AQUEOUS DISPERSION FOR ACTIVATING A METAL SURFACE AND METHOD FOR PHOSPHATIZING THEREOF

DE502019012513D1Active Publication Date: 2024-12-05HENKEL KGAA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012513
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-11
Filing Date
2019-06-07
Publication Date
2024-12-05
Estimated Expiration
2039-06-07

AI Technical Summary

Technical Problem

Existing phosphating processes face challenges in achieving uniform and comprehensive activation of metal surfaces, particularly in composite structures, leading to issues with sedimentation, paint adhesion, and electrocoating performance, especially when treating materials with high aluminum content.

Method used

An aqueous dispersion containing a dispersed particulate component of polyvalent metal cations, polymeric organic compounds with styrene and maleic acid units, and a thickener, which forms stable agglomerates that prevent sedimentation and ensure uniform activation, even after dilution, with a D50 value above 10 μm and thixotropic flow behavior.

Benefits of technology

The solution provides stable and uniform activation, enhancing paint adhesion and electrocoating performance while minimizing the use of the dispersion, preventing sedimentation, and ensuring easy handling and dosing, resulting in high-quality, defect-free phosphate coatings.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to an aqueous dispersion as a concentrate for the activation stage of a phosphating process for metal surfaces, comprising a dispersed particulate component and a thickener. The particulate component contains, in addition to dispersed inorganic compounds of polyvalent metal cations, polymeric organic compounds as dispersing aids, which are at least partially composed of styrene and / or an α-olefin having no more than 5 carbon atoms, as well as maleic acid, its anhydride and / or its imide, and which additionally contain polyoxyalkylene units. The aqueous dispersion is further characterized by a D50 value above 10 µm. Furthermore, the present invention relates to a process for the corrosion-protective pretreatment of the surfaces of a metallic material, in particular for zinc phosphating.

[0002] Phosphate-forming coatings have been practiced and intensively researched for decades for applying crystalline, corrosion-protective coatings to metallic surfaces, particularly iron, zinc, and aluminum. Zinc phosphating, which is particularly well-established for corrosion protection, is applied in a layer thickness of a few micrometers and involves corrosive pickling of the metallic material in an acidic aqueous solution containing zinc ions and phosphates. During the pickling process, an alkaline diffusion layer forms on the metal surface. This layer extends into the solution. Within this layer, sparingly soluble crystallites form, precipitate directly at the interface with the metallic material, and continue to grow there.To support the pickling reaction on aluminum materials and to mask the aluminum poison, which, in dissolved form, interferes with the formation of coatings on metal materials, water-soluble compounds are often added. These compounds serve as a source of fluoride ions. Zinc phosphating always begins with the activation of the metallic surfaces of the component to be phosphated. Wet-chemical activation is conventionally carried out by bringing the components into contact with colloidal, aqueous solutions of phosphates ("activation step"), which, immobilized on the metal surface, serve as growth nuclei for the formation of the crystalline coating within the alkaline diffusion layer during the subsequent phosphating process.Suitable dispersions are colloidal, mostly neutral to alkaline, aqueous compositions based on phosphate crystallites, whose crystal structure exhibits only minor crystallographic deviations from the type of zinc phosphate layer to be deposited. In addition to titanium phosphate, often referred to in the literature as Jernstedt salt, water-insoluble bivalent and trivalent phosphates are also suitable as starting materials for preparing a colloidal solution suitable for activating a metal surface for zinc phosphating. For example, WO 98 / 39498 A1 teaches, in particular, bivalent and trivalent phosphates of the metals Zn, Fe, Mn, Ni, Co, Ca, and Al in this context, with phosphates of the metal zinc being technically preferred for activation for subsequent zinc phosphating.

[0003] Each type of layer-forming phosphating, a process sequence of activation and zinc phosphating, has its own characteristics, which are particularly important when treating components composed of a mix of different metallic materials, or when treating new types of materials. Closed crystalline zinc phosphate coatings can no longer form on steel surfaces of components activated with Jernstedt salts if the proportion of dissolved aluminum in the zinc phosphating bath exceeds a certain threshold, for example, in components with a high aluminum content, so activation according to WO 98 / 39498 A1 must be used. This type of activation also offers the advantage of producing thinner phosphate coatings on aluminum surfaces that provide better corrosion protection compared to activation with Jernstedt salts.However, activation with bi- and trivalent phosphates in zinc phosphating baths, which are also intended to form coatings on aluminum surfaces, often results in defect-rich coatings on the zinc surfaces. These coatings are characterized by the presence of loose adhesions of components of the zinc phosphate coating, which noticeably reduce the paint adhesion to the zinc surfaces in the subsequent dip coating. Furthermore, the loose phosphate adhesions are partially carried over into a subsequent dip coating process, where they are partially dissolved in the aqueous binder dispersion.Dissolved phosphates carried over into the dip coating can, on the one hand, negatively impact the deposition characteristics of the dispersed coating components and, on the other hand, reduce the effective concentration of essential catalysts / crosslinkers based on selected heavy metals through precipitation reactions. Phosphate carryover can therefore be the cause of increased baking temperatures, especially for dip coatings that contain water-soluble or water-dispersible salts of yttrium and / or bismuth in addition to the dispersed resin.

[0004] EP 1 566 466 A1 teaches the activation for a layer-forming zinc phosphate coating based on a dispersion of zinc phosphate particles with a D50 value not exceeding 3 µm, which is well suited for aluminum substrates. In one embodiment, a copolymer based on carboxyl-containing monomers and, for example, styrene is included to stabilize the dispersion.

[0005] But also in all other phosphating processes, for example in the case of zinc phosphating of composite structures, which is designed to form non-layers on the surfaces of materials made of aluminum, there is still a need, with regard to the established wet-chemical activation processes, to further stabilize the aqueous dispersions from which the application baths for activation are prepared against sedimentation or to optimize their ability to activate metal surfaces for phosphating.The latter aspect primarily involves the ability to achieve the most uniform and comprehensive activation possible of the metal surfaces to be phosphated, thus resulting in the formation of homogeneous, fine-crystalline coatings in the phosphating stage. This ensures excellent paint adhesion properties and, in turn, high electrical resistance, thus enabling a correspondingly good coverage of the paint in the subsequent electrocoating. Furthermore, sufficient activation should be achieved while minimizing the use of the complexly produced and stabilized aqueous dispersion used as the concentrate for the application bath. With regard to stabilizing such a concentrate against sedimentation, the difficulty of simply redispersing already sedimented active components after extended standing times and making them available for activation is a recurring challenge.At the same time, the concentrate must be easy to handle in terms of process technology and, in particular, after redispersion, it must be easy to pump into the activation application bath for subsequent dosing.

[0006] This complex task is surprisingly solved by combining a specific polymeric dispersing agent in the presence of a thickener. This special combination ensures the required flow behavior and the necessary stability against sedimentation through the association of the dispersed primary particles, which activate a metal surface upon contact, to form stabilized agglomerates. Furthermore, the specific dispersing agent ensures that when the concentration of the dispersion components is reduced, for example, by dilution with water, primary particles are gradually released from the agglomerates without losing their stability against sedimentation.

