Effect pigments coated with organic binders for powder coatings; and a method for producing these coated effect pigments and their use.

DE502017016484D1Active Publication Date: 2024-10-31ECKART GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016484
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-03-30
Filing Date
2017-03-30
Publication Date
2024-10-31
Estimated Expiration
2037-03-30

AI Technical Summary

Technical Problem

Existing methods for coating effect pigments with organic binders, such as those used in powder coatings, face issues like separation of pigments and binders due to differences in specific weights and electrostatic charging, leading to poor storage stability and limited opacity, especially with larger pigments.

Method used

A process involving spontaneous precipitation of polymers in organic solvents, where binders with polyester functions are dissolved and then precipitate out, forming a crystalline layer on effect pigments, enhancing their coverage and stability without altering external parameters like temperature or pH.

Benefits of technology

The process ensures excellent coverage and stability of effect pigments, reducing separation and improving storage stability, allowing for higher pigment loads and maintaining optical properties, while being cost-effective and simple to implement.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to the coating of effect pigments with organic binders by spontaneous precipitation, as well as to a process for producing these coated effect pigments and their use.

[0002] Effect pigments are widely used in the pigmentation of paints, varnishes, powder coatings, printing inks, plastics, and cosmetics. The incorporation and wetting of these pigments into binder systems often poses problems, especially in powder coatings.

[0003] Effect pigments cannot be incorporated into powder coatings by extrusion and subsequent comminution of the extrudate, as is common with organic or inorganic colored pigments, because this would break the platelet-shaped pigments and lose their optical effect. Instead, so-called dry-blend or bonding processes are used.

[0004] The dry-blend process is a simple mixing procedure in which commercially available powder coatings and effect pigments are blended together in a dry state. Optionally, additional additives such as flow agents can be added to the mixing process. A disadvantage of such dry blends is that, due to differences in specific weight and electrostatic charging behavior during powder coating, such as the separation of effect pigments and binders. The recyclability of the powder coating, which in itself is one of the major advantages of powder coating systems, is no longer possible with powder coatings pigmented with effect pigments produced using this process.

[0005] The bonding process involves mixing a commercially available powder coating and an effect pigment, in which a physical bond between the effect pigment particles and the powder coating particles is achieved by heating the mixture. The bonding process thus causes the effect pigments to adhere to the surface of the powder coating particles. Bonded effect pigments exhibit less color change because there is only a greatly reduced separation of the powder coating and the effect pigment during application. A disadvantage, however, is that the bonding process is a very "hands-on" process that requires a great deal of experience and know-how. Local overheating in the reactor is possible, which then leads to an undesirable curing reaction of the powder coating. The resulting buildup in the reactor must then be laboriously removed.If the buildup is not completely removed by protective screening downstream of the process, specks may form in the coating. Furthermore, depending on the particle size, only a maximum of approximately 7% by weight of effect pigment can be incorporated in the bonding process. Especially with larger pigments (D50 > 35 µm), these small amounts are often insufficient to achieve adequate coverage.

[0006] A disadvantage of both the dry-blend and bonding processes is that the effect pigments are not completely coated by the binder and are therefore applied to a substrate without a binder coating. During the subsequent curing process, usually a stoving process, these pigments are not fully wetted by the binder. As a result, metallic effect pigments, for example, are not completely coated by the binder after the powder coating has cured and therefore do not receive optimal corrosion protection.

[0007] Another disadvantage of bonded effect pigments is that they sometimes have limited storage stability. Since the binders are inherently reactive, these products can agglomerate over extended storage periods, particularly at higher temperatures in the summer months or in hot climates, due to partial crosslinking of the binder, and thus become unusable.

[0008] An alternative to bonded products was proposed in EP 1 699 884 B1 and EP 1 893699 B1. Here, a reactive binder with the corresponding hardener is applied to the platelet-shaped metallic or pearlescent effect pigments by spray drying. For this purpose, the components are necessarily dissolved beforehand in a suitable organic solvent. The binder-hardener system is not cured in the coating state. Rather, it is cured together with the powder coating after a dry-blend process.

[0009] These products have the advantages of bonded products and, in the case of metallic effect pigments, improved resistance in relevant chemical tests and mortar tests compared to the metallic effect pigments used, as well as a special appearance (3-D effect) (U. Hirth, A. Albrecht and B. Schreiber, 1 PPCJ December 2008).

[0010] However, these products suffer from relatively poor storage stability. Furthermore, due to the complex manufacturing process, these pigments can only be produced in limited quantities and at relatively high manufacturing costs.

[0011] Therefore, there is a need for coated effect pigments which, like bonded products, have a reduced separation of effect pigment and powder coating and have improved storage stability compared to the state of the art.

[0012] DE 10 2008 060 228 A1 and US Pat. No. 7,578,879 B2 describe effect pigments coated with LCST and UCST polymers. An LCST polymer is a polymer that is soluble in a solvent at low temperatures and becomes insoluble above a certain temperature. A UCST polymer is a polymer that is soluble in a solvent at high temperatures and becomes insoluble below a certain temperature. However, these are already cured polymers and not binders. Furthermore, these binders do not contain polyester functional groups. Furthermore, the teaching of these documents includes a subsequent reaction to immobilize the polymers on the effect pigment surface.

[0013] These pigments do not have adequate opacity and tend to agglomerate.

[0014] EP 1332182 B1 described the precipitation of polymers onto pigments from a dispersion of the pigments with the polymer in a solvent in which the polymers are soluble, by adding a solvent in which the polymers are insoluble. DE 2603211 disclosed the reverse process: A dispersion of a pigment or pearlescent pigment and a polymer in a solvent readily soluble for the polymer was added to a solvent in which the polymer is sparingly soluble. Furthermore, a similar process for the use of pigment concentrates in plastics was disclosed in DE 1544830.

[0015] However, no crystalline polymer layers are deposited. Furthermore, these precipitation processes result in highly agglomerated precipitates, making further processing virtually impossible. In the case of effect pigments, sticky powders are obtained that are unsuitable for application.

[0016] Also known are effect pigments, particularly metallic effect pigments, which are coated with polymer layers that are polymerized in situ from monomers in a liquid phase onto the effect pigments. Most known systems are or comprise polyacrylates (EP 2479224 A1, US 20120065298 A1, EP 2115075 A1, EP 1950257 A1, EP 1837380 A1, EP 477433 B1). Some of these pigments are coated with a metal oxide layer before the polyacrylate coating (US 20090117281 A1, EP 2688962 A1, EP 2773704 A1). In this case, multifunctional acrylate monomers (crosslinkers) are always used. The resulting polymer layers are non-crystalline. These products exhibit quite good chargeability and often high chemical stability in powder coatings.

[0017] However, such coated pigments are usually used in powder coatings using the dry-blend process and therefore have the associated disadvantages, such as excessive separation. Application in the bonding process is cumbersome, as the additional polymerization step unnecessarily complicates and increases the cost of the process.

[0018] Furthermore, semi-crystalline or amorphous polyesters are known as binders for powder coatings, as described, for example, in US Pat. No. 6,635,721 B1 or US Pat. No. 3,371,108. They are produced by polycondensation of the corresponding acid and alcohol components in the melt of the starting materials (melt polymerization). Due to their use in powder coatings and their cost-effective manufacturing process, such polymers do not come into contact with organic solvents during their life cycle.

[0019] There is therefore a need for coated effect pigments that do not have the aforementioned disadvantages. In particular, the effect pigments should have very good storage stability and the low tendency to separate that bonded pigments exhibit.

[0020] Furthermore, there is a need for a simple and cost-effective process for producing these pigments.

[0021] The object of the present invention was achieved by providing a coated effect pigment comprising a platelet-shaped substrate and a coating applied thereto comprising a binder for powder coating, characterized bythat in a DSC diagram at a forward speed of 5 °C / min it has at least one endothermic peak with a maximum from a range of T max = 100 to 150 °C and an enthalpy ΔH associated with this peak from a range of 15 J / g to 80 J / g, wherein the enthalpy is calculated on the amount of binder and wherein the binder has polyester functions and is produced by melt polymerization.

[0022] Further embodiments of the coated effect pigment are described in subclaims 2 to 12. I Spontaneous precipitation of polymers:

[0023] The present invention is based on a completely unexpected effect. This effect consists in the polymers initially dissolving in an organic solvent at a certain temperature T dissolving. The dissolving process is usually supported by auxiliary measures such as stirring and / or ultrasonic treatment. However, after a certain period of time t dissolving, a precipitate of the polymer forms in the solution. This process occurs spontaneous , i.e. without changing external parameters such as temperature, pH or by adding salt or another solvent.

[0024] In the context of this invention, this behavior is referred to as "spontaneous precipitation" of the polymer. To the inventor's knowledge, such behavior of polymers has not been previously known.

[0025] According to the invention, spontaneous precipitation is also understood to mean a slight temperature change, for example, due to the release of heat of dissolution. Slight temperature changes are understood here as changes in the range of 0 to 5 °C, preferably 0.5 to 2 °C.

[0026] The precipitation of dissolved polymers by changing the temperature, pH, or adding salts (salting out) has long been known in the prior art. Precipitation by adding a solvent in which the polymer is poorly soluble to the polymer solution is also known. The latter method is used, for example, in EP 1332182 B1 for coating pigments with organic polymers.

[0027] UCST or LCST polymers are also known, but in these cases a temperature change is always necessary to cause precipitation.

[0028] The effect of spontaneous precipitation is exploited in this invention to coat effect pigments with organic binders. The binders are preferably binders suitable for powder coatings. The binders used for this purpose are particularly preferably powder coating binders.

[0029] In particularly preferred embodiments, the binder used is a binder which is spontaneously precipitable in an organic solvent at a temperature T insoluble.

[0030] In suitable embodiments, the time period t insoluble ranges from approximately half a minute to 48 hours. During this time period, at least 50%, preferably 60%, more preferably 70%, particularly preferably at least 80%, and most preferably at least 90% of the previously dissolved polymer is precipitated.

[0031] However, time spans of less than half a minute are unsuitable for coating effect pigments, as the precipitation is too uncontrolled. Time spans longer than 48 hours make the precipitation process costly due to the long batch times.

[0032] It is therefore preferred that at least 50%, preferably 60%, further preferably 70%, particularly preferably at least 80% and very particularly preferably at least 90% of the previously dissolved polymer is precipitated in an organic solvent within a time period t insoluble from a range of 0.5 h to 12 h and further particularly preferably from a range of 1 h to 10 h and very particularly preferably from a range of 2 h to 8 h.

[0033] Most preferably, at least 90% of the binder is precipitated in an organic solvent within a time period t insol in a range of 2 to 8 hours.

[0034] In general, it has been observed that the precipitation of the polymers occurs largely quantitatively. Typically, 90 to 100%, preferably 92 to 97%, of the dissolved polymers are reprecipitated.

[0035] The temperature of spontaneous precipitation T insoluble is preferably in a range from 0°C to 80°C, particularly preferably in a range from 10°C to 70°C, further particularly preferably in a range from 15°C to 50°C, and most preferably in a range from 18°C ​​to 30°C. At lower temperatures, precipitation occurs more quickly than at higher temperatures.

[0036] The solvent used for the dissolution process should not be too non-polar. For example, it has been observed that binders can be dissolved in non-polar solvents such as carbon tetrachloride, but not that they precipitate again.

[0037] Preferred organic solvents are solvents from the group of ketones and esters. Particularly preferred solvents are acetone, methyl ethyl ketone (MEK), ethyl acetate, and mixtures thereof.

[0038] Although the dissolution of the polymers prior to spontaneous precipitation occurred without any visible residues, the solutions always exhibited a certain opacity, suggesting the presence of a colloidal state due to aggregation of the dissolved polymer. In contrast, clear solutions were obtained in nonpolar solvents such as carbon tetrachloride, where spontaneous precipitation did not occur.

