Battery module
The battery module design with controlled weld bead geometry and material composition addresses the instability of laser welding heterogeneous materials, enhancing tensile strength and reducing resistance in battery modules.
Patent Information
- Application Number
- DE202020006073
- Authority / Receiving Office
- DE · DE
- Patent Type
- Utility models
- Current Assignee / Owner
- Priority Date
- 2020-11-19
- Filing Date
- 2020-11-20
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2030-11-30
AI Technical Summary
Existing laser welding methods for connecting electrode strips to busbars in battery modules result in inconsistent tensile strength and high probability of defects, particularly when using heterogeneous materials like aluminum and copper, leading to increased process complexity and cost.
A battery module design with a bus bar featuring holes for electrode strips, where the strips are inserted and welded with a controlled weld bead shape and composition, ensuring stable connections by adhering to specific geometric parameters and material ratios.
Achieves a stable weld with twice the tensile strength and reduced electrical resistance, minimizing defects and process complexity while maintaining electrical properties.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery module, and in particular to a battery module with improved mechanical and electrical properties. [State of the art]
[0002] Recently, the demand for high-capacity and high-performance secondary batteries has increased, and it is necessary to develop secondary batteries that require high energy density, high performance, and a high level of reliability to meet these requirements.
[0003] Particularly for the electrical connection between cells, which requires a high degree of reliability, various methods such as ultrasonic welding, laser welding, and mechanical bonding (screws / nuts) have been used. Among these, laser welding is the most common connection method used to meet the increasing demands for energy density.
[0004] Laser welding typically employs an overlap welding process involving one or more electrode strips and a busbar. However, this method exhibits significant variation in tensile strength after welding and a high probability of welding defects, such as weak welds, depending on the pressure conditions. As in Fig. As shown in Figure 1, electrode strips of multiple specifications must be bent and cut in a single module for welding, resulting in increased process complexity and manufacturing costs.
[0005] Furthermore, the resistance of each cell within a module is uneven due to the varying lengths of the electrode strips for each cell specification, which most likely has a negative impact on long-term durability. In particular, when using existing laser welding processes, it is quite difficult to ensure stable weld quality (tensile strength, electrical resistance, etc.) when welding the electrode strips to a busbar, especially when they are made of different materials. Prior to the present invention, a stable weld between an aluminum strip and a copper busbar could not be achieved. [Invention][Technical Problem]
[0006] One objective of the present invention is to provide a battery module that has a welded part with excellent tensile strength and contact resistance by appropriately controlling the welding of heterogeneous materials between an electrode strip and a busbar.
[0007] The aims and objectives of the present invention are not limited to those mentioned above. That is to say, other aims and objectives not mentioned can be obviously understood by those skilled in the art in the field to which the present invention belongs from the following description. [Technical solution]
[0008] In a general aspect, a battery module comprises: a plurality of battery cells, each containing an electrode strip; and a busbar connected to the electrode strip to electrically connect the plurality of battery cells together, the busbar comprising a plate in which a plurality of holes is formed, the electrode strips of each of the battery cells being inserted into at least a part of the plurality of holes in the plate, the electrode strips inserted into the hole and the plate being connected together by a weld bead, and the weld bead satisfying equations 1 and 2 below. 0 <W<7T
[0009] In equation 1, W is the width of the weld bead, based on the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip. 0 <H<3T
[0010] In equation 2, H is the height of the weld bead, relative to the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip.
[0011] W can range from 2T to 6T, and H can range from 0.5T to 2T.
[0012] In another aspect, a battery module comprises: a plurality of battery cells, each containing an electrode strip; and a busbar connected to the electrode strip to electrically connect the plurality of battery cells together, the busbar comprising a plate in which a plurality of holes is formed, the electrode strips of each of the battery cells being inserted into at least a part of the plurality of holes in the plate, the electrode strip inserted into the hole and the plate being connected together by a weld bead, and the weld bead satisfying Equation 3 below. 0 <A<21T2
[0013] In equation 3, A is the cross-sectional area of the weld bead, based on the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip.
[0014] A can T 2 up to 12T 2 be.
[0015] The weld bead can also satisfy equation 4 below. 0.4T≤D≤2T
[0016] In equation 4, D is the penetration depth of the weld bead into a hole, based on the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip.
[0017] The electrode strip and the plate can be made of different materials.
[0018] This is particularly effective in ensuring a stable weld between an electrode strip and a busbar made of different materials. For example, a stable weld can be achieved between an aluminum electrode strip and a copper busbar.
[0019] The weld bead can be made from 70 to 99 wt% of a first base material and a remainder of a second base material, by using the electrode strip as the first base material for welding and the plate as the second base material for welding.
[0020] The electrode strip can be made of aluminum and the plate of copper.
[0021] The plate or electrode strip may contain a surface plating layer.
[0022] The surface plating layer may contain Ni, Sn, Si, Mg, Fe, Mn, Zn, Cr, Li, Ca or an alloy thereof.
