airtight state for a prolonged period, reducing the likelihood of deterioration by effectively managing internal pressure and preventing seal cracks.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The present invention relates to a battery.
[0002] This application claims priority to Japanese Patent Application No. 2022-004113, filed on January 14, 2022, the contents of which are incorporated herein by reference. [State of the art]
[0003] Traditionally, batteries house an electrical storage element in a housing. The interior of the housing is sealed with a gasket, thus making the interior of the housing airtight.
[0004] For example, Patent Document 1 describes a coin-like lithium battery in which a negative electrode made of lithium or a lithium alloy and a positive electrode are arranged opposite each other via a separator and stored in a battery case. In this coin-like lithium battery, at least one of the negative electrode and the positive electrode is swollen into a curved shape in the central part, and the battery can is elastically deformed along the curved surface. Furthermore, Patent Document 1 describes that a negative electrode cap and a positive electrode can configuring the battery are sealed by an insulating gasket. Furthermore, Patent Document 1 describes as a negative electrode cap a cap having a side wall formed by folding and doubling the material of a peripheral portion. [Citation list][Patent document]
[0005] [Patent Document 1] Unexamined Japanese Patent Application, First Publication No. H7-201323 [Summary of the invention][Technical problem]
[0006] In conventional batteries, the electrical storage element inside the case expands or gas leaks from the electrical storage element, causing the internal pressure in the case to rise and the case to deform. If this forces the seal that maintains the airtight condition of the case to exceed its elastic limit, it may crack the seal. If a crack occurs in the seal, the sealing performance of the seal deteriorates, making it difficult to maintain the airtight condition of the case, and the battery becomes prone to deterioration.
[0007] For this reason, conventional batteries require that the airtight condition in the housing be maintained over a long period of time, even when the internal pressure increases, in order to slow down the deterioration of the batteries.
[0008] The present invention has been made in consideration of the above-described circumstances, and an object of the present invention is to provide a battery capable of maintaining the airtight state in the casing for a long period of time and less likely to deteriorate. [Solution to the problem]
[0009] [1] Having a battery: an electrical storage element having a positive electrode, a negative electrode, and an insulating film disposed between the positive electrode and the negative electrode and electrically separating the positive electrode and the negative electrode; and a housing that houses the electrical storage element in an airtight manner, wherein the housing comprises: a first part having a bottom portion and a tubular portion; a second part having a lid-like portion covering an opening of the first part and a surrounding wall portion covering the tube-like portion from an external environment; and a seal continuously disposed between an end face of the first part and the second part and between the tubular portion and the second part, and a non-contact portion with which the seal does not contact, which is provided in either a part of a first surface of the first part facing the seal or a part of a second surface of the second part facing the seal, or both.
[0010] [2] The battery according to [1], in which the non-contact portion is provided on the second surface.
[0011] [3] The battery according to [2], wherein the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a percentage of a length of the non-contact portion provided on the second surface with respect to a distance L2 in a longitudinal direction of the tubular portion from an outer surface of the lid-like portion to an end surface of the surrounding wall portion is 20% to 95%.
[0012] [4] The battery according to any one of [1] to [3], wherein the non-contact portion is provided on the first surface.
[0013] [5] The battery according to [4], in which the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a percentage of a length of the non-contact portion provided on the first surface with respect to a length L1 of the tubular portion facing the surrounding wall portion is 40% to 80%.
[0014] [6] The battery according to any one of [1] to [5], wherein the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a plurality of non-contact portions having a length of 10 µm or more are present.
[0015] [7] The battery according to any one of [1] to [6], wherein the tubular portion of the first part has a cylindrical shape and comprises: a first outer diameter portion; a second outer diameter portion having a larger outer diameter than the first outer diameter portion; and a step portion connecting the first outer diameter portion and the second outer diameter portion, wherein the first outer diameter portion is arranged closer to the bottom portion than the second outer diameter portion, and wherein, in a sectional area passing through a center of the tubular portion, the step portion is provided within a length range of 1 / 3 of a length L1 of the tubular portion facing the surrounding wall portion from a central position of the length L1 of the tubular portion facing the surrounding wall portion.
[0016] [8] The battery according to any one of [1] to [7], wherein the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a length L3 of the seal in a longitudinal direction of the tubular portion is greater than a distance L2 in the longitudinal direction of the tubular portion from an outer surface of the lid-like portion to an end surface of the surrounding wall portion. [Advantageous effects of the invention]
[0017] A battery of the present invention comprises a case that accommodates an electric storage element in an airtight state, the case having a first member including a bottom portion and a tubular portion, a second member including a lid-like portion covering an opening of the first member, and a surrounding wall portion covering the tubular portion from an external environment, and a gasket continuously disposed between an end surface of the first member and the second member and between the tubular portion and the second member, and a non-contact portion with which the gasket is not in contact is provided in either a part of a first surface of the first member facing the gasket or a part of a second surface of the second member facing the gasket, or both.Therefore, the battery of the present invention is capable of maintaining the airtight state in the case for a long period of time and is less likely to deteriorate. [Brief description of the drawings] Fig. 1 is a schematic cross-sectional view showing a battery according to a first embodiment, and is a cross-sectional view of a cut surface along a planar view center of a tubular portion 1b of a first part 1. Fig. 2(a) and Fig. 2(b) are cross-sectional views for describing the overall structure of the battery of the first embodiment. Fig. 2(a) is a cross-sectional view taken along a line AA' in Fig. 2(b). Fig. 2(b) is a cross-sectional view of the cut surface along the planar view center of the tubular portion 1b of the first part 1. Fig.3 is a schematic cross-sectional view showing a battery of a second embodiment, and is a cross-sectional view of a cut surface along a planar view center of a tubular portion 11b of a first part 1. [Description of the embodiments]
[0018] A battery according to the present invention will be described in detail below with reference to the drawings. <Erste Ausführungsform> [Battery]
[0019] Fig. 1, Fig. 2(a) and Fig. 2(b) are schematic cross-sectional views showing a battery according to a first embodiment. Fig. 1 and Fig. 2(a) are cross-sectional views of a cut surface along a planar view center of a tubular portion 1b having a tubular shape of a first part 1. Fig. 2(a) is a cross-sectional view taken along a line AA' in Fig. 2(b). A Fig. 1, Fig. 2(a) and Fig. The battery 10 shown in Fig. 2(b) is a coin-like battery and has an electric storage element 12 and a case 11 which airtightly houses the electric storage element 12.
[0020] The casing 11 of the battery 10 of the present embodiment includes a first part 1, a second part 2, and a gasket 3. The interior of the casing 11 is sealed with the gasket 3; thereby, the interior of the casing 11 is made airtight and placed in an airtight state. (First part)
[0021] The first part 1 has a bottom portion 1a and a tubular portion 1b which is connected to the edge portion of the bottom portion 1a and integrated with the bottom portion 1a, as shown in Fig. 1. The bottom section 1a has a round shape in a plan view, and the tubular section 1b has a cylindrical shape (see Fig. 2(a) and Fig.2(b)). The tubular portion 1b has a first outer diameter portion 1e, a second outer diameter portion 1f having a larger outer diameter than the first outer diameter portion 1e, and a step portion 1g connecting the first outer diameter portion 1e and the second outer diameter portion 1f, as shown in Fig. 1. The first outer diameter portion 1e is arranged closer to the bottom portion 1a than the second outer diameter portion 1f. The first outer diameter portion 1e and the second outer diameter portion 1f extend in a direction substantially perpendicular to the extension direction of the bottom portion 1a, as shown in Fig. 1 shown.
