METHOD FOR WELDING FOAM PARTICLES

DE502019012529D1Inactive Publication Date: 2024-12-05KURTZ GMBH & CO KG +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012529
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-24
Filing Date
2019-11-25
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for welding foam particles using electromagnetic waves face challenges in achieving uniform heat distribution, leading to uneven welding in particle foam parts, particularly with low-energy plastics that are hydrophobic and difficult to wet, resulting in poor wettability and absorption of heat transfer media.

Method used

Surface modification of foam particles using polymers that form intra- or intermolecular covalent bonds, creating a hydrophilic net-like coating that improves wettability and absorption of electromagnetic radiation, allowing for uniform welding without additional heat transfer media.

Benefits of technology

The surface modification enhances the uniformity and efficiency of heat input during welding, improving the quality of particle foam parts by ensuring even absorption of electromagnetic energy and reducing electrostatic charges, delamination risks, and enabling better integration with reactive matrices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to methods for welding foam particles provided with a surface modification by means of electromagnetic waves.

[0002] In the production of molded particle foam parts from foam particles, foam particles are fused together under the influence of heat. The heat required for this can be transferred to the foam particles being fused using electromagnetic waves, among other methods. Additional heat-transfer materials may be required to improve the heat transfer to the foam particles.

[0003] WO 2013 / 050581 A1 discloses a process for producing particle foam parts. A mixture of foam particles and a dielectric transfer fluid is heated using electromagnetic waves to fuse the foam particles into a particle foam part. Radio waves or microwaves are used as the electromagnetic waves. The foam particles are made of polypropylene (PP).

[0004] US Pat. No. 3,060,513 describes a process for sintering moist thermoplastic foam particles. The particles are dielectrically heated and simultaneously compressed in the mold. Electromagnetic waves are applied at a frequency of approximately 2 to 1000 MHz.

[0005] A similar process is described in US 3,242,238, in which foam particles are moistened with an aqueous solution and exposed to an electromagnetic field with a frequency of approximately 5 to 100 MHz.

[0006] GB 1,403,326 describes a process for welding expandable polystyrene foam particles, in which the particles are moistened with an aqueous solution and exposed to an electromagnetic field of 5 to 2000 MHz.

[0007] WO 01 / 64414 A1 discloses another process in which polymer particles made of polyolefins, wetted with a liquid medium, are heated with electromagnetic waves, particularly microwaves. The temperature in the mold is regulated by controlling the pressure within it.

[0008] WO 2008 / 043700A1 describes coated foam particles and processes for producing fire-resistant particle foam bodies. DE 10 2007 035 560 A1 describes the use of coated particles for producing expanded polystyrene (EPS).

[0009] In the processes explained above, moist foam particles are heated with electromagnetic waves, whereby the electromagnetic energy is absorbed by the liquid and transferred to the particles.

[0010] US Pat. No. 5,128,073 discloses thermoplastic particles coated with a high-frequency energy-absorbing material. These particles can be heated with electromagnetic waves, whereby the coating absorbs the electromagnetic energy and transfers it to the foam particles in the form of heat. Electromagnetic waves in the range of 40 MHz to 2450 MHz are used to weld the foam particles. The described coating is achieved by mixing with high-frequency absorbing organic materials. Examples include: alkanolamines such as triethanolamine, tripropanolamine, monohydroxyamines, and dihydroxyamines; alkyl glycols such as 2-hydroxyethyl ether; polyalkylene glycols such as polyethylene glycol; and aqueous solutions thereof.According to the embodiments, the respective coating materials are applied to foam particles either with or without solvent by mixing them with them, whereupon the respective mixture is heated by means of radiation in a shaping environment.

[0011] Some of the aforementioned processes have been known for decades. However, they have not yet been able to gain practical acceptance. There are various reasons for this. These processes work very well in laboratory samples. However, the transition to industrial production is difficult and, at least until recently, has not been successful. A key reason for this is that heat cannot always be applied evenly to the foam particles, resulting in uneven welding within the particle foam part.