[0023] The thickness of the electrode strip can be 0.2 mm or more.
[0024] The thickness of the electrode strip can range from 0.2 mm to 1.0 mm.
[0025] The thickness of the plate can be 0.5 mm or more.
[0026] The weld bead may include: a cover part with a convex shape that covers the hole on one of the two opposing surfaces in the thickness direction of the plate; and a column part that is loaded into the hole based on the cross-section of the weld bead in the thickness direction of the plate.
[0027] In the cross-section of the weld bead in the thickness direction of the plate, the weld bead can be left-right asymmetrical with respect to a center line of the hole.
[0028] In the cross-section of the weld bead in the thickness direction of the plate, the weld bead can exhibit a left-right asymmetry in the ratio L1 : L2 by defining as a boundary point a point where an interface between the weld bead and one of two opposite surfaces in the thickness direction of the plate and a surface of one of the surfaces meet.
[0029] The plate may have a protruding area formed around the point where the hole is created.
[0030] The plate may contain a strip connecting part that protrudes outwards from the plate from an outer circumference of the hole.
[0031] The hole can have an insertion part with an open side, so that the electrode strip can be inserted.
[0032] The battery cell can be a bag-type battery cell. [Beneficial Effects]
[0033] According to the present invention of the configuration described above, it is possible to ensure stable welding quality, and in particular, it is possible to provide a high-quality welded part with an equivalent level of contact resistance and a higher tensile strength, which is more than twice as high as in the conventional method in the case of welding heterogeneous materials of an electrode strip and a busbar.
[0034] Furthermore, it is possible to reduce the resistance in a module by minimizing the length of an electrode strip, and it is possible to ensure and manage stable weld quality by controlling the height, width, or area of a weld bead formed after welding in a specific area.
[0035] Furthermore, it is possible to ensure and control stable weld quality by controlling the elemental composition of a welded part that is formed after welding. [BRIEF DESCRIPTION OF THE DRAWINGS] Fig. Figure 1 is a diagram showing a conventional battery module with a C-shaped busbar. Fig. Figure 2 is a diagram showing a battery module according to an embodiment of the present invention. Fig. Figure 3 is a diagram showing a busbar forming the battery module according to the present invention. Fig. Figure 4 is a diagram showing a battery module with a weld bead according to an embodiment of the present invention. Fig. Figure 5 is a diagram showing a busbar according to another embodiment of the present invention. Fig.Figure 6 is a diagram showing a busbar according to another embodiment of the present invention. Fig. Figure 7 is a diagram illustrating a state in which a laser L is irradiated with respect to a longitudinal direction d1 of an electrode strip according to another embodiment of the present invention. Fig. Figure 8 is a diagram showing an imaginary surface for producing a cross-section of a weld bead in the thickness direction of a plate according to another embodiment of the present invention. Fig. Figure 9 is a schematic cross-sectional diagram illustrating that the weld bead is formed together with the plate by heating and melting an end section of an electrode strip, which penetrates through a hole in the plate according to the embodiment of the present invention, with a laser. Fig.10 is a photograph showing the shape of the weld bead when an Al electrode strip is welded to a Cu busbar with heterogeneous materials according to the method of Fig. 7 is welded. [Detailed description]
[0036] A battery module of the present invention is described in detail below with reference to the accompanying drawings. The drawings below are exemplary to adequately convey the content of the present invention to those skilled in the art. Therefore, the present invention is not limited to the drawings shown below, but can be modified in many different ways. Furthermore, the accompanying drawings suggested below may be exaggerated to clarify the content and scope of the present invention.Technical and scientific terms used in this description have the general meaning understood by those skilled in the field to which the present invention relates, unless otherwise defined, and any description of the known function and configuration which unnecessarily obscures the core of the present invention is omitted from the following description and the accompanying drawings.
[0037] Furthermore, a singular form used in the description and the accompanying claims may include a plural form unless otherwise indicated by the context.
[0038] In this description and the attached claims, terms such as "first", "second", etc. are used to distinguish the individual components, not in a restrictive sense.
[0039] In this description and the accompanying claims, the terms “contain” or “have” mean that the features or elements described in the description are present, unless expressly limited, and do not preclude the possibility of adding one or more other features or components, unless expressly limited.
[0040] In the present description and the attached claims, if a part, such as a film (layer), area, component, etc., is located above or on another part, this includes not only the case where a part is directly above it in contact with another part, but also the case where another film (layer), area, or component is arranged in between.
[0041] In conventional overlap welding, especially when welding a copper busbar and an aluminum electrode strip made of heterogeneous copper-aluminum material, the weld strength (tensile strength) is generally 3.5 kgf / mm². 2 or more. This corresponds to approximately 70% or more of the tensile strength of 5.5 kgf / mm². 2 of pure Al, which meets the weldability generally required for products, as well as the requirements for mechanical strength such as vibration and shock resistance of products.