[0022] An inner surface-side curvature radius r1 and an outer surface-side curvature radius r2 of the first member 1 formed by the step portion 1g are not particularly limited, but are preferably 50 μm or more, and more preferably 60 μm to 200 μm. This is because when the curvature radius r1 and the curvature radius r2 are 50 μm or more, a non-contact portion 41, in which the length of a portion where a first surface 1d and the gasket 3 are not in contact with each other is 10 μm or longer, can be easily formed in the vicinity of the step portion 1g. In addition, when the curvature radius r1 and the curvature radius r2 are 200 μm or less, the difference in outer diameter between the first outer diameter portion 1e and the second outer diameter portion 1f does not become too large, which is preferable.The inner surface-side radius of curvature r1 and the outer surface-side radius of curvature r2 may be the same or different from each other.
[0023] The difference in outer diameter between the first outer diameter portion 1e and the second outer diameter portion 1f (in other words, a length twice the extension of the step portion 1g in the thickness direction of the tubular portion 1b) can be set, for example, to 50 μm to 200 μm, and preferably to 60 μm to 100 μm. When the difference in outer diameter between the first outer diameter portion 1e and the second outer diameter portion 1f is 50 μm or more, the height of the step portion 1g becomes sufficiently large. As a result, it becomes easy for the non-contact portion 41 to be formed in a wider area with which the gasket 3 is not in contact, near the step portion 1g on the first surface 1d in the bottom portion 1a side.In addition, when the difference in outer diameter between the first outer diameter portion 1e and the second outer diameter portion 1f is 200 μm or less, it becomes easy to secure the airtightness in the case 11 with the gasket 3 after the completion of the battery 10 (when the battery 10 is completed), and the airtightness in the case 11 becomes more favorable.
[0024] In a sectional view along the center of the tubular portion 1b of the first part 1, the step portion 1g connecting the first outer diameter portion 1e and the second outer diameter portion 1f is within a length range of 1 / 3 of a length L1 of the tubular portion 1b facing a surrounding wall portion 2b from a central position of the length L1 of the tubular portion 1b facing the surrounding wall portion 2b of the second part 2, as shown in Fig.1. Therefore, it is possible to sufficiently secure the length of the first outer diameter portion 1e and the second outer diameter portion 1f, and in a case where the internal pressure in the housing 11 has increased, the step portion 1g acts as a fulcrum of deformation, and the first outer diameter portion 1e and the second outer diameter portion 1f of the tubular portion 1b expand in a curved shape. As a result, it is possible to effectively absorb a force due to the deformation of the housing 11 with a gap between the first outer diameter portion 1e and the gasket 3 and a gap between the second outer diameter portion 1f and the gasket 3 in a case where the internal pressure in the housing 11 has increased.Therefore, in a case where the step portion 1g is provided in a length range of 1 / 3 of the length L1, it becomes easy to secure the airtightness in the casing 11 with the gasket 3, and the airtightness in the casing 11 becomes more favorable.
[0025] Furthermore, in a housing in which the step portion 1g is provided within a length range of 1 / 3 of the length L1, the position of the step portion 1g is not positioned too close to an end surface 1c of the first member 1. Therefore, in a case where the internal pressure in the housing 11 has increased, the end surface 1c of the first member 1 acts as a fulcrum of deformation, and the tubular portion 1b of the first member 1 expands in a curved shape, and it is not difficult for the force associated with the deformation of the housing 11 to be absorbed by the space between the first outer diameter portion 1e and the gasket 3. Furthermore, in a housing in which the step portion 1g is provided within a length range of 1 / 3 of the length L1, the position of the step portion 1g is not brought too close to the bottom portion 1a of the first member 1.Therefore, in a case where the internal pressure in the housing 11 has increased, the force due to the deformation of the housing 11 can be prevented from reaching the second part 2 without being sufficiently absorbed by the space between the first outer diameter portion 1e and the gasket 3, and the second part 2 can be prevented from deforming.
[0026] For example, the material used for the first part 1 may be a conductive material such as a foil or plate made of a metal selected from nickel, stainless steel, aluminum, and copper. (Second part)
[0027] The second part 2 has a lid-like portion 2a covering the opening of the first part 1 and the surrounding wall portion 2b covering the tube-like portion 1b of the first part 1 from the outside, as shown in Fig.1. The lid-like portion 2a is arranged substantially parallel to the bottom portion 1a of the first part 1. The surrounding wall portion 2b is connected to the edge portion of the lid-like portion 2a and integrated with the lid-like portion 2a. The lid-like portion 2a has, in a planar view, a substantially concentrically round shape, the center of which is located substantially at the same position as that of the bottom portion 1a of the first part 1, as shown in Fig. 2(a) and Fig. 2(b). The surrounding wall portion 2b has a cylindrical shape that is substantially concentric with the tubular portion 1b, and the inner diameter of the surrounding wall portion 2b is longer than the outer diameter of the tubular portion 1b of the first part 1. The surrounding wall portion 2b has an inner diameter and an outer diameter that are substantially constant.
[0028] The length from the inner surface of the lid-like portion 2a to an end surface 2c of the surrounding wall portion 2b is shorter than the length from the outer surface of the bottom portion 1a of the first part 1 to the end surface 1c of the tubular portion 1b. Therefore, a part of the tubular portion 1b of the first part 1 is exposed on the outer surface of the housing 11.
[0029] For example, the material of the second part 2 can be a conductive material such as a foil or plate made of a metal selected from nickel, stainless steel, aluminum, and copper. The material of the second part 2 can be identical to or different from the material of the first part 1. (Seal)
[0030] The seal 3 is arranged continuously between the end face 1c of the first part 1 and the second part 2 and between the tubular section 1b and the second part 2, as shown in Fig. 1 shown.
[0031] As in Fig.1, in the sectional area along the center of the tubular portion 1b of the first member 1, a length L3 of the gasket 3 in the longitudinal direction of the tubular portion 1b is preferably longer than a distance L2 of the second member 2 in the longitudinal direction of the tubular portion 1b from the outer surface of the lid-like portion 2a to the end surface 2c of the surrounding wall portion 2b. When the length L3 of the gasket 3 in the longitudinal direction of the tubular portion 1b is greater than the distance L2, the gasket 3 is disposed over the entire area between the end surface 1c of the first member 1 and the second member 2 and between the tubular portion 1b and the second member 2. Therefore, the gasket 3 is disposed over the entire area of an intrusion path of moisture that might penetrate into the housing 11 from the end surface 2c of the surrounding wall portion 2b.As a result, it becomes easy to more reliably secure the airtightness in the housing 11 with the gasket 3, and the airtightness in the housing 11 becomes even more favorable.
[0032] As the material of the seal 3, for example, a known insulating material such as acid-modified polyethylene, polypropylene, acid-modified polypropylene, an epoxy resin, polyvinylidene fluoride (PVDF) or polyvinylidene chloride (PVDC) can be used. (non-contact section)
[0033] In the battery 10 of the present embodiment, as shown in Fig. 1, Fig. 2(a) and Fig.As shown in Figure 2(b), the non-contact portion 41 with which the gasket 3 is not in contact is provided in a part of the first surface 1d of the first member 1 that is opposite to the gasket 3. The planar shape of the non-contact portion 41 may have any shape, such as a substantially round shape or a substantially polygonal shape, or it may be an irregular shape. The number of non-contact portions 41 may be one or more, but a plurality of non-contact portions is preferably provided because it is possible to more effectively maintain airtightness in the casing 11. The plurality of non-contact portions 41 may be arranged regularly or irregularly. The plurality of non-contact portions 41 may each have a different planar shape, or some or all of the portions may have the same planar shape.
