IMAGE PRINTING FORM AND METHOD FOR MAKING A PRINTING FORM

DE502018015237D1Active Publication Date: 2024-10-31CONTITECH DEUTSCHLAND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502018015237
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-20
Filing Date
2018-10-16
Publication Date
2024-10-31
Estimated Expiration
2038-10-16

AI Technical Summary

Technical Problem

Conventional methods for producing imaging printing forms, particularly in gravure printing, are complex, energy-intensive, and environmentally unfavorable due to the need for multiple layers including soft copper and hard chrome plating, which are costly and toxic, making them unsuitable for small batch sizes.

Method used

A single hard rubber layer based on butadiene-acrylonitrile rubber (NBR), carboxyl-containing nitrile rubber (XNBR), or hydrogenated acrylonitrile-butadiene rubber (HNBR) is used as the elastomer coating for the printing form, replacing the copper and chrome layers, allowing for engraving and printing without the need for electroplating and with reduced material usage.

Benefits of technology

This solution simplifies the production process, reduces environmental impact, and maintains printing quality by using a durable hard rubber layer that can be reused multiple times with minimal wear, eliminating the need for galvanic processes and allowing for efficient ink transfer and printing performance comparable to conventional methods.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to an imaging printing form which comprises a base body with an elastomer coating, wherein the elastomer coating bears an engraved pattern, wherein the elastomer coating consists essentially of hard rubber and has a hardness of greater than 70 ShoreD according to DIN ISO 7619-1, characterized in that the hard rubber is a hard rubber based on butadiene-acrylonitrile rubber (NBR), carboxyl group-containing nitrile rubber (XNBR), hydrogenated acrylonitrile-butadiene rubber (HNBR) or combinations thereof. Furthermore, the present invention comprises a method for producing an imaging printing form and a method for gravure printing.

[0002] Intaglio printing is a printing technique in which the elements to be reproduced are present as depressions (cells) in the printing form. The printing process is carried out by first inking the entire printing form, removing the excess ink with a squeegee or wiper so that the printing ink remains only in the depressions, and then transferring the ink to the paper.

[0003] The printing form can be a printing plate or a gravure cylinder. In the industrial sector, however, doctor blade gravure or rotary gravure printing is particularly important, in which the printing form is a gravure cylinder. This process is used, for example, for printing magazines or catalogs.

[0004] The production of the imaging (printing) surfaces of the printing form is carried out in the conventional way by first machining a soft copper layer with a Mohs hardness of, for example, 2 using electromechanical or laser engraving, and then engraving the printing cells. The softness of the copper layer is necessary to create the engraving using the engraving tools used in the prior art without immediately wearing them out. If these tools become excessively worn, this process would no longer be economical. Subsequently, a hard chromium layer with a Mohs hardness of, for example, 8 is applied in a galvanic process to protect the engraving layer from wear caused by the squeegee during the printing process. However, this conventional process has disadvantages.This process requires the application of two layers to the printing form, making it comparatively complex and energy-intensive. Furthermore, this process involves a galvanic process step for applying the chromium layer, which is extremely unfavorable from a health and environmental perspective. Hard chromium plating typically uses chromium(VI) trioxide, which is highly toxic during application until it is deposited. Furthermore, the proper disposal of chromium compounds is problematic from both an environmental and cost perspective. As batch sizes for print jobs become increasingly smaller, the disadvantages associated with this conventional process for producing printing forms no longer outweigh the benefits.

[0005] AT 3237 61 B, DE 198 17 104 A1, WO 03 / 037630 A1, JP 2005 254696 A, JP 2009023181 A and EP 2 301 759 A1 disclose imaging printing plates which comprise a base body with an elastomer coating and wherein the elastomer coating carries an engraved pattern.

[0006] The present invention is therefore based on the object of providing an imaging printing form whose production avoids the above-described disadvantages of conventional methods. The present invention is further based on the object of providing a correspondingly improved production method.

[0007] These objects are achieved by the embodiments characterized in the claims.

[0008] In particular, an imaging printing form is provided which comprises a base body with an elastomer coating, wherein the elastomer coating bears an engraved pattern, wherein the elastomer coating consists essentially of hard rubber and has a hardness of greater than 70 ShoreD according to DIN ISO 7619-1, characterized in that the hard rubber is a hard rubber based on butadiene-acrylonitrile rubber (NBR), carboxyl group-containing nitrile rubber (XNBR), hydrogenated acrylonitrile-butadiene rubber (HNBR) or combinations thereof.