[0039] In embodiments according to the invention, the binder has polyester functions. In particularly preferred embodiments, the binder is a polyester, which can be used as a powder coating binder. Such binders are produced via melt polymerization. The monomers (monomers containing carboxylic acid functions as the acid component and monomers containing alcohol functions as the alcohol component) are melted and polymerized or oligomerized by polycondensation in the presence of suitable catalysts. This results in polyesters that may have hydroxyl groups or carboxylic acid groups as terminal functional groups. These polyesters are naturally not fully cured, since, as binders in the powder coating, they must cure further after the coating process during the baking of the coating.Examples of the production of such polyesters can be found in EP 0521992 B1, US 6,660,398 B1, US 6,635,721 B1, WO 2001 / 138432 A1, US 6,384,102 B1, WO 2004 / 083326 A1 and WO 2002 / 50201 A1.

[0040] In further preferred embodiments, the polyester contains, as the acid component, a major portion of monomers from the group consisting of isophthalic acid and terephthalic acid, and mixtures thereof. In particularly preferred embodiments, the binder contains, as the acid component, at least 14 mol% of isophthalic acid, based on all acid components.

[0041] The proportion of isophthalic acid and terephthalic acid is preferably 50 to 100 mol% and particularly preferably 70 to 96 mol%, based on all acid components.

[0042] Other acid components that may be present, preferably not as the main component, include adipic acid, phthalic acid, succinic acid, glutaric acid, pimelic acid, azelaic acid, sebacic acid, fumaric acid, maleic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and mixtures of these compounds. Furthermore, tri- or polyfunctional carboxylic acids such as trimellitic acid or pyromellitic acid may be present in small amounts (less than 10 mol%) as branching units.

[0043] With regard to the alcohol components of the polyester binder, preferred embodiments are those that have a major proportion of neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol as the alcohol component. The proportion of neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol is preferably 50 to 100 mol%, particularly preferably 70 to 98 mol%, and very particularly preferably 80 to 95 mol%, based on all alcohol components. Neopentyl glycol is very particularly preferred as the major alcohol component.

[0044] Polyester binders with such alcohol contents are more likely to be classified as "amorphous" polyesters in the literature (US 6,660,398 B1, US 6635721 B1).

[0045] Other alcohol components, which are preferably present in a total of less than 50 mol% of all alcohol components, include, for example, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,3-propanediol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, neopentyl glycol hydroxypivalate, and mixtures of these compounds. Furthermore, tri- or polyfunctional hydroxylated compounds containing at least three hydroxyl groups, such as trimethylolpropane, ditrimethylolpropane, pentaerythritol, and mixtures thereof, may be present in small amounts (less than 10 mol%) as branching units.

[0046] In further preferred embodiments, with regard to the alcohol components of the polyester, the molar ratio of linear α,ω-alcohols such as ethylene glycol to neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol is below 20%, more preferably below 15%; even more preferably below 12% and most preferably below 10%. Polyesters with an excessively high content of linear α,ω-alcohols such as ethylene glycol have proven to be less suitable for spontaneous precipitation.

[0047] Such polyesters are known in the literature as "amorphous" polyesters. Polyesters with a high proportion of more symmetrical monomers, such as linear α,ω-alcohols and / or a high proportion of terephthalic acid, are known in the literature as "semicrystalline" polymers (EP 0 521 992 B1, US Pat. No. 4,217,426).

[0048] The spontaneous precipitation process of the polymers is due to an increased crystallization of the polymers, which occurs after dissolution of the polymers in the solvent. This is demonstrated below using various measurement methods.

[0049] Without being bound to any theory, this is explained, particularly in the case of polyester binders suitable for powder coatings, by the fact that, due to their melt production, these polyesters may already exhibit a certain degree of partial crystallinity, but are extremely sterically strained. The dissolution process gives the polymer chains more freedom of movement, allowing suitable polymer segments to be found and crystalline regions to form. Thus, the polymer ultimately becomes insoluble and precipitates.

[0050] Remarkably and completely surprisingly, this happens without any further changes to external parameters.

[0051] This is particularly surprising in the case of polyesters with a high proportion of neopentyl glycol as alcohol component and / or a high proportion of isophthalic acid as acid component, since these binders have been described in the literature as amorphous polyesters (US 6,660,398 B1, EP 0521992 B1). II Characterization of the polymers IIa DSC measurements:

[0052] Differential scanning calorimetry (DSC) is a standard method for analyzing polymers. The degree of crystallinity can be estimated based on the specific energy of endothermic melting peaks. However, determining an accurate degree of crystallinity always requires standardization using known polymers with a similar structure.

[0053] In this invention, the position of melting peaks is primarily determined by the maximum temperature T max . The polymers precipitated according to the invention can also exhibit melting peaks with multiple maxima. In this case, T max is chosen for the highest peak. If two peaks have largely equal intensities (+ / - 5%), the average of the two maxima is taken.

[0054] The effect pigments coated with binders according to the invention have, in a DSC diagram at a forward speed of 5 °C / min, at least one endothermic peak with a maximum from a range of T max = 100 to 150 °C and an enthalpy ΔH associated with this peak from a range of 15 J / g to 80 J / g, wherein the enthalpy is calculated based on the amount of binder.

[0055] This endothermic peak is attributed to the melting process of the crystalline components of the binder.

[0056] More preferably, T max is in a range from 110 to 140°C. Furthermore, the enthalpies of fusion are in a range from 20 to 70 J / g and particularly preferably in a range from 30 to 65 J / g, with the enthalpy being calculated based on the amount of binder.

[0057] The T max positions of the enthalpies of fusion are astonishing in the case of polyester binders. If one performs a DSC scan of the unprecipitated binders, one obtains a rather small peak with a T max of approximately 65 to 72 °C in the first DSC run for the preferred polyester binders.

[0058] This peak is likely due to certain small portions of crystalline regions of the polymer.

[0059] Thus, the effect pigments coated with binder according to the invention exhibit an increase in the enthalpy of fusion in the DSC ΔT Max from the crystallized state compared to the uncrystallized state from a range of 40 to 75 °C and preferably from a range of 50 to 70 °C.

[0060] The melting enthalpies of the non-precipitated binders, preferably polyester binders, ΔH AGM are in a range of only approximately 5 to 10 J / g.

[0061] Thus, the effect pigments coated with binder according to the invention have a ratio of the endothermic enthalpies of fusion ΔH / ΔH AGM , which can be determined by means of the precursor of a DSC measurement at a precursor rate of 5 °C / min and which are based on the amount of binder, after precipitation (ΔH) in relation to the binder before precipitation (ΔH AGM ) in a range from 2 to 10. This ratio is preferably in a range from 3 to 8 and very particularly preferably in a range from 4 to 7.5. Ilb Powder diffraction (PXRD):

[0062] Powder diffraction using the Debye-Scherrer geometry is a common method for determining the degree of crystallinity of polymers. This requires that the sample be spatially statistically distributed and, if possible, exhibit no preferred directions. This method can only detect crystalline fractions above a certain size, as no diffraction occurs in crystallites that are too small.

[0063] Preferably, the PXRD diffractograms are recorded in the Debye-Scherrer geometry with a capillary with a diameter of 0.3 mm, using Cu Kα1 as the X-ray source and germanium(111) with a slit width of 0.5 mm as the monochromator.

[0064] All these parameters influence the width of the peaks obtained.

[0065] Effect pigments coated according to the invention exhibit structured diffractograms. The peaks can be attributed to the (semi-)crystalline binder. These peaks have half-widths in the range of 0.7 to 2.0° (in 2θ).

[0066] However, no structured spectra are obtained from the unprecipitated polymers. IIc 13< C-MAS NMR spectroscopy and relaxation:

[0067] Since NMR relaxation measurement on solids is well known in the scientific literature for the characterization of crystalline and amorphous parts of polymers, but is less frequently mentioned in the patent literature, a general description of the method is given first. MAS spectroscopy:

[0068] Solid-state NMR spectroscopy is characterized by the influence of strong nucleus-nucleus interactions, which affect the spectrum. In liquid-state NMR, these interactions are largely averaged out by Brownian motion. This results in narrow resonance lines, from which in-depth information about the chemical composition of the sample under investigation can be extracted. For materials in the condensed phase (solid state), where fixed structures are present, Brownian motion is weak or absent. Consequently, spin interactions are always present, resulting in structureless, very broad NMR spectra. Among these interactions, dipolar interactions, chemical shift anisotropy, and quadrupole interactions play the most important roles.Since quadrupole interactions only play a role for nuclei with a nuclear spin I > 1, they can be neglected in 13< C NMR (analogous to 1< H, for 13< C the spin = ½).

[0069] Chemical shift anisotropy (CSA) describes the difference in the chemical shift of the NMR signal between isotropic and anisotropic states. The chemical shift is known to be a measure of the local magnetic field of a specific atomic nucleus, which induces a specific magnetic moment. In liquid NMR, the chemical shifts of polymers are usually averaged values ​​of all possible conformations due to the rapid conformational changes around the polymer's chemical bonds. In solids, the chemical shift—the interaction between the nuclear spin and the electrons in the molecular orbitals—is influenced by every structural change. Therefore, it contains valuable information not only about the chemical identities but also about the molecular orientations of the molecular groups involved.

[0070] Dipolar interactions, also called dipolar couplings, describe the direct interactions between two spins with a magnetic moment. In the case of a 13< C nucleus and a bound proton ( 1< H), the dipolar coupling depends on the distance r (~1 / r 3< ) and their orientation (θ) relative to the external magnetic field B 0 [Isao Ando, ​​Tetsuo Asakura, Solid State NMR of Polymers, Vol. 84].

[0071] To reduce these effects, a new method was introduced by Andrew et al. in 1958 [ER Andrew, A. Brandbury, RG Eades, Nature 1959, 183, 1802.]. This new technique (MAS for m agic a angle spinning) consisted of measuring the sample in a ceramic rotor that rotates at a specific, "magic," angle θ m , with a rotation frequency v rot ranging from ~1 kHz to 70 kHz. The magic angle θ m is the angle between the rotation axis and the external magnetic field B 0 at which the term cos 2 < θ m = 1 / 3, representing the average spatial orientation, is valid. It is exactly 54.74°. At this angle, spin interactions that broaden the NMR lines are partially averaged out, so that the linewidth is significantly reduced. However, it is still approximately 10 to 100 times the linewidth of the corresponding liquid NMR signals. Geometrically, the magic angle can be described as the angle of the diagonal to the edge of a cube.A characteristic feature of a MAS NMR spectrum is the presence of a central line at the position of the isotropic chemical shift, as well as sidebands, the so-called "rotational sidebands" (ssb). The rotational sidebands (ssb) always appear at integer multiples of the rotation frequency v rot . They are always denoted by a superscript asterisk (*) in the spectrum.

[0072] In the case of a polymer sample with many resonances, the overlap of the rotational sidebands with the actual chemical shift signals of different chemical groups complicates the analysis of the recorded spectra. Therefore, a rotation frequency is usually used at which at least the central lines of relevant chemical groups are free of overlap. Higher rotation frequencies will usually remove the rotational sidebands from the spectrum. For groups with a large chemical anisotropy shift (e.g., polymers with COO groups), high rotation frequencies and / or special techniques are used to suppress the rotational sidebands [WT Dixon, J. Chem. Phys., 77, 1800 (1982); ON Antzutkin, Z. Song, X. Feng, and MH Levitt. J. Chem. Phys., 100, 130 (1994)].