[0012] Recently, the efficiency and reliability of welding foam particles using electromagnetic radiation have been improved through the development of the forming tools used for this purpose. DE 10 2016 123 214 A1 and WO 2018 / 10054 describe corresponding devices. This also shows that the need for a heat transfer medium depends on the properties of the particles to be welded.

[0013] Particle foam parts can therefore be manufactured, for example, from foam particles based on polyurethane (eTPU). Polyurethane has a dielectric loss factor D of 0.2 for electromagnetic radiation with a frequency of 1 MHz. In contrast, the dielectric loss factor of polypropylene (PP) for electromagnetic radiation with a frequency of 1 MHz is only 0.00035. The absorption capacity of polyurethane is therefore significantly higher than that of polypropylene. This makes it possible to introduce the heat required to weld the foam particles into the foam particles without additional heat-transfer substances, in particular without aqueous solutions, since the foam particles themselves absorb the electromagnetic waves.

[0014] Instead of polyurethane-based foam particles, foam particles made of expandable thermoplastics based on polyether block amide (ePEBA), polylactate (PLA), polyamide (ePA), polybutylene terephthalate (ePBT), polyester ether elastomer (eTPEE) or polyethylene terephthalate (ePET) can also be used.

[0015] These materials each contain functional groups (amide group, urethane group, or ester group) that create a dipole moment. These functional groups are responsible for the molecules' ability to absorb radio frequency radiation (RF radiation). Therefore, other thermoplastics containing such dipole moment-causing functional groups are also suitable for RF welding.

[0016] Foam particles based on ePP (expandable polypropylene) or ePS (expandable polystyrene) can also be welded to form particle foam parts. Since these materials absorb electromagnetic radiation only to a very low degree, it is necessary to add a dielectric heat transfer medium, such as water, in these cases.

[0017] In general, foam particles consist of so-called low-energy plastics, i.e. plastics that have at least one of the following characteristics: the free surface energy is below 40 mN / m, the contact angle of water is greater than 45°, i.e. the water wettability is low or non-existent, the material is hydrophobic, they are not dyeable from the aqueous phase, they have a surface resistance of more than 106 W.

[0018] Non-limiting examples include plastics from the material classes of aramids, polyesters, polyamides, polyacrylates, polyacrylonitriles, (thermoplastic) polyurethanes, (per)fluorinated polyolefins, e.g. polytetrafluoroethylene or polyvinylidene (di)fluoride, polysulfones, polyimides, polyolefins, carbon, etc., as well as co- or terpolymers thereof.

[0019] The term "particles" refers to molded bodies made from the aforementioned polymers, which, due to their structure, are primarily characterized by their diameter, which lies in both the nanometer and centimeter range. They also have a (rotationally) symmetrical or irregular shape. The surface of the molded bodies is flat, rough, or fissured, or exhibits a combination of these characteristics. The molded bodies consist of pore-free polymer or of open- and / or closed-pore polymer.

[0020] The porosity of the polymers is also described by the term "expanded", for example ePET stands for expanded polyethylene terephthalate and eTPU for expanded thermoplastic polyurethane.

[0021] In the following, shaped bodies with such properties are referred to as "particles." The term "material" is also used, particularly in connection with surface modification(s).

[0022] Particles made from low-energy plastics, especially those made from polyolefins or polyesters, have a number of disadvantages: the materials are easily electrostatically charged, which makes handling and further processing more difficult, the materials are not water-wettable, which limits their use as filter material for aqueous media, the material surfaces have no functional groups or these can only be activated with (chemically) drastic means.

[0023] This is disadvantageous for use as a filler material in composites: Even when using a reactive epoxy resin as the matrix material, the contact between the filler material and the matrix remains purely physical-mechanical. If moisture penetrates this area, it can lead to delamination. Surface coloring directly from the aqueous phase is also not possible.For use in connection with the welding of foam particles using electromagnetic waves, the hydrophobic properties of the foam particles used are particularly disadvantageous because they make uniform wettability with aqueous heat transfer media considerably more difficult. This can lead to a lot of heat being transferred to the foam particles in some places and little heat in other places during production in a forming tool. This in turn can lead to inferior particle foam parts that are not bonded evenly everywhere.