[0034] As in Fig.1, in the battery 10 of the present embodiment, in the sectional area along the center of the tubular portion 1b of the first member 1, the percentage of the length of the non-contact portion 41 provided on the first surface 1d with respect to the length L1 of the tubular portion 1b facing the surrounding wall portion 2b of the second member 2 is preferably 40% to 80%, and more preferably 40% to 50%. When the percentage of the length of the non-contact portion 41 with respect to the length L1 is 40% or more, a crack can be effectively prevented from being generated in the gasket 3 due to a force attributable to the deformation of the casing 11 of the battery 10.When the percentage of the length of the non-contact portion 41 with respect to the length L1 is 80% or less, the sealing ability of the gasket 3 becomes favorable at the time of completion of the battery 10, and the airtightness in the case 11 thus becomes more favorable at the time of completion of the battery 10.
[0035] As in Fig.1, in the battery 10 of the present embodiment, the first member 1 has the stepped portion 1g connecting the first outer diameter portion 1e and the second outer diameter portion 1f. The non-contact portion 41 provided on the first surface 1d in the first outer diameter portion 1e often has a large area compared with the non-contact portion 41 provided on the first surface 1d in the second outer diameter portion 1f. This is because the surrounding wall portion 2b of the second member 2 is connected to the tubular portion 1b of the first member 1 by caulking; and thereby, the gasket 3 is pressed against the first surface 1d in the second outer diameter portion 1f.Therefore, as the percentage of the first outer diameter portion 1e in the tubular portion 1b facing the surrounding wall portion 2b of the second part 2 increases, the percentage of the length of the non-contact portion 41 with respect to the length L1 may increase.
[0036] As in Fig. 1, Fig. 2(a) and Fig.As shown in Fig. 2(b), in the battery 10 of the present embodiment, a non-contact portion 42 with which the gasket 3 is not in contact is also provided in a part of a second surface 2d of the second part 2 that is opposite to the gasket 3. The planar shape of the non-contact portion 42 may have any shape, such as a substantially round shape or a substantially polygonal shape, or it may be an irregular shape. The number of non-contact portions 42 may be one or more, but a plurality of non-contact portions is preferably provided because it is possible to more effectively maintain airtightness in the case 11. The plurality of non-contact portions 42 may be regularly or irregularly arranged. The plurality of non-contact portions 42 may each have a different planar shape, or a part or all of them may have the same planar shape.
[0037] As in Fig.1, in the battery 10 of the present embodiment, in the sectional area along the center of the tubular portion 1b of the first member 1, the percentage of the length of the non-contact portion 42 provided on the second surface 2d with respect to the distance L2 of the second member 2 in the longitudinal direction of the tubular portion 1b from the outer surface of the lid-like portion 2a to the end surface 2c of the surrounding wall portion 2b is preferably 20% to 95%, and more preferably 40% to 60%. When the percentage of the length of the non-contact portion 42 with respect to the distance L2 is 20% or more, a crack in the gasket 3 due to the force attributable to the deformation of the casing 11 of the battery 10 can be effectively prevented.When the percentage of the length of the non-contact portion 42 with respect to the distance L2 is 95% or less, the sealing ability of the gasket 3 becomes favorable at the completion of the battery 10, and the airtightness in the case 11 thus becomes favorable after the completion of the battery 10.
[0038] As in Fig.1, in the battery 10 of the present embodiment, in the sectional area along the center of the tubular portion 1b of the first member 1, it is preferable to provide a plurality of non-contact portions 41 and / or 42 having a length of 10 μm or more in either or both of the first surface 1d and the second surface 2d, and it is even more preferable to provide a plurality of non-contact portions 41 and 42 having a length of 10 μm or more in both the first surface 1d and the second surface 2d. The non-contact portions 41 and 42 having a length of 10 μm or more are capable of effectively absorbing the force due to the deformation of the case 11 with the space between the first surface 1d or the second surface 2d and the gasket 3.This can more effectively prevent a crack from occurring in the seal 3, which is opposite to the non-contact portions 41 and 42, due to the force resulting from the deformation of the housing 11. (electrical storage element)
[0039] The electrical storage element 12 in the battery 10 of the present embodiment has, in a planar view, a substantially round shape with a smaller diameter than the bottom portion 1a of the first part 1, as shown in Fig. 1, Fig. 2(a) and Fig.2(b). The electric storage element 12 has a laminate structure in which a negative electrode having a negative electrode active material layer 61 formed on a negative electrode current collector 6, a positive electrode having a positive electrode active material layer 71 formed on a positive electrode current collector 7, and a separator 5 disposed between the negative electrode active material layer 61 and the positive electrode active material layer 71 are laminated together.
[0040] For example, a known current collector made of a metal foil, such as a copper foil, can be used as the negative electrode current collector 6. The negative electrode current collector 6 has a substantially round shape in a plan view, as shown in Fig. 2(a) and Fig.2(b). The negative electrode current collector 6 is electrically connected to the bottom portion 1a of the first part 1 of the housing 11 via a tape-like negative electrode lead 62 made of a metal foil, such as a copper foil, and integrated into the edge portion of the negative electrode current collector 6.
[0041] As the negative electrode active material layer 61, a layer containing a known negative electrode active material such as graphite and a known binder such as polyvinylidene fluoride (PVDF) can be used.
[0042] As the positive electrode current collector 7, a known current collector made of a metal foil, such as an aluminum foil, can be used. The positive electrode current collector 7 has a substantially round shape in plan view, which is substantially concentric with the negative electrode current collector 6 and has a smaller diameter than the negative electrode current collector 6, as shown in Fig. 2(a) and Fig. 2(b). The positive electrode current collector 7 is electrically connected to the lid-like portion 2a of the second part 2 of the housing 11 via a band-shaped positive electrode lead 72 made of a metal foil, such as an aluminum foil, which is integrated into the edge region of the positive electrode current collector 7.
[0043] As the positive electrode active material layer 71, a layer containing a known positive electrode active material such as lithium cobaltate, a known binder such as polyvinylidene fluoride (PVDF), and a known conductive aid such as acetylene black can be used.
[0044] The separator 5 electrically separates the positive electrode from the negative electrode. A known insulating film made of a resin or the like can be used as the separator 5. The separator 5 has a substantially circular shape in plan view, which is substantially concentric with the negative electrode current collector 6 and has a larger diameter than the negative electrode current collector 6 and the positive electrode current collector 7, as shown in Fig. 2(a) and Fig. 2(b).
[0045] The electrical storage element 12 in the Fig. 1, Fig. 2(a) and Fig.The battery 10 shown in Figure 2(b) can be manufactured by a conventionally known method. For example, a positive electrode slurry is made into a paste by mixing the positive electrode active material, the binder, the conductive aid, and a known solvent such as N-methyl-2-pyrrolidone (NMP). Then, the positive electrode paste is coated onto the metal foil to serve as the positive electrode current collector 7 using a doctor blade method or the like to a predetermined thickness. Then, the metal foil to which the positive electrode slurry has been applied is dried at, for example, 150°C. After that, the dried, coated foil is pressed by a known method to achieve high densification; this forms the positive electrode active material layer 71.