[0073] In general, rotation frequencies of a few kHz up to 20 kHz are sufficient to average out the dipolar interactions between 13< C nuclei and bound protons. Dipolar interactions between 1< H nuclei are even stronger, so higher rotation frequencies of up to 70 kHz must be used. As a result, 1< H MAS solid-state NMR requires an extremely high material expenditure and is therefore rarely used. In the case of polymers, 13< C MAS NMR has long been proven to be sensitive enough to investigate structures and dynamic processes. Since 13< C nuclei have a significantly lower natural abundance than 1< H nuclei, techniques are commonly used in which the magnetizations of the more abundant species (in polymers therefore usually 1< H) are transferred to the rarer species (13< C).One of the most common techniques is Hartmann-Hahn cross-polarization, in which the magnetizations of the excited proton nuclei are transferred to the 13< C nuclei. In this case, a maximum sensitivity enhancement of a factor of 4, determined by the gyromagnetic ratio of the involved nuclei (γ H / γ C ), can be achieved [SR Hartmann, EL Hahn, Phys. Rev. 1962, 128, 2042].

[0074] In a crystal, the molecules exist in inequivalent positions or frozen conformations. The solid-state MAS NMR spectrum will exhibit more signals with slightly altered chemical shifts, whereas in a solvent NMR the signals would be equivalent. This effect can be used in solid-state NMR to study tautomerism and its dynamic changes [F. Laupretre, L. Monnerie, J. Virlet. Macromolecules 17 (1984) 1397].

[0075] For amorphous polymer samples below the Tg, the relatively high disorder of the chains will induce broader NMR bands than for crystalline samples. The differences between the broad NMR signals for the amorphous and narrower signals for the crystalline phases can be used to determine the degree of polymerization of the polymers [Isao Ando, ​​Tetsuo Asakura, Solid State NMR of Polymers, Vol. 84]. Since the chain conformations in amorphous and crystalline phases of polymers differ, their NMR spectra and dynamic NMR behavior will also differ. For semicrystalline polymers, the dynamic behavior can be used as a criterion to distinguish the behavior of the amorphous phase with highly mobile chains from that of the crystalline phase with very restricted chain mobility. One of the methods that is intensively used is the T1 longitudinal relaxation technique [WS Veeman, EM Mengen, HHC de Moor, Proc.IUPAC IUPAC Macromol. Svmp. 28rh. 1982. 2. ; FC Schilling, FA Bovery, AE Tonelli. Polvm. Marer. Sci. Eng. 50 (1984) 256, DA Torch. J. Magn. Reason. 30 (1978) 613.]. 13< C-MAS NMR relaxation:

[0076] Longitudinal relaxation or spin-lattice relaxation is the mechanism that describes the evolution of the magnetization vector in a spin system towards equilibrium, which occurs when the magnetization vector is parallel to the external field B o . By applying a suitable 90 x' ° pulse, the macroscopic magnetization M 0 in the rotating coordinate system, which by definition points in the z-direction (parallel to the external magnetic field) in the equilibrium state, is shifted in the y'-direction. The population ratios of the affected energy levels change such that equal population occurs instead of the population according to a Boltzmann distribution that applies at rest. Subsequently, relaxation to the equilibrium state occurs according to an exponential function with the time constant T 1 .

[0077] Due to the high mobility of the chains in the amorphous phase, T 1 is significantly shorter than the relaxation time in the crystalline phase. This effect means that in the case of a semicrystalline polymer, the relaxation curve can no longer be described by a simple exponential function of the type [Bloch F. Phys. Rev. 1946; 70: 460-474.]: M t = M 0 1 − e − t T 1 Rather, a biexponential function must be used to separate the fast relaxation time T 1 s< of the amorphous part from the slow relaxation time T 1 l< of the crystalline part: M t M 0 a c T 1 s T 1 l = M 0 ⋅ 1 − c ⋅ 1 − a ⋅ e − t T 1 s + c ⋅ 1 − a ⋅ e − t T 1 l The following assignments apply:

[0078] M 0 : Equilibrium magnetization M(t,M 0 ,a,c,T 1 s< , T 1 l< ): Magnetization at time tc: Fraction of the crystalline polymer as a mole fraction t: Time after the 90° pulse a: This parameter takes into account non-zero initial magnetizations and is not relevant for determining the crystalline fraction in the polymers and coated Al particles. Parameter a reflects the efficiency of the saturation block and the baseline correction and should be close to 1.0 with complete elimination of the magnetization at t = 0. T 1 s< : Spin-lattice relaxation time "short": Relaxation time of amorphous fractions T 1 l< : Spin-lattice relaxation time "long": Relaxation time of crystalline fractions

[0079] Appropriate waiting times are inserted between the 90° pulses.

[0080] Overall, this method is very sensitive for detecting crystalline portions of a polymer. Since the method is always interpreted at the molecular level, even very small crystalline domains in the polymer can be detected. IId 13< C-NMR MAS measurements on polymers and on effect pigments coated according to the invention

[0081] The experimental details of the measurements to be performed can be found in the experimental section.

[0082] The effect pigments coated according to the invention are characterized in that the binder has a crystalline and an amorphous portion, which is determined by means of 13< C-NMR MAS relaxation measurements, wherein the relaxation of the 13< C nuclei is described as a biexponential relaxation according to the formula M t M 0 a c T 1 s T 1 l = M 0 ⋅ 1 − c ⋅ 1 − a ⋅ e − t T 1 s + c ⋅ 1 − a ⋅ e − t T 1 l is fitted, wherein the degree of crystallinity c is in a range between 40 to 85% and wherein a short average relaxation time T 1 s< and a long average relaxation time T 1 l< are present and wherein T 1 l< is in a range of 65 to 130 s.

[0083] In other embodiments, the binder has a degree of crystallinity c of 45 to 75%.

[0084] In preferred embodiments, the long average relaxation time T 1 l< is in a range of 70 to 110 s, particularly preferably in a range of 71 to 100 s. III Effect pigments:

[0085] The effect pigments are taken from the group consisting of metallic effect pigments, pearlescent pigments and interference pigments as well as their mixtures.

[0086] The metallic effect pigments are based on a platelet-shaped metal core. "Platelet-shaped" refers to a metal core whose aspect ratio, i.e., the ratio of average size d 50 to average thickness h 50 , is greater than 5. Metal cores with an aspect ratio of 10 to 500 and 40 to 100 are also preferred.

[0087] Metal cores with a higher form factor exhibit better metallic properties such as light-dark flop or luster. According to the invention, it is preferred that the platelet-shaped metal core contains or consists of metals from the group consisting of aluminum, copper, zinc, tin, gold bronze, brass, iron, titanium, chromium, nickel, silver, gold, steel, as well as their alloys and mixtures thereof. According to a further variant of the invention, the platelet-shaped metal core is an aluminum or gold bronze pigment. Aluminum pigments are particularly preferred.

[0088] The metallic effect pigments are either platelet-shaped and essentially round (so-called silver dollar type) or platelet-shaped and essentially "cornflake-like" in shape (so-called cornflake type).

[0089] The platelet-shaped metal core of the metallic effect pigments according to the invention, ie without subsequent coating with polymer, preferably has an average thickness h 50 of approximately 20 nm to approximately 2 µm, more preferably of 25 nm to 1 µm and even more preferably of 30 nm to 600 nm.

[0090] The h 50 value refers to the cumulative frequency distribution of the thickness distribution. The thickness distribution can be determined by SEM measurements on 70 to 100 pigments according to the method described in WO 2004 / 087816 A2 (pages 24 and 25).

[0091] The sizes of the effect pigments according to the invention are determined in the usual way using laser granulometry. This yields a cumulative frequency distribution of the volume-averaged size distribution function. The D 50 value indicates the value at which 50% of the measured effect pigments have a volume-averaged diameter equal to or smaller than the specified value. The scattered light signals are evaluated according to the Fraunhofer theory, which also includes the refraction and absorption behavior of the particles. The size distribution is preferably measured using the Cilas 1064 device from Quantachrome.

[0092] The D 50 values ​​of the size distribution of the effect pigments according to the invention are preferably in a range from 3 to 200 µm, more preferably in a range from 5 to 100 µm and particularly preferably in a range from 8 to 90 µm.

[0093] In further embodiments, the platelet-shaped substrate is a metallic effect pigment coated with a metal oxide or a pearlescent pigment.

[0094] The metal oxide is preferably selected from the group consisting of silicon (di)oxide, silicon oxide hydrate, silicon hydroxide, aluminum oxide, aluminum oxide hydrate, aluminum hydroxide, and mixtures thereof. Silicon dioxide (SiO 2 ) is particularly preferred.

[0095] Metallic effect pigments precoated with a metal oxide in this way can be coated much more easily with the binder suitable for powder coatings according to the invention. Furthermore, the metal oxide coating contributes to improved chemical and gassing stability of the entire effect pigment.

[0096] The metal oxide preferably has a geometric layer thickness of at least 10 nm. Below this layer thickness, chemical stability will be insufficient.

[0097] The preferred maximum layer thickness of the metal oxide is 200 nm, preferably 50 nm.

[0098] At layer thicknesses above 200 nm, the optical properties of the effect pigment can become detrimental.

[0099] In a particularly preferred embodiment, the platelet-shaped substrate is an aluminum effect pigment coated with SiO2.

[0100] In a further development of the invention, it is possible to precoat the metallic pigment with a substance that improves the adhesion between the effect pigment surface and the powder coating resin deposited thereon. These substances can be, for example, functionalized silanes, functionalized polymers, and organophosphorus compounds.

[0101] Preferably, functionalized silanes are used. The silanes preferably have the general formula (III) (Y)R (4-z) Si(X) z (III)

[0102] In the silane compound according to formula (III), z is an integer from 1 to 3, R is a substituted or unsubstituted, unbranched or branched alkyl chain having 1 to 12 carbon atoms, Y is a functional group that can react with corresponding functionalities of the precipitated polymer, and X represents a halogen and / or alkoxy group. R can also be cyclically bonded to Si, in which case z is usually 2. X is preferably a methoxy or ethoxy group. The Y group can be terminally bonded to the alkyl radical R. Multiple Y groups can also be bonded to an alkyl radical.

[0103] The silanes bind to the metal pigment surface following a condensation reaction between the Si(X) group and the surface OH groups. The reactive function Y, on the other hand, can cause a bond to the subsequently precipitated powder coating binder. This can involve covalent bonds or weaker interactions such as hydrogen bonds. The decisive factor is that the powder coating binder is anchored so firmly to the metal pigment surface by the silanes acting as adhesion promoters that it remains largely bound to the effect pigment during subsequent processing of the effect pigment, e.g. by sieving or further processing into a powder coating. The silanes therefore act as adhesion promoters between the metal pigment surface and the powder coating binder of the coating.

[0104] Isocyanate, epoxy, amino, hydroxy, carboxy, acrylate, or methacrylate groups are preferred as functional groups Y. These groups react with corresponding chemically compatible countergroups of the powder coating binder. However, the binder itself does not cure, i.e., the oligomeric / polymeric binder retains its chemical crosslinkability or curability. The functional group Y of the silane can, for example, react with functional groups of the powder coating binder that are not or only partially involved in the curing of the powder coating binder. For example, the functional group of the powder coating binder can be present in a stoichiometric excess relative to the functional group Y of the silane.On the metal pigment surface precoated with at least one silane compound according to formula (III), the functional groups (Y) are regularly present in a stoichiometric deficit, based on the corresponding chemically compatible functional countergroup of the subsequently applied powder coating binder.

[0105] For example, Y can be an isocyanate or epoxy group, while the binder comprises polyester components with polyol and polycarboxy functions. The isocyanate groups can, optionally with the addition of a catalyst, react with OH groups of the binder even at room temperature. Only after the metallic pigment has been coated and incorporated into a coating system does the polyester coating cure during baking of the coating system. The Y group is preferably a terminal group, as this offers the highest reactivity due to the lowest steric hindrance. However, it can also be a largely terminal group, in which up to 3 carbon atoms can still be present up to the chain end before the Y function.

