AI Technical Summary
Existing additive manufacturing processes face challenges in producing complex-shaped foam objects with internal geometries due to the mechanical limitations of 3D printed cases, which often fail under the pressure of rising foam and released propellants, and struggle with reusability and cost-effectiveness of construction materials.
A method involving the production of a shell using additive manufacturing, followed by the introduction of a polyisocyanate and polyol reaction mixture that reacts to form a polymer within the shell, allowing for a longer setting time to prevent shell damage and enabling the creation of complex foam structures with mechanical reinforcement.
This method allows for the production of complex-shaped foam objects with internal geometries that were previously inaccessible, while reducing production time and enhancing the mechanical properties of the objects, and promoting cost-effective and resource-saving production with reusable materials.
Description
[0001] The present invention relates to a method for producing an article, comprising the steps of: producing a shell which comprises a volume for receiving a fluid, by means of an additive manufacturing process from a building material; providing a reaction mixture comprising a polyisocyanate component and a polyol component in the volume and allowing the reaction mixture to react in the volume to obtain a polymer present at least partially in the volume. The invention further relates to an article obtainable by a method according to the invention, comprising a shell which defines a volume located within the shell and a foam which completely or partially fills the volume. The shell can be subsequently completely or partially removed in order to obtain complexly shaped foam bodies.
[0002] Additive manufacturing processes are those that build objects layer by layer. They therefore differ significantly from other manufacturing processes such as milling, drilling, or machining. In the latter processes, an object is processed in such a way that it achieves its final geometry by removing material.
[0003] Additive manufacturing processes use different materials and process techniques to build objects layer by layer. In Fused Deposition Modeling (FDM), for example, a thermoplastic wire is liquefied and deposited layer by layer onto a movable build platform using a nozzle. Upon solidification, a solid object is created. The nozzle and build platform are controlled based on a CAD drawing of the object. If the geometry of this object is complex, for example, with geometric undercuts, additional support materials must be printed and removed after the object is completed.
[0004] There are also additive manufacturing processes that use thermoplastic powder to build objects layer by layer. In this process, thin layers of powder are applied using a so-called coater and then selectively melted using an energy source. The surrounding powder supports the component geometry. Complex geometries can therefore be manufactured more economically than with the previously described FDM process. In addition, various objects can be arranged or manufactured tightly packed in the so-called powder bed. Due to these advantages, powder-based additive manufacturing processes are considered to be among the most economical additive manufacturing processes on the market. They are therefore predominantly used by industrial users. Examples of powder-based additive manufacturing processes are so-called laser sintering (SLS, Selective Laser Sintering) and high-speed sintering (HSS).They differ in the method used to introduce the energy for selective melting into the plastic. In the laser sintering process, the energy is introduced via a guided laser beam. In the so-called High Speed Sintering (HSS) process (EP 1648686), the energy is introduced via infrared (IR) emitters in combination with an IR absorber selectively printed into the powder bed. Selective Heat Sintering (SHS) uses the printing unit of a conventional thermal printer to selectively melt thermoplastic powders.
[0005] Another group of additive manufacturing processes uses radically crosslinkable resins, which, if necessary, achieve their final strength in the resulting object via a second curing mechanism. Examples of such processes are stereolithography processes and the derived DLP process.
[0006] In the technical field of coatings, so-called "dual cure" systems are known in which the liquid coating material is first crosslinked radically, for example photochemically, and then further cured via reactions of NCO groups with suitable reaction partners.
[0007] The presence of foam or other fillings between 3D-printed walls is known, for example, from patent applications WO 2015 / 065936 A2, WO 2015 / 139095 A1, WO 2016 / 086268 A1, WO 2016 / 124432 A1, or US 2016 / 059485 A1. WO 2015 / 139095 A1 discloses a method for producing a composite object using a computer-controlled device and discloses such a device. The device comprises a reservoir containing a liquid, curable first material, means for selectively solidifying the first material, and means for selectively depositing a second material. The method comprises the steps of selectively depositing portions of the second material and selectively solidifying portions of the first material such that the solidified portions of the first material and the deposited portions of the second material form the composite object.
[0008] WO 2016 / 086268 A1 describes a method for manufacturing a buoyancy module for a subsea buoyancy system, comprising the steps of: forming a shell, at least partially, by an additive manufacturing process; introducing a buoyancy material into the shell; and sealing the shell.
[0009] WO 2016 / 142930 A1 discloses, among other things, a method for producing a three-dimensional object using a "3D object manufacturing machine" with a main and a satellite material distribution head. The satellite material distribution head can be used to distribute a two-component material such as "EasyFlo Spray Foam FR8 Liquid Plastic" or similar polyurethane foams into the interior of the three-dimensional object, creating a reinforced, durable inner shell without compromising the external appearance of the model.
[0010] The introduction of foam-forming reaction mixtures into cavities, as is common in the production of PUR or PUR / PIR foam bodies, cannot be easily transferred to 3D-printed shells. Reaction mixtures for so-called "foam in place" or "reaction injection molding" processes are designed for high reaction rates and correspondingly short demolding times. However, the resulting pressures from the rising foam and the released blowing agent can easily exceed the mechanical strength of 3D-printed shells.
[0011] One object of the present invention is to at least partially overcome at least one disadvantage of the prior art. Furthermore, the invention aims to provide an additive manufacturing process in which the objects to be produced can be obtained as cost-efficiently and / or individually and / or resource-efficiently as possible, particularly with regard to the recyclability of construction materials.
[0012] According to the invention, the object is achieved by a method according to claim 1 and an object according to claim 13. Advantageous further developments are specified in the subclaims. They can be combined in any desired manner unless the context clearly indicates otherwise.
[0013] A method for manufacturing an article comprises the steps: Producing a shell comprising a volume for receiving a fluid from a construction material by means of an additive manufacturing process; providing a reaction mixture comprising a polyisocyanate component and a polyol component in the volume; allowing the reaction mixture to react in the volume to obtain a polymer present at least partially in the volume.
[0014] In the process, the reaction mixture has a setting time of ≥ 2 minutes.
[0015] The process according to the invention makes it possible to produce objects whose external shape is limited only by the performance of the selected additive manufacturing process and the equipment used. Mechanical reinforcement of the objects is achieved by the polymer obtained by reaction. This also reduces production times for the objects, since only the outer shell needs to be manufactured.
[0016] Furthermore, the process according to the invention makes it possible to produce a complex-shaped foam article with internal foam geometries that are not accessible by conventional methods. In this process, the molding material manufactured by an additive process can be at least partially removed again, preferably, for example, by melting, thermolysis, or hydrolysis.
[0017] Preferably, the setting time is ≥ 3 minutes, more preferably ≥ 5 minutes. It is further preferred that the setting time is ≥ 3 minutes to ≤ 90 minutes or ≥ 5 minutes to ≤ 60 minutes.
[0018] The setting time is the time required for the polyaddition reaction between NCO-reactive components and polyisocyanate components to produce a theoretically infinitely expanded polymer. The setting time can be determined experimentally by dipping a thin wooden stick into the foaming reaction mixture at short intervals. The time from mixing the components until the stick begins to slough off its surface when pulled out is the setting time.
[0019] Reaction mixtures with the setting times according to the invention, which are considered slow in the art, ensure that the undesirable side effects of the exothermic reaction of the reaction mixture to form a PUR or PUR / PIR material do not damage the shell or, in the case of complex geometries, lead to an undesirable, highly inconsistent formation of the foam structure. One undesirable effect is, for example, the melting or softening of a thermoplastic shell with loss of the intended shape. A slower reaction allows the released reaction heat to be dissipated more effectively. In the case of closed shells, the pressure buildup inside the shell due to the reaction is also undesirable, particularly in combination with melting or softening of thermoplastic shell material. The slower the reaction progresses, the more gas can diffuse through the shell to the outside.For the method according to the invention, it may be desirable that the additively manufactured shell is not completely gas-tight and / or liquid-tight.