[0042] In recent years, however, the requirements for the mechanical strength of lithium secondary batteries for motor vehicles have improved significantly, and it is difficult to guarantee the safety factor and reliability of products that meet the requirements of vibration and shock tests with existing weld strength. Therefore, it is urgently necessary to improve weld strength and ensure reliability. Furthermore, the state of the art exhibits a large variation in tensile strength after welding and a high probability of welding defects, such as weak welds, which depend on the pressing conditions of the electrode strips. As in Fig. As shown in Figure 1, electrode strips of multiple specifications must be bent and cut in a single module for welding, resulting in an increase in process and administrative costs.
[0043] In contrast to the prior art, the present invention can standardize an electrode strip processing die for all unit cells forming a module without requiring the electrode strips of several adjacent cells (battery cells) to be bent or cut into more than one die to weld them together for electrical connection. The processed unit cells are stacked to form a laminate with a predetermined number of cells, and then a plate can be mounted in a direction in which the electrode strips are inserted for electrical connection. The plate can have holes (e.g.,The plates have slots arranged at predetermined regular intervals through which pre-processed electrode strips can be inserted at one end of the holes, facing the battery module, to a certain depth. In some embodiments, the strips pass through the holes and emerge at the side of the holes. The number of slots corresponds to the number of electrode strips. Furthermore, the shape and size of each slot correspond to the shape and size of the electrode strips, ensuring that, after insertion, the distance between each strip and the surrounding hole is minimized. In one embodiment, the plate may have a projecting surface or area surrounding each slot and projecting in a direction along which the corresponding electrode strip runs around an outer circumference of the slot.
[0044] After assembly in this manner, each electrode strip protrudes through the plate, and welding is then performed by irradiating the protruding welded portion of the electrode strip with a laser beam. Since various shapes and qualities of electrode strips can be formed depending on the thickness, material, protruding quantity, plate material, plating material, weld length, weld speed, laser power, and laser irradiation pattern of the electrode strip, the inventors were able to establish optimal quality control criteria by identifying the degree of influence of the various factors through the experimental design method.The inventors investigated the correlation between the mechanical / electrical properties and the cross-sectional shape of the weld bead through repeated research and analysis during the welding of heterogeneous materials where the electrode strip material and the plate material differ, particularly when welding heterogeneous Cu-Al materials. This led to the derivation of the weld bead shape described below. When welding heterogeneous materials, especially heterogeneous Cu-Al materials, if the weld bead conforms to the shape described below, the weld strength can be more than doubled without degrading the electrical properties of the welded part, and the electrical resistance of the module can be reduced.Although not necessarily limited to this analysis, the mechanical properties can be improved without significant deterioration of the electrical properties by the composition of the weld bead, which varies depending on the external shape of the weld bead and the shape of the weld bead when welding heterogeneous materials, for example by Cu-Al dilution in the case of heterogeneous Cu-Al material.
[0045] In general, dilution represents the degree of contribution of each weld base material (in the case of the present invention, the plate and the electrode strip) to the overall weld, with or without filler material addition. In a cross-sectional diagram of the weld metal, dilution can be measured as the area in which each component has melted and blended. It is known that this dilution varies depending on the applied welding heat, the thermal properties, and the shape and dimensions of the initial joint.
[0046] In the present invention, the weld bead can be produced by using the electrode strip as the first base material for welding and the plate as the second base material for welding, consisting of 70 to 99 wt.% of the first base material and the remainder (1 to 30 wt.%) of the second base material, and advantageously of 75 to 99 wt.% of the first base material and the remainder (1 to 25 wt.%) of the second base material. That is, the dilution of the first base material can be 85 to 99% and the dilution of the second base material can be 1 to 15%, and advantageously the dilution of the first base material can be 89 to 99% and the dilution of the second base material 1 to 11%. In this case, a surface cladding layer can be formed on the electrode strip, which serves as the first base material (welding base material), and / or on the plate, which serves as the second base material.This means that the electrode strip and / or the plate may contain the surface plating layer, and in particular, the electrode strip, where electrical / chemical stability with respect to an electrolyte is to be ensured, may contain the surface plating layer. As is known, the surface plating layer, to ensure electrical / chemical stability with respect to the electrolyte, may contain Ni, Sn, Si, Mg, Fe, Mn, Zn, Cr, Li, Ca, or an alloy thereof. If the surface plating layer is present on the electrode strip and / or the plate, the thinness of the surface plating layer itself can also be calculated by analyzing the elemental weight percentage (wt%) of the weld bead containing the first base material, the second base material, and the plating component described above.