[0024] The above-mentioned loose mixing of foam particles with high-frequency energy-absorbing substances has the disadvantage that such substances are not permanently bonded to the particles.

[0025] A process for surface modification using an aqueous solution of polyvinyl alcohol containing silanol(ate) groups described in EP 2 670 906 or WO 2012 / 103876 relates exclusively to textile substrates.

[0026] The invention is based on the object of further developing methods for welding expandable thermoplastic foam particles by means of electromagnetic waves in such a way that the welding is as uniform as possible during the production of particle foam parts from foam particles, the latter being welded uniformly.

[0027] The object is achieved by methods for welding foam particles with electromagnetic waves, wherein foam particles with a surface modification are welded in a mold with electromagnetic waves, wherein the surface modification is produced by contacting the foam particles with a solution containing polymers capable of forming intra- or intermolecular covalent bonds under the conditions required for this purpose.

[0028] The way in which the surface modification is produced by forming intra- and / or intermolecular covalent bonds creates a net-like coating that completely or partially envelops the foam particles, so that the surface modification is permanently bonded to the particle, even if no covalent bond is formed to the foam particle.

[0029] In processes according to the invention, the surface modification can be hydrophilic.

[0030] Hydrophilic surface modifications are advantageous because they improve the wettability of foam particles with heat transfer media such as water or aqueous solutions, which in turn improves wetting uniformity and promotes more uniform welding of the foam particles. Hydrophilicity can be adjusted by incorporating suitable hydrophilic groups into the polymers used to create the surface modification. The degree of hydrophilicity can be tailored by varying the type and / or number of hydrophilic groups used.

[0031] The permanent functionalization of the material surfaces allows the ionogenic and / or covalent bonding of water-soluble chemicals, e.g., dyes, metal-binding ligands, or biologically active compounds, improves water wettability, thereby reducing electrostatic chargeability, improves water absorption and retention capacity, allows capillary water transport, etc. Functional groups stably anchored to the material surface also enable covalent bonding between particles and chemically reactive matrices, thus providing composite materials with improved delamination resistance.

[0032] In processes according to the invention, the surface-modified foam particles can be wetted with an aqueous solution before they are welded in the mold using electromagnetic waves.

[0033] In this way, water can be used as a medium for absorbing electromagnetic waves during welding, which is particularly advantageous and therefore preferred in combination with a hydrophilic surface modification, which improves the wettability of an otherwise hydrophobic foam particle.

[0034] In the case of the foam particles used in the processes according to the invention, the production of the surface modification may comprise, as an additional step, the removal of the solvent used therein.

[0035] Removing solvent after surface modification but before welding allows for solvent-free handling of surface-modified foam particles. Solvent-free, i.e., essentially dry, foam particles can be stored longer than solvent-treated foam particles. The latter can, in principle, be welded using electromagnetic waves, with or without a heat transfer medium. Removing the solvent used in manufacturing enables wetting with a heat transfer medium that is different from the solvent used in the surface modification process. This is particularly advantageous when the solvent and heat transfer medium are not compatible.

[0036] In the process according to the invention, the surface modification may comprise polar groups to improve the absorption of electromagnetic radiation, particularly in the radio frequency range.

[0037] This can improve the absorption capacity at the particle surface, which improves the heat input at the particle surface and thus promotes uniform welding.

[0038] Corresponding polar groups can be selected from: ester, acetal or urethane group.

[0039] The polymers capable of forming intra- or intermolecular covalent bonds have functional groups selected from sulfonic acid, thio, ammonium, carboxyl or silanol groups, which are components of polyvinyl alcohol, polyvinylpyrrolidone.

[0040] The functional groups mentioned enable the polymers of which they are a component to form intra- or intermolecular covalent bonds in a simple manner, although in principle other functional groups and polymers are also possible.

[0041] Preferably, the foam particles are provided with a surface modification by contacting them with an aqueous polyvinyl alcohol solution containing carboxyl or silanol groups, wherein the pH of the aqueous polyvinyl alcohol solution containing carboxyl or silanol groups is between 2 and 5, and wherein the aqueous polyvinyl alcohol solution containing carboxyl or silanol groups optionally comprises further substances which influence the surface tension and / or the viscosity of the solution.