[0046] Subsequently, the metal foil with the positive electrode active material layer 71 is punched into a predetermined shape using, for example, a PINNACLE DIE (registered trademark). This shapes the metal foil with the positive electrode active material layer 71 into a shape corresponding to the positive electrode current collector 7 having a substantially circular shape and the shape of the band-shaped positive electrode lead 72 extending from the edge portion of the positive electrode current collector 7. Next, the positive electrode active material layer 71 formed at a location on the metal foil to serve as the positive electrode lead 72 is peeled off. The positive electrode composed of the positive electrode current collector 7 and the positive electrode active material layer 71, and the positive electrode lead 72 integrated with the positive electrode current collector 7, is obtained through the above-described steps.
[0047] Subsequently, a negative electrode slurry is prepared by mixing the negative electrode active material, the binder, and a well-known solvent such as N-methyl-2-pyrrolidone (NMP) to form a paste. Next, the negative electrode consisting of the negative electrode current collector 6 and the negative electrode active material layer 61, as well as the negative electrode lead 62 integrated with the negative electrode current collector 6, are prepared in the same manner as in the case of preparing the positive electrode and the positive electrode lead 72, except that the metal foil to serve as the negative electrode current collector 6 is used instead of the metal foil to serve as the positive electrode current collector 7, and the negative electrode slurry is used instead of the positive electrode slurry.
[0048] Next, the separator 5 is applied to the negative electrode active material layer 61 of the negative electrode, and the positive electrode is laminated so that the positive electrode active material layer 71 comes into contact with the separator 5. Thereafter, the laminated negative electrode, the separator 5, and the positive electrode are brought into close contact with each other and, if necessary, fixed with insulating tape (not shown). Fig. 1, Fig. 2(a) and Fig. The electrical storage element 12 shown in Fig. 2(b) is manufactured by the steps described above.
[0049] The electrical storage element in the battery 10 of the present embodiment is not limited to the Fig. 1, Fig. 2(a) and Fig.2(b). For example, the planar shape of the electric storage element may be a substantially non-circular shape, or it may be a substantially elliptical shape or a substantially polygonal shape, and may be determined as appropriate depending on the planar shape or the like of the first part 1. Moreover, in the electric storage element, a plurality of laminate structures in which the positive electrode, the separator, and the negative electrode are laminated together may be laminated together.
[0050] Furthermore, the electric storage element must include a positive electrode, a negative electrode, and an insulating film interposed between the positive electrode and the negative electrode, electrically separating the positive electrode and the negative electrode. A conventionally known electric storage element may be used. For example, an electric storage element including a positive electrode, a negative electrode, a separator (insulating film), and an electrolytic solution, such as those used in lithium batteries or the like, may be used. The electric storage element may, for example, comprise a wound body obtained by winding a tape-like complex with a separator interposed between a positive electrode and a negative electrode.In a housing in which the electrical storage element has the wound body described above, the central position of the wound complex and the central position of the cylindrical tubular portion 1b of the first part 1 may substantially overlap in a planar view.
[0051] At the Fig. 1, Fig. 2(a) and Fig. In the battery 10 shown in Fig. 2(b), the first part 1 and the second part 2 are made of a conductive material, the negative electrode in the electrical storage element 12 is electrically connected to the first part 1, the positive electrode is electrically connected to the second part 2, and the first part 1 and the second part 2 are electrically insulated from each other by the seal 3.
[0052] In the battery 10 of the present embodiment, it is required that one of the positive electrode or the negative electrode in the electric storage element 12 is electrically connected to the first part 1, the other is electrically connected to the second part 2, the first part 1 and the second part 2 are electrically insulated from each other by the gasket 3, the positive electrode in the electric storage element 12 may be electrically connected to the first part 1, and the negative electrode may be electrically connected to the second part 2. [Process for manufacturing a battery]
[0053] The Fig. 1, Fig. 2(a) and Fig. Battery 10 shown in Figure 2(b) can be manufactured, for example, by a method to be described below.
[0054] A substantially circular first metal foil is prepared to serve as the first part 1. The first metal foil is then subjected to a drawing process according to a known method, thereby forming the first part 1 having a predetermined shape and including the bottom portion 1a and the tubular portion 1b.
[0055] Next, the electrical storage element 12 is housed in the first part 1, and the first part 1 and the negative electrode of the electrical storage element 12 are connected by a resistance welding method of the negative electrode lead 62 (see Fig. 2(a)) of the electrical storage element 12 is electrically connected to the bottom portion 1a of the first part 1.
[0056] Next, a tape-like insulating layer having a substantially uniform thickness is prepared to serve as a gasket 3. Subsequently, a plurality of depressed portions are formed on one or both surfaces of the insulating layer. These plurality of depressed portions may be regularly or irregularly arranged. Furthermore, the plurality of depressed portions may be formed on the entire surface of the insulating layer or only on a part of the insulating layer. In a housing in which the plurality of depressed portions are formed only on a part of the insulating layer, the plurality of depressed portions are preferably formed on a portion located between the tubular portion 1b of the first part 1 and the second part 2.The recessed portions on the insulating layer can be formed, for example, by a method in which a roller having predetermined unevennesses on the surface is pressed against the insulating layer.
[0057] Subsequently, the insulating layer is applied so that it covers the end face 1c of the first part 1 and covers part of the tubular portion 1b of the first part 1 from the outside. In a housing in which the plurality of recessed portions are provided only on one surface of the insulating layer, the insulating layer is preferably applied so that the surface with the recesses is on the outside. This is because the non-contact portion 42, with which the gasket 3 is not in contact, can be easily formed on the second surface 2d of the second part 2.
[0058] Next, a round second metal foil is prepared to serve as the second member 2. Then, the second metal foil is attached to the first member 1 with the insulating layer having a plurality of recessed portions interposed therebetween. After that, the end portion of the second metal foil is folded along the tubular portion 1b of the first member 1, and the folded portion is joined to the tubular portion 1b of the first member 1 by caulking according to a known method. Thus, the second member 2 having a predetermined shape and including the lid-like portion 2a and the surrounding wall portion 2b is formed, and the interior of the casing 11 is placed in an airtight state.
[0059] Subsequently, the second part 2 and the positive electrode of the electrical storage element 12 are connected by a resistance welding process of the positive electrode lead 72 (see Fig.2(b)) of the electrical storage element 12 is electrically connected to the lid-like portion 2a of the second part 2.
[0060] The Fig. 1, Fig. 2(a) and Fig. The battery 10 shown in Figure 2(b) is manufactured by the steps described above.
[0061] The Fig. 1, Fig. 2(a) and Fig.The battery 10 shown in Fig. 2(b) has the case 11 that accommodates the electric storage element 12 in an airtight state, and the case 11 includes: the first member 1 having the bottom portion 1a and the tubular portion 1b; the second member 2 having the lid-like portion 2a covering the opening of the first member 1 and the surrounding wall portion 2b covering the tubular portion 1b from the outside; and the gasket 3 continuously disposed between the end surface 1c of the first member 1 and the second member 2 and between the tubular portion 1b and the second member 2. Furthermore, in the battery 10, the non-contact portions 41 and 42 with which the gasket 3 is not in contact are provided in both a part of the first surface 1d of the first part 1 facing the gasket 3 and a part of the second surface 2d of the second part 2 facing the gasket 3.