[0047] The composition of the weld metal (weld bead) during welding can be quantified for various process factors using energy-dispersive spectroscopy (EDS). Table 1 below summarizes the composition (wt%) of the weld metal under different welding conditions, based on preliminary tests, and the calculated dilution during welding of heterogeneous materials consisting of Cu-plate-Al electrode strips. The method for calculating the dilution is well known in the art and is therefore not described separately. [Table 1] Thickness of the aluminum strip (mm) Cu range (wt%) Average copper content (wt%) Si + Ni (wt%) Si + Mg + Fe + etc. (wt.%) Al (wt%) Calculated range of Cu dilution (%) 0,4 18~42 27~37 / 2.5 ∠3 rest 6~18 1,1 3~15 5~11 / 2.5 ∠3 rest 1~5
[0048] As a result of testing the mechanical properties of the welded part at various dilutions, as shown in Table 1, it was confirmed that Cu, i.e. the weld metal with a composition where the dilution of the plate is more than 11%, exhibits significant formation of intermetallic compounds (IMC) and the appearance of cracks, and it was also confirmed that the composition and dilution of the weld metal can be controlled by the thickness of the aluminum electrode strip.
[0049] Meanwhile, it has been established that the weld bead size is a very important indicator for determining the overall composition and dilution. In particular, the weld bead size is directly related to the strength of the weld metal. When welding heterogeneous materials consisting of copper plate and aluminum electrode strips, this generally means that with increasing weld bead size, more aluminum is contained, and it has been found that copper dilution and IMC formation are reduced, thus decreasing the occurrence of cracks and resulting in stronger welded parts. Based on the research results, including these preliminary experiments, the present invention exhibits a weld strength of 7.0 kgf / mm². 2 or more, which is more than double the existing overlap weld strength of 3.5 kgf / mm 2is, and the present invention is presented by determining the specific conditions of the weld bead in which a stable weld quality is achieved by minimizing the occurrence of intermetallic compounds (IMC) such as Al x Cu x or Cu x Al x is achieved.
[0050] The present invention is described in detail below with reference to the accompanying drawings.
[0051] Fig. Figure 2 is a diagram illustrating a structure in which the battery strips 120 of each battery cell 110 are electrically connected by a busbar 150 in a laminate in which the battery cells 110 are stacked according to an embodiment of the present invention. Fig. Figure 3 is a diagram showing a busbar 150 in a battery module according to an embodiment of the present invention.
[0052] As in Fig. 2 and Fig.As shown in Figure 3, the battery module 100 according to the embodiment of the present invention contains a plurality of battery cells 110 and electrode strips 120 which are brought out of the battery cells 110.
[0053] As in Fig. As shown in Figure 3A, the battery module 100 of the present invention includes the busbar 150, and the busbar 150 includes a plate 150a with a plurality of holes 150c formed in the plate 150a. In this case, the plate 150a contains three holes 150c, each hole being shaped to accommodate a corresponding electrode strip 120 from the plurality of electrode strips 120. Each hole 150c has a slot shape dimensioned to correspond to a cross-section of the electrode strip 120, so that an end section of an electrode strip 120 can be inserted into the hole 150c.
[0054] In the Fig.In the example shown in Figure 3B, each hole 150c can contain an inserter 151 that is open on one side to allow the electrode strip 120 to be inserted into the hole 150c. The inserter 151 can, for example, have a tapered shape that widens towards the open side so that the electrode strip 120 can be easily inserted into the hole 150c; however, the shape of the inserter 151 is not limited to this. If both end sections of the hole 150c are blocked, as shown in Figure 3B, the inserter 151 can be inserted into the hole 150c in a tapered shape that widens towards the open side, allowing the electrode strip 120 to be easily inserted into the hole 150c. Fig. As shown in Figure 3A, the electrode strip 120 can be inserted into the hole 150c of the plate 150a in the projection direction of the electrode strip 120, and if an end section of the hole 150c is open, as ... direction of the projection of the electrode strip 120. Fig. As shown in Figure 3B, the electrode strip 120 can be inserted into the hole 150c of the plate 150a in a lateral direction (broad direction) of the electrode strip through the insertion part 151.
[0055] Although there are three 150cm holes in each of the 150mm power rails Fig. 3a and Fig. As shown in Figure 3b, it should be noted that the present invention is not limited by the number of holes 150c in each of the busbars 150. Therefore, in general, one or more holes 150c can be formed in each of the plates 150a, and each of the electrode strips 120 can be inserted into a corresponding hole 150c and welded to the busbar 150. In this way, the plurality of welded battery cells 110 can be electrically connected to one another via the busbar 150.
[0056] Fig.Figure 4 is a diagram showing a battery module with a plurality of battery cells 110 and a plurality of electrode strips 120 projecting from opposite sides of the battery module. Each electrode strip 120 on one side of the battery module is shown connected to the busbar 150 via a weld bead 170. According to the present invention, in the battery module, each electrode strip 120 is inserted into a corresponding hole 150c formed in the plate 150a of the busbar 150, and then the electrode strips 120 are connected to the busbar 150 by welding. In this way, the electrode strips 120 of the electrode cells 110 can be electrically connected without having to deform the shape of the electrode strips 120 separately, as in the prior art.
[0057] Within the scope of the present invention, one or more holes 150c can be formed in the plate 150a, corresponding to the number of battery cells 110 to be connected. Therefore, to electrically connect the battery cells 110, they can be connected regardless of the number of battery cells 110 to be connected, without changing the shape of the electrode strips 120.