[0009] According to the present invention, the printing form according to the invention comprises an elastomer coating consisting essentially of hard rubber. This elastomer coating is also referred to below as the hard rubber layer. Thus, according to the invention, a printing form with a printing layer is provided which replaces the two layers in conventional printing forms (namely the copper layer and the chromium layer) with a single hard rubber layer. The base body of the printing form according to the invention thus comprises the elastomer coating as a single layer. The hard rubber layer enables engraving using the engraving techniques known in the gravure printing industry, completely dispensing with the electroplating surface treatment described in the prior art.

[0010] The hard rubber of the printing form according to the invention is a hard rubber based on butadiene-acrylonitrile rubber (NBR), carboxyl group-containing nitrile rubber (XNBR), hydrogenated acrylonitrile-butadiene rubber (HNBR) or combinations thereof.

[0011] The elastomer coating of the printing form according to the invention has a hardness of greater than 70 Shore D. This hardness is determined according to DIN ISO 7619-1. Thus, in contrast to conventional elastomers, the hard rubber layer of the printing form according to the invention exhibits a higher hardness (corresponding to a higher modulus of elasticity) and thus lower deformation and recovery (rubber elasticity).

[0012] The imaging printing form according to the invention can be any suitable printing form. Preferably, the imaging printing form is a gravure cylinder or a printing plate. A gravure cylinder is particularly preferred because it is the most frequently used in commercial printing. If the printing form according to the invention is a gravure cylinder, the base body is preferably a hollow cylinder, an axial cylinder, or a sleeve as a cylindrical strength support. The base body can be formed from any suitable material. The base body can, for example, consist of plastic or metal. In a preferred embodiment, the base body consists of aluminum and / or steel. Particularly preferably, the base body is a hollow cylinder or an axial cylinder made of aluminum and / or steel.

[0013] The elastomer coating of the printing form according to the invention can have any suitable thickness. Preferably, the elastomer coating has a thickness of at least 30 µm. In a particularly preferred embodiment, the elastomer coating has a thickness in the range of 30 µm to 30 mm. The large range of 30 µm to 30 mm allows the printing form to be used multiple times without re-rubbering. To do this, an engraving is simply sanded off after use, and a new engraving is applied.

[0014] The roughness of the elastomer coating can be suitably adjusted by grinding and polishing, for example to an average roughness depth of less than 2 µm Rz. According to a preferred embodiment of the present invention, the surface of the elastomer coating has an average roughness depth of less than 1 µm Rz. The roughness ensures that an ink film allows the doctor blade to glide on the surface of the printing form during subsequent printing.

[0015] The present invention further relates to a method for producing an imaging printing form, comprising (a) providing a base body, (b) providing an elastomer coating on the base body, and (c) providing an engraving pattern on the elastomer coating by engraving, characterized in that the elastomer coating consists essentially of a hard rubber and has a hardness of greater than 70 ShoreD according to DIN ISO 7619-1, and wherein the hard rubber is a hard rubber based on butadiene-acrylonitrile rubber (NBR), carboxyl-containing nitrile rubber (XNBR), hydrogenated acrylonitrile-butadiene rubber (HNBR), or combinations thereof.

[0016] The imaging printing form produced by this process can be any suitable printing form. Preferably, the imaging printing form is a gravure cylinder or a printing plate. A gravure cylinder is particularly preferred, as it is the most commonly used printing form in commercial printing.

[0017] According to the method according to the invention, a base body is first provided (step (a)). If the printing form produced by the method according to the invention is a gravure cylinder, the base body is preferably a hollow cylinder, an axial cylinder, or a sleeve as a cylindrical strength support. The base body can be formed from any suitable material. The base body can be made of plastic or metal, for example. In a preferred embodiment, the base body is made of aluminum and / or steel. The base body is particularly preferably a hollow cylinder or an axial cylinder made of aluminum and / or steel.

[0018] In step (b) of the inventive method, an elastomer coating is provided on the base body. This can be done using conventional methods. In a preferred embodiment of the inventive method, step (b) comprises the substeps (b.1) of coating the base body with an elastomer or an elastomer mixture, (b.2) vulcanizing the elastomer or the elastomer mixture to form the hard rubber, (b.3) removing excess hard rubber by lathing, and (b.4) grinding the surface of the elastomer coating.