[0062] Regarding the battery 10, there are cases where the electric storage element 12 housed in the case 11 expands, a gas is generated from the electric storage element 12, or the internal pressure in the case 11 increases due to a change over time. In the non-contact portions 41 and 42, even if the internal pressure in the case 11 increases and the case 11 expands or deforms, part of a force associated with the deformation of the case 11 is absorbed by the space between the first surface 1d and / or the second surface 2d and the gasket 3. Therefore, the force opposing the non-contact portions 41 and 42 and associated with the deformation of the case 11, which is applied to the gasket 3, is relieved.This can prevent a crack from occurring in the seal 3 facing the non-contact sections 41 and 42 due to the force associated with the deformation of the housing 11.
[0063] In addition, when the force associated with the deformation of the case 11 becomes large, air between the non-contact portions 41 and 42 and the gasket 3 is forced outward, the space between the first surface 1d and / or the second surface 2d and the gasket 3 collapses, and the gasket 3 facing the non-contact portions 41 and 42 is pressed against the non-contact portions 41 and 42. As a result, even in a case where a crack is generated in the gasket 3 in contact with the first surface 1d and the second surface 2d when the battery 10 is completed due to the force attributed to the deformation of the case 11, the airtight state in the case 11 is maintained by the sealing ability of the gasket 3 pressed against the non-contact portions 41 and 42.
[0064] For these reasons, it is possible to maintain the airtight state in the case 11 for a long period of time, and it makes the battery 10 of the present embodiment less susceptible to deterioration and excellent in reliability.
[0065] In contrast, for example, in a battery in which the gasket 3 is in contact with the entire first surface 1d of the first part 1 facing the gasket 3 and the entire second surface 2d of the second part 2 facing the gasket 3, the airtightness of the case after completion of the battery is favorable. However, in this battery, a crack was easily generated in the gasket 3 by a force resulting from the deformation of the case combined with an increase in the internal pressure in the case, and it was not possible to maintain the airtight state in the case for a long period of time.
[0066] Furthermore, it is in the Fig. 1, Fig. 2(a) and Fig.2(b) such that the tubular portion of the first part 1 has a cylindrical shape and includes the first outer diameter portion 1e, the second outer diameter portion 1f has a larger outer diameter than the first outer diameter portion 1e, and the stepped portion 1g connects the first outer diameter portion 1e and the second outer diameter portion 1f, and the first outer diameter portion 1e is arranged at a position closer to the bottom portion 1a than the second outer diameter portion 1f. Moreover, in the sectional area along the center of the tubular portion 1b, the stepped portion 1g is within a length range of 1 / 3 of the length L1 of the tubular portion facing the surrounding wall portion 2b of the second part 2 from the central position of the length L1 of the tubular portion 1b facing the surrounding wall portion 2b, as shown in Fig.1. Therefore, even when the internal pressure in the housing 11 increases, the airtight state in the housing 11 can be maintained for a longer period of time due to the sealing ability of the gasket 3 for the reasons (1) to (3) described below.
[0067] (1) A force generated by caulking the surrounding wall portion 2b of the second member 2 with the tubular portion 1b becomes weak in the bottom portion 1a-side region of the step portion 1g compared to the end surface 1c-side region of the step portion 1g. Therefore, when the internal pressure in the casing 11 increases, the bottom portion 1a-side region of the step portion 1g preferentially expands, while the deformation in other portions of the casing 11 is dampened. The generation of a crack in the gasket 3 located outside the bottom portion 1a-side region of the step portion 1g can be prevented.
[0068] (2) It becomes easy to form the non-contact portion 41 having a wide area with which the seal 3 is not in contact in the bottom portion 1a-side portion of the step portion 1g on the first surface 1d, and it becomes easy to form the non-contact portion 42 having a wide area with which the seal 3 is not in contact on the second surface 2d located so as to oppose the first outer diameter portion 1e. Therefore, even if the bottom portion 1a-side portion of the step portion 1g expands, a force attributed to the expansion is absorbed by the non-contact portions 41 and 42 having a large area, and the force attributed to the expansion of the housing 11 and exerted on the seal 3 facing the non-contact portions 41 and 42 is relieved.
[0069] (3) When the internal pressure in the housing 11 increases, the gasket 3 facing the second outer diameter portion 1f where the distance between the surrounding wall portion 2b of the second member 2 and the tubular portion 1b is narrow is pressed against the non-contact portions 41 and 42. Thereafter, as the internal pressure in the housing 11 further increases, the expansion of the bottom portion 1a-side area of the step portion 1g becomes even larger and can no longer be absorbed by the non-contact portions 41 and 42, and the gasket 3 facing the non-contact portions 41 and 42 is pressed against the non-contact portions 41 and 42.Therefore, even if a crack occurs in the gasket 3 which was in contact with the first surface 1d and the second surface 2d after the completion of the battery 10, the airtight state in the case 11 is maintained by the sealing ability of the gasket 3 pressed against the non-contact portions 41 and 42. <Zweite Ausführungsform>
[0070] Fig. Fig. 3 is a schematic cross-sectional view showing a battery of a second embodiment. With respect to a battery 10a of the second embodiment shown in Fig. 3, the same parts as in the battery 10 of the first embodiment described above are designated by the same reference numerals and will not be described again. In a first part 1 in a housing 11a of the Fig. 3, a tubular portion 11b has a cylindrical shape as in the battery 10 of the first embodiment. Fig.3 is a schematic cross-sectional view of a cut surface along a planar view center of the tubular portion 11b.
[0071] The battery 10a of the second embodiment differs from the battery 10 of the first embodiment in that the tubular portion 11b in the first part 1 of the housing 11a has a substantially constant outer diameter and has no stepped portions. The tubular portion 11b extends in a direction substantially perpendicular to the extension direction of a bottom portion 1a, as shown in Fig. 3 shown.
[0072] Similar to the battery 10 of the first embodiment, the one shown in Fig.3 has the housing 11a which houses an electrical storage element 12 in an airtight state, and the housing 11a comprises a first part 1, a second part 2, and a gasket 3. In addition, non-contact portions 41 and 42 with which the gasket 3 is not in contact are provided in both a part of a first surface 1d of the first part 1 facing the gasket 3 and a part of a second surface 2d of the second part 2 facing the gasket 3. Therefore, the Fig. 3, similarly to the battery 10 of the first embodiment, is capable of maintaining the airtight state in the casing 11a for a long period of time, is less susceptible to deterioration, and has excellent reliability. (More examples)
[0073] The battery of the present invention is not limited to the embodiments described above.
[0074] In the Fig. 1 and Fig. For example, in the batteries 10 and 10a shown in Fig. 3, a case has been described in which the non-contact portions 41 and 42 with which the gasket 3 is not in contact are provided in a part of the first surface 1d of the first part 1 opposite to the gasket 3 and in a part of the second surface 2d of the second part 2 opposite to the gasket 3, respectively, but the non-contact portion may be provided only in a part of the first surface 1d or a part of the second surface 2d.
[0075] In a case where the non-contact portion is provided only in either a part of the first surface 1d or a part of the second surface 2d, it is preferable that the non-contact portion 42 be provided in a part of the second surface 2d of the second member 2 that is opposite to the gasket 3. This is because when the space between the second surface 2d has a larger surface area than the first surface 1d and the gasket 3, a force due to the deformation of the housing 11 or 11a can be more effectively absorbed, and it is possible to more effectively prevent a crack from being generated in the gasket 3.