[0020] The setting time intended according to the invention can be achieved by various measures, individually or in combination. For example, the reaction mixture can contain an amine catalyst. Another measure is the use of slower-reacting aliphatic polyisocyanates. Finally, the polyol component can contain difunctional polyols, which reduce the crosslinking density in the final product and also in the reacting reaction mixture and thus potentially also extend the setting time.
[0021] To simplify preparation, the reaction mixture can be adjusted to a low viscosity. For example, the reaction mixture can have an initial viscosity (20 °C, ASTM D 2393), i.e., immediately after mixing the polyol component and isocyanate component, of ≥ 100 mPas to ≤ 5000 mPas.
[0022] The volume can be, for example, ≥ 1 cm 3< to ≤ 5000 cm 3<.
[0023] After the reaction mixture has been provided in the volume, the shell together with the reaction mixture contained therein can be rotated or pivoted in the space so that the reaction mixture can be evenly distributed in the available shell.
[0024] Cases are conceivable in which the reaction mixture does not contain a blowing agent and thus does not cure into a foam. In this case, the resulting polymer would act as a solid layer on the inside of the shell, providing mechanical reinforcement. However, the advantages of the process according to the invention are particularly evident when the reaction mixture also contains a blowing agent. This can be a physical and / or chemical blowing agent.
[0025] The construction material preferably comprises a polyurethane polymer. Components in the reaction mixture can then react with any remaining reactive groups of the polyurethane polymer present in the shell, forming a cohesive bond. Thermoplastic polyurethanes (TPU), especially thermoplastic polyurethane elastomers (TPE), are particularly preferred.
[0026] Suitable for producing the polyurethane polymer in the building material are organic aliphatic, cycloaliphatic, araliphatic, and / or aromatic polyisocyanates with at least two isocyanate groups per molecule, as well as mixtures thereof, known to those skilled in the art. For example, NCO-terminated prepolymers can be used.
[0027] All compounds known to the person skilled in the art that have an average OH or NH functionality of at least 1.5 can be used as NCO-reactive compounds with Zerewitinoff-active hydrogen atoms for producing the polyurethane polymer in the building material. These can be, for example, low-molecular-weight diols (e.g., 1,2-ethanediol, 1,3- or 1,2-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol), triols (e.g., glycerol, trimethylolpropane), and tetraols (e.g., pentaerythritol), short-chain amino alcohols, polyamines, but also higher-molecular-weight polyhydroxy compounds such as polyether polyols, polyester polyols, polycarbonate polyols, polyether carbonate diols, polysiloxane polyols, polyamines, polyether polyamines, and polybutadiene polyols.
[0028] The NCO groups in the polyurethane polymer of the building material may be partially blocked. In this case, the process according to the invention further comprises the step of deblocking these NCO groups. After deblocking, they are available for reactions with the reaction mixture, forming a cohesive bond.
[0029] The blocking agent is chosen so that the NCO groups are at least partially unblocked upon heating. Examples of blocking agents are alcohols, lactams, oximes, malonic esters, alkyl acetoacetates, triazoles, phenols, imidazoles, pyrazoles and amines, such as butanone oxime, diisopropylamine, 1,2,4-triazole, dimethyl-1,2,4-triazole, imidazole, malonic acid diethyl ester, acetoacetic ester, acetone oxime, 3,5-dimethylpyrazole, ε-caprolactam, N-methyl-, N-ethyl-, N-(iso)propyl-, Nn-butyl-, N-iso-butyl-, N-tert-butyl-benzylamine or 1,1-dimethylbenzylamine, N-alkyl-N-1,1-dimethylmethylphenylamine, adducts of benzylamine with compounds with activated double bonds such as malonic acid esters, N,N-dimethylaminopropylbenzylamine and other tertiary amino groups containing optionally substituted benzylamines and / or dibenzylamine or any mixtures of these blocking agents.
[0030] In a preferred embodiment, the building material is radically crosslinkable and comprises groups with Zerewitinoff-active H atoms, the shell is obtained from a precursor and the process comprises the steps: I) Depositing radically crosslinked building material onto a carrier to obtain a layer of building material bonded to the carrier, which corresponds to a first selected cross-section of the precursor; II) Depositing radically crosslinked building material onto a previously applied layer of building material to obtain a further layer of building material, which corresponds to a further selected cross-section of the precursor and is bonded to the previously applied layer; III) Repeating step II) until the precursor is formed; wherein the deposition of radically crosslinked building material takes place at least in step II) by exposing and / or irradiating a selected region of a radically crosslinkable building material, corresponding to the respectively selected cross-section of the precursor, and wherein the radically crosslinkable building material has a viscosity (23 °C, DIN EN ISO 2884-1) of ≥ 5 mPas to ≤ 100,000 mPas, wherein the radically crosslinkable building material comprises a curable component in which NCO groups and olefinic C=C double bonds are present and step IV) is further carried out after step III): IV) heating the precursor obtained after step III) to a temperature of ≥ 50 °C, so that the shell is obtained.
[0031] In this variant, the shell is thus obtained in two production steps. The first production step can be considered the build-up step. This build-up step can be realized using optical-ray additive manufacturing processes such as inkjet printing, stereolithography, or DLP (digital light processing) and is the subject of steps I), II), and III). The second production step can be considered the curing step and is the subject of step IV). Here, the precursor or intermediate shell obtained after the build-up step is converted into a mechanically more durable shell without further changing its shape.
[0032] In step I) of this variant of the process, a radically cross-linked build material is deposited on a substrate. This is usually the first step in inkjet, stereolithography, and DLP processes. This results in a layer of build material bonded to the substrate, corresponding to a first selected cross-section of the precursor.
[0033] According to the instructions of step III), step II) is repeated until the desired precursor is formed. In step II), a radically cross-linked build material is deposited onto a previously applied layer of build material, resulting in a further layer of build material that corresponds to another selected cross-section of the precursor and is bonded to the previously applied layer. The previously applied layer of build material can be the first layer from step I) or a layer from a previous run of step II).
[0034] In this process variant, the deposition of a radically crosslinked build-up material is carried out at least in step II) (preferably also in step I) by exposing and / or irradiating a selected area of a radically crosslinkable resin, corresponding to the respective selected cross-section of the precursor. This can be achieved either by selective exposure (stereolithography, DLP) of the crosslinkable build-up material or by selective application of the crosslinkable build-up material, followed by an exposure step that no longer needs to be selective due to the previous selective application of the crosslinkable build-up material (inkjet process).
[0035] In the context of this process variant, the terms "radically crosslinkable build material" and "radically crosslinked build material" are used. The radically crosslinkable build material is converted into the radically crosslinked build material by exposure and / or irradiation, which triggers radical crosslinking reactions. "Exposure" refers to the exposure to light in the range between near IR and near UV light (1400 nm to 315 nm wavelength). The other shorter wavelength ranges are covered by the term "irradiation," for example, far UV light, X-rays, gamma radiation, and electron beams.
[0036] The selection of the respective cross-section is conveniently carried out using a CAD program that has been used to create a model of the shell to be manufactured. This operation is also called "slicing" and serves as the basis for controlling the exposure and / or irradiation of the radically crosslinkable resin.
[0037] In this process variant, the radically crosslinkable build material has a viscosity (23 °C, DIN EN ISO 2884-1) of ≥ 5 mPas to ≤ 100,000 mPas. Thus, at least for the purposes of additive manufacturing, it is considered a liquid resin. Preferably, the viscosity is ≥ 50 mPas to ≤ 10,000 mPas, more preferably > 500 mPas to ≤ 5,000 mPas.
[0038] Furthermore, in the process, the radically crosslinkable resin comprises a curable component containing NCO groups and olefinic C=C double bonds. In this curable component, the molar ratio of NCO groups to olefinic C=C double bonds can range from ≥ 1:5 to ≤ 5:1 (preferably ≥ 1:4 to ≤ 4:1, more preferably ≥ 1:3 to ≤ 3:1). The molecular ratio of these functional groups can be determined by integrating the signals of a sample in the 13< C NMR spectrum.
[0039] In addition to the curable component, the radically crosslinkable building material can also comprise a non-curable component, which may include, for example, stabilizers, fillers, and the like. In the curable component, the NCO groups and the olefinic C=C double bonds can be present in separate molecules and / or in a single molecule. If NCO groups and olefinic C=C double bonds are present in separate molecules, the body obtained after step IV) of this process variant has an interpenetrating polymer network.