[0042] Appropriately modified polyvinyl alcohols are particularly suitable for crosslinking, have hydrophilic groups in the form of hydroxyl (-OH) groups, and, depending on the manufacturing process, possibly acetyl (-OOC-CH 3 ) groups, which are polar and also allow further modifications.

[0043] The lower limit of the concentration of the carboxyl or silanol group-containing polyvinyl alcohol solution can be 0.001, 0.01, 0.5 or 1% (w / v), the upper limit 40% (w / v), 10% (w / v), 2% (w / v), or 1% (w / v).

[0044] Here and in the following, the respective concentration specification "% (w / v)" means the same as "g / 100 ml", ie 1% (w / v) means 1 g / 100 ml, 2% (w / v) means 2 g / 100 ml, etc.

[0045] Concentrations of 1% (w / v) have proven particularly advantageous. Higher upper limits can be advantageous when providing surface modifications with greater layer thickness. This can be advantageous, for example, to increase the concentration of certain functional groups located on or near the surface. Lower concentrations can be advantageous when providing surface modifications with thinner layer thicknesses. The latter is particularly advantageous when excessive layer thicknesses would prevent the particles from welding together.

[0046] Surface modifications containing OH groups can be further modified by covalent bonding of water-soluble substances to the hydroxyl (-OH) groups present there by means of ester, acetal, urethane or ether bonds.

[0047] In this way, the particles used for welding can be "tailored" by providing further suitable modifications. For example, additional electromagnetic radiation-absorbing groups can be introduced near the particle surface, and / or the hydrophilicity of the particle surface can be further modified, and / or it can be used to color particles, and so on.

[0048] In processes according to the invention, the foam particles can consist of: polyurethane (ePU), expandable thermoplastics based on polyether block amide (ePEBA), based on polylactate (PLA), based on polyamide (ePA), based on polybutylene terephthalate (ePBT), based on polyester ether elastomer (eTPEE), based on polyethylene terephthalate (ePET), or of expandable polyethylene (ePE), expandable polypropylene (ePP) or expandable polystyrene (ePS).

[0049] These materials are particularly preferred materials for foam particles.

[0050] The electromagnetic waves used in the method according to the invention are preferably electromagnetic RF waves. The electromagnetic RF waves preferably have a frequency of at least 30 kHz or at least 0.1 MHz, in particular at least 1 MHz or at least 2 MHz, and preferably at least 10 MHz.

[0051] The electromagnetic RF waves preferably have a maximum frequency of 300 MHz.

[0052] The generator for generating electromagnetic waves preferably generates electromagnetic waves with an amplitude of at least 10 3 < V and in particular at least 10 4 < V. Commercially available generators generate RF waves with a frequency of 27.12 MHz.

[0053] The electromagnetic waves can also be microwaves in the frequency range of 300 MHz to 300 GHz.

[0054] In the following, the invention is explained in more detail with reference to the figures and embodiments.

[0055] The term "surface modification" or "surface modification" used here describes that the surfaces of non-surface-modified materials differ from those of surface-modified materials in at least one of the following respects: in the results of surface analysis, e.g. using ESCA (Electron Spectroscopy for Chemical Analysis) or SIMS (Secondary Ion Mass Spectroscopy), in water wettability, in electrostatics, in chemical reactivity, e.g. in dyeability with water-soluble dyes from the aqueous phase.

[0056] Particles made from low-energy plastics can be surface-modified as described in EP 2 670 906. Additional compounds can advantageously be used for surface modification.

[0057] According to the invention, the surface modification of particles made from low-energy plastics is carried out by contacting them with a solution containing polymers capable of forming covalent inter- and intramolecular bonds under the conditions required for this purpose, such as solvent (mixture), pH, temperature, pressure, energy input, and removing the solvent again.