[0019] The coating of the base body with an elastomer or an elastomer mixture according to step (b.1) can be carried out, for example, using a calender plate that is wound around the base body. Alternatively, the elastomer or elastomer mixture can be extruded onto the base body. This can be done, for example, using a ring extruder. It is also possible to coat the base body by strip coating or by doctoring / dipping from a solution of the elastomer or elastomer mixture. The coating is carried out with a layer thickness such that the required or desired final layer thickness can be achieved after vulcanization and grinding.

[0020] The elastomer or elastomer mixture to be applied is preferably butadiene-acrylonitrile rubber (NBR), carboxyl-containing nitrile rubber (XNBR), hydrogenated acrylonitrile-butadiene rubber (HNBR) or a combination thereof.

[0021] Vulcanization of the elastomer or elastomer mixture to form the hard rubber according to step (b.2) can be carried out by any conventional method. The hard rubber is obtained by crosslinking the elastomer or elastomer mixture. Vulcanization can be carried out, for example, in an autoclave. According to a preferred embodiment, the base body coated with an elastomer or elastomer mixture can be bandaged before vulcanization. This additional step is advantageous with regard to optimized vulcanization.

[0022] The hard rubber obtained after vulcanization has a hardness greater than 70 Shore D. This hardness is determined according to DIN ISO 7619-1.

[0023] The removal of excess hard rubber by turning according to step (b.3) can also be done by any conventional method.

[0024] The surface of the elastomer coating is preferably ground using a diamond milling machine ("Polishmaster") to produce the final dimension. The elastomer coating obtained by the process according to the invention can have any suitable thickness. Preferably, the elastomer coating has a thickness of at least 30 µm after grinding. In a particularly preferred embodiment, the elastomer coating has a thickness in the range of 30 µm to 30 mm.

[0025] The roughness of the elastomer coating can also be suitably adjusted by grinding, for example to an average roughness depth of less than 2 µm Rz. According to a preferred embodiment of the present invention, the surface of the elastomer coating has an average roughness depth of less than 1 µm Rz after grinding.

[0026] It is also possible to create an additional grinding surface on the elastomer coating using, for example, two stone grinding wheels. This is advantageous because such a grinding surface later allows the printing ink to act as a lubricating film between the squeegee and the printing form. However, compared to conventional processes, this step is not absolutely necessary. Since even hard rubbers with hardnesses greater than 70 Shore D still contain elastic components, the squeegee seals, and a clean print can be achieved without additional surface grinding.

[0027] In step (c) of the method according to the invention, an engraving pattern is provided on the elastomer coating by engraving. The engraving is preferably carried out by electromechanical engraving or laser engraving.

[0028] In electromechanical engraving, a diamond stylus cuts cells into the printing form. If the printing form is a gravure cylinder, the diamond stylus cuts the cells into the rotating cylinder, with a sliding foot keeping the stylus at a constant distance from the cylinder. The arrangement and size of the cells determine the final printed image. Electromechanical engraving produces cells with a depth of approximately 45 to 55 µm, for example.

[0029] Laser engraving is particularly preferred. Laser engraving creates cells with a depth of approximately 35 to 45 µm, for example, allowing imaging speeds to be increased by up to 75% compared to electromechanical engraving.

[0030] According to a preferred embodiment, a quality control check can be performed after engraving. This check is typically performed before delivery and checks, in particular, the print quality and surface quality.

[0031] The inventive method offers a number of advantages over conventional methods for producing printing plates. In particular, the invention eliminates the need for electroplating processes, which are disadvantageous from a cost and environmental perspective. Furthermore, significantly fewer process steps are required to produce the inventive printing plate using the inventive method, since only one coating layer needs to be applied. Furthermore, the inventive method also offers the possibility of utilizing existing technology. Thus, no additional investment is required by the user.

[0032] Furthermore, the present invention relates to methods for gravure printing, comprising (a) providing the above-described image-forming printing form according to the invention, (b) applying an ink to the surface of the printing form and (c) transferring the ink from the surface of the printing form to a printable substrate.