[0040] In this variant of the process, step IV) is carried out after step III). In this step, the precursor obtained in step III) is heated to a temperature of ≥ 50 °C, preferably ≥ 65 °C, more preferably ≥ 80 °C, particularly preferably ≥ 80 °C to ≤ 200 °C, so that the shell is obtained. The heating can take place for a period of ≥ 1 minute, preferably ≥ 5 minutes, more preferably ≥ 10 minutes to ≤ 24 hours, preferably ≤ 8 hours, particularly preferably < 4 hours.
[0041] Preferably, the reaction is carried out until ≤ 20%, preferably ≤ 10%, and more preferably ≤ 5% of the originally present NCO groups are still present. This can be determined by quantitative IR spectroscopy.
[0042] It is preferred that step IV) is only performed once the entire precursor build-up material has reached its gel point. The gel point is considered to have been reached when, in a dynamic mechanical analysis (DMA) using a plate-on-plate oscillation viscometer according to ISO 6721-10 at 20 °C, the graphs of the storage modulus G' and the loss modulus G" intersect. Optionally, the precursor is subjected to further light exposure and / or irradiation to complete the radical crosslinking. The radically crosslinked build-up material can have a storage modulus G' (DMA, plate-on-plate oscillation viscometer according to ISO 6721-10 at 20 °C and a shear rate of 1 / s) of ≥ 10 6 < Pa.
[0043] The radically crosslinkable building material may further contain additives such as fillers, UV stabilizers, radical inhibitors, antioxidants, mold release agents, water scavengers, slip additives, defoamers, flow control agents, rheology additives, flame retardants, and / or pigments. These auxiliaries and additives, with the exception of fillers and flame retardants, are typically present in an amount of less than 10 wt.%, preferably less than 5 wt.%, particularly preferably up to 3 wt.%, based on the radically crosslinkable resin. Flame retardants are typically present in amounts of at most 70 wt.%, preferably at most 50 wt.%, particularly preferably at most 30 wt.%, calculated as the total amount of flame retardants used based on the total weight of the radically crosslinkable building material.
[0044] Suitable fillers include, for example, AlOH 3 , CaCO 3 , metallic pigments such as TiO 2 , and other known conventional fillers. These fillers are preferably used in amounts of at most 70 wt.%, preferably at most 50 wt.%, particularly preferably at most 30 wt.%, calculated as the total amount of fillers used based on the total weight of the radically crosslinkable resin.
[0045] Suitable UV stabilizers can preferably be selected from the group consisting of piperidine derivatives, such as 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-1,2,2,6,6-pentamethylpiperidine, bis-(2,2,6,6-tetra-methyl-4-piperidyl)-sebacate, bis(1,2,2,6,6-pentamethyl-1-4-piperidinyl)-sebacate, bis-(2,2,6,6-tetramethyl-4-piperidyl)-suberate, bis-(2,2,6,6-tetramethyl-4-piperidyl)-dodecanedioate; benzophenone derivatives such as 2,4-dihydroxy, 2-hydroxy-4-methoxy, 2-hydroxy-4-octoxy, 2-hydroxy-4-dodecyloxy or 2,2'-dihydroxy-4-dodecyloxy-benzophenone; Benztriazole derivatives, such as2-(2H-Benzotriazol-2-yl)-4,6-di-tert-pentylphenol, 2-(2H-Benzotriazol-2-yl)-6-dodecyl-4-methylphenol, 2-(2H-Benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(5-Chlor-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)-4-methylphenol, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2-(2H-Benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, Isooctyl-3-(3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenylpropionat), 2-(2H-Benzotriazol-2-yl)-4,6-bis(1,1-dimethylethyl)phenol, 2-(2H-Benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(5-Chlor-2H-benzotriazol-2-yl)-4,6-bis(1,1-dimethylethyl)phenol; Oxalaniliden, wie z.B. 2-Ethyl-2'-ethoxy- oder 4-Methyl-4'-methoxyoxalanilid; Salicylsäureestern, wie z.B. Salicylsäurephenylester, Salicylsäure-4-tert-butylphenylester, Salicylsäure-4-tert-octylphenylester; Zimtsäureesterderivaten, wie z.B.Methyl α-cyano-β-methyl-4-methoxycinnamate, butyl α-cyano-β-methyl-4-methoxycinnamate, ethyl α-cyano-β-phenylcinnamate, isooctyl α-cyano-β-phenylcinnamate; and malonic ester derivatives, such as dimethyl 4-methoxybenzylidenemalonate, diethyl 4-methoxybenzylidenemalonate, and dimethyl 4-butoxybenzylidenemalonate. These preferred light stabilizers can be used individually or in any combination.
[0046] Particularly preferred UV stabilizers are those that completely absorb radiation with a wavelength < 400 nm. These include, for example, the benzotriazole derivatives mentioned. Very particularly preferred UV stabilizers are 2-(5-chloro-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)-4-methylphenol, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, and / or 2-(5-chloro-2H-benzotriazol-2-yl)-4,6-bis(1,1-dimethylethyl)phenol.
[0047] If appropriate, one or more of the UV stabilizers mentioned by way of example are added to the radically crosslinkable building material, preferably in amounts of 0.001 to 3.0% by weight, particularly preferably 0.005 to 2% by weight, calculated as the total amount of UV stabilizers used based on the total weight of the radically crosslinkable building material.
[0048] Suitable antioxidants are preferably sterically hindered phenols, which can preferably be selected from the group consisting of 2,6-di-tert-butyl-4-methylphenol (ionol), pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, triethylene glycol bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, 2,2'-thio-bis(4-methyl-6-tert-butylphenol) and 2,2'-thiodiethyl bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]. These can be used individually or in any combination with one another if required. These antioxidants are preferably used in amounts of 0.01 to 3.0 wt.%, particularly preferably 0.02 to 2.0 wt.%, calculated as the total amount of antioxidants used based on the total weight of the radically crosslinkable building material.
[0049] Suitable radical inhibitors or retarders are particularly those that specifically inhibit uncontrolled radical polymerization of the resin formulation outside the desired (irradiated) area. These are crucial for good edge sharpness and imaging accuracy in the precursor. Suitable radical inhibitors must be selected according to the desired radical yield from the irradiation / exposure step and the polymerization rate and reactivity / selectivity of the double bond carriers. Suitable radical inhibitors include, for example, 2,2-(2,5-thiophenediyl)bis(5-tert-butylbenzoxazole), phenothiazine, hydroquinones, hydroquinone ethers, quinone alkyds and nitroxyl compounds, as well as mixtures thereof, benzoquinones, copper salts, pyrocatechols, cresols, nitrobenzene, and oxygen. These antioxidants are preferably used in amounts of 0.001 wt% to 3 wt%.
[0050] In a further preferred embodiment, the olefinic double bonds in the radically crosslinkable building material are at least partially in the form of (meth)acrylate groups.
[0051] In a further preferred embodiment, the radically crosslinkable building material comprises a compound which is obtainable from the reaction of an NCO-terminated polyisocyanate prepolymer with a molar deficit of a hydroxyalkyl (meth)acrylate, based on the free NCO groups.
[0052] In a further preferred embodiment, the radically crosslinkable building material comprises a compound which is obtainable from the reaction of an NCO-terminated polyisocyanurate with a molar deficit of a hydroxyalkyl (meth)acrylate, based on the free NCO groups.