[0058] Polymers capable of forming covalent inter- and intramolecular bonds possess additional functional groups, such as sulfonic acid, thio, ammonium, carboxyl, or silanol groups, which are components of polyvinyl alcohol (PVA) and polyvinylpyrrolidone. Examples include polyvinyl alcohol containing carboxyl groups or polyvinyl alcohol containing silanol groups. These polyvinyl alcohols, equipped with carboxyl or silanol groups, are commercially available from Kuraray Europe GmbH, Hattersheim, Germany, as KURARAY POVAL™< K (new product name: KURARAY POVAL™< 25-88 KL) or KURARAY POVAL™< R (new product name: KURARAY POVAL™< 25-98 R). In this context, reference is made to the company's current data sheets.

[0059] For permanent surface modification, aqueous solutions of polyvinyl alcohol containing carboxyl or silanol groups are preferred. The polymer concentration used depends primarily on the intended use of the particles or the product manufactured from them and can vary between 0.001% (w / v) and 40% (w / v). Typically, the concentrations are between 0.01% (w / v) and 10% (w / v), preferably 0.5 to 2% (w / v), and particularly preferably 1% (w / v). The preparation of such solutions is known; see, for example, the data sheets mentioned above.

[0060] Other substances that reduce the surface tension of water, such as lower aliphatic alcohols, surfactants, and wetting agents, can be added to these polymer solutions. Compounds that modify the viscosity of the solution, such as fumed silica or metal salts, can also be included in the solution. Their selection, as is familiar to those skilled in the art, is based on the intended use of the surface-modified materials, their compatibility with the dissolved polymer capable of forming covalent intra- and intermolecular bonds, the material types and properties to be modified, and the contacting and drying conditions.

[0061] The pH of the polymer solution used depends on the reactivity of the polymer used; for polyvinyl alcohol containing carboxyl and silanol groups, it is preferably acidic, at 3 ± 1, for the formation of ester or siloxane bonds.

[0062] The temperature of the polymer solution used can be between 3°C and 95°C, preferably between 15 and 65°C, most preferably at room temperature.

[0063] The low-energy materials are brought into contact with a solution containing polymers capable of forming inter- and intramolecular bonds. The term "contacting" here describes the process of enabling all or certain parts of the surface of the low-energy material to enter into physical-chemical interactions with the dissolved substances in the solution. At the molecular level, this includes terms such as physisorption and chemisorption, and at the production level, terms such as bringing into intimate contact, coating, enveloping, painting, wetting, impregnating, spraying, painting, dipping, etc.

[0064] Contacting can be done either manually or inline using known tools and at production speed.

[0065] The contact time of the low-energy materials with the polymer solution ranges from seconds to several days and is determined and optimized taking into account the polymer concentration used, the intended use of the material, its properties such as texturing, compactness, density, etc., as well as economic aspects.

[0066] After the low-energy materials have been contacted with the polymer solution, the solvent, preferably water, is removed if necessary, which is usually done by drying the materials wetted with the polymer solution. Drying temperatures can range from 1°C to over 170°C. They are determined on a case-by-case basis, taking into account the intended use and the properties of the material used. They are preferably at room temperature, more preferably between 30 and 70°C, and most preferably between 70 and 130°C.

[0067] The degree of drying depends on the intended use of the materials, so that they can have a residual moisture content between 0% and 40%, based on non-surface-modified materials.

[0068] The detection of the permanent presence of functional groups is advantageously carried out using water-soluble (addition) dyes capable of covalent bonding. For example, simplicol® from Brauns-Heitmann, Warburg, is suitable for detecting hydroxyl groups. Developed for the permanent coloration of cotton, this dye cannot be washed off even after repeated washing with hot water, which is considered proof of the stability of the surface modification.

[0069] It is assumed that the contacting described above and the subsequent drying causes the polymers capable of forming covalent inter- and intramolecular bonds to initially accumulate on the surface of the particles as the solvent water evaporates. In the case of polyvinyl alcohol containing carboxyl groups, the progressive evaporation of the solvent leads to a reaction in which the carboxyl and hydroxyl groups react with each other, predominantly intermolecularly, to form ester bonds. In the case of polyvinyl alcohol containing silanol groups, the silanol groups then react with each other (via condensation reaction and with the elimination of water, predominantly intermolecularly) as evaporation progresses. In both cases, a giant molecule is formed that envelops the particle surface and adheres firmly to it. By specifically adjusting the concentration of the carboxyl or hydroxyl groups, the resulting ester bonds can be reduced.Using a polyvinyl alcohol solution containing silanol groups, it is possible to apply not only thin, possibly monomolecular layers to the surface, but also thick layers that firmly bond the individual particles together or close gaps (gussets) between the particles.