[0076] In the batteries 10 and 10a, which are in Fig. 1 and Fig.3, a housing has been described in which the bottom portion 1a of the first part 1 has a round shape in a plan view and the tubular portions 1b and 11b have a cylindrical shape, but the planar shapes of the bottom portion 1a of the first part 1 and the tubular portions 1b and 11b do not necessarily have to be a round shape, but may have, for example, a polygonal shape such as a square shape, a rectangular shape or a hexagonal shape, an elliptical shape or an oval shape, and are not particularly limited.
[0077] In the Fig. 1 and Fig.3, a case where the lid-like portion 2a of the second part 2 has a round shape in a plan view has been described as an example, but the planar shape of the lid-like portion 2a is not limited to a round shape, is preferably a substantially similar shape to the planar shape of the bottom portion 1a of the first part 1, and can be appropriately selected depending on the planar shape of the bottom portion 1a.
[0078] In the Fig. 1 and Fig.3, a case where the surrounding wall portion 2b of the second part 2 has a cylindrical shape has been described as an example, but the planar shape of the surrounding wall portion 2b is not limited to a round shape, is preferably a substantially similar shape to the planar shapes of the tubular portions 1b and 11b of the first part 1, and can be appropriately selected depending on the planar shapes of the tubular portions 1b and 11b.
[0079] So far, the embodiments of the present invention have been described in detail, but each configuration in each embodiment, a combination thereof, or the like is an example, and addition, omission, replacement, and other changes of the configuration are possible within the scope of the features of the present invention. [Examples]“Example 1” (Production of an electrical storage element)
[0080] A positive electrode slurry was prepared by mixing lithium cobaltate as the positive electrode active material, polyvinylidene fluoride (PVDF) as the binder, acetylene black as the conductive auxiliary, and N-methyl-2-pyrrolidone (NMP) as the solvent into a paste. The positive electrode slurry was then coated onto an aluminum foil, which would serve as the positive electrode current collector 7, using a doctor blade method. The aluminum foil, onto which the positive electrode slurry had been coated, was then dried at 150°C. The dried, coated foil was then pressed and highly densified, forming a positive electrode active material layer 71.
[0081] Subsequently, the aluminum foil with the positive electrode active material layer 71 was punched out using a PINNACLE DIE (registered trademark). The aluminum foil with the positive electrode active material layer 71 was formed into a shape corresponding to the positive electrode current collector 7, which had a circular shape with a diameter of 10 mm, and a band-shaped positive electrode lead 72, which was 20 mm long and 5 mm wide, extended from the edge portion of the positive electrode current collector 7. Subsequently, the positive electrode active material layer 71, which had been formed at a portion of the aluminum foil to serve as the positive electrode lead 72, was peeled off. A positive electrode composed of the positive electrode current collector 7 and the positive electrode active material layer 71, as well as the positive electrode lead 72 integrated with the positive electrode current collector 7, was obtained through the steps described above.
[0082] Subsequently, a negative electrode slurry was prepared by mixing graphite as the negative electrode active material, polyvinylidene fluoride (PVDF) as the binder, and N-methyl-2-pyrrolidone (NMP) as the solvent to form a paste. Next, a negative electrode consisting of a negative electrode current collector 6 with a round shape and a diameter of 13 mm, a positive electrode active material layer 61, and a tape-like negative electrode lead 62 with a length of 3 mm and a width of 5 mm integrated with the negative electrode current collector 6 was prepared in the same manner as in the preparation of the positive electrode and the positive electrode lead 72, except that a copper foil to serve as the negative electrode current collector 6 was used instead of the aluminum foil, and the negative electrode slurry was used instead of the positive electrode slurry.
[0083] Subsequently, a circular separator 5 with a larger diameter than the negative electrode current collector 6 was applied to the negative electrode active material layer 61, and the positive electrode was laminated so that the positive electrode active material layer 71 came into contact with the separator 5. Afterward, the negative electrode, the separator 5, and the laminated positive electrode were brought into close contact with each other and fixed with insulating tape. An electrical storage element 12 as shown in Fig. 1 was obtained by the steps described above. (manufacturing of batteries)
[0084] Next, a first metal foil consisting of a 100 µm thick, substantially round stainless steel foil was prepared to serve as the first part 1. Thereafter, the first metal foil was subjected to a drawing process, forming a 4.0 mm high first part 1 having a round bottom portion 1a and a tubular portion 1b.
[0085] As the first part 1, the tubular portion 1b was formed, which included a first outer diameter portion 1e with an outer diameter of 20.0 mm, a second outer diameter portion 1f with an outer diameter of 20.4 mm, and a step portion 1g connecting the first outer diameter portion 1e and the second outer diameter portion 1f. An inner surface-side curvature radius r1 of the first part 1 formed by the step portion 1g was 100 μm, and an outer surface-side curvature radius r2 was 100 μm. The step portion 1g was formed to be located at the center of a length L1 of the tubular portion 1b, which is opposed to the surrounding wall portion 2b of the second part 2.
[0086] Next, the electric storage element 12 was housed in the first part 1, and the first part 1 and the negative electrode of the electric storage element 12 were electrically connected to each other by a method in which the negative electrode lead 62 of the electric storage element 12 was resistance-welded to the bottom portion 1a of the first part 1.
[0087] Next, a tape-shaped insulating layer made of polypropylene with a substantially uniform thickness of 100 µm was prepared to serve as gasket 3. Subsequently, a plurality of recessed portions were formed on both surfaces of the insulating layer. The recessed portions on the insulating layer were formed by a process in which a roller with a plurality of rectangular protrusions with a height of 30 µm, a length of 50 mm, and a width of 50 µm at intervals of 200 µm on the roller surface was pressed against the insulating layer.
[0088] Subsequently, the insulating layer was applied in such a way that it covers an end face 1c of the first part 1 and covers part of the tubular section 1b of the first part 1 from the outside.
[0089] Next, a second metal foil consisting of a 100 µm thick, substantially circular stainless steel foil was prepared to serve as the second part 2. Furthermore, the second metal foil was applied to the first part 1 with the insulating layer having a plurality of recessed portions sandwiched between them. Afterward, the end portion of the second metal foil was folded along the tubular portion 1b of the first part 1, and the folded portion was joined to the tubular portion 1b of the first part 1 by caulking.
[0090] The second part 2 was formed with the round lid-like section 2a and the surrounding wall section 2b with an outer diameter of 20.6 mm and the interior of a housing 11 was placed in an airtight state.
[0091] Subsequently, the second part 2 and the positive electrode of the electrical storage element 12 were electrically connected to each other by a resistance welding process of the positive electrode lead 72 of the electrical storage element 12 to the lid-like portion 2a of the second part 2.
[0092] A battery 10 of the Fig. Example 1 shown in Figure 1 was prepared by the steps described above.