[0106] The binder functionalities that react with Y can also be the same ones that build up the polymer during curing of the binder. This is possible because, as already explained above, the Y-reactive functional groups of the powder coating binder are usually present in a stoichiometric excess to the Y functional group on the pigment surface, so that after the reaction of the Y reactive group with the oligomeric / polymeric binder, sufficient functional groups remain on the oligomeric and / or polymeric binder for crosslinking or curing. The Y-reactive functional group of the powder coating binder can also be different from the functional group(s) involved in the curing of the binder.

[0107] Organofunctional silanes with appropriate functional groups suitable as surface modifiers are commercially available. For example, many of the products manufactured by Evonik, Rheinfelden, and marketed under the trade name "Dynasylan ®<" are available, as are the Silquest ®< silanes produced by OSi Specialties, and the GENOSIL ®< silanes produced by Wacker.

[0108] Examples include 3-methacryloxypropyltrimethoxysilane (Dynasylan MEMO, Silquest A-174NT), 3-mercaptopropyltri(m)ethoxysilane (Dynasylan MTMO or 3201; Silquest A-189), 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO, Silquest A-187), tris-(3-trimethoxysilylpropyl)isocyanurate (Silquest Y-11597), gamma-mercaptopropyltrimethoxysilane (Silquest A-189), beta-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (Silquest A-186), gamma-isocyanatopropyltrimethoxysilane (Silquest A-Link 35, Genosil GF40), (methacryloxymethyl)trimethoxysilane (Genosil XL 33), Isocyanatomethyl)trimethoxysilane (Genosil XL 43), aminopropyltrimethoxysilane (Dynasylan AMMO;Silquest A-1110), Aminopropyltriethoxysilan (Dynasylan AMEO) oder N-(2-Aminoethyl)-3-aminopropyltrimethoxysilan (Dynasylan DAMO, Silquest A-1120) oder N-(2-Aminoethyl)-3-aminopropyltriethoxysilan, Triaminofunktionelles Trimethoxysilan (Silquest A-1130), bis-(gamma-Trimethoxysilylpropyl)amin (Silquest A-1170), N-ethyl-gamma-aminoisobytyltrimethoxysilan (Silquest A-Link 15), N-Phenyl-gammaaminopropyltrimethoxysilan (Silquest Y-9669), 4-Amino-3,3-dimethylbutyltrimethoxysilan (Silquest Y-11637), (N-Cyclohexylaminomethyl)triethoxyosilan (Genosil XL 926), (N-Phenylaminomethyl)trimethoxysilan (Genosil XL 973) und deren Mischungen.;

[0109] The silanes, preferably silanes according to formula (I), can be applied directly to the metallic surface of effect pigments. According to a preferred embodiment, the effect pigments are metallic pigments provided with an SiO 2 coating, preferably coated with an SiO 2 coating, with the silanes applied to the SiO 2 coating. The powder coating binder is then applied to the thus precoated metallic pigments. IV Procedure:

[0110] A process for producing an effect pigment coated according to the invention comprises the following steps: a1) dissolving a binder which is spontaneously precipitable in an organic solvent or solvent mixture within a first time period of t solv at a temperature T solv from a range of 0°C to 80°C, b1) subsequently adding an effect pigment to the solvent or solvent mixture from a1) while dispersing the effect pigment, c1) coating the effect pigment with the binder within a second time period t solv at a temperature T solv from a range of 0°C to 80°C, or a2) dispersing an effect pigment in a solvent or solvent mixture, b2) subsequently adding a binder which is spontaneously precipitable to the solvent or solvent mixture which has a temperature T solv c2) coating the effect pigment with the binder within a time period t solv , d) separating the coated effect pigment from the solvent or solvent mixture and e) optionally drying the coated effect pigment.

[0111] Accordingly, there are two main processes for producing the effect pigments coated according to the invention. In the first process, the binder, which is spontaneously precipitated, is first dissolved in an organic solvent or solvent mixture. The time period t dissolution is not important per se and will be determined by practical considerations. The time period t dissolution is preferably in a range of approximately 0.25 to 3 hours. The dissolution process is advantageously facilitated by stirring and / or ultrasonic treatment of the solution.

[0112] The binder concentration should be in the range of approximately 10 to 40 wt.%, preferably 15 to 25 wt.%, based on the solvent quantity. To save solvent, you can work at a relatively high concentration, but it should be noted that the effect pigment is still easy to disperse.

[0113] The second step (b1) of adding the effect pigment to the solvent and dispersing it in the solution should ideally be performed as soon as the binder has dissolved. If you wait too long, spontaneous precipitation of the binder may begin.

[0114] Before being added to the dissolved polymer, the effect pigment can already be present as a separate dispersion in a solvent, preferably in the solvent or solvent mixture already used for step a1). This makes addition easier, for example, by metering it using conventional equipment. This also avoids dust formation, which is possible with an effect pigment powder, and the addition is virtually residue-free.

[0115] The second process is even simpler and is preferred according to the invention. Here, the effect pigment according to step a2) is already dispersed in the solvent or solvent mixture.

[0116] It has been shown that in step a2) the dissolution process of the added polymer in the solvent or solvent mixture is largely unaffected by the already dispersed effect pigment. The precipitation onto the effect pigment in step c2) takes place virtually seamlessly. Steps b2) and c2) can also overlap in time. This is not necessarily a disadvantage, since polymer that has not yet dissolved largely does not affect the precipitation of the polymer that has already dissolved. The time period t undissolved in step c1) or c2) is in a range from 0.5 h to 12 h and more particularly preferably in a range from 1 h to 10 h and very particularly preferably in a range from 2 h to 8 h. Time periods of 0.5 h to 1.5 h are also possible. The precipitation of the polymer takes place largely quantitatively, preferably to 92 to 100%. However, it has been shown that not all of the polymer always coats the effect pigments; a certain proportion can also be present as secondary precipitates.However, this is not a disadvantage, especially in powder coating applications.

[0117] However, the effect pigments are coated very homogeneously and their surface is largely quantitatively coated by the binder.

[0118] The temperature of the binder precipitation T unlös in steps c1) or c2) is preferably in a range from 0°C to 80°C, particularly preferably in a range from 10°C up to 5°C below the boiling point of the solvent or solvent mixture, further particularly preferably in a range from 15°C to 50°C and very particularly preferably in a range from 18°C ​​to 30°C.

[0119] Precipitation occurs faster at lower temperatures than at higher temperatures. The temperature is advantageously at or near room temperature. This saves energy consumption associated with heating or cooling the dispersion.

[0120] The temperature T solv for step a1) or b2) is also preferably in a range from 0°C to 80°C, particularly preferably in a range from 10°C to 5°C below the boiling point of the solvent or solvent mixture, further particularly preferably in a range from 15°C to 50°C, and very particularly preferably in a range from 18°C ​​to 30°C. Here, too, working at or near room temperature offers the most advantages.

[0121] In particularly preferred processes according to the invention, the difference ΔT=T insoluble - T soluble in both processes is in a range of 0 to 5 °C, thus resulting in spontaneous precipitation. Naturally, the process is particularly easy to control here, since heating or cooling steps can largely be dispensed with.

[0122] However, different temperatures can also be chosen for T soluble or T insoluble. For example, in the first process, the binder can be dissolved at a higher temperature, which usually occurs more quickly than at lower temperatures, and then the precipitation can take place at a lower temperature.

[0123] However, process variants with different temperatures for T soluble or T insoluble are not a process according to the LCST or UCST polymers, since according to the invention preferably no LCST or UCST polymers are used as binders.

[0124] Preferably, t unsolv in step c1) or c2) is in a range from 0.5 h to 12 h, and particularly preferably in a range from 2 to 8 h. Furthermore, precipitation times t unsolv can also be selected from a range from 1 h to 2 h.

[0125] If t unsolv is below 0.5 h, the precipitation may be uncontrolled with an excessively high proportion of secondary precipitates, ie binder not precipitated onto the surface of the effect pigment.

[0126] If t unlös is above 12 h, no disadvantages are to be expected on the product side, but the otherwise very simple process becomes unnecessarily long.

[0127] Advantageously, a solvent is selected in which both the failure times t unlös are short in the range of approximately 1 h to 3 h and the temperatures T unlös are at or close to room temperature, preferably between 18 °C and 30 °C.

[0128] The effect pigment to be coated can be in the form of a paste or a powder. Due to the manufacturing process, metallic effect pigments are often in the form of a white spirit-containing paste with a solids content of approximately 50 to 70 wt.%. In this case, an additional solvent is added to the system, which is relatively non-polar. This does not necessarily impair the precipitation process, but preliminary tests with appropriate solvent mixtures should be conducted to determine whether the binder used is precipitable in these systems.

[0129] The effect pigment is preferably in powder form. This provides better-defined conditions for the precipitation of the polymer, but also improves the processability of the solvent if it is not a solvent mixture.

[0130] For both processes, the organic solvent is preferably selected from the group consisting of acetone, methyl ethyl ketone, ethyl acetate and mixtures thereof.

[0131] It is advantageous to avoid mixing and opt for one of the solvents.

[0132] If the effect pigment is a metallic effect pigment initially present as a white spirit-containing paste, the solvents mentioned above will be present in a mixture with white spirit. In this case, care should be taken to ensure that the white spirit or another non-polar solvent present in the metallic effect pigment paste is present in the dispersion in concentrations of preferably less than 20% by weight, particularly preferably less than 10% by weight, based on the total solvent.

[0133] Steps d) and optionally e) of the methods are known standard steps and can be carried out in the usual manner.

[0134] Overall, the methods according to the invention are characterized by their great simplicity and low costs.

[0135] The solvent used can be recycled, ie solvent separated after step d) can be returned to the coating process, if necessary after a simple processing.

[0136] The binders used in the process according to the invention are spontaneously precipitable within the meaning of this invention. In preferred embodiments, the binder has polyester functions. In particularly preferred embodiments, the binder is a polyester which can be used as a powder coating binder. Such binders are produced via melt polymerization. The monomers (monomers containing carboxylic acid functions as the acid component and monomers containing alcohol functions as the alcohol component) are melted and polymerized or oligomerized by polycondensation in the presence of suitable catalysts. This produces polyesters which may have hydroxyl groups or carboxylic acid groups as terminal functional groups. These polyesters are naturally not fully cured, since as binders in the powder coating they must cure further after the coating process during the baking of the coating.

[0137] In further preferred embodiments, the polyester contains, as the acid component, a major portion of monomers from the group consisting of isophthalic acid and terephthalic acid, and mixtures thereof. In particularly preferred embodiments, the binder contains, as the acid component, at least 14 mol% of isophthalic acid, based on all acid components.

[0138] The proportion of isophthalic acid and terephthalic acid is preferably 50 to 100 mol% and particularly preferably 70 to 96 mol%, based on all acid components.

[0139] Other acid components that may be present, preferably not as the main component, include adipic acid, phthalic acid, succinic acid, glutaric acid, pimelic acid, azelaic acid, sebacic acid, fumaric acid, maleic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and mixtures of these compounds. Furthermore, tri- or polyfunctional carboxylic acids such as trimellitic acid or pyromellitic acid may be present in small amounts (less than 10 mol%) as branching units.

[0140] With regard to the alcohol components of the polyester binder, preferred embodiments are those that have a major proportion of neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol as the alcohol component. The proportion of neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol is preferably 50 to 100 mol%, particularly preferably 70 to 98 mol%, and very particularly preferably 80 to 95 mol%, based on all alcohol components. Neopentyl glycol is very particularly preferred as the major alcohol component.