[0058] That is, in the present invention, the plate 150a, which forms the busbar 150, contains a plurality of holes 150c arranged at a predetermined regular interval. The shape, size, and positioning of the holes 150c are such that the busbar can be easily positioned on the side of the battery module with the protruding electrode strips 120, so that each electrode strip 120 can be firmly inserted into a corresponding hole 150c. By welding the electrode strips 120 in their respective holes 150c, the plurality of battery cells 110 can be electrically connected to the busbar 150 and to each other. Since the electrode strips 120 are inserted into and welded into each hole 150c, the plurality of battery cells 110, which are welded together by the busbar 150, are thus electrically connected to each other.In the illustrated embodiment of the present invention, the holes 150c, which have an elongated rectangular shape, are referred to as slots or slot shapes. However, the invention is not limited to this shape, but includes shapes and sizes that closely enclose the electrode strips 120.
[0059] Fig. 5 is a diagram showing a busbar 150 according to another embodiment of the present invention. As in Fig. As shown in Figure 5, the plate 150a of the busbar 150 has a plurality of projecting areas 150b separated by valley areas 150v. The holes 150c are formed centrally in the projecting areas 150b. In other words, the projecting areas 150b are formed around the positions where the holes 150c are formed. The in Fig.Figure 5 shows a busbar 150 with three projecting regions 150b and two valley regions 150v. Each projecting region 150b forms a cavity 150k on the side facing the battery cells 110 of the battery module. Each hole 150c has a tapered section 150t at a first end, facing the cavity 150k and the battery cells 110 of the battery module. The tapered section 150t enlarges the opening of the hole 150c towards the battery cells 110. The cavity 150k of the projecting region 150b and the tapered section 150t serve to guide the electrode strip 120 so that it can be inserted into the hole 150c. Therefore, in the embodiment of Fig. 5 the plate 150a of the busbar 150 has a plurality of holes 150c formed at a predetermined regular distance from each other, and a corresponding number of protruding areas 150b formed around the holes 150c.
[0060] Fig. Figure 6 is a diagram showing the busbar 150 according to another embodiment of the present invention. As in Fig.As shown in Figure 6, according to another embodiment of the present invention, the plate 150a contains a plurality of strip connectors 151a, the number of which corresponds to the holes 150c. Each strip connector 151a is configured to project from the outer circumference of a corresponding hole 150c in the direction in which the electrode strip 120 projects from the side of the busbar 150 facing away from the battery cells 110. When the battery cells 110 are then electrically connected to each other by laser welding, the electrode strip 120, melted by the laser L, can contact the strip connector 151a to be electrically connected to the busbar 150. In this case, a cavity 151b is formed on the opposite surface of the strip connector 151a around the hole 150c to insert the electrode strip 120 into the hole 150c.The cavity 151b has a smoother spherical profile than the cavity 150k of the embodiment of . Fig. 5. Furthermore, the strip connecting part 151a is generally smaller than the projection area 150b of the embodiment of Fig. 5.
[0061] Fig. Figure 7 is a diagram illustrating a state in which a laser L is irradiated in a longitudinal direction “d”, that is, in the extension direction of the electrode strip 120. As in Fig.As shown in Figure 7, the laser L is irradiated obliquely in a longitudinal direction d with respect to a central axis of the protruding electrode strip 120, which is inserted into the hole 150c. Accordingly, if the electrode strip 120 is irradiated perpendicularly to a distal surface of the electrode strip 120, the laser L will not shine directly onto the battery cell 110 due to a welding error, thus minimizing the possibility of an accident. Furthermore, since the laser L is irradiated obliquely, the welding process on the distal surface of the electrode strip 120 can be inspected with the naked eye, thereby improving the quality and production speed of the manufacturing process for the battery module.
[0062] In the battery module of the present invention, weld beads of various shapes can be formed by laser welding after the electrode strip 120 has penetrated the hole 150c in the plate 150a. As described above, the inventors have found that the shape and size of the weld bead are closely related to the composition of the weld metal based on the dilution of the base material, and it has been confirmed that the mechanical properties, including the tensile strength of the weld, can be significantly improved without impairing the electrical properties if the weld bead has a specific shape and size, as described in this invention.
[0063] Based on this finding, in one aspect of the present invention, the electrode strip inserted into the hole and the plate are connected to each other by the weld bead, and the weld bead has a width W and a height H that satisfy the following equations 1 and 2. 0 <W<7T
[0064] In equation 1, W is the width of the weld bead, based on the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip. 0 <H<3T
[0065] In equation 2, H is the height of the weld bead, relative to the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip. Therefore, T can be measured in millimeters "mm".