[0093] In the battery 10 of Example 1, in a sectional area along the center of the tubular portion 1b of the first part 1, a length L3 of the gasket 3 in the longitudinal direction of the tubular portion 1b was 3.5 mm, and a distance L2 of the second part 2 in the longitudinal direction of the tubular portion 1b from the outer surface of the lid-like portion 2a to the end surface 2c of the surrounding wall portion 2b was 3.0 mm. “Example 2”
[0094] A battery 10 according to Example 2 was manufactured in the same manner as Example 1, except that the arrangement of the insulating layer was changed. In the battery 10 of Example 2, the length L3 of the gasket 3 in the longitudinal direction of the tubular portion 1b in a sectional area along the center of the tubular portion 1b of the first part 1 was 2.8 mm. “Example 3”
[0095] A 10a battery of the Fig. Example 3 shown in Figure 3 was manufactured in the same manner as Example 1, except that the tubular portion 11b of the first part 1 had a constant outer diameter of 20.4 mm and had no step portions. “Example 4”
[0096] A battery 10 according to Example 4 was manufactured in the same manner as Example 1, except that a roller having a plurality of rectangular projections having a height of 30 µm, a length of 10 mm, and a width of 10 µm at intervals of 200 µm on the roller surface was used as the roller. “Example 5”
[0097] A battery 10a according to Example 5 was manufactured in the same manner as Example 3, except that a roller having a plurality of rectangular projections having a height of 30 µm, a length of 10 mm, and a width of 10 µm at intervals of 200 µm on the roller surface was used as the roller. “Example 6”
[0098] A battery 10a according to Example 6 was manufactured in the same manner as in Example 3, except that the arrangement of the insulating layer was changed. In the battery 10a of Example 6, the length L3 of the gasket 3 in the longitudinal direction of the tubular portion 1b in a sectional area along the center of the tubular portion 1b of the first part 1 was 2.8 mm. “Example 7”
[0099] A battery 10a according to Example 7 was manufactured in the same manner as Example 6, except that a plurality of recessed portions were formed on only one surface of the insulating layer and the insulating layer was attached so that the surface of the insulating layer having the recessed portions was on the inside. “Example 8 and Example 9”
[0100] The batteries 10a of Example 8 and Example 9 were manufactured in the same manner as Example 7, except that the number of times the roller was pressed against the insulating layer was changed. The number of times the roller was pressed against the insulating layer in Example 8 was smaller than the number of times in Example 7, and the number of times the roller was pressed against the insulating layer in Example 9 was larger than the number of times in Example 7. “Example 10”
[0101] A battery 10a of Example 10 was manufactured in the same manner as in Example 6, except that a plurality of recessed portions were formed on a surface of the insulating layer by using a roller having a plurality of rectangular projections having a height of 30 µm, a length of 10 mm, and a width of 10 µm and arranged at intervals of 200 µm on the surface of the roller, and the insulating layer was installed so that the surface having the recessed portions of the insulating layer was outside. “Example 11 and Example 12”
[0102] Batteries 10a of Example 11 and Example 12 were manufactured in the same manner as Example 10, except that the number of times the roller was pressed against the insulating layer was changed. The number of times the roller was pressed against the insulating layer was set higher in both Example 11 and Example 12 than the number of times in Example 10, and the number of times in Example 11 was set higher than that in Example 12. “Example 13 to Example 16”
[0103] Batteries 10a of Examples 13 to 16 were manufactured in the same manner as in Example 6, except that the number of times the roller was pressed against the insulating layer was changed on each of the two surfaces of the insulating layer. On the surface of the insulating layer facing the tubular portion 1b of the first part 1, the number of times the roller was pressed against the insulating layer in Examples 13 and 14 was set smaller than the number in Example 6, and the number of times the roller was pressed against the insulating layer in Examples 15 and 16 was set larger than the number in Example 6.In addition, on the surface of the insulating layer facing the second part 2, the number of times the roller was pressed against the insulating layer in Example 13 and Example 15 was set smaller than the number of times in Example 6, and the number of times the roller was pressed against the insulating layer in Example 14 and Example 16 was set larger than the number of times in Example 6. “Comparison Example 1”
[0104] A battery 10 of Comparative Example 1 was manufactured in the same manner as in Example 6, except that the insulating layer was used without forming the recessed portions. “Comparison example 2”
[0105] A battery 10 of Comparative Example 2 was manufactured in the same manner as in Example 1, except that the insulating layer was used without forming the recessed portions. [Measurement of percentage deterioration]
[0106] With respect to each of the batteries 10 and 10a of Example 1 to Example 16, Comparative Example 1, and Comparative Example 2 obtained as described above, using a battery charging / discharging system (SM-8: manufactured by Meiden Hokuto Corporation), constant current charging was performed up to 4.2 V at a current of 0.1 C, and after the voltage reached 4.2 V, constant voltage charging was performed until a current of 0.05 C was reached. Subsequently, constant current discharging was performed to 3.0 V at a current of 0.1 C, and the discharge capacity was measured (capacity before storage).
[0107] Thereafter, each of the batteries 10 and 10a, whose capacity had been measured before storage, was charged, brought to a fully charged state, and stored for one month at an ambient temperature of 60 °C and a humidity of 95%.
[0108] For each of the batteries 10 and 10a, a constant current discharge to 3.0 V was performed at a current of 0.1 C after storage. Afterward, the battery was charged and discharged under the same conditions as before the pre-storage capacity measurement, and the discharge capacity was measured in the same manner as the pre-storage capacity measurement (capacity after storage).
[0109] Subsequently, the percentage deterioration of capacity ([capacity after storage / capacity before storage] × 100 (%)) was calculated from the capacities before storage and after storage. The results are shown in Table 1. [Table 1] 1f - 1e Percentage of non-contact section 41 Presence or absence of a plurality of non-contact sections 41 of 10 µm or more Percentage of non-contact section 42 Presence or absence of a plurality of non-contact sections 42 of 10 µm or more Presence or absence of a step section s 1g L3 - L2 Degree of deterioration Example 1 0.2 mm 50% Available 50% Available Available More than 0 90% Example 2 0.2 mm 50% Available 50% Available Available 0 or less 88% Example 3 0.0 mm 50% Available 50% Available Missing More than 0 88% Example 4 0.2 mm 50% Missing 50% Missing Available More than 0 87% Example 5 0.0 mm 50% Missing 50% Missing Missing More than 0 85% Example 6 0.0 mm 50% Missing 50% Missing Missing 0 or less 85% Example 7 0.0 mm 50% Missing 0% Missing Missing 0 or less 83% Example 8 0.0 mm 19% Missing 0% Missing Missing 0 or less 79% Example 9 0.0 mm 96% Missing 0% Missing Missing 0 or less 76% Example 10 0.0 mm 0% % Missing 39% Missing Missing 0 or less 78% Example 11 0.0 mm 0% % Missing 81% Missing Missing 0 or less 79% Example 12 0.0 mm 0% Missing 70% Missing Missing 0 or less 82 % Example 13 0.0 mm 19% Missing 39% Missing Missing 0 or less 78% Example 14 0.0 mm 19% Missing 81% Missing Missing 0 or less 78% Example 15 0.0 mm 96% Missing 39% Missing Missing 0 or less 76% Example 16 0.0 mm 96% Missing 81% Missing Missing 0 or less 74% Comparison example 1 0.0 mm 0% Missing 0% Missing Missing 0 or less 65% Comparison example 2 0.2 mm 0% % Missing 0% Missing Available More than 0 69%
[0110] The battery 10 of Example 1, on which the capacity deterioration rate had been measured, was embedded in a resin, and two arbitrary locations along the center of the tubular portion 1b of the first part 1 were cut out using a precision cutting machine (trade name: ISOMET, manufactured by Buhler). The resulting cut surfaces of the two locations were each polished with sandpaper. Afterward, the surface was milled by irradiating each cut surface with an Ar ion beam using an ion milling machine (trade name: IM4000, manufactured by Hitachi High-Tech Corporation), and a cross-sectional observation sample was obtained.