[0007] The present invention therefore relates in a first aspect to an aqueous dispersion having a D50 value of more than 10 µm containing (a) at least 5% by weight of a dispersed particulate component comprising (a1) at least one particulate inorganic compound of a polyvalent metal cation, and (a2) at least one polymeric organic compound which is at least partly composed of styrene and / or an α-olefin having not more than 5 carbon atoms and maleic acid, its anhydride and / or its imide and which additionally comprises polyoxyalkylene units, and (b) at least one thickener.

[0008] The dispersed particulate component (a) of the aqueous dispersion according to the present invention is the solids content remaining after drying the retentate of an ultrafiltration of a defined subvolume of the aqueous dispersion with a nominal molecular weight cut-off of 10 kD (NMWC). Ultrafiltration is carried out with the addition of deionized water (κ < 1 µScm -1< ) ​​until a conductivity of less than 10 µScm -1< is measured in the filtrate.

[0009] For the purposes of the present invention, an organic compound is polymeric if its weight-average molar mass is greater than 500 g / mol. The molar mass is determined using the molar mass distribution curve of a sample of the respective reference quantity, determined experimentally using size-exclusion chromatography with a concentration-dependent refractive index detector at 30 °C and calibrated against polyethylene glycol standards. The molar mass averages are evaluated computer-assisted using the strip method with a third-order calibration curve. Hydroxylated polymethacrylate is suitable as the column material, and an aqueous solution of 0.2 mol / L sodium chloride, 0.02 mol / L sodium hydroxide, and 6.5 mmol / L ammonium hydroxide is used as the eluent.

[0010] In its function as a concentrate for the activation stage of phosphating, the aqueous dispersion according to the invention contains a sufficient amount of particulate constituents (a), with a proportion of preferably at least 10% by weight, particularly preferably at least 15% by weight, being more advantageous in this regard. A proportion of particulate constituent (a) above 40% by weight should not be set due to the typically poorer process-technical handling of the dispersion. Therefore, the proportion of the particulate fraction is particularly preferably not more than 30% by weight. Quantitative data regarding the composition of the aqueous dispersion according to the invention always refer to the dispersion as a reference quantity within the scope of the present invention, unless another reference quantity is explicitly specified.

[0011] Typically, the use of polyvalent metal cations in the form of phosphates, which are present in the particulate constituent (a) in a correspondingly high proportion for activation, is preferred for the activation. Accordingly, the at least one particulate inorganic compound (a1) of the dispersed particulate constituent (a) is preferably composed at least partially of phosphates. The proportion of these phosphates, based on the dispersed inorganic particulate constituent, calculated as PO4, is preferably at least 25% by weight, more preferably at least 35% by weight, especially preferably at least 40% by weight, and most preferably at least 45% by weight.The inorganic particulate component of the aqueous dispersion is the one that remains when the particulate component (a) obtained from drying the ultrafiltration retentate is pyrolyzed in a reaction furnace at 900 °C without the addition of catalysts or other additives while supplying a CO2-free oxygen stream until an infrared sensor in the reaction furnace outlet delivers a signal identical to that of the CO2-free carrier gas (blank value). The phosphates contained in the inorganic particulate component are determined as phosphorus content directly from the acid digestion using atomic emission spectrometry (ICP-OES) after acid digestion of the same with an aqueous 10 wt.% HNO3 solution at 25 °C for 15 min.

[0012] The active components of the aqueous dispersion, which effectively promote the formation of a continuous phosphate coating on the metal surfaces and, in this sense, activate the metal surfaces, are, as already mentioned, preferably composed primarily of phosphates, which in turn, for the formation of fine-crystalline coatings, preferably comprise at least partially hopeite, phosphophyllite, scholzite, and / or hureaulite, particularly preferably at least partially hopeite, phosphophyllite, and / or scholzite, particularly preferably at least partially hopeite and / or phosphophyllite, and very particularly preferably at least partially hopeite. A preferred activation within the meaning of the present invention is therefore based essentially on the phosphates in particulate form contained in the aqueous dispersion according to the invention.The phosphates hopeite, phosphophyllite, scholzite, and / or hureaulite can be dispersed into an aqueous solution as component (a1) to provide the aqueous dispersion according to the invention as finely ground powders or as a powder paste ground with the polymeric organic compound (a2) as a dispersing aid. Hopeites stoichiometrically comprise, without taking into account water of crystallization, Zn 3 (PO 4 ) 2 and the nickel- and manganese-containing variants Zn 2 Mn(PO 4 ) 3 , Zn 2 Ni(PO 4 ) 3 , whereas phosphophyllite consists of Zn 2 Fe(PO 4 ) 3 , scholzite of Zn 2 Ca(PO 4 ) 3 , and hureaulite of Mn 3 (PO 4 ) 2 .The existence of the crystalline phases hopeite, phosphophyllite, scholzite and / or hureaulite in the aqueous dispersion according to the invention can be detected by X-ray diffraction methods (XRD) after separation of the particulate component (a) by ultrafiltration with a nominal exclusion limit of 10 kD (NMWC, Nominal Molecular Weight Cut Off) as described above and drying of the retentate to constant mass at 105°C.

[0013] Due to the preference for the presence of phosphates which comprise zinc ions and have a certain crystallinity, it is preferred for the formation of firmly adhering crystalline zinc phosphate coatings after activation if the aqueous dispersion according to the invention contains at least 20% by weight, preferably at least 30% by weight, particularly preferably at least 40% by weight of zinc in the inorganic particulate component of the aqueous dispersion, based on the phosphate content of the inorganic particulate component, calculated as PO 4 .

[0014] However, activation within the meaning of the present invention should preferably not be achieved using colloidal solutions of titanium phosphates, since otherwise the layer-forming zinc phosphating on iron, especially steel, cannot be reliably achieved. In a preferred embodiment of the process according to the invention, the proportion of titanium in the inorganic particulate component of the aqueous dispersion is therefore less than 0.1 wt. %, particularly preferably less than 0.01 wt. %, based on the aqueous dispersion. In a particularly preferred embodiment, the aqueous dispersion of the activation contains a total of less than 10 mg / kg, particularly preferably less than 1 mg / kg, of titanium.

[0015] Due to the excellent dispersing properties of the polymeric organic compounds (a2), it is also advantageous that a high proportion of inorganic particulate constituent can be achieved, which is essential for the activation of the metal surfaces. In the aqueous dispersion, a proportion of the dispersed inorganic particulate constituent of preferably at least 60 wt. %, particularly preferably at least 80 wt. %, based on the amount of dispersed particulate constituent (a), can be successfully adjusted.