[0066] Specifically, the cross-section of the weld bead in the thickness direction of the plate means a cross-section that is intersected by an imaginary plane parallel to the thickness direction of the plate (an imaginary plane that is in-plane with the thickness direction). However, it can also mean the cross-section of the weld cut, thus minimizing the area of the weld bead. As a practical example, as in the Fig. In the example shown in Figure 8, an imaginary plane p, which forms the cross-sectional area of the weld bead, can be an imaginary plane that runs parallel to a thickness direction t1 of the plate and parallel to a thickness direction t2 of the electrode strip, and the cross-section of the weld bead can mean a cross-section that is cut by the imaginary plane p described above.
[0067] Equations 1 and 2 described above are particularly important when the electrode strip and the plate are made of different materials (metallic materials). Specifically, if the weld bead width W is 7T or greater when welding heterogeneous materials, the formation of intermetallic compounds between these materials can be induced. As a more concrete example, if the electrode strip is made of aluminum and the plate (busbar) is made of copper, the melt volume of the copper plate (busbar) increases, and the formation of an intermetallic compound at the copper-aluminum interface is induced if the weld bead width is 7T or greater. This can lead to a deterioration in the quality of the welded part, such as microcracks and increased resistance.Furthermore, if the weld bead height H is 3T or greater, the penetration depth decreases, which can lead to a problem because the interfacial adhesion between the heterogeneous materials is weakened. That is, Equation 1 represents a geometric parameter that strongly influences the dilution between the base metals in the weld bead, and Equation 2 represents a geometric parameter that strongly influences the shape of the weld bead itself.
[0068] The weld bead contains, for example: a cover section 171 with a convex shape, which covers the hole on one of the two opposing surfaces in the thickness direction of the plate, based on the cross-section of the weld bead in the thickness direction of the plate; and a column section 172, which is loaded into the hole. When the molten metal produced from the weld base materials is cooled to form the weld bead during welding, not only the composition of the weld bead but also the shape of the weld bead itself, including the cover section 171 and the column section 172, affects the mechanical properties of the welded part. Equation 2 is a geometric parameter that affects the shape of the weld bead itself. If the height H of the weld bead is 3T or more, the length of the column section 172 of the weld bead is shortened, which can lead to a problem because the interfacial adhesion decreases.
[0069] To ensure consistent weld quality, the width W of the weld bead can advantageously be 2T to 6T, or even more advantageously 3T to 6T, and the height H can advantageously be 0.5T to 2T, or even more advantageously 1T to 2T. When the width and height of the weld bead are met, the weld bead exhibits improved tensile strength and low contact resistance, thus displaying excellent welding properties. Furthermore, when the width and height of the weld bead are met, it is possible to ensure stable and reproducible weld quality (improved weld strength, excellent electrical properties of the weld, etc.), even when certain welding conditions, such as a heat gradient generated during welding, or changes in specific welding conditions, such as the use of a laser irradiation method during welding, are observed.
[0070] The width and height of the weld bead described above directly affect the cross-sectional area of the weld bead. Accordingly, in another embodiment, the electrode strip inserted into the hole and the plate are connected to each other by the weld bead, and the weld bead can satisfy equation 3 below. 0 <A<21T2
[0071] In equation 3, A is the cross-sectional area of the weld bead, based on the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip. In this case, the cross-sectional area of the weld bead in the thickness direction of the plate is the same as described above based on equations 1 and 2.
[0072] The cross-sectional area A of a weld bead 170 can be less than 21T 2 If the cross-sectional area is 21T 2 (mm 2If the cross-sectional area of the weld bead is greater than or greater than this, various problems can occur, such as the increased formation of intermetallic compounds (IMC), reduced weld strength, and the appearance of cracks in the welded part. Preferably, the cross-sectional area of the weld bead, relative to the cross-sectional area of the weld bead, can be determined by the cross-sectional area of the weld bead. 2 up to 12T 2 and even more advantageously 3T 2 up to 12T 2 If the cross-sectional area of the weld bead is sufficient, the weld bead has improved tensile strength and low contact resistance, and can therefore exhibit excellent welding properties and can maintain consistent welding characteristics without being significantly affected by the specific welding conditions.
[0073] The weld bead can satisfy equation 1 and equation 2 and also equation 3, and independently it can satisfy equation 3 and also equation 1, equation 2 or equation 1 and equation 2.
[0074] Fig. Figure 9 is a schematic cross-sectional view illustrating that the weld bead 170 is formed by heating and melting an end section of the electrode strip 120 that has penetrated through the hole 150c of the plate 150a of the busbar 150.
[0075] As in Fig.As shown in Figure 9, the width W of the weld bead can be the width of the cover part 171, relative to the cross-section of the weld bead. In particular, the width W of the weld bead can represent the distance between the left and right boundary points p1 and p2, by defining the boundary points p1 and p2 at a point where an interface between the weld bead 170 and one of the two opposing surfaces in the thickness direction of the plate 150a meets a surface of one of the surfaces in the cross-section of the weld bead in the thickness direction of the plate. In this case, in which Fig. In example 9, the width of the weld bead is as shown in Fig.Figure 9 shows that if the left and right boundary points p1 and p2 are at the same height, and if the left and right boundary points p1 and p2 are not at the same height, the width of the weld bead can be defined as the shortest distance between the two boundary points.