[0033] The invention will now be explained in more detail using an embodiment. Example:

[0034] A black colored HNBR compound with the following properties was produced: Color: CA.9005 RAL Hardness: 77D Shore A Density: 1.245 g / cm 3<

[0035] The raw rubber mixture was prepared in a homogeneous form as a drawn calendered sheet with a thickness of approximately 1.2 mm and wound around a hollow aluminum cylinder. The raw rubber exhibited very little stickiness and was therefore easy to wind.

[0036] The material was then vulcanized at a temperature of 135°C for 16 hours. It was then slowly cooled to prevent spalling.

[0037] Subsequently, the workpiece was turned to a rough dimension of 143.39 mm using a turning tool. The feed rate was limited to 50 mm / min, and the surface temperature was monitored to ensure it remained within a range of 40 to 50 degrees Celsius.

[0038] The elastomer-coated aluminum hollow cylinder was then polished. This involved a two-step fine polishing to a final dimension of 143.24 mm. After fine polishing, the surface had an average roughness of less than 0.6 µm Rz.

[0039] The surface was then sanded to adjust the average surface roughness to 0.7 Rz for the ink sliding layer under squeegee.

[0040] The elastomer coating had a hardness of 82 ShoreD.

[0041] Subsequently, electromechanical engraving was performed using a 120° diamond stylus. Stylus wear was continuously monitored.

[0042] Figure 1 shows a microscope image of the engraved surface. The quality of the cutting contours / cup edges corresponded to that of a conventional printing plate with a copper coating.

[0043] The gravure cylinder produced in this way was used in a gravure printing test.

[0044] Figure 2 shows a microscope image of the resulting print.

[0045] The resulting print showed a color density of 1.7. Toning and area coverage were acceptable.

[0046] Finally, a wear test was conducted using a Moser proofing press with an MDC softblade. The print quality was acceptable up to 150,000 linear meters, compared to the required 50,000 linear meters. The gravure cylinder thus showed minimal wear.

[0047] In summary, the hard rubber coated gravure cylinder showed just as good printing results as a conventional copper coated and hard chrome plated gravure cylinder.

Claims

1. Image-providing printing template comprising a base with an elastomer coating, where the elastomer coating bears an engraved pattern, where the elastomer coating consists essentially of hard rubber and has a hardness above 70 Shore D according to DIN ISO 7619-1, characterized in that the hard rubber is a hard rubber based on butadiene-acrylonitrile rubber (NBR), on carboxylated nitrile rubber (XNBR), on hydrogenated acrylonitrile-butadiene rubber (HNBR) or combinations thereof.

2. Image-providing printing template according to Claim 1 in the form of an intaglio printing cylinder or of a printing plate.

3. Image-providing printing template according to either of Claims 1 and 2, where the base is a hollow cylinder, an axial cylinder or a sleeve as cylindrical reinforcing structure.

4. Image-providing printing template according to any of Claims 1 to 3, where the thickness of the elastomer coating is at least 30 µm.

5. Image-providing printing template according to any of Claims 1 to 4, where the average roughness depth Rz of the surface of the elastomer coating is below 1 µm.

6. Process for the production of an image-providing printing template, comprising a. the provision of a base, b. the provision of an elastomer coating on the base, and c. the provision of an engraved pattern on the elastomer coating by engraving, characterized in that the elastomer coating consists essentially of a hard rubber and has a hardness above 70 Shore D according to DIN ISO 7619-1, and wherein the hard rubber is a hard rubber based on butadiene-acrylonitrile rubber (NBR), on carboxylated nitrile rubber (XNBR), on hydrogenated acrylonitrile-butadiene rubber (HNBR) or combinations thereof.

7. Process according to Claim 6, wherein the step b. of the provision of an elastomer coating on the base comprises the following steps: b.1 the covering of the base with an elastomer or an elastomer mixture, b.2 the vulcanization of the elastomer or the elastomer mixture with formation of the hard rubber, b.3 the removal of excess hard rubber by a turning procedure, and b.4 the removal of material by grinding from the surface of the elastomer coating.

8. Process according to Claim 6 or 7, wherein the engraving is achieved by an electromechanical engraving procedure or by a laser engraving procedure.

9. Process for intaglio printing, comprising a. the provision of an image-providing printing template according to any of Claims 1 to 5, b. the application of an ink to the surface of the printing template and c. the transfer of the ink from the surface of the printing template to a printable substrate.