[0070] However, crosslinking begins even without removing the solvent. Therefore, it is not necessary to remove the solvent. Especially if the solvent can also serve as a heat transfer medium, it may be advantageous not to remove the solvent, or to remove it incompletely.

[0071] When using polyvinyl alcohol containing carboxyl or silanol groups, the hydroxy (-OH) groups anchored firmly on the surface are available for the covalent bonding of water-soluble substances via ester, acetal, urethane, or ether bonds. Esterification can occur with inorganic or organic acids. For example, the -OH groups can be esterified with di-, tri-, or polycarboxylic acids, so that the material surface is negatively, anionically charged in aqueous solution. Through esterification with zwitterions, e.g., amino acids, the surface acquires a cationic, positive charge, which can be used for further reactions. Compounds containing aldehyde groups, such as glyceraldehyde, can be added to the -OH groups under acid catalysis, forming an acetal bond; in this case, the number of -OH groups on the material surface increases. Compounds containing double bonds, such asVinylsulfonic acid, for example, can be added to the -OH groups under peroxide catalysis, forming hydrolysis-stable ether bonds. In this case, at pH >2, the surface acquires a negative, anionic charge from the -SO 3 -< groups.

[0072] These additional surface modifications expand the range of applications of such surface-modified particles made from low-energy plastics in technical applications, including applications in medicine, environmental technology and biotechnology.

[0073] The surface-modified particles produced from low-energy plastics according to the process can be used for the production of molded bodies by near-surface heat development by means of electromagnetic radiation, e.g. by means of microwaves, as fillers for composite materials, as moisture-binding insulating material, as filter materials, as drainage material, as substrates for the immobilization of biologically active substances, as cell culture substrates, as electroless metallizable substrates, etc.

[0074] With regard to the processes according to the invention, the surface modification results in improved wettability with water. The inventors also assume that, independently of this, the functional groups present improve the absorption capacity of electromagnetic radiation at the surface. This leads to better welding overall.

[0075] The locally enhanced ability to absorb electromagnetic radiation on the surface of the particles results from the structure of the surface modification. Functional groups present there (e.g., ester groups, amide groups, urethane groups) create a dipole moment. Such functional groups are conducive to the absorption of electromagnetic radiation, especially radiofrequency radiation.

[0076] Foam particles based on polyurethane (ePU), polyether block amide (ePEBA), polylactate (PLA), polyamide (ePA), polybutylene terephthalate (ePBT), polyester ether elastomer (eTPEE), or polyethylene terephthalate (ePET) can also be used, as these materials absorb electromagnetic waves well. These materials, which absorb electromagnetic radiation, especially RF waves, well, each have a functional group (here: amide group, urethane group, or ester group) that creates a dipole moment. These functional groups are responsible for the molecules absorbing electromagnetic radiation. Therefore, other thermoplastics that have such functional groups that create a dipole moment are also suitable for heating with electromagnetic radiation, using RF waves.The same applies to coatings containing such groups, regardless of the type of foam particles.

[0077] The improved wettability with water results from the presence of polar functional groups. In the case of polyvinyl alcohol, these are alcohol (-OH) groups and, if present in the polyvinyl alcohol due to its manufacturing process, acetate groups (carboxylic acid ester groups). In addition, there are silanol or carboxyl groups when appropriately modified polyvinyl alcohols are used.

[0078] The methods according to the invention are superior to prior art methods in that they enable improved and, above all, more uniform heat input. This will be discussed in more detail below using the exemplary embodiments. Example 1:

[0079] KURARAY POVAL ™< R (new product name: KURARAY POVAL ™< 25-98 R) from Kuraray Europe GmbH, Hattersheim, is used as the polyvinyl alcohol containing silanol groups.