[0141] Polyester binders with such alcohol contents are more likely to be classified as "amorphous" polyesters in the literature (US 6,660,398 B1, US 6635721 B1).

[0142] Other alcohol components, which are preferably present in a total of less than 50 mol% of all alcohol components, include, for example, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,3-propanediol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, neopentyl glycol hydroxypivalate, and mixtures of these compounds. Furthermore, tri- or polyfunctional hydroxylated compounds containing at least three hydroxyl groups, such as trimethylolpropane, ditrimethylolpropane, pentaerythritol, and mixtures thereof, may be present in small amounts (less than 10 mol%) as branching units.

[0143] In further preferred embodiments, with regard to the alcohol components of the polyester, the molar ratio of linear α,ω-alcohols such as ethylene glycol to neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol is below 20%, more preferably below 15%; even more preferably below 12% and most preferably below 10%. Polyesters with an excessively high content of linear α,ω-alcohols such as ethylene glycol have proven to be less suitable for spontaneous precipitation.

[0144] In further embodiments, the precipitation of the powder coating binders, especially the polyester powder coating binders, can, quite surprisingly, take place in the presence of additives that act as precipitation control agents. These additives cause more effective precipitation of the powder coating binders on the effect pigment surface. This is noticeable in a higher coverage of the pigments with binder and correspondingly lower secondary precipitation.

[0145] These additives are preferably comb copolymers based on maleic anhydrides with vinyl aromatics, preferably with substituted or unsubstituted styrene. Furthermore, these additives preferably contain polyether units (EO and / or PO) linked to acid groups via ester, amide, or imide groups.

[0146] These additives preferably have acid numbers of 4 to 45 mg KOH / g, more preferably of 5 to 40 mg KOH / g.

[0147] Further preferred salts are those in which the acid number is approximately equal to the amine number.

[0148] Such additives are described, for example, in EP 2125909 B1, EP 2106412 B1, EP 2125910 B1, EP 2240543 B1, DE 102010049642 A1, EP 2723779 B1 or EP 2864373 B1.

[0149] Commercially available additives include Byk 190, Disperbyk 2060, Disperbyk 2010, Byk ES80 or Byk 187 (all from Byk Additives & Instruments, Abelstrasse 26, D-46483 Wesel, Germany).

[0150] Such additives are typically used predominantly as wetting and dispersing additives, particularly for the formation of pigment pastes. A function as an aid to the spontaneous polymer precipitation onto effect pigments described in this invention was not foreseeable.

[0151] In a further embodiment of the present invention, the effect pigment is treated with an adhesion promoter after step a2) and before the addition of the binder and optionally before the addition of an additive. The adhesion promoters, in particular functional silanes, are described above.

[0152] The invention further relates to the use of the effect pigments according to the invention.

[0153] The effect pigments coated according to the invention are used in paints, powder coatings, printing inks, toners, or plastics. Use in powder coatings is particularly preferred.

[0154] Since the binders used according to the invention are suitable for powder coating binders, the effect pigments according to the invention are particularly easy to process in powder coatings. The binder of the powder coating into which the effect pigment is incorporated can be the same as or different from the binder of the coating.

[0155] In preferred embodiments, polyester resins will be chosen both as coating binder for the effect pigments and as binder for the powder coating. List of illustrations:

[0156] Fig. 1: DSC diagrams recorded at 5 °K / min in a temperature interval from 30 to 210 °C plotted against temperature. Only the forward scans to higher temperatures are shown, not the reverse scans. - (Solid line): Preliminary test example 1: Powder coating CC 4540-0 after precipitation from acetone, -·-·-· (Line, dash, dot): Preliminary test comparison example 1: Powder coating CC 4540-0 as received from the manufacturer _ .. _ . ._ . (Line, dash, dot, dot): Preliminary test example 1b: Powder coating CC 4540-0 after precipitation, 2nd scan directly after 1st scan Fig. 2 : Schematic representation of the pulse sequences used for the 13< C-MAS NMR overview measurements ( Fig. 2a ) and the 13< C-NMR MAS relaxation measurements ( Fig. 2b ). Fig. 3: PXRD of preliminary test example 1 (CC 4540-0) for the amorphous phase according to preliminary test comparative example 1 (top) and semi-crystalline phase according to preliminary test example 1 (middle, dashed line) as well as the coated aluminum particles according to example 1 (bottom, dotted line).

[0157] The measurements were performed on a STOE StadiP diffractometer in Debye-Scherrer geometry using Cu Kα1 radiation (Ge(111) monochromator). SiO2 capillaries with a diameter of 0.3 mm were used. The measured data for the amorphous and semi-crystalline samples were shifted upwards by 50,000 and 25,000 counts, respectively, for clarity. The very sharp and high peaks in Example 1 are due to reflections from the aluminum substrate.

[0158] Fig. 4: 13< C CP-MAS spectra of the binder CC 4540-0 for the amorphous phase according to preliminary comparative example 1 (bottom, labeled "AGM"; ν red = 12.5 kHz), the semi-crystalline phase according to preliminary comparative example 1 (middle, labeled "ND 10%"; ν red = 12.5 kHz), and the coated aluminum particles according to example 1 (top, labeled "50 / 50 Alu pigment"; ν red = 8 kHz). Rotational sidebands are marked with asterisks, and the isotropic chemical shifts were assigned to the characteristic chemical units of the acid and alcohol components of the polyester.

[0159] Fig. 5 : Plot of relaxation strength versus waiting time for the 13< C resonance of the methylene group of the semi-crystalline polymer from preliminary test example 1 (binder CC 4540-0). The two different time constants for the amorphous and crystalline portions are reflected in two regions with significantly different slopes.

[0160] Fig. 6 : 13< C CP-MAS spectra of the binder CC 2506 for the amorphous phase according to preliminary comparative example 10 (bottom, labeled "AGM"; ν red = 6 kHz) and the semi-crystalline phase according to preliminary example 1 (middle, labeled "ND"; ν red = 6 kHz). Rotational sidebands are marked with asterisks, and the isotropic chemical shifts were assigned to the characteristic chemical building blocks.

[0161] Fig. 7 : Plot of relaxation strength versus waiting time for the 13< C resonance of the methylene group of the semicrystalline polymer from preliminary test example 10 (binder CC 2506-1). The two different time constants for the amorphous and crystalline portions are reflected in two regions with significantly different slopes. Examples A1 Preliminary tests 1 to 15:

[0162] In preliminary tests, various polyester binders, commercially available as powder coating binders, were dissolved in solvents such as acetone, methyl ethyl ketone (MEK), or ethyl acetate at room temperature and then tested for possible spontaneous precipitation. For this purpose, the solvent was placed in a beaker, the temperature was adjusted if necessary, and the binder powder (typically approximately 1 / 6 of the solvent quantity) was added while stirring.

[0163] All binders that exhibited spontaneous precipitation initially dissolved without residue, but were present as a slightly grayish solution, suggesting at least a partially colloidal state. Binders that did not exhibit spontaneous precipitation (comparative examples) always dissolved in a colorless, clear solution.

[0164] Spontaneous precipitation occurred over varying periods, ranging from a few minutes to approximately 48 hours. The precipitated polymers were filtered through VWR 454 filter paper (particle retention: 12-15 µm) and dried at 50°C for 6 hours in a vacuum drying oven. These polymer powders were then ready for further analysis.

[0165] Systematic investigations on some selected polymers showed that the precipitation occurred at least 90%, and in most cases largely quantitatively.

[0166] All results are summarized in Table 1. Preliminary test comparison examples 1 to 3:

[0167] The binders CC 340, CC 2818-0 (both Allnex) and Uralac P 1580 (DSM) were dissolved in acetone, ethyl acetate or methyl ethyl ketone, but did not precipitate.

[0168] These binders are therefore not spontaneously precipitable within the meaning of this invention. Preliminary test comparison examples 4 to 6:

[0169] In preliminary tests, attempts were made to dissolve the semi-crystalline powder coating polyester resins UVCOAT 9010, Additol P791, and Crylcoat-8078-0 (all from Allnex) in ethyl acetate, acetone, and methyl ethyl ketone at room temperature and at various temperatures up to 5 °C below their respective boiling points. However, the resins could not be dissolved to a sufficient degree for the invention.

[0170] These binders are therefore not spontaneously precipitable within the meaning of this invention.

[0171] These resins were analyzed, as analytically feasible, with regard to their monomer composition (see Table 1) and characterized by DSC (see Table 2). A2 Structure Binder

[0172] The binders were analyzed for their monomer composition using standard polymer analysis methods such as GC-mass spectroscopy, IR spectra, and NMR (1< H, 13< C, and 2D NMR). Some of the acid monomer components, which were present in very small amounts, were categorized as "other acids."

[0173] Table 1 provides an overview of the binders tested. It also provides a rough estimate of the precipitation time and the results of the monomer component analysis. For each sample, the amounts of isophthalic acid or terephthalic acid (preliminary comparative example 3) were set as 100 parts, and all other components were given in proportion to these amounts.

[0174] In further preliminary test examples, the procedure was as in Example 1, using various polyester resins suitable for powder coatings.

[0175] The results of the dissolution tests in acetone at room temperature as well as the analytically determined monomer compositions are shown in Table 1. Similar results were also obtained in solvents such as ethyl acetate or methyl ethyl ketone (MEK).

[0176] In very non-polar solvents such as chloroform, the binders dissolved completely, resulting in a clear solution. However, no precipitation occurred.

[0177] In total, fifteen of the twenty-one polyester binders tested showed spontaneous precipitation behavior (preliminary test examples 1-15), while three binders dissolved in the solvent but no longer precipitated spontaneously (preliminary test comparison examples 1-3) and three other binders were insoluble (preliminary test comparison examples 4-6).

[0178] Most of these binders were also tested in ethyl acetate and methyl ethyl ketone, yielding similar results. Table 1: Solubility in acetone and analytical monomer composition of the polyester binders according to preliminary tests Example binder Manufacturer Precipitation time Analytically determined relative amount of monomers (based on 100 parts of isophthalic acid or terephthalic acid) Isophthalic acid Terephthalic acid Other acids Neopentyl glycol Trimethylolpropane (TMP) Ethylene glycol / diethylene glycol Preliminary test example 1 CC* 4540-0 Allnex < 3 h 100 1,8 - 92,1 2,5 4,8 Preliminary test example 2 Uralac P 3480 DSM < 3 h 100 3 0,2 94 2 Preliminary test example I 3 Uralac P 3495 DSM < 20 h 100 362 9 442 Preliminary test example 4 CC 2578-0 Allnex < 42 h 100 450 4 505 8 Preliminary test example I 5 CC 4420-0 Allnex < 20 h 100 82 7 Preliminary test example 6 Uralac P800 DSM < 1 min 100 5,2 98,3 0,9 2,3 Preliminary test example 7 CC 4626-0 Allnex < 1 min 100 1,3 92,5 Preliminary test example I 8 Uralac P6800 DSM < 3 h 100 1,5 84,5 5 7,6 Preliminary test example 9 CC4655-2 Allnex < 3 h 100 < 1 87,7 3,6 5,9 Preliminary test example 10 CC 2506-1 Allnex < 3 h 100 435,8 508,2 Preliminary test example 11 CC 2505-4 Allnex < 3 h 100 545 17 587 47,2 Preliminary test example 12 P 3486 Allnex < 42 h 100 592,3 653,2 6 11,1 Preliminary test example 13 CC 4890-0 Allnex < 3 h 100 1,6 112 3 7,5 Preliminary test example 14 Sirales 7499 SIR < 3 h 100 2,6 98,2 Preliminary test example 15 Uralac P 5500 DSM < 3 h 100 12,4 90,7 1,8 Preliminary test comparison example 1 CC340** Allnex No felling 100 82,1 27,5 Preliminary test comparison example 2 Uralac P 1580 DSM No felling 100 67 18 15 Preliminary test comparison example 3 CC2818 Allnex No felling 0 100 0 14,7 89,6 Preliminary test example 4 UVCOAT 9010 Allnex No solution 100,5*** 100 to 105 (ethylene glycol) Preliminary test example 5 Additol***** P791 DSM No solution **** Preliminary test example 6 CC-8079-0 Allnex No solution 100***** 2,4 trans-1,4-dimethylolcyclohexane: 61.0; cis-1,4-dimethylolcyclohexane: 34.1 * The abbreviation CC stands for "Crylcoat" ** Binder of the examples from EP 1 699 884 B1 *** Dodecanoic acid **** This product dissolved only in very small amounts in DMSO and therefore could not be analyzed. It is an ester of 1,12-dodecanoic acid ***** Adipic acid

[0179] The binders of the preliminary comparative examples 1-3 had a high proportion of ethylene glycol or trimethylolpropane compared to neopentyl glycol.