[0111] The cut surface of each cross-sectional sample was observed with a laser microscope (trade name: VK-X, manufactured by Keyence Corporation), and the number and lengths of the non-contact sections 41 and 42 with a length of 100 μm or more were examined on the obtained image.
[0112] In addition, the cut surface of each cross-sectional sample was observed with a scanning electron microscope (SEM) (trade name: SU8220, manufactured by Hitachi High-Tech Corporation), and the number and length of the non-contact sections 41 and 42 with a length of less than 100 μm were examined on the obtained image.
[0113] Furthermore, the percentage of the length of the non-contact portions 41 provided on a first surface 1d with respect to the length L1 of the tubular portion 1b facing the surrounding wall portion 2b of the second part 2 in each section was calculated, and an average value thereof (hereinafter referred to as "the percentage of non-contact portions 41" in some packages) was determined. The results are shown in Table 1.
[0114] Furthermore, the percentage of the length of the non-contact portions 42 provided on a second surface 2d was calculated with respect to the distance L2 of the second part 2 in the longitudinal direction of the tubular portion 1b from the outer surface of the lid-like portion 2a to the end surface 2c of the surrounding wall portion 2b in each section, and an average value thereof (hereinafter referred to in some cases as "the percentage of the non-contact portions 42") was obtained. The results are shown in Table 1.
[0115] Furthermore, for each cut surface, images obtained by laser microscopy and scanning electron microscope (SEM) observation were examined to determine whether a majority of the non-contact portions 41 and 42 with a length of 10 µm or more were present. The results are shown in Table 1. In Table 1, "Present" was entered for a package in which multiple non-contact portions 41 with a length of 10 µm or more (or multiple non-contact portions 42 with a length of 10 µm or more) were provided on all cut surfaces, and "Missing" was entered for other cases.
[0116] In each of the batteries 10 and 10a of Example 2 to Example 16, Comparative Example 1, and Comparative Example 2 in which the deterioration rate of capacity was measured, the cut surfaces at two arbitrary positions along the center of the tubular portion 1b of the first part 1 were observed, and the number and lengths of the non-contact portions 41 and 42 were examined in the same manner as in Example 1 in which the deterioration rate of capacity was measured.
[0117] In each of the batteries 10 and 10a of Example 1 to Example 16, Comparative Example 1, and Comparative Example 2, the difference (1f - 1e) between the outer diameter of the first outer diameter portion 1e and the outer diameter of the second outer diameter portion 1f in the first part 1, the percentage of the non-contact portions 41, the percentage of the non-contact portions 42, whether a plurality of the non-contact portions 41 and 42 having a length of 10 µm or more were provided or not,the presence or absence of the step portion 1g and whether the difference (L3 - L2) between the length L3 of the gasket 3 in the longitudinal direction of the tubular portion 1b or 11b and the distance L2 of the second part 2 in the longitudinal direction of the tubular portion 1b or 11b from the outer surface of the lid-like portion 2a to the end surface 2c of the surrounding wall portion 2b in the sectional area along the center of the tubular portion 1b or 11b of the first part 1 is greater than zero or not are given in Table 1.
[0118] As shown in Table 1, the percentages of capacity deterioration in the batteries 10 and 10a of Example 1 to Example 16 having the non-contact portions 41 and / or the non-contact portions 42 were high compared to those in the batteries of Comparative Example 1 and Comparative Example 2 in which the gasket 3 and all the facing surfaces of the first part 1 and the second part 2 were in contact with each other (the percentages of the non-contact portions 41 and 42 were 0%). This is believed to be because the batteries 10 and 10a of Example 1 to Example 16 had the non-contact portions 41 and 42, and thus it was possible to maintain the airtight state in the cases 11 and 11a during storage.
[0119] Specifically, in the batteries 10 and 10a of Example 1 to Example 16, the batteries 10 and 10a of Example 1 to Example 7, and Example 12 in which the percentage of non-contact portions 41 was 20% to 95% and / or the percentage of non-contact portions 42 was 40% to 80%, the capacity deterioration rates were 80% or more, and it was confirmed that the batteries had a lower probability of deterioration. [Industrial applicability]
[0120] According to the present invention, it is possible to maintain the airtight state in the case for a long period of time and to provide a battery that is less susceptible to damage. List of reference symbols
[0121] [List of reference signs] 1 First Part 1a floor section 1b, 11b tubular section 1c End face 1d First surface 1e First outer diameter section 1f Second outer diameter section 1g step section 2 Second part 2a Lid-like section 2b Surrounding wall section 2c End face 2d Second Surface 3 Seal 5 Separator 6 Negative electrode current collector 7 Positive electrode current collector 10, 10a battery 11, 11a housing 12 Electrical storage element 41, 42 Non-contact section 61 Negative electrode active material layer 62 Negative electrode lead 71 Positive electrode active material layer 72 Positive electrode lead r1 Inner surface-side radius of curvature r2 Outer surface-side radius of curvature QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] Japanese Patent Application No. 2022-004113
[0002]
Claims
[1] A battery comprising: an electrical storage element having a positive electrode, a negative electrode, and an insulating film disposed between the positive electrode and the negative electrode and electrically separating the positive electrode and the negative electrode; and a housing that houses the electrical storage element in an airtight manner, wherein the housing comprises a first part with a bottom portion and a tubular portion; a second part having a lid-like portion covering an opening of the first part and a surrounding wall portion covering the tube-like portion from an external environment; and a seal continuously disposed between an end face of the first part and the second part and between the tubular portion and the second part, and a non-contact portion with which the seal is not in contact is provided in either a part of a first surface of the first part facing the seal or a part of a second surface of the second part facing the seal, or both. [2] The battery according to claim 1, wherein the non-contact portion is provided on the second surface. [3] The battery according to claim 2, wherein the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a percentage of a length of the non-contact portion provided on the second surface with respect to a distance L2 in a longitudinal direction of the tubular portion from an outer surface of the lid-like portion to an end surface of the surrounding wall portion is 20% to 95%. [4] The battery according to any one of claims 1 to 3, wherein the non-contact portion is provided on the first surface. [5] The battery according to claim 4, wherein the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a percentage of a length of the non-contact portion provided on the first surface with respect to a length L1 of the tubular portion facing the surrounding wall portion is 40% to 80%. [6] The battery according to any one of claims 1 to 5, wherein the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a plurality of non-contact portions having a length of 10 µm or more are present. [7] The battery according to any one of claims 1 to 6, wherein the tubular portion of the first part has a cylindrical shape and comprises: a first outer diameter portion; a second outer diameter portion having a larger outer diameter than the first outer diameter portion; and a step portion connecting the first outer diameter portion and the second outer diameter portion, wherein the first outer diameter portion is arranged closer to the bottom portion than the second outer diameter portion, and wherein, in a sectional area passing through a center of the tubular portion, the step portion is provided within a length range of 1 / 3 of a length L1 of the tubular portion facing the surrounding wall portion from a central position of the length L1 of the tubular portion facing the surrounding wall portion. [8] The battery according to any one of claims 1 to 7, wherein the tubular portion of the first part has a cylindrical shape, and in a sectional area along a center of the tubular portion, a length L3 of the seal in a longitudinal direction of the tubular portion is greater than a distance L2 in the longitudinal direction of the tubular portion from an outer surface of the lid-like portion to an end surface of the surrounding wall portion.
Citation Information
Patent Citations
Battery
JP2023103542A