[0080] For surface modification, a 0.5% (w / v) aqueous KURARAY POVAL™< R solution is used: 5 g of polymer are placed in 1,000 ml of deionized water at room temperature and then heated to approximately 90°C with continuous stirring until the polymer is completely dissolved. The pH is adjusted to 3 with dilute hydrochloric acid.

[0081] Particles: ArmaShape. These are particles or hollow spheres made of polyethylene terephthalate with a diameter of <0.5 µm from Armacell Benelux SA, Thimister-Clermont, Belgium.

[0082] Contacting: Approximately 200 ml of ArmaShape is poured into a plastic sieve. The sieve is placed on a suitable glass, and KURARAY POVAL™< R solution is poured onto the beads until they float to the surface. They are then pressed back into the solution using a suitable plastic lid. The contact time is approximately 5 minutes.

[0083] Drying: The polymer solution is allowed to drain from the sieve, then the beads are spread out on a glass plate and dried at approximately 70°C in a convection oven.

[0084] Result: Beads contacted with KURARAY POVAL™< R solution show a distinct, non-washable stain with simplicol®< (a cotton dye from Brauns-Heitmann, Warburg) – untreated controls do not bind any dye. Beads contacted with POVAL™< R solution are water-wettable. Example 2:

[0085] As example 1, except that a POVAL ™< K solution (new product name: KURARAY POVAL ™< 25-88 KL) is used. Example 3:

[0086] PET beads are surface-modified as described in Example 1, moistened with water, and filled into a glass syringe while still wet. They are compressed with the syringe plunger until no more water is visible from the syringe. The pressure of the syringe plunger on the beads is maintained by suitable clamps. This construct is exposed to the electromagnetic energy of a 600-watt microwave for 40 minutes. After cooling, a stable molded body made of baked PET beads that corresponds to the syringe interior can be removed. Example 4:

[0087] Beads or foam particles made of ePP from Kaneka are surface-modified as described in Example 1, moistened with water, and filled into a glass syringe while still wet. They are compressed with the syringe plunger until no more water is visible. The pressure of the syringe plunger on the beads is maintained by suitable clamps. This construct is exposed to the electromagnetic energy of a 600-watt microwave for 40 minutes. After cooling, a stable molded body made of baked or welded ePP beads, corresponding to the syringe interior, can be removed. Example 5:

[0088] Foam particles made of EPP from Kaneka or EPS from BASF and Knauf are welded together in a test forming tool using electromagnetic waves under various conditions, namely: Wetted with distilled water (as a comparative example); coated with PVA (1% w / v in water) in the presence of water (according to the invention); coated with polyethylene glycol in the presence of water (as a comparative example).

[0089] As PVA, KURARAY POVAL™< R solution (new product name: KURARAY POVAL™< 25-98 R) in the form of a 1% (w / v) aqueous solution was used, i.e., a polyvinyl alcohol containing silanol groups.

[0090] Each experiment is repeated five times. The supply voltage for frequency generation is approximately 6.5 kV, applied for a constant period of approximately 22 seconds. The molding chamber is shaped so that a cuboid foam plate measuring 100 mm x 100 mm x 25 mm is formed as the test molded part. The test molding tool, or the device supporting it, is equipped with an optical temperature sensor that measures the surface temperature of the workpiece made of foam particles to be welded or to be welded. At the same time, a sensor is contained in the mold wall that measures the foam pressure, i.e., the pressure in the mold. The circuit also contains a measuring device that measures the electrical power emitted to the capacitor in the form of radiation. This corresponds to the power of the radiation absorbed by the foam particles during welding.

[0091] The maximum power absorbed reflects the absorption capacity of the material being examined. The higher the measured maximum power, the higher the absorption capacity of the material being examined. The energy corresponds to the integral under the time-power curve and represents the absorbed radiation energy.

[0092] The results are shown in the bar charts of the Figures 1 to 3 This shows the maximum power and the energy consumed for each of the three different treatment types. Figure 1 summarizes the results for the foam particles made of EPS from BASF, Figure 2 for the EPS foam particles from Knauf and Figure 3 for the EPP foam particles from Kaneka.