[0180] Three other binders, marketed by their manufacturers as "semi-crystalline" powder coating binders, could not be sufficiently dissolved (preliminary comparative examples 4-6). These binders had a major proportion of adipic acid (preliminary example 5) or 1,12-dodecanoic acid as the acid component. As far as could be analyzed, no detectable amounts of neopentyl glycol were found as alcohol components, but instead ethylene glycol (preliminary example 4) or a mixture of cis- and trans-dimethylolcyclohexane.

[0181] Apparently, these binders already have such a crystalline content that they cannot be dissolved and therefore no longer exhibit "spontaneous polymerization". DSC investigations on binders from the preliminary tests:

[0182] DSC investigations were also carried out for examples of the preliminary tests according to the invention. Small, defined amounts (a few mg) of both the precipitated and dried binder (preliminary test examples) and, for comparison, the unprecipitated, dry binder as received from the manufacturer (preliminary test comparison examples) were weighed in, and DSC measurements were carried out (instrument manufacturer: Netzsch, Germany; type: STA 449 F3 Jupiter; comparison standard: indium). The flow rate was 5 °K / min and the temperature range generally extended from 30 °C to 250 °C. The sample was then cooled without waiting at 5 K / min to 40 °C and, after waiting for 20 minutes at this temperature, a second temperature run was recorded at 5 K / min to 250 °C. The measurements were carried out in air, as no reactivity with oxygen could be detected.

[0183] The unprecipitated comparison samples each exhibited an endothermic peak with a maximum in a range from above 60 to approximately 75 °C and a corresponding T onset of approximately 55 to below 70 °C. Below this peak, there is generally a glass transition temperature T g , which is known to be noticeable in DSC as a shift in the baseline. This glass transition temperature is primarily attributable to the amorphous portions of the polymer. This behavior in DSC is known and quite common for these polyester binders. The peak is likely due to the melting of certain small crystalline portions.

[0184] In contrast, the spontaneously precipitated samples exhibited significantly larger endothermic peaks, with a maximum T max in a range of approximately 120 to approximately 135 °C and a corresponding T onset of approximately 100 to 124 °C. Here, too, a glass transition temperature may still be below the peak. The temperature decline of all samples was essentially unstructured, with no clearly identifiable peaks.

[0185] This is a clear indication that the strongly shifted and enlarged endothermic peaks are due to a significant increase in the crystalline fractions of the investigated polyester resins due to spontaneous precipitation.

[0186] When a second measurement was carried out on the spontaneously precipitated samples after the first temperature cycle, a behavior similar to that of the unprecipitated samples was always observed.

[0187] Fig. 1shows, by way of example, the temperature gradients for Preliminary Test Example 1. The unprecipitated polymer, as received from the manufacturer (Preliminary Test Comparative Example 1), exhibits an endothermic peak with a maximum at 70.1 °C. The precipitated polymer, on the other hand, exhibits an endothermic peak at 126.2 °C and a much higher enthalpy (Preliminary Test Example 1). If a DSC spectrum is recorded again after returning to 30 °C, the next DSC scan is very similar to that of the unprecipitated polymer (Preliminary Test Comparative Example 1b, T max at 71.5 °C). Apparently, the crystalline structure obtained due to spontaneous precipitation was irreversibly destroyed at higher temperatures.

[0188] However, if this polymer were to be dissolved in the solvent again and precipitate spontaneously, a DSC curve similar to that of preliminary test example 1 would be obtained (not in the Fig. 1shown). The crystallization process is reversible in this sense.

[0189] In all DSC experiments, TGA measurements were always performed simultaneously. These showed mass reductions in the range of 1 to approximately 2 wt.% for some samples. Typically, an initial decrease occurred at a temperature of approximately 50°C. This can be interpreted as the removal of residual traces of solvent from the precipitated polymer.

[0190] The peaks were integrated to calculate the associated enthalpy ΔH. Table 2 provides an overview of the measured data obtained. It shows the onset temperatures T Onset , the maximum temperatures T Max , and the enthalpies ΔH (after subtracting a standard background correction) associated with the endothermic peaks for the unprecipitated binder samples (preliminary test comparison examples) and for the precipitated samples (preliminary test examples). Furthermore, the shifts of these parameters are shown, whereby the value of the unprecipitated binder was subtracted from that of the precipitated binder. For the enthalpies, the ratio of the precipitated to the unprecipitated polyester resin was calculated.

[0191] This enormous temperature shift of the T max values ​​as well as the strong increase in the associated enthalpy of the endothermic peaks can be attributed to a significant increase in the crystalline fraction of the polymers due to the spontaneous precipitation. Table 2: T onset , T max and ΔH parameters from DSC measurements on precipitated binders (preliminary test examples) and unprecipitated binders (preliminary test comparison examples) Example binder Unprecipitated binder (preliminary test comparison examples) Precipitated binder (inventive preliminary test examples) Comparison (precipitated minus unprecipitated binder) T onset [°C] Tmax [°C] ΔH AGM [J / g] T onset [°C] Tmax [°C] ΔH / [J / g] ΔT onset [°C] ΔT max [°C] ΔH precipitated / ΔH AGM Preliminary test example 1 CC4540-0 65,6 70,1 9,4 100,5 126,2 55,0 34,9 56,1 5,9 Preliminary test example 2 P 3480 66,9 71,2 8,0 104,5 128,8 44,0 37,6 57,6 5,5 Preliminary test example 3 P 3495 64,6 71,1 5,1 105,4 129 30,9 40,8 57,9 6,0 Preliminary test example 4 CC 2578-0 70,1 73,5 6,9 107,1 130,5 32,2 37,0 57 4,7 Preliminary test example 5 CC 4420-0 64 71,3 7,4 105,7 123,4 38,2 41,7 51,7 5,2 Preliminary test example 6 P800 65,4 69,3 7,9 124 132,5 38,2 58,6 67,2 6,1 Preliminary test example 7 CC 4626-0 63,8 67,7 10,1 127 134,1 51,4 63,2 66,4 5,1 Preliminary test example 8 P 6800 63,8 66,6 8,5 115,8 124,5 42,2 52,0 57,9 5,0 Preliminary test example 9 CC4655-2 67,8 72 8,5 117 125,3 41,9 49,2 53,3 4,9 Preliminary test example 10 CC 2506-1 68,3 71,7 6,2 106,2 132,2 35,0 37,9 60,6 5,6 Preliminary test example 11 CC 2505-4 64,8 68,9 6,0 110,1 130,7 32,8 45,3 61,8 5,5 Preliminary test example 12 P 3486 64,6 67,1 5,2 110,2 134,5 35,6 45,6 67,4 6,8 Preliminary test example 13 CC 4890-0 66,8 69,8 8,7 105,4 125,9 43,0 38,6 56,1 4,9 Preliminary test example 14 Sir 7499 66,8 69,9 8,3 106,8 126,7 45,3 40,0 56,8 5,5 Preliminary test example 15 P 5500 59,6 62,7 9,0 103,4 120 38, 43,8 53,3 4,2 Preliminary test example 4 UVCOAT 9010 79,5 84,1 105,1 -- -- -- -- -- -- Preliminary test example 5 Additol P791 86,5 94,3 191,1 -- -- -- -- -- -- Preliminary test example 6 Crylcoat-8079-0 86,4 92,5 / 99,7 34,6 -- -- -- -- -- --

[0192] The very high melting range values ​​of 120 to over 132 °C are similarly only known in the literature for so-called "semicrystalline" polyesters (EP 0 521 992 B1, US 4,217,426). Similar enthalpy values ​​are also reported there.

[0193] What's surprising, however, is that these binders are more commonly known as "amorphous" binders due to their monomer composition (e.g., US Pat. No. 6,660,398 B1). The degree of crystallization achieved by spontaneous precipitation is apparently very high.

[0194] The enthalpy values ​​of the preliminary comparative examples 4 and 5 (measured only in the first scan), at 105.1 and 191.1 J / g, were even higher than all measured enthalpy values ​​of the inventive examples after precipitation. This appears to reflect an even higher degree of crystallization. These binders are apparently so highly crystalline that they cannot be dissolved in the solvents used here and thus do not undergo spontaneous crystallization. B Coating effect pigments: Example 1:

[0195] An open 1-liter jacketed reactor was used, cooled to 15 °C using a cryostat. 60.0 g of SiO 2 -coated aluminum effect pigment (STANDART ®< PCS 3500, available from Eckart GmbH) with an average particle size D 50 of 35 µm were initially introduced and suspended in 250 g of acetone. 63.0 g of a carboxyl-containing, saturated polyester resin named Crylcoat 4540-0 (manufacturer: Allnex S.à.rl) were added to the suspension over a period of 60 minutes via a shaker. After the addition was complete, the suspension was stirred for 2 hours and then filtered with suction. The resulting precipitate was dried in a heatable duplex kneader (type HKD-T06D, IKA ®< -Werke GmbH & Co. KG) under vacuum at 35 °C and 80 mbar for one hour and then sieved through a sieve with a mesh size of less than 100 µm. Example 2:

[0196] The procedure was as in Example 1, but the polyester resin used was Sirales PE 7499 (manufacturer: SIR Industriale SpA) (corresponding to preliminary test 14). Example 3:

[0197] The procedure was as in Example 1, but the polyester resin used was CC 2506-1 (manufacturer: Allnex S.à.rl) (corresponding to preliminary test 10). Example 4:

[0198] The procedure was as in Example 1, but 60.0 g of SiO 2 coated gold bronze pigment Dorolan Rich Bleach Gold 17 / 0 was used as the effect pigment. Example 5:

[0199] The procedure was as in Example 1, but 60.0 g of pearlescent pigment Luxan E221 (Eckart GmbH, Germany) was used as effect pigment. Example 6:

[0200] The procedure was as in Example 1, except that ethyl acetate was used as the solvent instead of acetone. Before adding the binder, 1.0 g of Disperbyk 2060 was added to the metallic effect pigment suspension and stirred for 1 h before adding the binder. After the addition, the suspension was stirred for 2 hours and then allowed to stand for 1 h. A slightly cloudy solvent supernatant formed, while the coated metallic effect pigment settled.

[0201] When the formulation according to Example 1 was used without the addition of any additives, the supernatant was significantly more cloudy. Light microscopy and SEM images showed that the metallic effect pigment in Example 6 was better and more evenly coated with polymer than in Example 1, where some secondary precipitation was observed. Example 7:

[0202] The procedure was as in Example 6, but before adding Disperbyk 2060 to the suspension of the metallic effect pigment, 2.0 g of Dynasylan Glymo (Evonik Industries AG) were added and stirred for 1 h at room temperature.