[0016] The aqueous dispersion according to the invention is characterized by a D50 value of more than 10 µm. The agglomerates of the dispersed particles contained in the dispersion determine the thixotropic flow properties, which are favorable for its handling. The tendency of the agglomerates to be highly viscous at low shear promotes their high storage stability, while the loss of viscosity under shear determines their pumpability. Favorable flow properties are also obtained if the dispersion does not significantly exceed a D90 value of 150 µm, so that according to the invention, a D90 value of the aqueous dispersion of less than 150 µm, preferably less than 100 µm, in particular less than 80 µm, is preferred.

[0017] In the context of the present invention, the D50 value or the D90 value refers to the particle diameter which 50 vol.% or 90 vol.% of the particulate components contained in the aqueous dispersion do not exceed.

[0018] The D50 or D90 value can be determined according to ISO 13320:2009 by means of light scattering analysis according to the Mie theory from volume-weighted cumulative particle size distributions immediately after dilution of the dispersion to a dispersed particulate content of 0.05 wt.% with an appropriate amount of deionized water (κ < 1 µScm -1< ) ​​at 20 °C, assuming spherical particles and a refractive index of the scattering particles of n o = 1.52 - i 0.1. The dilution is carried out by adding an appropriate amount of the dispersion to a volume of 200 ml of deionized water into the sample vessel of the LA-950 V2 particle size analyzer from Horiba Ltd. added and mechanically circulated into the measuring chamber (setting of the circulation pump on the LA-950 V2: level 5 = 1167 rpm for a volume flow of 3.3 liters / minute).The particle size distribution is measured within 120 seconds after the dispersion is added to the dilution volume.

[0019] The particulate constituent (a) present in the aqueous dispersion according to the invention is present at least partially in agglomerates having particle sizes above 10 µm. The agglomerates themselves are in turn composed of primary particles, so that the aqueous dispersions according to the invention preferably have a bimodal particle size distribution and particularly preferably a distribution maximum at a particle size below 1 µm and another at a particle size above 10 µm. A bimodal particle size distribution exists when the volume-weighted particle size distribution curve has at least two separate distribution maxima, preferably such that the ratio of the intensities in the distribution maxima to the intensity in the distribution minimum lying between the distribution maxima is in each case greater than 2.

[0020] The polymeric organic compounds (a2) used as dispersing agents, which contain polyoxyalkylene units, are, for the purposes of the present invention, composed at least partially of styrene and / or an α-olefin having no more than 5 carbon atoms, and maleic acid, its anhydride, and / or its imide. The α-olefin is preferably selected from ethene, 1-propene, 1-butene, isobutylene, 1-pentene, 2-methylbut-1-ene, and / or 3-methylbut-1-ene, and particularly preferably selected from isobutylene. It is clear to the person skilled in the art that the polymeric organic compounds (a2) contain these monomers as structural units covalently linked to one another or to other structural units in unsaturated form.Suitable commercially available representatives include, for example, Dispex® CX 4320 (BASF SE), a maleic acid-isobutylene copolymer modified with polypropylene glycol, Tego® Dispers 752 W (Evonik Industries AG), a maleic acid-styrene copolymer modified with polyethylene glycol, or Edaplan® 490 (Münzing Chemie GmbH), a maleic acid-styrene copolymer modified with EO / PO and imidazole units. In the context of the present invention, preference is given to those polymeric organic compounds (a2) that are composed at least partially of styrene.

[0021] The polymeric organic compounds (a2) used as dispersing agents contain polyoxyalkylene units, which are preferably composed of 1,2-ethanediol and / or 1,2-propanediol, particularly preferably both 1,2-ethanediol and 1,2-propanediol, wherein the proportion of 1,2-propanediols in the totality of the polyoxyalkylene units is preferably at least 15 wt. %, but particularly preferably not exceeding 40 wt. %, based on the totality of the polyoxyalkylene units. Furthermore, the polyoxyalkylene units are preferably present in the side chains of the polymeric organic compounds (a2). A proportion of polyoxyalkylene units in the totality of the polymeric organic compounds (a2) of preferably at least 40 wt. %, particularly preferably at least 50 wt. %, but preferably not more than 70 wt. % is advantageous for the dispersibility.

[0022] For the anchoring of the dispersing aid with the inorganic particulate constituent of the aqueous dispersion, which in a preferred embodiment is formed at least partially by polyvalent metal cations in the form of phosphates, the organic polymeric compounds (a2) additionally also have imidazole units, preferably in such a way that the polyoxyalkylene units of the polymeric organic compounds (a2) are at least partially end-capped with an imidazole group, so that in the preferred embodiment terminal imidazole groups are present in the polyoxyalkylene side chain, wherein the covalent linkage of the polyoxyalkylene units with the imidazole group preferably takes place via a nitrogen atom of the heterocycle.In a preferred embodiment, the amine number of the organic polymeric compounds (a2) is at least 25 mg KOH / g, more preferably at least 40 mg KOH / g, but preferably less than 125 mg KOH / g, particularly preferably less than 80 mg KOH / g, so that in a preferred embodiment, the totality of the polymeric organic compounds in the particulate constituent (a) also has these preferred amine numbers. The amine number is determined in each case based on a weight of approximately 1 g of the respective reference quantity—organic polymeric compounds (a2) or totality of the polymeric organic compounds in the particulate constituent—in 100 ml of ethanol, titrating with 0.1 N HCl standard solution against the indicator bromophenol blue until the color changes to yellow at an ethanolic solution temperature of 20 °C.The amount of standard HCl solution used in milliliters multiplied by the factor 5.61 divided by the exact mass of the sample in grams corresponds to the amine number in milligrams of KOH per gram of the respective reference quantity.

[0023] The presence of maleic acid, provided it is a component of the organic polymeric compound (a2) as a free acid and not in the form of the anhydride or imide, can impart increased water solubility of the dispersing agent, particularly in the alkaline range. It is therefore preferred that the polymeric organic compounds (a2), preferably also the totality of the polymeric organic compounds in the particulate component (a), have an acid number according to DGF CV 2 (06) (as of April 2018) of at least 25 mg KOH / g, but preferably less than 100 mg KOH / g, particularly preferably less than 70 mg KOH / g, in order to ensure a sufficient number of polyoxyalkylene units.Furthermore, it is preferred if the polymeric organic compounds (a2), preferably also the totality of the polymeric organic compounds in the particulate constituent (a), have a hydroxyl number of less than 15 mg KOH / g, particularly preferably less than 12 mg KOH / g, especially preferably less than 10 mg KOH / g, in each case determined according to method A of 01 / 2008:20503 from European Pharmacopoeia 9.0.

[0024] For sufficient dispersion of the inorganic particulate constituents of the dispersion, it is sufficient if the proportion of the polymeric organic compounds (a2), preferably the totality of the polymeric organic compounds in the particulate constituent (a), based on the particulate constituent (a), is at least 3 wt.%, particularly preferably at least 6 wt.%, but preferably does not exceed 15 wt.%.