[0053] Suitable polyisocyanates for the preparation of the NCO-terminated polyisocyanurates and prepolymers are, for example, those which have a molecular weight in the range of 140 to 400 g / mol, with aliphatically, cycloaliphatically, araliphatically and / or aromatically bound isocyanate groups, such as. B. 1,4-Diisocyanatobutane (BDI), 1,5-Diisocyanatopentane (PDI), 1,6-Diisocyanatohexane (HDI), 2-Methyl-1,5-diisocyanatopentane, 1,5-Diisocyanato-2,2-dimethylpentane, 2,2,4- or 2,4,4-trimethyl-1,6-diisocyanatohexane, 1,10-diisocyanatodecane, 1,3- and 1,4-diisocyanatocyclohexane, 1,4-diisocyanato-3,3,5-trimethylcyclohexane, 1,3-diisocyanato-2-methylcyclohexane, 1,3-Diisocyanato-4-methylcyclohexane, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate;IPDI), 1-isocyanato-1-methyl-4(3)-isocyanatomethylcyclohexane, 2,4'- and 4,4'-diisocyanatodicyclohexylmethane (H 12 MDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane, bis-(isocyanatomethyl)-norbornane (NBDI), 4,4'-Diisocyanato-3,3'-dimethyldicyclohexylmethane, 4,4'-Diisocyanato-3,3',5,5'-tetramethyldicyclohexylmethane, 4,4'-Diisocyanato-1,1'-bi(cyclohexyl), 4,4'-Diisocyanato-3,3'-dimethyl-1,1'-bi(cyclohexyl), 4,4'-Diisocyanato-2,2',5,5'-tetra-methyl-1,1'-bi(cyclohexyl), 1,8-Diisocyanato-p-menthane, 1,3-Diisocyanato-adamantane, 1,3-Dimethyl-5,7-diisocyanatoadamantane, 1,3- and 1,4-bis-(isocyanatomethyl)benzene (xylylene diisocyanate; XDI), 1,3- and 1,4-bis(1-isocyanato-1-methylethyl)benzene (TMXDI) and bis(4-(1-isocyanato-1-methylethyl)phenyl) carbonate, 2,4- and 2,6-diisocyanatotoluene (TDI), 2,4'- and 4,4'-diisocyanatodiphenylmethane (MDI), 1,5-diisocyanatonaphthalene and any mixtures of such diisocyanates.;
[0054] Furthermore, according to the invention, aliphatic and / or aromatic isocyanate-terminated prepolymers, such as aliphatic or aromatic isocyanate-terminated polyether, polyester, polyacrylate, polyepoxide, or polycarbonate prepolymers, can also be used as starting materials for isocyanurate formation. Suitable trimerization catalysts are described below in connection with another embodiment.
[0055] Suitable hydroxyalkyl (meth)acrylates include alkoxyalkyl (meth)acrylates with 2 to 12 carbon atoms in the hydroxyalkyl radical. Preferred are 2-hydroxyethyl acrylate, the isomer mixture formed by the addition of propylene oxide to acrylic acid, or 4-hydroxybutyl acrylate.
[0056] The reaction between the hydroxyalkyl (meth)acrylate and the NCO-terminated polyisocyanurate can be catalyzed by conventional urethanization catalysts such as DBTL. In this reaction, the molar ratio between NCO groups and OH groups of the hydroxyalkyl (meth)acrylate can range from ≥10:1 to ≤1.1:1 (preferably ≥5:1 to ≤1.5:1, more preferably ≥4:1 to ≤2:1). The resulting curable compound can have a number-average molecular weight M n of ≥200 g / mol to ≤5000 g / mol. Preferably, this molecular weight is ≥ 300 g / mol to ≤ 4000 g / mol, more preferably ≥ 400 g / mol to ≤ 3000 g / mol.
[0057] Particularly preferred is a curable compound obtained from the reaction of an NCO-terminated polyisocyanurate with hydroxyethyl (meth)acrylate, the NCO-terminated polyisocyanurate being obtained from 1,6-hexamethylene diisocyanate in the presence of an isocyanate trimerization catalyst. This curable compound has a number-average molecular weight M n of ≥ 400 g / mol to ≤ 3000 g / mol and a molar ratio of NCO groups to olefinic C=C double bonds in a range from ≥ 1:5 to ≤ 5:1, particularly preferably ≥ 1:3 to ≤ 3:1, most preferably ≥ 1:2 to ≤ 2:1.
[0058] In a further preferred embodiment, the radically crosslinkable resin further comprises a radical initiator and / or an isocyanate trimerization catalyst. To prevent an undesirable increase in the viscosity of the radically crosslinkable resin, the radical initiator and / or isocyanate trimerization catalyst can be added to the resin only immediately before the start of the process according to the invention.
[0059] Thermal and / or photochemical radical initiators (photoinitiators) can be considered as radical initiators. It is also possible to use both thermal and photochemical radical initiators simultaneously. Suitable thermal radical initiators include azobisisobutyronitrile (AIBN), dibenzoyl peroxide (DBPO), di-tert-butyl peroxide, and / or inorganic peroxides such as peroxodisulfates.
[0060] Photoinitiators are generally divided into two types: unimolecular type (I) and bimolecular type (II). Suitable type (I) systems are aromatic ketone compounds, such as benzophenones in combination with tertiary amines, alkylbenzophenones, 4,4'-bis(dimethylamino)benzophenone (Michler's ketone), anthrone, and halogenated benzophenones, or mixtures of the aforementioned types. Also suitable are type (II) initiators such as benzoin and its derivatives, benzil ketals, acylphosphine oxides, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bisacylphosphine oxides, phenylglyoxylic acid esters, camphorquinone, α-aminoalkylphenones, α,α-dialkoxyacetophenones, and α-hydroxyalkylphenones. Specific examples are Irgacur ®< 500 (a mixture of benzophenone and (1-hydroxycyclohexyl)phenyl ketone, Ciba, Lampertheim, DE), Irgacure ®< 819 DW (phenylbis-(2, 4, 6-trimethylbenzoyl)phosphine oxide, Ciba,Ciba, Lampertheim, Germany) or Esacure ®< KIP EM (oligo-[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)-phenyl]-propanone], Lamberti, Aldizzate, Italy) and bis-(4-methoxybenzoyl)diethylgerman. Mixtures of these compounds can also be used.
[0061] When choosing photoinitiators, care should be taken to ensure they have sufficient reactivity with the radiation source used. A wide variety of photoinitiators are available on the market. Commercially available photoinitiators cover the entire UV-VIS spectrum. Photoinitiators are used in the production of coatings, printing inks, and adhesives, as well as in the dental field.
[0062] In this process variant, the photoinitiator is generally used in a concentration of 0.01 to 6.0 wt.%, preferably 0.05 to 4.0 wt.% and particularly preferably 0.1 to 3.0 wt.%, based on the amount of curable component containing olefinically unsaturated double bonds used.
[0063] In a further preferred embodiment, the method has the features: the carrier is arranged within a container and can be lowered vertically in the direction of gravity, the container contains the radically crosslinkable building material in an amount which is sufficient to cover at least the carrier and an uppermost surface, viewed in the vertical direction, of crosslinked building material deposited on the carrier, before each step II) the carrier is lowered by a predetermined distance so that a layer of the radically crosslinkable building material forms above the uppermost layer, viewed in the vertical direction, of the crosslinked building material and in step II) an energy beam exposes and / or irradiates the selected region of the layer of the radically crosslinkable building material, corresponding to the respectively selected cross-section of the precursor.
[0064] Thus, according to this embodiment, the additive manufacturing process of stereolithography (SLA) is covered. For example, the carrier can be lowered by a predetermined distance of ≥ 1 µm to ≤ 2000 µm.
[0065] In a further preferred embodiment, the method has the features: the carrier is arranged within a container and can be lifted vertically against the direction of gravity, the container provides the radically crosslinkable building material, before each step II) the carrier is lifted by a predetermined distance so that a layer of the radically crosslinkable building material forms under the lowest layer of the crosslinked building material seen in the vertical direction and in step II) a plurality of energy beams simultaneously expose and / or irradiate the selected region of the layer of the radically crosslinkable building material, corresponding to the respectively selected cross-section of the precursor.
[0066] Thus, according to this embodiment, the additive manufacturing process of DLP technology is covered when the plurality of energy beams generate the image to be provided by exposure and / or irradiation via an array of individually controllable micromirrors. The carrier can, for example, be raised by a predetermined distance of ≥ 1 µm to ≤ 2000 µm.
[0067] In a further preferred embodiment, the method has the features: In step II), the radically crosslinkable build-up material is applied from one or more print heads, according to the selected cross-section of the precursor, and is then exposed and / or irradiated.