[0203] The quantity of polymer precipitation was comparable to Example 6. Comparison example 1 (based on EP 1 699 884 B1):

[0204] 195 g of the polyester resin Crylcoat 2818-0 (Allnex S.à.rl) and 105 g of a polyisocyanate adduct called Vestagon BF 1320 (manufacturer: Evonik) as a hardener component were dissolved in 1,800 g of acetone, and 200 g of SiO 2 -coated aluminum effect pigment (STANDART®< PCS 3500, available from Eckart GmbH) were dispersed. The dispersion was sprayed in a spray dryer at a rate of 30 g / min and a spray pressure of 2.5 bar in a 55 °C air stream. After drying, a yield of 380 g of coated effect pigment was obtained. Comparison example 2:

[0205] Coating as in comparative example 1, only 200 g of pearlescent pigment Luxan E221 (Eckart GmbH, Germany) was used as substrate. Comparative Example 3: Use of a UCST polymer based on DE 102 43 438 A1

[0206] The metallic effect pigment was suspended as described in Example 1, except that 250 g of deionized water was used as the solvent. 63 g of LUVITEC®< VPC 55 K 65 W (a UCST polymer from BASF with a cloud point of approximately 65 °C in water) were added as the polymer. The temperature was then raised to 75 °C within one hour, and the mixture was left at this temperature for one hour. The still-warm dispersion was then filtered.

[0207] In contrast to the inventive examples, the resulting precipitate exhibited high viscosity, which was due to severe agglomeration of the pigment particles. The agglomeration proved to be so severe that further testing of the pigments was deemed impractical.

[0208] In further comparative experiments, the precipitation temperature was varied and ethyl acetate was used as solvent instead of water, but agglomerates were always formed. B1 Application properties B 1.1 Storage stability tests:

[0209] In accordance with DIN EN ISO 8130-8, 50 g of pigment powder from the inventive examples and the comparative examples were each placed in a sealable aluminum container and stored for 28 days in an oven at 60 °C. After this time, the consistency was assessed and graded according to the criteria below compared to a reference sample stored at room temperature. Table 3: The storage tests are based on the following evaluation system: Key figure Extent of solidification or agglomeration 0 No change 1 Slight signs of consolidation; agglomerates can be easily broken up. 2 Significant solidification. Some effort is required to disperse the powder coating. Agglomerates can be broken up by applying pressure by hand. 3 1)< Significant solidification, making it difficult or impossible to disperse the powder coating. Agglomerates are very stable and require the use of mechanical means for breaking them up. 1)< If a product is classified as 3, consideration should be given to whether further testing is necessary, as the powder coating is unlikely to be used satisfactorily. Table 4: Results of the storage tests: sample Key figure storage test Example 1 0 Example 2 0 Example 3 0 Example 4 0 Example 5 0 Example 6 0 Example 7 0 Comparison example 1 3 Comparison example 2 3

[0210] All examples according to the invention and Comparative Examples 2 to 5 exhibited excellent storage stability (index 0). However, the storage stability of Comparative Examples 1 and 2 could only be rated with index 3.

[0211] The improved storage stability is most likely due to the increased degree of crystallization of the binder coatings of the examples according to the invention. B 1.2: Adhesion resistance of the polymer layer:

[0212] An important criterion for the product according to the invention is the adhesion of the resin layer to the effect pigment surface. The resin layer is subjected to significant stress during the drying and screening production steps, as well as during the subsequent processing steps by the user of the product according to the invention.

[0213] To determine adhesion to the resin layer on the effect pigment surface, the samples of inventive examples 1, 6, and 7 were subjected to particle number and size measurements. Size measurements were performed using a Sysmex FPIA-3000S. The CE 50 value is the size value at which 50% of the equivalent circle size of the measured particles in a cumulative size distribution is smaller than this value (number average). The instrument was equipped with an ultrasonic unit for dispersing the samples. This unit operates at 15 watts with adjustable amplitude and a frequency of 30 kHz.

[0214] The samples were measured without ultrasonic loading and, to simulate mechanical stresses during processing steps, with ultrasound at 20% and 60% amplitude The following Table 5 illustrates the results:

[0215] Table 5: CE 50 values ​​and the measured particle number (determined with Sysmex FPIA 3000S): Measured quantities sample Ultrasound 15 W, frequency 30 kHz amplitude without 20% 60% CE 50 / µm Example 7 3,20 1,98 1,80 Example 6 2,79 1,64 1,58 particle number Example 7 1958 5482 7066 Example 6 2810 8484 10992

[0216] The samples of Example 6 consistently exhibited lower CE 50 values ​​and higher particle counts than those of Example 7. This is due to increased secondary precipitates in the polymer coating. These secondary precipitates are usually significantly smaller than the effect pigments. As the amplitude and thus the energy input of the ultrasonic treatment increase, the CE 50 values ​​decrease in both cases. Apparently, the pigments are being crushed or the polymer coating is partially abrasive.

[0217] Thus, the polymer coating in Example 7 is better bonded to the pigment surface than in Example 6, which is probably due to the adhesion-promoting effect of the epoxy silane. B2 Analytical Investigations B 2.1 DSC measurements:

[0218] Analogous to the preliminary tests, DSC analyses were conducted using a Netzsch instrument (type STA 449 F3 Jupiter) based on the inventive examples. The binder contents of the coated effect pigments were determined analytically. The curves of the DSC measurements corresponded to those of the preliminary tests. The positions of the onset and maximum temperatures of the endothermic peaks largely corresponded to those of the corresponding preliminary tests. The enthalpies of the endothermic peaks were converted to these binder amounts. The results showed very good agreement with the preliminary tests, with deviations in the range of + / - 5%. B 2.2 PXRD powder diffractograms

[0219] All powder diffraction measurements were carried out on a STOE StadiP diffractometer in Debye-Scherrer geometry in transmission at room temperature. The diffractometer is equipped with copper radiation and a germanium monochromator (111), so that only the Cu Kα1 band (λ = 1.5406 Å) is used for diffraction. The generator power was adjusted to 40 kV and 40 mA to ensure an optimal ratio of background to Bragg scattering. To limit beam divergence, a 0.5 mm collimator was used in front of the sample. All measurements were performed in a 2Θ range between 5° and 70° using a Mythen detector (Dectris) with a detection window of 64x8 mm, which corresponds to an aperture angle of 19° in 2Θ. The detector was moved in 0.2° steps and an exposure time of 90 s for each step. The individual measurements are summed. This results in a measurement time of 8 h and 8 min for each sample. The samples were prepared in 0.3 mm borosilicate glass capillaries (Hilgenberg, Markröhrchen). B 2.3 C 13< -MAS NMR overview measurements

[0220] All high-resolution one-dimensional 13< C NMR spectra (e.g. Fig. 4 and 6) were recorded on a Bruker Avance III HD Fourier transform NMR spectrometer. The spectrometer is equipped with three channels and a wide-bore magnet (cryomagnet) with a magnetic field strength of 9.4 T. This corresponds to Larmor frequencies of 400.13 MHz for 1< H nuclei and 100.62 MHz for 13< C nuclei. The samples were filled into 4 mm zirconia rotors and transferred into a Bruker 4 mm MAS double-resonance probe head. During the measurements, the rotation frequency of the sample container was 12.5 kHz for the pure polymers (preliminary test examples 1, 10, and 15, as well as preliminary comparative examples 1, 10, and 15) and 8.0 kHz for the coated aluminum particles (Example 1). Excitation was achieved by cross-polarization using a CW pulse on the 13< C channel and a shape pulse on the 1< H channel. The shape pulse transferred the 1< H polarization to the 13< C nuclei in the usual way. Fig. 2aoutlines the pulse sequences used.

[0221] During the shape pulse, the pulse amplitude was increased linearly by a factor of two during the Hartmann-Hahn block. The initiating proton 90° pulse was adjusted to a length of 2.5 µs, and the nutation frequencies of 1<H and 13<C during the Hartmann-Hahn block were 65 kHz (averaged over shape) and 53 kHz, respectively. The Hartmann-Hahn condition for the transfer of magnetization from the protons to the 13<C nuclei is known to be: <ν( 1<H)> - ν( 13<C) = n* ν rot , where n is usually ±1. A duration of the Hartmann-Hahn block (contact time) of 3 ms provided optimal transfer efficiency. The repetition time of 1 s was chosen so that in all cases more than 90% of the proton magnetization could relax to thermal equilibrium. During FID acquisition, broadband proton decoupling was performed using a SPINAL64 sequence (described in BM Fung, AK Khitrin, K. Ermolaev, J. Magn. Reson.2000, 142, 97-104), with the proton nutation frequency set to 73 kHz and the time interval between the individual phase shifts to 7.2 µs. With an acquisition time of 40 ms, 4,096 points were acquired for the FID (. F ree I induction D ecay). While 4,096 transients were accumulated for the pure polymer samples (preliminary tests), the low sensitivity in the case of the coated aluminum particles (Example 1) required 51,600 repetitions. The 1D spectra were obtained by subsequent Fourier transformation with a zerofilling of 4,096 points and a convolution with a Lorentzian line with a half-width of 10 Hz. All chemical shifts for 13< C are given relative to the standard TMS (0 ppm).

[0222] 13< C-MAS NMR survey measurements were made for the polymer samples of the preliminary test examples 1, 10 and 17 (spontaneously precipitated polymers) as well as the corresponding preliminary comparison examples 1, 10 and 17 (polymer samples in the initial state) and for Example 1. The Fig. 4 shows the spectra of Example 1, Preliminary Test Example 1 and Preliminary Test Comparative Example 1. Also shown are the chemical formulas of the structural elements of the polyester and their assignment to the peaks in the NMR spectrum.

[0223] Fig. 6 shows the spectra of Example 10, Preliminary Test Example 10 and Preliminary Test Comparison Example 10. Compared to the Fig. 4 In the range of 130 ppm a double structure can be seen due to the high terephthalic acid content of the binder.

[0224] The precipitated, semi-crystalline polymers each exhibit significantly better-structured 13< C NMR spectra than the unprecipitated, amorphous polymers. For the coated aluminum pigment (Example 1), the structures are not quite as pronounced as for the pure polymer (Preliminary Test Example 1). This is likely due to the larger susceptibility differences in this sample.

[0225] The half-widths of the 13< C MAS spectra were between 250 and 350 Hz for the amorphous samples (preliminary comparative examples 1, 10 and 17) and between 100 and 180 Hz for the semi-crystalline polymers (preliminary examples 1, 10 and 17). Those of the coated Al particles (Example 1) were between 180 and 270 Hz.

[0226] Since the degree of crystallization could not be determined from the half-widths alone, additional 13< C-NMR MAS relaxation measurements were performed. B 2.4 13< C-NMR MAS relaxation measurements:

[0227] All 13<C spin-lattice relaxation (T 1 ) measurements were performed on a Bruker Avance II Fourier transform NMR spectrometer. This spectrometer is equipped with three channels and a wide-bore magnet with a magnetic field strength of 7.05 T. This corresponds to Larmor frequencies for 1<H and 13<C of 300.15 MHz and 75.48 MHz, respectively. The samples were loaded into 7 mm zirconia rotors and transferred to a Bruker 7 mm MAS triple resonance probe head. During the measurements, the sample container's rotation frequency was 6 kHz. This low rotation frequency was chosen to minimize the influence of the rotation frequency on spin-lattice relaxation by quenching spin diffusion in the proton bath. The acquisition was performed using a saturation sequence.The saturation block contained ten 13< C-90° pulses with a duration of 3.5 µs for the pure polymers of the preliminary and comparative examples and 7.0 µs for the coated Al particles (Example 1), with a dephasing interval of 20 ms between them. At the end of the saturation block, the residual magnetization was less than 0.1%, with the majority of the magnetization decrease being caused by the rapid relaxation of the methyl resonance. The saturation block was followed by a variable waiting time between 100 µs and 1400 s, during which the longitudinal magnetization rebuilds, depending on this waiting time and the time constant T 1 . The waiting times were chosen with an exponential spacing so that six values ​​were measured every full decade.To detect the restored polarization, it was converted into transverse, observable magnetization using a 90° read pulse on the 13< C channel, again with a duration of 3.5 µs and 7.0 µs. The resulting FID was recorded with an acquisition time of 15 ms and 2048 points under broadband proton decoupling using a SPINAL64 sequence. For the latter, the proton nutation frequency was 75 kHz and the time interval between the individual phase shifts was 7.4 µs. For the pure polymer samples (preliminary and comparative examples), 64 transients were recorded for each FID at each waiting time. For the coated Al particles (Example 1), the number of repetitions for each FID was 1200. Fig. 2b gives a schematic overview of the pulse sequences used.