[0025] The presence of a thickener according to component (b), in combination with its particulate constituent, imparts the desired, previously mentioned flow behavior to the aqueous dispersion and prevents the irreversible formation of agglomerates in the particulate constituent from which primary particles can no longer be dissolved. According to the invention, the addition of the thickener makes it possible to obtain preferred aqueous dispersions according to the invention which, in the shear rate range from 0.001 to 0.25 reciprocal seconds, have a maximum dynamic viscosity at a temperature of 25°C of at least 1000 Pa s, but preferably below 5000 Pa s, and preferably exhibit shear-thinning behavior at shear rates above that present at the maximum dynamic viscosity at 25°C, i.e. a decrease in viscosity with increasing shear rate, so that the aqueous dispersion as a whole exhibits thixotropic flow behavior.The viscosity over the specified shear rate range can be determined using a plate / cone viscometer with a cone diameter of 35 mm and a gap width of 0.047 mm.

[0026] A thickener according to component (b) according to the present invention is a polymeric chemical compound or a defined mixture of chemical compounds which, as a 0.5 wt. % constituent in deionized water (κ < 1 µScm -1< ) ​​at a temperature of 25 °C, has a Brookfield viscosity of at least 100 mPa s at a shear rate of 60 rpm (= rounds per minute) using a size 2 spindle. When determining this thickening property, the mixture with water is to be prepared in such a way that the appropriate amount of the polymeric chemical compound is added to the water phase with stirring at 25 °C. The homogenized mixture is then freed of air bubbles in an ultrasonic bath and left to stand for 24 hours. The measured viscosity value is then read immediately within 5 seconds after applying a shear rate of 60 rpm using spindle number 2.

[0027] To provide a D50 value of more than 10 µm and the associated advantageous thixotropic flow behavior, an aqueous dispersion according to the invention preferably contains a total of at least 0.5 wt. %, but preferably not more than 4 wt. %, particularly preferably not more than 3 wt. %, of one or more thickeners according to component (b), wherein the total proportion of polymeric organic compounds in the non-particulate constituent of the dispersion according to the invention preferably does not exceed 4 wt. % (based on the dispersion). The non-particulate constituent is the solids content of the dispersion according to the invention in the permeate of the ultrafiltration described above after drying to constant mass at 105°C – i.e., the solids content after separation of the particulate constituent by ultrafiltration.

[0028] Certain polymeric compound classes are particularly suitable thickeners according to component (b) of the first aspect of the present invention and are also readily available commercially.Thus, the thickener according to component (b) is first preferably selected from polymeric organic compounds, which in turn are preferably selected from polysaccharides, cellulose derivatives, aminoplasts, polyvinyl alcohols, polyvinylpyrrolidones, polyurethanes and / or urea urethane resins, and particularly preferably from urea urethane resins, which in combination with the dispersed components associate in such a way that even small amounts of such a thickener are sufficient to form stable agglomerates in the dispersion, which bring about the desired D50 value of more than 10µm and also cause the previously described preferred thixotropic flow behavior, so that the dispersion has both a high storage life and excellent pumpability, which plays an important role in terms of process technology when metering in the dispersion to further sharpen the activation stage.

[0029] A urea urethane resin as a thickener according to component (b) of the present invention is a mixture of polymeric compounds resulting from the reaction of a polyfunctional isocyanate with a polyol and a mono- and / or diamine. In a preferred embodiment, the urea urethane resin is derived from a polyfunctional isocyanate, preferably selected from 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, 2,2(4),4-trimethyl-1,6-hexamethylene diisocyanate, 1,10-decamethylene diisocyanate, 1,4-cyclohexylene diisocyanate, p-phenylene diisocyanate, m-phenylene diisocyanate, 2,6-toluene diisocyanate, 2,4-toluene diisocyanate and mixtures thereof, p- and m-xylylene diisocyanate, and 4-4'-diisocyanatodicyclohexylmethane, particularly preferably selected from 2,4-toluene diisocyanate and / or m-xylylene diisocyanate.In a preferred embodiment, the urea urethane resin is derived from a polyol selected from polyoxyalkylene diols, particularly preferably from polyoxyethylene glycols, which in turn are preferably composed of at least 6, particularly preferably at least 8, especially preferably at least 10, but preferably less than 26, particularly preferably less than 23 oxyalkylene units.

[0030] Particularly suitable and therefore preferred urea urethane resins according to the invention are obtainable by a first reaction of a diisocyanate, for example, toluene-2,4-diisocyanate, with a polyol, for example, a polyethylene glycol, to form NCO-terminated urethane prepolymers, followed by further reaction with a primary monoamine and / or with a primary diamine, for example, m-xylylenediamine. Urea urethane resins that contain neither free nor blocked isocyanate groups are particularly preferred.As a component of alkaline, aqueous dispersions according to the invention, such urea urethane resins promote the formation of loose agglomerates of primary particles and thus both the preferred thixotropic flow behavior and the provision of dispersions exhibiting the advantageous bimodal particle size distribution according to the invention. However, the agglomerates are stabilized in the aqueous phase and protected against further agglomeration to such an extent that sedimentation of the particulate constituent is largely prevented. To further promote this property profile, urea urethane resins that contain neither free or blocked isocyanate groups nor terminal amine groups are preferably used as component (b).In a preferred embodiment, the thickener according to component (b), which is a urea urethane resin, therefore has an amine number of less than 8 mg KOH / g, more preferably less than 5 mg KOH / g, especially preferably less than 2 mg KOH / g, in each case determined by the method as described above for the organic polymeric compound a2). Since the thickener is essentially dissolved in the aqueous phase and can thus be assigned to the non-particulate constituent of the aqueous dispersion, while component (a2) is essentially bound in the particulate constituent, an aqueous dispersion is accordingly preferred in which the totality of the polymeric organic compounds in the non-particulate constituent preferably has an amine number of less than 16 mg KOH / g, more preferably less than 10 mg KOH / g, especially preferably less than 4 mg KOH / g.Furthermore, it is preferred that the urea urethane resin has a hydroxyl number in the range of 10 to 100 mg KOH / g, particularly preferably in the range of 20 to 60 mg KOH / g, determined according to Method A of 01 / 2008:20503 from European Pharmacopoeia 9.0. With regard to the molecular weight, a weight-average molar mass of the urea urethane resin in the range of 1000 to 10,000 g / mol, preferably in the range of 2000 to 6000 g / mol, is advantageous according to the invention and therefore preferred, in each case determined experimentally as described above in connection with the inventive definition of a polymeric compound.

[0031] The pH of the dispersion, without the addition of auxiliaries, is typically in the range of 6.0 - 9.0, and such a pH range is therefore preferred according to the invention. However, for compatibility with the actual, and usually alkaline-adjusted, colloidal aqueous solution in the activation stage, it is advantageous if the pH of the aqueous dispersion, optionally also by adding alkaline-reacting compounds, is above 7.2, particularly preferably above 8.0. The alkalinity of the aqueous dispersion according to the invention is ideally limited, since some polyvalent metal cations have amphoteric character and can therefore be dissolved out of the particulate constituent at higher pH values, so that the pH of the aqueous dispersion is preferably below 10 and particularly preferably below 9.0.The "pH value" as used in the present invention corresponds to the negative decimal logarithm of the hydronium ion activity at 20 °C and can be determined using pH-sensitive glass electrodes.