[0068] Thus, according to this embodiment, the additive manufacturing process of the inkjet method is covered: the crosslinkable build material is selectively applied, optionally separately from the catalysts according to the invention, by one or more print heads, and the subsequent curing by irradiation and / or exposure can be non-selective, for example by a UV lamp. The print head(s) for applying the crosslinkable build material can be a (modified) print head for inkjet printing processes. The carrier can be designed to be movable away from the print head, or the print head can be designed to be movable away from the carrier. The increments of the spacing movements between the carrier and the print head can, for example, be in a range from ≥ 1 µm to ≤ 2000 µm.
[0069] In a further preferred embodiment, the production of the shell by means of the additive manufacturing process comprises the steps: Applying a layer of particles comprising the build material to a target surface; applying energy to a selected portion of the layer, corresponding to a cross-section of the shell, such that the particles in the selected portion are bonded; repeating the steps of applying and applying energy for a plurality of layers such that the bonded portions of the adjacent layers bond to form the shell.
[0070] According to this embodiment, the process is a powder sintering or powder melting process. It is preferred that at least 90% by weight of the particles have a particle diameter of ≤ 0.25 mm, preferably ≤ 0.2 mm, particularly preferably ≤ 0.15 mm. The energy source for bonding the particles can be electromagnetic energy, such as UV to IR light. An electron beam is also conceivable. The bonding of the particles in the irradiated part of the particle layer is usually achieved by (partial) melting of a (semi-)crystalline material and bonding the material upon cooling. However, it is also possible for other shape transformations of the particles, such as a glass transition, i.e., heating the material to a temperature above the glass transition temperature, to cause the particles to bond to one another.
[0071] In a further preferred embodiment, the action of energy on a selected part of the layer, corresponding to a cross-section of the shell, so that the particles in the selected part are bonded, comprises the following step: Irradiating a selected part of the layer, corresponding to a cross-section of the shell, with an energy beam so that the particles in the selected part are bonded.
[0072] This process can be considered a selective sintering process, particularly a selective laser sintering (SLS) process. The energy beam for bonding the particles can be a beam of electromagnetic energy, such as a "light beam" from UV to IR light. The energy beam is preferably a laser beam, particularly preferably with a wavelength between 600 nm and 15 µm. The laser can be a semiconductor laser or a gas laser. An electron beam is also conceivable.
[0073] In a further preferred embodiment, the action of energy on a selected part of the layer, corresponding to a cross-section of the shell, so that the particles in the selected part are bonded, comprises the following steps: Applying a liquid to a selected portion of the layer, corresponding to a cross-section of the shell, wherein the liquid increases the absorption of energy in the regions of the layer contacted by it relative to the regions not contacted by it; irradiating the layer such that the particles in regions of the layer contacted by the liquid are bonded together and the particles in regions of the layer not contacted by the liquid are not bonded together.
[0074] In this embodiment, for example, a liquid containing an IR absorber can be applied to the layer using an inkjet process. Irradiating the layer leads to selective heating of those particles that are in contact with the liquid including the IR absorber. In this way, bonding of the particles can be achieved. Optionally, a second liquid can also be used, which is complementary to the energy-absorbing liquid in terms of its behavior towards the energy used. In areas where the second liquid is applied, the energy used is not absorbed but reflected. The areas beneath the second liquid are thus shaded. In this way, the selectivity between areas of the layer that are to be melted and those that are not to be melted can be increased.
[0075] In a further preferred embodiment, the production of the shell by means of the additive manufacturing process comprises the steps: Applying a layer of particles comprising the building material to a target surface; applying a liquid to a selected portion of the layer, corresponding to a cross-section of the shell, wherein the liquid is selected such that it bonds the particles to one another in the areas of the layer contacted by it, by bonding, fusing, and / or dissolving. Repeating the steps of applying the layer and the liquid so that the bonded portions of the adjacent layers bond to form the shell.
[0076] This process can be considered a so-called "binder jetting" process. As described above, the liquid can come into contact with the powder layer in a variety of ways and solidify it in a targeted manner.
[0077] Preferred building materials that are processed in this way are either inorganic sands such as SiO 2 or gypsum or organic polymer powders such as polystyrene, polyvinyl chloride, polymethyl methacrylate and polyurethane.
[0078] In a further preferred embodiment, the production of the shell by means of the additive manufacturing process comprises the steps: Applying a filament of an at least partially melted building material to a carrier to obtain a layer of the building material corresponding to a first selected cross-section of the shell; applying a filament of the at least partially melted building material to a previously applied layer of the building material to obtain a further layer of the building material corresponding to a further selected cross-section of the shell and connected to the previously applied layer; repeating the step of applying a filament of the at least partially melted building material to a previously applied layer of the building material until the shell is formed.
[0079] This embodiment is a fused deposition modeling (FDM) process. The individual filaments deposited can have a diameter of ≥ 30 µm to ≤ 2000 µm, preferably ≥ 40 µm to ≤ 1000 µm, and particularly preferably ≥ 50 µm to ≤ 500 µm.
[0080] The first step of this embodiment of the method involves building up the first layer onto a carrier. The second step is then carried out by applying further layers to previously applied layers of build material until the desired final result in the form of the object is achieved. The at least partially melted build material bonds with existing layers of material to build up a structure in the z-direction. However, it is possible for only one layer of build material to be applied to a carrier.
[0081] In a further preferred embodiment, the reaction mixture reacts to form a foam with a compressive strength at 10% compression (DIN EN 826) of ≥ 50 kPa, preferably ≥ 95 kPa to ≤ 800 kPa or to form a foam with a compression hardness at 40% compression (ISO 3386-1) of ≤ 15 kPa, preferably ≤ 12 kPa, most preferably ≥ 1 kPa to ≤ 10 kPa.
[0082] The foams preferred according to the invention have a bulk density (ISO 845) of ≤ 300 g / l, particularly preferably ≤ 200 g / l and particularly preferably ≤ 100 g / l.
[0083] In a further preferred embodiment, the polyol component comprises a difunctional polyether polyol and / or a difunctional polyester polyol and / or a difunctional polyether carbonate polyol.
[0084] The difunctional polyether polyol is preferably a polyoxyalkylene polyol with a hydroxyl number (DIN 53240) of ≥ 150 to ≤ 550 mg KOH / g. It can also be used, for example, in a proportion of ≥ 3 to ≤ 25 wt.%, preferably ≥ 5 to ≤ 20 wt.%, based on the total weight of the polyol component.
[0085] It is further preferred that the difunctional polyester polyol has a hydroxyl number (DIN 53240) of ≥ 200 to ≤ 500 mg KOH / g.
[0086] An example of a reaction mixture which can be used in the process according to the invention contains the polyisocyanate component A) and / or polyol component B) shown below, which are also described in patent application EP 2 784 100 A1: Polyisocyanate component A) comprising: A1) 0 to 10 wt.%, preferably 0.1 to 8 wt.%, particularly preferably 0.1 - 5 wt.%, based on the organic polyisocyanate component A), 2,2'-diphenylmethane diisocyanate, A2) 0 to 30 wt.%, preferably 10 to 25 wt.%, based on the organic polyisocyanate component A), 2,4'-diphenylmethane diisocyanate and A3) 25 to 75 wt.%, preferably 35 to 55 wt.%, based on the polyisocyanate component A), 4,4'-diphenylmethane diisocyanate Polyol component B) comprising: B1) 20 to 70 wt.%, preferably 25 to 45 wt.%, based on component B, polyoxyalkylene polyols having a hydroxyl number of 25 to 60 mg KOH / g and a number-average functionality of 2 to 4, B2) 20 to 50 wt.%, based on the component B, polyoxypropylene polyols having a hydroxyl number of 300 to 900 mg KOH / g and a number-average functionality of 2.5 to 4, B3) 0 to 25 wt.%, preferably 5 to 20 wt.-%, based on component B, of polyoxyalkylene polyols having a hydroxyl number of 150 to 550 mg KOH / g and a functionality of 2, B4) 0 to 20 wt.%, based on component B, of ester group-containing polyols having a hydroxyl number of 200 to 500 mg KOH / g and a number-average functionality of 2 to 5, B5) 0.1 to 15 wt.%, preferably 0.1 to 5 wt.%, based on component B, of propylene oxide-ethylene oxide copolymers having a hydroxyl number of 25 to 200 mg KOH / g and a functionality of 5 to 8, preferably 6, B6) 0 to 3 wt.%, based on component B, of glycerol B7) 1 to 7 wt.%, preferably 4 to 6.5 wt.%, particularly preferably 5.6 to 6.6 wt.%, based on component B, of water, B8) 0.5 to 4 wt.-%, based on component B, catalysts B9) optionally auxiliaries and / or additives, wherein the NCO index (ratio of the number of NCO groups to the number of NCO-reactive groups multiplied by 100) is 85 to 125, preferably 100 to 120 and the sum of components B1) to B9) is 100 wt.%.