[0228] To enable a frequency-resolved analysis of the spin-lattice relaxation, the obtained pseudo-2D data were Fourier transformed along the F2 domain. This involved zerofilling of 2048 points and convolution with a Lorentzian line with a half-width of 50 Hz. All chemical shifts for 13<C are again given relative to the standard TMS (0 ppm). The resulting spectra were baseline corrected by fitting the spectra for the shortest waiting time, which did not yet contain any significant spectral intensity, with a cubic spline interpolation. The resulting fitting curve was then subtracted from all other spectra. Integration was then performed over the resonances of the characteristic chemical building blocks by summing the intensities. The MATLAB program package version R2014b (8.4.0.150421) from MathWorks was used for baseline correction and integration.The following spectral ranges were integrated: 17-28 ppm (Me-), 61-78 ppm (-CH 2 -), 30-40 ppm (C q ), 124-140 ppm (-C aromatic -), and 160-170 ppm (-CO 2 -). The integral intensities were biexponentially fitted as a function of the waiting time t using equation (1). For this purpose, a Levenberg-Marquardt algorithm was used, as implemented in the program gnuplot (version 4.6 patch level 5), with a weighting of 1.0 for each data point in the sum of the least squares errors. M t M 0 a c T 1 s T 1 l = M 0 ⋅ 1 − c ⋅ 1 − a ⋅ e − t T 1 s + c ⋅ 1 − a ⋅ e − t T 1 l

[0229] The equilibrium magnetization M 0 was adjusted separately as the average of the intensities for the longest waiting times and was not changed in the global refinements. With the Levenberg-Marquardt algorithm used, only the variables a, c, T 1 s< and T 1 l< were changed. To achieve this, it is important to ensure that the intensities no longer increase systematically for at least the last three measured values. Parameter a takes into account initial magnetizations other than zero and is therefore to be regarded as a technical variable for the refinement, which is otherwise not relevant for determining the crystalline fraction in the polymers and coated Al particles. Parameter a reflects the efficiency of the saturation block and the baseline correction and should be close to 1.0 with complete elimination of the magnetization at t = 0. For the measurements performed here, a fluctuated between 0.92 and 1.1.

[0230] Thus, three variables remain for the determination of the degree of crystallinity – the two time constants of the spin-lattice relaxation T 1 s< and T 1 l< as well as the weighting c. T 1 s< and T 1 l< differed significantly and could therefore be easily separated. Together with the powder diffractograms ( Fig. 3 ) this suggests a heterogeneous nature of the samples, in which a disordered (amorphous) and ordered (crystalline) region can be distinguished. The fast spin-lattice relaxation with the time constant T 1 s< is assigned to the amorphous region due to the more efficient relaxation, in which stronger dynamics are to be expected. Accordingly, T 1 l< is characteristic of the crystalline region. The constant c describes the proportion of crystalline regions in atomic percent. Fig. 5 and 7show, as an example, the typical course of the relaxation strength Φ = (M 0 -M(t)) / M 0 against the waiting time t. The y-axis is plotted logarithmically, so that the individual relaxation components appear as straight lines.

[0231] The results of the evaluation of the relaxation measurements performed are shown in Table 6. The signals of the methyl groups were not taken into account, as they are known to relax very quickly due to the spin-rotation relaxation between C and neighboring H atoms, so that no difference between the crystalline and amorphous parts can be detected. Table 6: Results of the evaluation of the 13< C-MAS realaxation measurements Binder / Sample: Determined size - CO2 - Car - CH2 - Cq Mean values ​​of determined quantities c, T 1 s< and T 1 l< CC 4540-0 "AGM" (amorphous) Preliminary Test Comparison Example 1 M 0 2,02 6,49 1,75 1,06 a 1,00 1,00 1,00 1,00 c 0,66 0,81 0,64 0,64 0,69 T 1 s< / s 16 7,2 2,1 4,8 7,5 T 1 l< / s 73 45,9 28 22 42,2 (CC 2506-1 "AGM") Preliminary test comparison example 10 M 0 3,12 8,33 2,82 1,87 a 1,00 0,99 0,98 0,99 c 0,73 0,74 0,66 0,4 0,63 T 1 s< / s 12,2 4,4 1,2 8,3 6,5 T 1 l< / s 55,4 43,2 24,1 36 39,7 (Sirales PE 7499 "AGM") Preliminary test comparison example 15 M 0 2,28 6,01 2,09 1,18 a 1,00 1,00 0,98 1,00 c 0,79 0,75 0,65 0,79 0,75 T 1 s< / s 11,5 9,4 1,6 1,6 6,0 T 1 l< / s 71,4 61,1 35,9 22,8 47,8 CC 4540-0 "Nd" Preliminary Test Example 1 M 0 1,15 3,15 0,76 0,59 a 1,10 1,00 1,00 1,03 c 0,77 0,54 0,47 0,33 0,5275 T 1 s< / s 1,6 14 9,6 7,2 8,1 T 1 l< / s 93 140 83 77 98,25 CC 4540-0 coated Al substrate Example 1 M 0 7,5 19,8 2,8 3,4 a 1,002 0,964 0,95 1,02 c 0,69 0,76 0,73 0,65 0,7075 T 1 s< / s 14,9 8,8 0,5 1,3 6,4 T 1 l< / s 123 84,6 57 29,8 73,6 CC 2506-1 "Nd" Preliminary Test Example 10 M 0 2,49 6,25 2,11 1,29 a 1,00 0,99 0,99 0,99 c 0,73 0,62 0,72 0,33 0,6 T 1 s< / s 10,2 12,5 2,1 7,4 8,1 T 1 l< / s 105 103 50,1 47 76,3 Sirales PE 7499 "ND" Preliminary Test Example 15 M 0 1,79 4,27 1,58 0,86 a 1,00 0,99 0,98 0,99 c 0,68 0,63 0,75 0,7 0,69 T 1 s< / s 16,8 14,8 2,1 4 9,4 T 1 l< / s 116 114 57 23,4 77,6

[0232] The relaxations of the 13< C nuclei of the acid groups (abbreviated -CO 2 -), the aromatic group of the acid component (abbreviated C ar ), as well as the methylene groups (abbreviated -CH 2 -) and the quaternary C atom (abbreviated C q ) of the neopentyl alcohol component were used for the evaluation. The methyl groups were not included due to their notoriously rapid relaxation. For the determined values ​​c, T 1 s< and T 1 l<, the mean values ​​of all individual groups were used, which corresponds to the usual procedure for this method.

[0233] The short relaxation frequencies associated with the amorphous portion differ significantly from the long relaxation frequencies associated with the crystalline portion. Example 1 according to the invention and the preliminary test examples 1, 10, and 15 exhibit significantly higher relaxation times T 1 l< (73.6 to 98.25 s) than the corresponding preliminary test examples (39.7 to 47.8 s). However, no clear demarcations can be seen in the parameter c, as with the value T 1 l<. All samples tested exhibit degrees of crystallization c of approximately 70%.

[0234] Overall, these findings can be interpreted as meaning that the unprecipitated binder polymers already exhibit a certain degree of preorder with a very small spatial extent. However, in the precipitated binder polymers, the ordered regions increase significantly in spatial extent, leading to longer relaxation times T 1 l<.

[0235] Since the 13< C NMR relaxation measurements described here are an extremely sensitive method at the molecular level, even regions with very low order can lead to high c values. This method detects local order in the polymer starting from approximately 3 to 4 unit cells.

[0236] This interpretation of the NMR findings fits very well with the results of the PXRD investigations. The unprecipitated samples of the preliminary test comparison examples always showed unstructured spectra. The preordering of the polymers that was already present here was apparently too spatially weak to produce signals in the Debye-Scherrer geometry. With this method, which is based on rather long-range interactions, structured signals are only obtained when at least approximately twenty unit cells of the crystalline regions are present. The precipitated polymers showed clearly structured spectra, both in the pure polymer samples (preliminary test examples) and in the polymer precipitated onto the aluminum platelets (Example 1). In the NMR relaxation experiments, the greatly increased domain size of the crystalline portions of the precipitated polymers led to the observed longer relaxation times T 1 l<

Claims

1. Coated effect pigment comprising a platelet-shaped substrate and a coating applied thereon and comprising a binder for powder coating, characterized in that in a DSC diagram at a rate of advance of 5°C / min it exhibits at least one endothermic peak having a maximum from a range of Tmax = 100 to 150°C and also having an enthalpy ΔH associated with this peak from a range from 15 J / g to 80 J / g, the enthalpy being calculated on the amount of the binder, and the binder having polyester functions and being prepared via a melt polymerization.

2. Coated effect pigment according to Claim 1, characterized in that the binder exhibits an increase in the enthalpy of fusion in the DSC ΔTmax of the crystallized state, in comparison to the uncrystallized state, from a range from 40 to 75°C.

3. Coated effect pigment according to Claim 1 or 2, characterized in that the binder in the PXRD diffractogram recorded in the Debye-Scherrer geometry with a capillary 0.3 mm in diameter, using Cu Kα1 as x-ray source and using germanium(111) with a slit width of 0.5 mm as monochromator, has structured peaks with full widths at half maximum in the range from 0.7 to 2.0° (in 2θ).

4. Coated effect pigment according to any of Claims 1 to 3, characterized in that the binder is not an LCST or UCST polymer.

5. Coated effect pigment according to any of Claims 1 to 3, characterized in that the binder is a polyester containing acid and alcohol components and as acid components a main fraction is taken from monomers of the group consisting of isophthalic acid and terephthalic acid and mixtures thereof.

6. Coated effect pigment according to any of Claims 1 to 3, characterized in that the binder comprises as acid component at least 14 mol% of isophthalic acid, based on all the acid components.

7. Coated effect pigment according to any of Claims 1 to 3, characterized in that the binder contains as alcohol component a fraction of neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol of 50 to 100 mol%, based on all the alcohol components.

8. Coated effect pigment according to Claim 7, characterized in that with regard to the alcohol components of the polyester it has a molar ratio of ethylene glycol to neopentyl glycol and / or 2-butyl-2-ethyl-1,3-propanediol of less than 20%.

9. Coated effect pigment according to any of the preceding claims, characterized in that the platelet-shaped substrate is taken from the group consisting of metallic effect pigments, pearlescent pigments, and interference pigments, and also mixtures thereof.

10. Coated effect pigment according to Claim 1 to 9, characterized in that the platelet-shaped substrate is a pearlescent pigment or is a metallic effect pigment coated with a metal oxide.

11. Coated effect pigment according to Claim 10, characterized in that the metal oxide is taken from the group consisting of silicon (di)oxide, silicon oxide hydrate, silicon hydroxide, aluminium oxide, aluminium oxide hydrate, aluminium hydroxide, and mixtures thereof.

12. Use of a coated effect pigment according to any of Claims 1 to 11 in paints, powder coatings, printing inks, toners or plastics.