[0032] A previously described aqueous dispersion according to the invention is preferably obtainable by i) Providing a pigment paste by grinding 10 parts by mass of a particulate inorganic compound (a1) with 0.5 to 2 parts by mass of the polymeric organic compound (a2) in the presence of 4 to 7 parts by mass of water and grinding until a D90 value of less than 5 µm is achieved; ii) Diluting the pigment paste with such an amount of water and a thickener (b) that a dispersed particulate component (a) of at least 5 wt.% and a maximum dynamic viscosity of at least 1000 Pa s at a temperature of 25 °C in the shear rate range of 0.001 to 0.25 reciprocal seconds is achieved; and iii) Adjusting a pH value in the range of 7.2 to 10.0 with the aid of an alkaline compound, wherein preferred embodiments of the dispersion are obtained in an analogous manner by selecting corresponding components (a1), (a2) and (b) in the amount possibly provided or required in each case.

[0033] The aqueous dispersion according to the invention may additionally contain auxiliaries, for example selected from preservatives, wetting agents, and defoamers, which are present in the amount required for the respective function. The proportion of auxiliaries, particularly preferably of other compounds in the non-particulate component that are not thickeners or alkaline-reacting compounds, is preferably less than 1 wt.%. In the context of the present invention, an alkaline-reacting compound is water-soluble (water solubility: at least 10 g per kilogram of water with κ < 1 µScm -1< ) ​​and has a pK B value for the first protonation stage above 8.0.

[0034] In a further, second aspect, the present invention relates to a process for corrosion-protective pretreatment based on phosphating, incorporating an aqueous dispersion according to the first aspect of the present invention. The process according to this second aspect relates to the corrosion-protective pretreatment of a metallic material selected from zinc, iron, or aluminum, or of a component composed at least partially of such metallic materials, in which the metallic material or the component is first subjected to activation (i) and then to phosphating (ii) in successive process steps, wherein the activation in process step (i) is effected by bringing the metallic material, or at least one metallic material of the component, into contact with a colloidal, aqueous solution that is available as a by a factor of 20 to 100.000 diluted aqueous dispersion according to the first aspect of the present invention.

[0035] For sufficient activation of all metallic materials selected from zinc, aluminum, and iron, the proportion of the particulate component of the colloidal, aqueous solution should be adjusted accordingly. The aqueous dispersion according to the first aspect of the present invention is characterized precisely in that a relatively low proportion of inorganic particulate components in the colloidal, aqueous solution of the activation stage is required for activation of the metal surfaces, in particular a relatively low proportion of phosphates in the inorganic particulate component.Therefore, in the context of the second aspect of the present invention, a process is preferred in which the proportion of the inorganic particulate constituent, based on the colloidal, aqueous solution of the activation stage in process step (i), is at least 5 mg / kg, preferably at least 20 mg / kg, particularly preferably at least 50 mg / kg, preferably in each case as the proportion of phosphates in the inorganic particulate constituent calculated as PO4 and based on the colloidal, aqueous solution. For economic reasons and for reproducible coating results, activation should be carried out with colloidal, aqueous solutions that are as dilute as possible.It is therefore preferred that the proportion of the inorganic particulate component relative to the colloidal, aqueous solution of the activation stage is less than 0.5 g / kg, particularly preferably less than 0.4 g / kg, especially preferably less than 0.3 g / kg, preferably in each case as the proportion of phosphates in the inorganic particulate component calculated as PO 4 and relative to the colloidal, aqueous solution.

[0036] The particulate constituents of the colloidal aqueous solution of the activation stage in the second aspect of the present invention are determined in an analogous manner to those of the aqueous dispersion according to the first aspect of the present invention and are therefore also defined analogously.

[0037] When, in the context of the second aspect of the present invention, reference is made to the treatment of a metallic material selected from zinc, iron, or aluminum, this includes all materials that contain more than 50 at.% of the respective element. Corrosion-protective pretreatment always affects the surfaces of the material or component. The material can be a uniform material or a coating. Thus, according to the invention, galvanized steel grades consist of both steel and zinc, whereby iron surfaces can be exposed at the cut edges and grinding points, for example of an automobile body made of galvanized steel, and according to the invention, the iron material is then pretreated.

[0038] The components treated according to the second aspect of the present invention can be any spatial structures of any shape and design that originate from a manufacturing process, in particular also semi-finished products such as strips, sheets, rods, pipes, etc. and composite structures assembled from the aforementioned semi-finished products, wherein the semi-finished products are preferably connected to one another by gluing, welding and / or flanging to form the composite structure.

[0039] A rinsing step may be performed between activation and phosphating to reduce the carryover of alkaline components into the usually acidic phosphating process. However, a rinsing step is preferably avoided to fully maintain the activation performance. A rinsing step serves exclusively to completely or partially remove soluble residues, particles, and active components that are carried over from a previous wet-chemical treatment step from the component to be treated. This step does not require the rinsing fluid itself to contain active components based on metallic or semi-metallic elements, which are consumed simply by bringing the metallic surfaces of the component into contact with the rinsing fluid.The rinsing liquid can be simply town water or deionized water or, if necessary, a rinsing liquid that contains surface-active compounds to improve wettability with the rinsing liquid.

[0040] For layer-forming phosphating and the formation of semi-crystalline coatings, which are the targets of the activation of the metallic materials, it is preferred that the phosphating in process step (ii) be carried out by contacting the surfaces with an acidic aqueous composition containing 5-50 g / kg of phosphates dissolved in water, calculated as PO4, and preferably additionally containing at least one source of free fluoride. According to the invention, the amount of phosphate ions comprises the orthophosphoric acid and the anions of the salts of orthophosphoric acid dissolved in water, calculated as PO4.

[0041] In a particular embodiment of the second aspect of the present invention, the subsequent phosphating is a zinc phosphating and the phosphating in process step (ii) is based on an acidic aqueous composition containing 0.3 - 3 g / kg of zinc ions, preferably on an acidic aqueous composition containing 5 - 50 g / l of phosphate ions, 0.3 - 3 g / l of zinc ions and an amount of free fluoride.