[0087] Mixtures of 4,4'-, 2,4'-, and 2,2'-diphenylmethane diisocyanates and polyphenyl polymethylene polyisocyanates (crude MDI) are preferred as polyisocyanate components. Crude MDI grades with a diphenylmethane diisocyanate isomer content of 50 to 70 wt.% have proven particularly effective.
[0088] As component B1), polyoxyalkylene polyols in the hydroxyl number range of 25 to 40 mg KOH / g are preferably used, which are preferably obtainable by reacting ethylene oxide and / or propylene oxide with trivalent polyols, such as glycerol, trimethylolpropane or with divalent polyols, such as ethylene glycol, water, 1,2-propylene glycol, neopentyl glycol, bisphenols, and others.
[0089] As component B2) preferably polyoxyalkylene polyols in the hydroxyl number range of 380 to 650 mg KOH / g are used, which are preferably obtainable by reacting ethylene oxide and / or propylene oxide with polyols, such as glycerol, trimethylolpropane, triethanolamine, ethylenediamine, ortho-toluyldiamine, mixtures of sugar and / or sorbitol with glycols, among others.
[0090] As component B3), difunctional polyoxyalkylene polyols in the hydroxyl number range from 150 to 550 are used, which are preferably accessible by reacting ethylene oxide and / or propylene oxide with glycols, such as ethylene, diethylene, 1,2- or 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, bisphenols and others.
[0091] As component B4), ester-containing polyols with a hydroxyl number range of 200 to 500 mg KOH / g are preferably used, which can preferably be prepared by esterification of phthalic anhydride, terephthalic acid, isophthalic acid, glutaric acid, succinic acid, and / or adipic acid with ethylene, diethylene, propylene glycol, butanediol, hexanediol, trimethylolpropane, glycerol, and others. The use of a reaction product of phthalic anhydride, diethylene glycol, and ethylene oxide is particularly preferred.
[0092] As component B5), hexafunctional propylene oxide-ethylene oxide copolymers with a hydroxyl number range of 25 to 200 are preferably used, which are preferably obtainable by reacting ethylene oxide and propylene oxide with sorbitol and its isomers. A proportion of ≥ 10 wt.% ethylene oxide units, based on (B5), is particularly preferred.
[0093] The catalysts (B8) include compounds that accelerate the reaction to produce the foam. Suitable organic metal compounds are preferably organic tin compounds, such as tin(II) salts of organic carboxylic acids, for example tin(II) acetate, tin(II) octoate, tin(II) ethylhexanoate, tin(II) laurate and the dialkyltin(IV) salts of organic carboxylic acids, for example dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate, dioctyltin diacetate, bismuth and zinc salts as well as tertiary amines such as triethylamine, tributylamine, dimethylcyclohexylamine, dimethylbenzylamine, N-methylimidazole, N-methyl-, N-ethyl-, N-cyclohexylmorpholine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutylenediamine, N,N,N',N'-tetramethylhexylene-1,6-diamine, Pentamethyldiethylenetriamine, tetramethyl diaminoethyl ether, bis(dimethylaminopropyl) urea, dimethylpiperazine, 1,2-dimethylimidazole, 1-aza-bicyclo-[3,3,0]-octane, 1,4-diazabicyclo-[2,2,2]-octane,and alkanolamine compounds such as triethanolamine, tris-isopropanolamine, N-methyl- and N-ethyl-diethanolamine, and dimethylethanolamine. Other suitable catalysts include: tris-(dialkylamino)-s-hexahydrotriazines, especially tris-(N,N-dimethylamino)-s-hexahydrotriazine, tetraalkylammonium salts such as N,N,N-trimethyl-N-(2-hydroxypropyl)ammonium formate, N,N,N-trimethyl-N-(2-hydroxypropyl)ammonium 2-ethylhexanoate, tetraalkylammonium hydroxides such as tetramethylammonium hydroxide, alkali metal hydroxides such as sodium hydroxide, alkali metal alcoholates such as sodium methylate and potassium isopropylate, and alkali metal or alkaline earth metal salts of fatty acids having 1 to 20 carbon atoms and optionally pendant OH groups.
[0094] Tertiary amines which are reactive towards isocyanates are preferred, such as, for example, N,N-dimethylaminopropylamine, bis-(dimethylaminopropyl)amine, N,N-dimethylaminopropyl-N'-methylethanolamine, dimethylaminoethoxyethanol, bis-(dimethylaminopropyl)amino-2-propanol, N,N-dimethylaminopropyl-dipropanolamine, N,N,N'-trimethyl-N'-hydroxyethyl bisaminoethyl ether, N,N-dimethylaminopropylurea, N-(2-hydroxypropyl)imidazole, N-(2-hydroxyethyl)imidazole, N-(2-aminopropyl)imidazole, 2-((dimethylamino)ethyl)methylaminopropanol, 1,1'-((3-(dimethylamino)propyl)imino)bis-2-propanol and / or the reaction products of ethyl acetoacetate, polyether polyols and 1-(Dimethylamino)-3-aminopropane and in particular the tall oil acid amide salt of N,N-dimethylaminopropylamine are used.
[0095] As auxiliaries and / or additives B9) colorants, foam stabilizers, inorganic fillers, emulsifiers, cell openers and flame retardants can be used.
[0096] Suitable foam stabilizers include, for example, siloxane-polyoxyalkylene copolymers, organopolysiloxanes, ethoxylated fatty alcohols and alkylphenols, fatty acid-based amine oxides and betaines, and castor oil or ricinoleic acid esters.
[0097] Cell openers include paraffins, polybutadienes, fatty alcohols and, if necessary, polyalkylene oxide-modified dimethylpolysiloxanes.
[0098] Further examples of auxiliaries and / or additives B9) that may optionally be used according to the invention are emulsifiers, reaction retarders, stabilizers against aging and weathering influences, plasticizers, inorganic flame-retardants, phosphorus- and / or halogen-containing organic flame retardants, fungistatic and bacteriostatic substances, pigments and dyes, as well as the conventional organic and inorganic fillers known per se. Examples of emulsifiers include ethoxylated alkylphenols, alkali metal salts of fatty acids, alkali metal salts of sulfated fatty acids, alkali metal salts of sulfonic acids, and salts of fatty acids and amines.
[0099] Further information on the use and mode of action of the above-mentioned auxiliaries and / or additives can be found, for example, in the Kunststoff-Handbuch, Polyurethane, Volume VII, Carl Hanser Verlag, Munich, Vienna, 2nd edition, 1983.
[0100] The foam can be produced by mixing the polyol formulation with the polyisocyanate component, typically in a weight ratio of 100:150 to 100:200. This mixing is typically performed using a low-pressure foaming machine.