[0076] As in Fig.As shown in Figure 9, the height H of the weld bead can be the maximum height of the cover part 171 based on the cross-section of the weld bead. Specifically, the height H of the weld bead can be a distance (shortest distance) between the imaginary line connecting the left and right boundary points p1 and p2 and a highest point of the cover part 171, by defining the boundary points p1 and p2 at the point where the interface between the weld bead 170 and one of the two opposing surfaces in the thickness direction of the plate 150a and the surface of one of the surfaces in the cross-section of the weld bead in the thickness direction of the plate meet. Since the weld bead in Figure 9 is a cross-section of the plate 150a, the height H of the weld bead can be determined by defining the boundary points p1 and p2 at the point where the interface between the weld bead 170 and one of the two opposing surfaces in the thickness direction of the plate 150a meets the surface of the weld bead in the cross-section in the thickness direction of the plate. Fig. In the example shown in Figure 9, where the left and right boundary points p1 and p2 are at the same height, the width of the weld bead in this case is only as shown in Figure 9. Fig.9 shown, and the height of the weld bead can be defined as the shortest distance between the imaginary line connecting the two boundary points and the highest point of the cover part 171.
[0077] In one embodiment, the weld bead can also satisfy equation 4. 0.4T≤D≤2T
[0078] In Equation 4, D is the penetration depth of the weld bead into the hole, based on the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip. The penetration depth can be, for example, the distance (shortest distance) between the imaginary line connecting the left and right boundary points p1 and p2 and the deepest point of the weld bead within the hole. The penetration depth can correspond to the length of the column section 172. The penetration depth can be a factor related to the mechanical properties and the plate thinning due to the shape of the weld bead itself. If the penetration depth is 0.4T to 2T, preferably 0.5T to 1.5T, and even more preferably 0.5T to 1.0T, the plate thinning is controlled to 5% or less, and the mechanical properties can be improved by the shape of the weld bead.
[0079] In one embodiment, the weld bead 170 can be left-right symmetrical or left-right asymmetrical in the cross-section of the weld bead in the thickness direction of the plate with respect to a centerline CL of the hole. In this case, the centerline of the hole can coincide with the centerline of the battery strip inserted into the hole. With reference to Fig. 9. Left-right symmetry can mean that the ratio of L1 : L2 is 1 : 1 to 1.2, by defining the shortest distance between the two left and right boundary points p1 and p2 and the center line of the hole as L1 and L2, and defining the greater distance as L2 if L1 and L2 are different. With reference to Fig.9. Left-right asymmetry can mean that the ratio of L1 : L2 is greater than 1 : 1.2; in particular, the ratio of L1 : L2 is 1 : 1.2 to 3, and especially 1 : 1.2 to 2.5. The left-right asymmetric structure can be mainly influenced by the direction of laser irradiation, and as above, based on Fig.As described in Figure 7, such asymmetrical structures can occur when the laser beam is directed at an oblique angle. It is known that the left-right asymmetrical structure of the weld bead is detrimental to the mechanical properties of the weld. However, according to one embodiment of the present invention, the mechanical properties (weld strength) of the weld are not significantly affected by the asymmetrical structure of the weld bead if the parameters of the bead width, bead thickness, or cross-sectional area of the bead are satisfied. That is, even with the left-right symmetrical structure or the left-right asymmetrical structure, the welding properties can be essentially constant and uniform and exhibit improved mechanical properties.
[0080] In an advantageous example, the electrode strip material plate material can be an aluminum-copper material or a copper-aluminum material. In this case, the aluminum material can be aluminum with a purity of 90% or greater, particularly aluminum with a purity of 95% or greater, 99% or greater, or 99.5% or greater. The aluminum material can be, for example, industrial-grade pure aluminum, and commercially available products may include the Al1000 series (UNS #) such as A11050, A11100, or Al1200. The copper material can be copper with a purity of 98% or greater, 99% or greater, or 99.3% or greater. The copper material may be, for example, industrial pure copper, and commercially available products may contain the C10100 to C13000 series (UNS #), such as C11000, C10100, C10200 and C12500.
[0081] In the present invention, the electrode strip 120 is arranged to penetrate the hole 150c in a direction perpendicular to the surface of the plate 150a, and its thickness is preferably 0.2 mm or more. Preferably, the thickness of the electrode strip can be 0.2 to 1.0 mm. Having a thickness of 0.2 mm or more is advantageous because the weld bead with the specific shape described above can be produced by laser welding, and the weld bead can be produced with a plate thinning of 11% or less.
[0082] Furthermore, the plate 150a in the present invention preferably has a thickness of 0.5 mm or more, and can, for example, have a thickness of 0.5 mm to 10 mm, 1 mm to 8 mm or 1 mm to 6 mm, but is not necessarily limited thereto.