[0042] A source of free fluoride ions is essential for the layer-forming zinc phosphating process, as the desired layer formation is achieved on all metallic materials selected from zinc, iron, or aluminum. This is necessary, for example, in the zinc phosphating of automobile bodies that are at least partially made of aluminum. If all surfaces of the metallic materials of a component are to be coated with a phosphate coating, the amount of particulate components in the activation process often needs to be adjusted to the amount of free fluoride required for layer formation in the zinc phosphating process.In a process according to the second aspect based on activation followed by zinc phosphating, in which the components to be pretreated are made of metallic materials of zinc and iron, in particular steel, it is advantageous for a continuous and defect-free phosphate coating if the amount of free fluoride in the acidic aqueous composition is at least 0.5 mmol / kg. If the component is additionally made of the metallic material aluminum and its surfaces are also to be provided with a continuous phosphate coating, it is further preferred in the process according to the second aspect of the invention that the amount of free fluoride in the acidic aqueous composition is at least 2 mmol / kg.The concentration of free fluoride should not exceed values ​​above which the phosphate coatings predominantly exhibit adhesions that are easily wiped off, since these cannot be avoided even by a disproportionately increased amount of particulate components in the colloidal, aqueous solution of the activation. Therefore, it is also advantageous for economic reasons and therefore preferred if, in the process according to the second aspect of the present invention based on activation followed by zinc phosphating, the concentration of free fluoride in the acidic aqueous composition of the zinc phosphating is below 15 mmol / kg, particularly preferably below 10 mmol / kg, and especially preferably below 8 mmol / kg.

[0043] The amount of free fluoride is to be determined potentiometrically at 20 °C in the respective acidic aqueous composition after calibration with fluoride-containing buffer solutions without pH buffering using a fluoride-sensitive measuring electrode. Suitable sources of free fluoride are hydrofluoric acid and its water-soluble salts, such as ammonium bifluoride and sodium fluoride, as well as complex fluorides of the elements Zr, Ti and / or Si, in particular complex fluorides of the element Si. Preferably, the source of free fluoride in a phosphating according to the second aspect of the present invention is therefore selected from hydrofluoric acid and its water-soluble salts and / or complex fluorides of the elements Zr, Ti and / or Si. Salts of hydrofluoric acid are water-soluble within the meaning of the present invention if their solubility in deionized water (κ < 1 µScm -1< ) ​​at 60 °C is at least 1 g / L calculated as F.

[0044] To suppress so-called speck formation on the surfaces of metallic materials made of zinc, it is preferred, within the scope of the second aspect of the present invention and in a constellation in which activation is followed by zinc phosphating, if the source of free fluoride is at least partially selected from complex fluorides of the element Si, in particular from hexafluorosilicic acid and its salts. In phosphating, those skilled in the art understand speck formation to be the phenomenon of the local deposition of amorphous, white zinc phosphate in an otherwise crystalline phosphate layer on the treated zinc surfaces or on the treated galvanized or alloy-galvanized steel surfaces. The speck formation is caused by a locally increased pickling rate of the substrate.Such point defects in the phosphating process can be the starting point for the corrosive delamination of subsequently applied organic coating systems, so that the occurrence of specks can be largely avoided in practice. In this context, it is preferred if the concentration of silicon dissolved in water in the acidic aqueous composition of the zinc phosphating process in process step (ii) is at least 0.5 mmol / kg, more preferably at least 1 mmol / kg, especially preferably at least 2 mmol / kg, but preferably less than 15 mmol / kg, more preferably less than 12 mmol / kg, especially preferably less than 10 mmol / kg, and most preferably less than 8 mmol / kg.The upper limits for the silicon concentration are preferred, as above these values, phosphate coatings are favored, which predominantly exhibit loose adhesions, which cannot be avoided even by a disproportionately increased amount of particulate components in the colloidal aqueous solution of the activation stage. The concentration of silicon in the acidic aqueous composition, dissolved in water, is to be determined in the filtrate of a membrane filtration of the acidic aqueous composition, which was carried out using a membrane with a nominal pore size of 0.2 µm, using atomic emission spectrometry (ICP-OES).

[0045] With regard to the interplay between activation and zinc phosphating, it has been found that the proportion of particulate components contributing to activation must be adjusted to the amount of free fluoride and silicon in the zinc phosphating process to ensure that the higher levels of free fluoride present in the phosphating bath during layer-forming phosphating on components containing aluminum as the metallic material do not adversely affect layer formation. This is particularly important for consistent phosphate coating quality when pretreating a large number of components. The aqueous dispersion according to the first aspect of the present invention has a particularly supportive effect on the formation of defect-free zinc phosphate coatings.

[0046] In this sense, a method according to the second aspect of the present invention is preferred, in which a series of components is to be pretreated, which comprises components which are at least partially made of the materials zinc and aluminum, in which the components of the series are successively subjected in successive process steps, first to activation (i) and then to phosphating (ii), wherein the activation in process step (i) is carried out by bringing the component into contact with a colloidal, aqueous solution which is obtainable as an aqueous dispersion diluted by a factor of 20 to 100,000 according to the first aspect of the present invention, the dispersed particulate component (a) of which is at least partially composed of phosphates, and the phosphating in process step (ii) is carried out by bringing the component into contact with an acidic aqueous composition containing (a) 5-50 g / l of phosphate ions, (b) 0.3-3 g / l of zinc ions, and (c) at least one source of free fluoride, where the quotient of the concentration of phosphates in the inorganic particulate component of the colloidal aqueous solution of the activation in mmol / kg related to PO 4 to the sum of the concentration of free fluoride and the concentration of silicon in the acidic aqueous composition of the zinc phosphating and in each case in mmol / kg is greater than 0.2, preferably greater than 0.3, particularly preferably greater than 0.4.

[0047] The concentration of phosphates contained in the inorganic particulate component of the colloidal aqueous solution can be determined as phosphorus content directly from the acid digestion by means of atomic emission spectrometry (ICP-OES) after acid digestion of the same with aqueous 10 wt% HNO 3 solution at 25 °C for 15 min.

[0048] Typically, auxiliaries are added to the colloidal, aqueous solution to ensure the stability of the inorganic particulate constituent dispersed therein. Particularly when the colloidal, aqueous solution is obtained by diluting an aqueous dispersion according to the first aspect of the present invention, the inorganic particulate constituent of which is at least partially composed of phosphates, it is preferred if water-soluble phosphates, in particular pyrophosphates, are additionally present in the colloidal, aqueous solution of activation and are added, preferably in an amount of at least 5 mg / kg, particularly preferably at least 20 mg / kg, especially preferably at least 50 mg / kg, but preferably not more than 500 mg / kg, particularly preferably not more than 200 mg / kg. The non-particulate constituent of the colloidal, aqueous solution is determined orseparated as that of the aqueous dispersion according to the first aspect of the present invention.

[0049] Furthermore, complexing agents can be added to the colloidal aqueous solution of activation (i) in the process according to the second aspect of the present invention to stabilize the polyvalent metal cations dissolved in the aqueous phase, which are in chemical equilibrium with the particulate phosphate fraction. Particularly advantageous is the addition of α-hydroxycarboxylic acids such as gluconic acid, citric acid, tartaric acid, tartronic acid, glycolic acid, lactic acid, and / or organic phosphonic acids such as aminotrimethylenephosphonic acid, diethylenetriaminepenta(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or 1-hydroxyethane-(1,1-diphosphonic acid).

[0050] The addition of 1-hydroxyethane-(1,1-diphosphonic acid) as a complexing agent has proven particularly effective in this context.