[0101] A specific example (Example 1 from EP 2 784 100 A1) of a polyol component B) which can be used according to the invention is a mixture comprising: 30.0 parts by weight of polyether alcohol (B1) based on glycerol / propylene oxide / ethylene oxide, OH number 28 mg KOH / g, functionality 3, 34.0 parts by weight of polyether alcohol (B2) based on trimethylolpropane / propylene oxide, OH number 550 mg KOH / g, functionality 3, 15.0 parts by weight of polyester ether alcohol (B4) based on phthalic anhydride / diethylene glycol / ethylene oxide, OH number 300 mg KOH / g, functionality 2, 12.0 parts by weight of polyether alcohol (B3) based on propylene glycol / propylene oxide, OH number 512 mg KOH / g, functionality 2, 0.50 parts by weight of polyoxyalkylene polyols (B5), based on sorbitol / propylene oxide / ethylene oxide, OH number 100 mg KOH / g and a functionality of 6 6.40 parts by weight of water (B7) 1.80 parts by weight of a reaction product as described in EP 0629607 A2 from ethyl acetoacetate, polyether polyols and 1-(dimethylamino)-3-aminopropane with a functionality of approx. 2-3 and an OH number of 111 mg KOH / g (B8) 0.30 parts by weight.-Parts silicone foam stabilizer (Niax ®< Silicone SR 234 from Momentive Performance Materials) (B9), .
[0102] This polyol component can, for example (Example 1 from EP 2 784 100 A1) be reacted with the following isocyanate component A): 182 parts by weight of a technical isocyanate with a proportion of approximately 14 wt.%, based on organic polyisocyanate component A), 2,4'-diphenylmethane diisocyanate and approximately 45 wt.%, based on organic polyisocyanate component A), 4,4'-diphenylmethane diisocyanate, and an NCO content of 31.8 wt.%
[0103] As documented in Example 1 of EP 2 784 100 A1, foam blocks produced from this material can have the following average properties: bulk density (DIN 53420) 23.0 kg / m 3<; compressive strength (10% compression, DIN EN 826) 98 kPa and elongation at break (DIN 53430) 19%.
[0104] Another specific example (Example 2 from EP 2 784 100 A1) of a polyol component B) which can be used according to the invention is a mixture comprising: 30.0 parts by weight of polyether alcohol (B1) based on glycerol / propylene oxide / ethylene oxide, OH number 28 mg KOH / g, functionality 3, 34.2 parts by weight of polyether alcohol (B2) based on trimethylolpropane / propylene oxide, OH number 550 mg KOH / g, functionality 3, 15.0 parts by weight of polyester ether alcohol (B4) based on phthalic anhydride / diethylene glycol / ethylene oxide, OH number 310 mg KOH / g, functionality 2, 12.0 parts by weight of polyether alcohol (B3) based on propylene glycol / propylene oxide, OH number 512 mg KOH / g, functionality 2, 0.30 parts by weight of polyoxyalkylene polyols (B5), based on sorbitol / propylene oxide / ethylene oxide, OH number 100 mg KOH / g, functionality of 6 1.9 parts by weight of reaction product of acetoacetate ethyl ester, a polyether alcohol based on trimethylolpropane / propylene oxide (OH number 550 mg KOH / g) and 1-(dimethylamino)-3-aminopropane analogous to EP 0 629 607 (B8) 0.30 parts by weight of silicone foam stabilizer (Niax ®< Silicone SR 234 from Momentive Performance Materials) (B9), 5.8 parts by weight of water (B7)
[0105] This polyol component can, for example (Example 2 from EP 2 784 100 A1) be reacted with the following isocyanate component A): 172 parts by weight of a technical isocyanate with a proportion of approximately 21% by weight, based on organic polyisocyanate component A), 2,4'-diphenylmethane diisocyanate and approximately 44% by weight, based on organic polyisocyanate component A), 4,4'-diphenylmethane diisocyanate, and an NCO content of approximately 31.9% by weight
[0106] As documented in Example 1 of EP 2 784 100 A1, foam blocks produced from this material can have the following average properties: bulk density (DIN 53420) 24.2 kg / m 3<; compressive strength (10% compression, DIN EN 826) 97 kPa and elongation at break (DIN 53430) 19.83%.
[0107] In a further preferred embodiment, the polyol component comprises a blowing agent which is a mixture of water and at least one physical blowing agent.
[0108] In another preferred embodiment, the reaction mixture is introduced into the volume without interruption. This uninterrupted introduction could thus be characterized as a "one-shot" process.
[0109] In a further preferred embodiment, the shell produced in the additive manufacturing process encloses the volume in a partially interrupted form. Thus, the shell can have an opening for filling the reaction mixture, with this opening having an area (relative to the total surface area of the additively manufactured shell) of ≤ 10%, preferably ≤ 5%, and particularly preferably ≤ 3%.
[0110] In a further preferred embodiment, the shell produced in the additive manufacturing process encloses the volume without interruption. Thus, the shell is a completely closed shell. The reaction mixture can be introduced by injection through the shell using an injection cannula.
[0111] In a further preferred embodiment, the shell produced using the additive manufacturing process comprises one or more temporarily openable sections designed to release excess gas pressure built up within the volume. Such sections can be in the form of valves, the integration of which into the shell should pose no difficulties given that the shell was produced using an additive manufacturing process. So-called duckbill valves are particularly suitable. Such openable sections can help prevent the internal pressure in closed volumes from rising so sharply during foaming of the reaction mixture with the release of gaseous propellant that the shell bursts. These sections can also be mechanically removed during post-treatment after the object has been produced.
[0112] The invention further relates to an article obtainable by a method according to the invention, comprising a shell which defines a volume located within the shell and a foam which completely or partially fills the volume, wherein the shell comprises a thermoplastic polyurethane polymer, the foam comprises a polyurethane foam with a compressive strength at 10% compression (DIN EN 826) of ≥ 50 kPa, preferably ≥ 95 kPa to ≤ 800 kPa or a compression hardness at 40% compression (ISO 3386-1) of ≤ 15 kPa, preferably ≤ 12 kPa, very particularly preferably ≥ 1 kPa to ≤ 10 kPa and the foam and the shell are at least partially bonded to one another.
[0113] The filled volume can be, for example, ≥ 1 cm 3< to ≤ 5000 cm 3<.
[0114] In a preferred embodiment of the article, the shell comprises temporarily openable sections designed to release excess gas pressure built up in the volume. Such sections can be in the form of valves, the integration of which into the shell should pose no difficulties given that the shell was produced using an additive manufacturing process. So-called duckbill valves are particularly suitable. Such openable sections can help prevent the internal pressure in closed volumes from rising so sharply during foaming of the reaction mixture with the release of gaseous propellant that the shell bursts. These sections can also be mechanically removed during post-treatment after the article has been manufactured.
[0115] In a further preferred embodiment of the article, the shell comprises elements that protrude into the volume. In this way, structural reinforcement of the article can be achieved.
[0116] In a further preferred embodiment of the article, the article is a ball. The ball is preferably used as a game or sports equipment, for example, as a soccer ball, basketball, handball, tennis ball, softball, or the like. Such a ball can also have elements protruding from the shell into the volume. The ball preferably has a closed shell and a foam filling with a bulk density (ISO 845) of ≤ 100 g / l and a compressive strength at 10% compression (DIN EN 826) of ≥ 50 kPa. In this case, the foam is considered a hard, elastic foam. Description of the characters
[0117] Figure 1shows a bottom view of the 3D-printed shell (4) of an article (10) according to the invention according to Example 1, comprising three intertwined elements (2, 2', 2") with walls (1) and the polymer-filled volumes (3, 3', 3") enclosed thereby. Figure 2 shows a side view of the mold from example 1 consisting of three intertwined elements (2, 2', 2"). Figure 3 shows a top view of the mold from example 1 consisting of three intertwined elements (2, 2', 2"). Examples Inventive Example 1
[0118] An inventive article 10 was produced by first additively manufacturing a shell 4 and then filling it with a reaction mixture. The shell 4 was produced using the SLA process. The UV-reactive resin used was the photopolymer resin Greay FLGPGR03 from the manufacturer Formlabs and was processed in the SLA printer Form 2 from the manufacturer Formlabs. The shell forms a shape of three intertwined, hollow elements (2, 2', 2") with a wall thickness of 2 mm. The elements (2, 2', 2") were open at the bottom to allow filling with polymer, as shown in Figure 1 After printing and removing adhering liquid photopolymer, a reaction mixture was filled into this shell to form an article 10 as shown in Figure 2 to be shown. Figure 3 shows a plan view of the inventive article 10. The Figures 1 to 3However, the objects 10 shown are only examples and can have any shape achieved by 3D printing.