[0083] In one embodiment, the battery cell can be a pouch-type battery cell. A pouch-type battery cell can be a battery cell in which an electrode array comprising a cathode, an anode, and a separator located between the cathode and the anode is sealed in a pouch in a state of impregnation in an electrolyte (electrolytic solution). The pouch can have a multilayer film structure, in which a metal film, such as an aluminum film, is inserted between an outer and an inner film, but this is not limited to the pouch structure. In the battery module according to one embodiment, the electrode strips of each of the plurality of pouch-type battery cells stacked in one direction are inserted into each hole of the plate and welded together, so that the plurality of pouch-type battery cells can be electrically interconnected.
[0084] Fig.Figure 10 is a photograph showing the shape of the weld bead formed by welding the Al electrode strip to the Cu plate with the heterogeneous materials according to the process of Fig. 7 is formed. As in Fig. As shown in Figure 10, the surface of the plate in contact with the weld bead is inclined downwards in the longitudinal direction towards the outer periphery of the weld bead. In this way, the surface of the plate connected to the formed weld bead is positioned so that the hole slopes downwards from the center towards the outer periphery of the weld bead, thus ensuring a uniform weld bead shape and preventing a reduction in weld strength due to rough features such as a notch.
[0085] Although the present invention has been described by specific details such as detailed components, embodiments, and the accompanying drawings, these have been provided only to aid a complete understanding of the present invention. Therefore, the present invention is not limited to the embodiments described. Various modifications and alterations can be made by those skilled in the field to which the present invention relates, based on this description.
[0086] Therefore, the content of the present invention should not be limited to these embodiments, but the claims and all amendments that are equal or equivalent to the claims should fall within the scope and content of the present invention.
Claims
[1] Battery module, comprising: a plurality of battery cells, each containing at least one electrode strip; and at least one bus bar connected to the electrode strips of the battery cells to electrically connect the plurality of battery cells to one another, wherein the busbar includes a plate in which a plurality of holes are formed, the electrode strips of the battery cells are inserted into at least a portion of the plurality of holes in the plate, the electrode strip inserted into the hole and the plate are connected to each other by a weld bead, the electrode strip contains a first base material for welding and the plate contains a second base material for welding, and the dilution of the first base material is 85 to 99% and the dilution of the second base material is 1 to 15% in the weld bead. [2] The battery module according to claim 1, wherein the dilution of the first base material is 89 to 99% and the dilution of the second base material is 1 to 11%. [3] The battery module of claim 1, wherein the electrode strip contains aluminum and the plate contains copper. [4] The battery module according to claim 1, wherein the electrode strip includes a surface plating layer. [5] Battery module according to one of claims 1 to 4, wherein the weld bead satisfies the following equations 1 and 2, 0 <W<7T where in Equation 1, W is a width of the weld bead based on a cross section of the weld bead in a thickness direction of the plate and T is a thickness of the electrode strip, 0 <H<3T where in Equation 2, H is the height of the weld bead based on the cross section of the weld bead in the thickness direction of the plate and T is the thickness of the electrode strip. [6] The battery module according to claim 5, wherein W is 2T to 6T and H is 0.5T to 2T. [7] The battery module according to claim 5, wherein A, which is a cross-sectional area of the weld bead based on a cross section of the weld bead in a thickness direction of the plate, T 2 up to 12T 2 amounts. [8] The battery module of claim 5, wherein the weld bead further satisfies the following equation 4, 0.4T≤D≤2T where in Equation 4, D is the penetration depth of the weld bead into a hole based on the cross-section of the weld bead in the thickness direction of the plate, and T is the thickness of the electrode strip. [9] The battery module according to claim 4, wherein the surface plating layer contains at least one element selected from the group consisting of Ni, Sn, Si, Mg, Fe, Mn, Zn, Cr, Li, Ca and an alloy thereof. [10] The battery module according to claim 1, wherein the thickness of the electrode strip is 0.2 mm or more. [11] The battery module according to claim 1, wherein the thickness of the electrode strip is 0.2 mm to 1.0 mm. [12] The battery module according to claim 10, wherein the thickness of the plate is 0.5 mm or more. [13] The battery module according to claim 5, wherein the weld bead includes: a cover member having a convex shape covering the hole on one of two opposite surfaces in the thickness direction of the plate, and a column member loaded into the hole based on the cross section of the weld bead in the thickness direction of the plate. [14] The battery module according to claim 5, wherein in the cross section of the weld bead in the thickness direction of the plate, the weld bead is left-right asymmetrical with respect to a center line of the hole. [15] The battery module according to claim 14, wherein in the cross section of the weld bead in the thickness direction of the plate, by setting a point at which an interface between the weld bead and one of two opposite surfaces in the thickness direction of the plate and a surface of the one surface meet as a boundary point, the weld bead has a left-right asymmetry with a ratio of L1:L2 which is 1:1.2 to 3, where L1 is the shortest distance between the left boundary point and the center line of the hole and L2 is the shortest distance between the right boundary point and the center line.