[0051] The colloidal aqueous solution in the activation (i) of the process according to the second aspect of the present invention preferably has an alkaline pH, particularly preferably a pH above 8.0, especially preferably above 9.0, but preferably below 11.0, wherein compounds influencing the pH such as phosphoric acid, sodium hydroxide solution, ammonium hydroxide or ammonia can be used to adjust it.

[0052] A series of corrosion protection treatments of components occurs when a large number of components are brought into contact with the treatment solution provided in the respective treatment steps and usually stored in system tanks. The contacting of the individual components takes place one after the other and thus at different times. The system tank is the container containing the pretreatment solution for the purpose of the series corrosion protection treatment.

[0053] Insofar as zinc phosphating is the focus of process step (ii) within the scope of the second aspect of the present invention, the preferred pH of the acidic aqueous composition bringing about the zinc phosphating is above 2.5, particularly preferably above 2.7, but preferably below 3.5, particularly preferably below 3.3. The proportion of free acid in points in the acidic aqueous composition of the zinc phosphating in process step (ii) is preferably at least 0.4, but preferably not more than 3.0, particularly preferably not more than 2.0. The proportion of free acid in points is determined by diluting 10 ml of sample volume of the acidic aqueous composition to 50 ml and titrating it with 0.1 N sodium hydroxide solution to a pH of 3.6. The consumption in ml of sodium hydroxide solution indicates the number of points of free acid.

[0054] The usual additives for zinc phosphating can also be carried out analogously within the scope of the second aspect of the present invention, so that the acidic aqueous composition can contain the usual accelerators such as hydrogen peroxide, nitrite, hydroxylamine, nitroguanidine, and / or N-methylmorpholine N-oxide, as well as cations of the metals manganese, calcium, and / or iron in the form of water-soluble salts, which exert a positive influence on layer formation. In an embodiment preferred for environmental hygiene reasons, a total of less than 10 ppm of nickel and / or cobalt ions are contained in the acidic aqueous composition for zinc phosphating in process step (ii).

[0055] The process according to the invention creates a good paint adhesion primer for subsequent dip coating, during which a substantially organic topcoat is applied. Accordingly, in a preferred embodiment of the process according to the invention, the zinc phosphating, with or without an intermediate rinsing and / or drying step, but preferably with a rinsing step but without a drying step, is followed by dip coating, particularly preferably electrocoating, especially preferably cathodic electrocoating, which preferably contains, in addition to the dispersed resin, which preferably comprises an amine-modified polyepoxide, water-soluble or water-dispersible salts of yttrium and / or bismuth. Examples of implementation:

[0056] The properties of a dispersion according to the invention with regard to stability, flow behavior and suitability for activation in a zinc phosphating process are described below. Production of the pigment paste

[0057] To prepare a pigment paste for providing a dispersion according to the invention, 15 parts by mass of Edaplan®< 490 (Münzing Chemie GmbH) were predispersed as a dispersing agent in 25 parts by mass of demineralized water (κ < 1 µScm -1< ) ​​and then mixed with 60 parts by mass of zinc phosphate of quality grade PZ 20. This phase was transferred to a Dyno®< -Mill type KDL ball mill, and the zinc phosphate particles were continuously ground for two hours (grinding parameters: 75% bead fill level, 2000 revolutions per minute, 20 L volume flow per hour, 40-45 °C milling temperature). This resulted in an average particle size of approximately 0.35 µm, determined using a Malvern Zetasizer Nano ZS. Based on the dispersing aids to be used according to the invention, here Edaplan ®< 490, an optimal primary particle size for activation can be achieved with a usual acceptable mechanical or time expenditure. Preparation of the dispersion according to the invention

[0058] Subsequently, 2.5 parts by mass of a urea-urethane resin solution containing 40 wt.% of the resin based on an amine-modified prepolymer of TDI / XDI and PEG-16 (amine number < 1 mg KOH / g; hydroxyl number approx. 40 mg KOH / g) were initially introduced as a thickener in approx. 64 parts by mass of deionized water (κ < 1 µScm -1< ), homogenized, and adjusted to pH 9 with 10% sodium hydroxide solution. Approx. 33 parts by mass of the pigment paste were then added with stirring, adjusted to pH 9 with 1 wt.% NaOH solution, and stirred until completely homogenized. A sample of the inventive dispersion prepared in this way was analyzed by laser diffraction according to ISO 13320:2009 as stated in the description.For this purpose, 110 mg of the dispersion was added to 200 ml of deionized water (κ < 1 µScm -1< ). The resulting sample volume was transferred to the Retsch Horiba LA-950 particle analyzer. After 60 seconds, the particle size distribution curve in the sample volume was determined using laser diffraction. After evaluation as described in the description, a D50 value of 29 µm (D10 value: 0.4 µm; D90 value: 57 µm) was obtained.

[0059] The dispersion according to the invention possesses pronounced thixotropic flow behavior with a viscosity maximum of 2200 Pas at a shear rate of 0.002 s -1< and a dynamic viscosity below 100 Pas at a shear rate of 0.1 s -1<, each determined at 25 °C using a plate / cone viscometer with a cone diameter of 35 mm and a gap width of 0.047 mm. This is advantageous for preventing sedimentation during storage of the dispersion and also facilitates pumpability and thus the preparation and refilling of activation baths in zinc phosphating. Preparation of an activation solution for a zinc phosphating according to the invention

[0060] Five liters of demineralized water (κ < 1µScm -1< ) ​​were placed in a 5L beaker. 3 grams of an additive solution containing 20.4 wt% potassium pyrophosphate and 28 wt% potassium phosphate were added. The pH was adjusted to 10.5 with phosphoric acid while stirring. 10 grams of the dispersion according to the invention were then added. The pH was then adjusted to 10.5 using 1% sodium hydroxide solution while stirring. Use of the activation solution in a zinc phosphating according to the invention

[0061] For a layer-forming phosphating by means of an activation based on the dispersion according to the invention, sheets of cold-rolled steel (CRS), hot-dip galvanized steel (HDG) and aluminum (AA6014) were used: a) firstly, by immersion for 5 minutes in a degreasing bath containing 4 wt.% Bonderite ®< C-AK 1565 A and 0.6 wt.% Bonderite ®< C-AD 1561, each available from Henkel AG & Co. KGaA, prepared in process water (pH: 10.2-10.9; 55 °C) with stirring, were subjected to alkaline cleaning; b) were subjected to rinsing under process water and then under demineralised water (κ < 1µScm -1< ) ​​for approximately 30 seconds each; c) were brought into contact with the activating solution by immersion for 60 seconds while wetted with water; d) and immediately thereafter and without further rinsing steps in a hydroxylamine accelerated phosphating bath with a free acid content of 0.9 - 1.4 points (titrated to a pH of 3.6), a total acid content of 25 - 30 points (titrated to a pH of 8.5) and a free fluoride content of approx. 150 mg / kg containing 4.6 wt.% Bonderite ®< M-ZN 1994, 0.8 wt.% Bonderite ®< M-AD 565, 0.24 wt.% Bonderite ®< M-AD 338 and 0.38 wt.-% Bonderite ®< M-AD 110, each available from Henkel AG & Co. KGaA, immersed in demineralized water (κ < 1µScm -1< ) ​​for 3 min with stirring at 52 °C; e) subjected to a rinse with demineralized water (κ < 1µScm -1< ) ​​for about 30 s; and f) provided with an approx. 20 µm thick layer of an electrocoat type Cathoguard ®< 800 (BASF SE) and then cured at 180 °C for 35 min.