[0119] As a reaction mixture for the polymer to fill the hollow elements (2, 2', 2"), a prepolymer consisting of 51 wt.% methylenediphenyl isocyanate, 29 wt.% trifunctional polypropylene polyether polyol with a hydroxyl number of 35, 18 wt.% of a linear polypropylene polyether polyol with a hydroxyl number of 28, 1 wt.% paratoluenesulfonyl isocyanate, 0.6 wt.% of a polyether-modified polysiloxane as a foam stabilizer (Tegostab B 1903 purchased from Evonik Industries AG), and 0.4 wt.% dibutyltin dilaurate as a catalyst was initially used. 25 g of this prepolymer were mixed with 2.5 g of water as a chemical blowing agent to form a prepolymer mixture and stirred rapidly within 2 to 3 minutes using a wooden spatula. Immediately thereafter, the prepolymer mixture was poured into the additively produced shell 4 to form the article 10, as shown in Figures 2 and 3The prepolymer mixture has a drying time of 3 h, determined in a moisture-curing system at 23 °C and 50% relative humidity.
[0120] After 24 hours, the excess foam at the openings 5, 5', 5" was removed with a sharp knife. This results in an article 10 according to the invention consisting of an additively manufactured shell 4 that is completely foamed with a polymer. The shell 4 and the cured polymer are bonded together in a manner that exhibits little tension between the shell 4 and the volume 3, 3', 3" that surrounds the shell 4 formed by the walls 1. Due to this strong form fit, the article 10 exhibits high stability. The shell 4 and the polymer are firmly bonded together so that they preferably cannot be separated again without destroying the article 10. In this way, geometrically complex and voluminous structures can be created very quickly, which would not be possible without 3D printing. At the same time, producing the entire article using a 3D printing process would be extremely time-consuming.There is also a high degree of flexibility in the selection and combination of the properties of the shell materials and the polymer, which enables cost-effective production of a wide variety of geometries in combination with a wide range of material properties.
Claims
1. Method of producing an article (10), comprising the steps of: - producing a shell (4) encompassing a volume (3, 3', 3") for accommodating a fluid by means of an additive manufacturing method from a construction material; - providing a reaction mixture comprising a polyisocyanate component and a polyol component in the volume (3, 3', 3"); - allowing the reaction mixture to react in the volume (3, 3', 3") to obtain a polymer present at least in part in the volume (3, 3', 3"), characterized in that the reaction mixture has a setting time of ≥ 2 minutes.
2. Method according to Claim 1, characterized in that the construction material is free-radically crosslinkable and comprises groups having Zerewitinoff-active hydrogen atoms, in that the shell (4) is obtained from a precursor, and in that the method comprises the steps of: I) depositing free-radically crosslinked construction material on a carrier to obtain a ply of a construction material bonded to the carrier which corresponds to a first selected cross section of the precursor; II) depositing free-radically crosslinked construction material onto a previously applied ply of the construction material to obtain a further ply of the construction material which corresponds to a further selected cross section of the precursor and which is bonded to the previously applied ply; III) repeating step II) until the precursor is formed; wherein the depositing of free-radically crosslinked construction material at least in step II) is effected by exposure and / or irradiation of a selected region of a free-radically crosslinkable construction material corresponding to the respectively selected cross section of the precursor, and wherein the free-radically crosslinkable construction material has a viscosity, measured at 23°C to DIN EN ISO 2884-1, of ≥ 5 mPas to ≤ 100 000 mPas, wherein the free-radically crosslinkable construction material comprises a curable component in which there are NCO groups and olefinic C=C double bonds, and in that step III) is followed by a further step IV): IV) heating the precursor obtained by step III) to a temperature of ≥ 50°C to obtain the shell (4).
3. Method according to Claim 2, characterized in that - the carrier is disposed within a vessel and is lowerable vertically in the direction of gravity, - the vessel contains the free-radically crosslinkable construction material in an amount sufficient to cover at least the carrier and an uppermost surface of crosslinked construction material deposited on the carrier as viewed in vertical direction, - before each step II) the carrier is lowered by a predetermined distance so that a layer of the free-radically crosslinkable construction material is formed above the uppermost ply of the crosslinked construction material as viewed in vertical direction and - in step II) an energy beam exposes and / or irradiates the selected region of the layer of the free-radically crosslinkable construction material corresponding to the respectively selected cross section of the precursor.
4. Method according to Claim 2, characterized in that - the carrier is disposed within a vessel and is liftable vertically counter to the direction of gravity, - the vessel provides the free-radically crosslinkable construction material, - before each step II) the carrier is lifted by a predetermined distance so that a layer of the free-radically crosslinkable construction material is formed below the lowermost ply of the crosslinked construction material as viewed in vertical direction and - in step II) a multitude of energy beams simultaneously expose and / or irradiate the selected region of the layer of the free-radically crosslinkable construction material corresponding to the respectively selected cross section of the precursor.
5. Method according to Claim 2, characterized in that - in step II) the free-radically crosslinkable construction material is applied from one or more print heads corresponding to the respectively selected cross section of the precursor and is subsequently exposed and / or irradiated.
6. Method according to Claim 1, characterized in that the production of the shell (4) by means of the additive manufacturing method comprises the steps of: - applying a layer of particles including the construction material to a target surface; - introducing energy into a selected portion of the layer corresponding to a cross section of the shell (4) to bond the particles in the selected portion; - repeating the steps of applying and introducing energy for a multitude of layers to bond the bonded portions of the adjacent layers to form the shell (4).
7. Method according to Claim 1, characterized in that the production of the shell (4) by means of the additive manufacturing method comprises the steps of: - applying a layer of particles including the construction material to a target surface; - applying a liquid to a selected portion of the layer corresponding to a cross section of the shell (4), where the liquid is selected in such a way that it bonds the particles to one another in the regions of the layer with which it comes into contact by bonding, fusion and / or partial dissolution; - repeating the steps of applying the layer and the liquid to bond the bonded portions of the adjacent layers to form the shell (4).
8. Method according to Claim 1, characterized in that the production of the shell (4) by means of the additive manufacturing method comprises the steps of: - applying a filament of an at least partly molten construction material to a carrier to obtain a ply of the construction material corresponding to a first selected cross section of the shell (4); - applying a filament of the at least partly molten construction material to a previously applied ply of the construction material to obtain a further ply of the construction material which corresponds to a further selected cross section of the shell (4) and which is bonded to the ply applied beforehand; - repeating the step of applying a filament of the at least partly molten construction material to a previously applied ply of the construction material until the shell (4) has been formed.
9. Method according to any of Claims 1 to 8, characterized in that the reaction mixture reacts to form a foam having a compressive strength at 10% compression, measured to DIN EN 826, of ≥ 50 kPa or to form a foam having a compression hardness at 40% compression, measured to ISO 3386-1, of ≤ 15 kPa.
10. Method according to any of Claims 1 to 9, characterized in that the polyol component comprises a difunctional polyether polyol and / or a difunctional polyester polyol and / or a difunctional polyether carbonate polyol.
11. Method according to any of Claims 1 to 10, characterized in that the polyol component comprises a blowing agent which is a mixture of water and at least one physical blowing agent.
12. Method according to any of Claims 1 to 11, characterized in that the reaction mixture is provided in the volume (3, 3', 3") in an uninterrupted manner.
13. Article (10) obtainable by a method according to any of Claims 1 to 12, comprising a shell (4) that defines a volume (3, 3', 3") within the shell (4) and a foam that wholly or partly fills the volume (3, 3', 3"), characterized in that the shell (4) comprises a thermoplastic polyurethane polymer, the foam comprises a polyurethane foam having a compressive strength at 10% compression, measured to DIN EN 826, of ≥ 50 kPa or a compression hardness at 40% compression, measured to ISO 3386-1, of ≤ 15 kPa, and the foam and the shell (4) are at least partly cohesively bonded to one another.
14. Article (10) according to Claim 13, characterized in that the shell (4) comprises elements that project into the volume (3, 3', 3").