[0062] Table 1 summarizes the results of zinc phosphating in terms of coating weight and after exposure to corrosion testing. It shows that, at a relatively low coating weight, homogeneous, continuous zinc phosphate coatings are always produced, achieving excellent corrosion protection results. Table 1 Substrat Layer weight 1< / gm -2< Corrosion 2.3< / mm CRS 1,6 0,5 2< HDG 2,1 1,8 2< AA6014 1,6 3,5 3< 1 Differential gravimetric determination after removal of the phosphate layer in aqueous 5 wt.% chromic acid solution. 2 Delamination at the scribe after exposure to the VW PV 1210 alternating climate test for 6 weeks over 30 cycles 3 longest thread of filiform corrosion according to DIN EN 3665

Claims

1. An aqueous dispersion having a D50 value of more than 10 µm, determined according to the method according to the description: page 7, lines 19-31, containing (a) at least 5 wt.% of a dispersed particulate constituent, comprising (a1) at least one particulate inorganic compound of a polyvalent metal cation, and (a2) at least one organic compound having a weight-average molar mass greater than 500 g / mol, which is composed at least partially of styrene and / or an α-olefin having no more than 5 carbon atoms and maleic acid, its anhydride and / or its imide, and which additionally comprises polyoxyalkylene units, and (b) at least one thickener, wherein a thickener is a polymeric chemical compound or a defined mixture of chemical compounds that, as a 0.5 wt.% constituent in deionized water, κ < 1 µScm-1, at a temperature of 25 °C, has a Brookfield viscosity of at least 100 mPa·s at a shear rate of 60 rpm (=rounds per minute) using a size 2 spindle.

2. The dispersion according to claim 1, characterized in that the at least one particulate inorganic compound (a1) of the dispersed particulate constituent (a) is composed at least partially of phosphates and the proportion of these phosphates, based on the dispersed inorganic particulate constituent calculated as PO4, is preferably at least 25 wt.%, particularly preferably at least 35 wt.%, more particularly preferably at least 40 wt.%, most particularly preferably at least 45 wt.%.

3. The dispersion according to claim 2, characterized in that the entirety of the particulate inorganic compounds (a1), which are composed at least partially of phosphates, in the dispersed particulate constituent (a) is composed at least partially of hopeite, phosphophyllite, scholzite and / or hureaulite.

4. The dispersion according to one or more of the preceding claims, characterized in that the dispersion has a D90 value of less than 150 µm, preferably of less than 100 µm, particularly preferably of less than 80 µm.

5. The dispersion according to one or more of the preceding claims, characterized in that there is a bimodal particle size distribution, and preferably a distribution maximum for a particle size below 1 µm and another for a particle size above 10 µm.

6. The dispersion according to one or more of the preceding claims, characterized in that the organic compounds (a2) contain the polyoxyalkylene units in their side chains, the proportion of polyoxyalkylene units in the entirety of the organic compounds (a2) not exceeding preferably at least 40 wt.%, particularly preferably at least 50 wt.%, but more particularly preferably 70 wt.%.

7. The dispersion according to one or more of the preceding claims, characterized in that the organic compounds (a2) also have imidazole units, preferably such that the polyoxyalkylene units of the organic compounds (a2) are at least partially end-capped with an imidazole group.

8. The dispersion according to one or more of the preceding claims, characterized in that the entirety of organic compounds having a weight-average molar mass greater than 500 g / mol in the particulate constituent (a) has an amine value, determined according to the method according to the description: page 9, lines 16-23, of at least 25 mg KOH / g, particularly preferably of at least 40 mg KOH / g, but preferably of less than 125 mg KOH / g, particularly preferably of less than 80 mg KOH / g.

9. The dispersion according to one or more of the preceding claims, characterized in that the entirety of organic compounds having a weight-average molar mass greater than 500 g / mol in and based on the particulate constituent (a) is at least 3 wt.%, preferably at least 6 wt.%, but preferably does not exceed 15 wt.%.

10. The dispersion according to one or more of the preceding claims, characterized in that the thickener according to component (b) is selected from urea urethane resins, preferably urea urethane resins which have an amine value [determined according to the method according to the description: page 9, lines 16-23] of less than 8 mg KOH / g, particularly preferably of less than 5 mg KOH / g, most particularly preferably of less than 2 mg KOH / g.

11. The dispersion according to one or more of the preceding claims, characterized in that the proportion of thickeners according to component (b) is at least 0.5 wt.%, the total proportion of organic compounds having a weight-average molar mass greater than 500 g / mol in the non-particulate constituent preferably not exceeding 4 wt.%.

12. The dispersion according to one or more of the preceding claims, characterized in that the pH of the dispersion is above 7.2, preferably above 8.0, but preferably below 10.0, particularly preferably below 9.0.

13. The dispersion according to one or more of the preceding claims, characterized in that the maximum dynamic viscosity of the dispersion at a temperature of 25 °C in the shear rate range of from 0.001 to 0.25 reciprocal seconds is at least 1000 Pa s, but preferably below 5000 Pa s.

14. A method for anti-corrosion pretreatment of a metal material selected from zinc, iron or aluminum or of a component which is composed at least partially of such metal materials, in which method the metal material or the component undergoes firstly activation (i) and then phosphating (ii), in particular zinc phosphating, in consecutive method steps, wherein the activation in method step (i) is carried out by bringing the metal material or the component into contact with a colloidal aqueous solution which can be obtained as an aqueous dispersion according to one or more of the preceding claims 1 to 13, which is diluted by a factor of from 20 to 100,000.

15. The method according to claim 14, characterized in that components are pretreated in series, which components are made at least partially of the materials zinc and aluminum, and the activation in method step (i) - is carried out by contact with a colloidal aqueous solution prepared by diluting an aqueous dispersion according to one or more of the preceding claims 1 to 13, of which the entirety of particulate inorganic compounds (a1) is composed at least partially of phosphates, preferably at least partially of hopeite, phosphophyllite, scholzite and / or hureaulite, and the phosphating in process step (ii) - is carried out by contact with an acidic aqueous composition containing 5-50 g / kg of phosphates dissolved in water, calculated as PO4, 0.3-3 g / kg of zinc ions and an amount of free fluoride, the quotient of the concentration of the phosphates in the inorganic particulate constituent of the colloidal aqueous solution of the activation in mmol / kg, based on PO4, with respect to the sum of the concentration of free fluoride and the concentration of silicon in each case in the acidic aqueous composition of the phosphating and in each case in mmol / kg being greater than 0.2.