[0093] It follows that distilled water (both colorless) and polyethylene glycol (both gray) are almost equally poor heat transfer media, since the maximum absorbed power and converted energy are significantly lower for foam particles treated with distilled water or polyethylene glycol compared to particles treated with PVA (both black). Supplementary information

[0094] In Example 5 above, solvent removal was omitted during the preparation of the PVA coating. The particles coated with the surface modification solution were additionally treated with the same amount of water (14 g of water and 14 g of surface modification solution were used).

[0095] In order to avoid possible polymerization of polymer solution, e.g. PVA solution, and thus possible adhesion or sticking to tool surfaces, foam particles can be freed from solvent after the surface modification, i.e. dried, and then wetted with water in the molding device.

[0096] If removal of the solvent by drying is not planned, excess surface modification solution can be removed by centrifugation, for example in a tubular drum sieve, in such a way that only the (minimal) amount of surface modification solution required for welding remains on the surface of the particles.

[0097] The above discussions serve to explain the invention and are not to be construed as limiting.

[0098] Surface modification can also be done by: A process for the surface modification of particles made from low-energy plastics, characterized in that the particles are contacted with a solution containing polymers capable of forming covalent inter- and intramolecular bonds under the conditions required for this purpose, and the solvent is then removed. Similar processes, characterized in that aqueous solutions of polyvinyl alcohol containing carboxyl or silanol groups at pH 3 ± 1 are used.

[0099] Particles according to the invention made from low-energy plastics can be characterized by having been surface-modified by the aforementioned processes. Such particles according to the invention can serve as substrates for the covalent bonding of (predominantly) water-soluble substances via ester, urethane, acetal, or ether bonds.

[0100] The particles made from low-energy plastics and surface-modified as described in the two previous paragraphs can be used as substrates for the production of molded bodies by near-surface heat development, e.g. by means of microwaves, as moisture-binding insulating materials, as fillers for composite materials, as filter materials, as drainage materials, as substrates for the immobilization of biologically active substances, as cell culture substrates, as electroless metallizable substrates, etc.

Claims

1. A method for welding foam particles using electromagnetic waves, wherein foam particles undergoing a surface modification are welded in a molding tool using electromagnetic waves, wherein the surface modification is produced by the foam particles being brought into contact with a solution containing polymers which are capable of forming intramolecular or intermolecular covalent bonds, and wherein the polymers capable of forming intramolecular or intermolecular covalent bonds comprise functional groups selected from sulfonic acid, thio, ammonium, carboxyl or silanol groups which are part of polyvinyl alcohol or polyvinylpyrrolidone.

2. The method according to claim 1, wherein the surface modification is hydrophilic.

3. The method according to claim 1 or 2, wherein the foam particles with surface modification are wetted with an aqueous solution before they are welded in the molding tool using electromagnetic waves.

4. The method according to any of the preceding claims, wherein the production of the surface modification comprises, as an additional step, the removal of the solvent used in this method.

5. The method according to any of the preceding claims, wherein the surface modification for improving the absorption of electromagnetic radiation, in particular in the radiofrequency range, comprises polar groups.

6. The method according to claim 5, characterized in that the polar groups are selected from an ester, acetal or urethane group.

7. The method according to any of the preceding claims, wherein the foam particles are provided with a surface modification by contacting them with an aqueous carboxyl- or silanol group-containing polyvinyl alcohol solution, wherein the pH value of the aqueous carboxyl- or silanol group-containing polyvinyl alcohol solution is between 2 and 5, and wherein the aqueous carboxyl- or silanol group-containing polyvinyl alcohol solution optionally comprises further substances which affect the surface tension and / or the viscosity of the solution.

8. The method according to claim 7, characterized in that the concentration of the carboxyl or silanol group-containing polyvinyl alcohol solution is 0.001% (w / v) to 40% (w / v), 0.01% (w / v) to 10% (w / v), 0.5 to 2% (w / v), or is 1% (w / v).

9. The method according to any of the preceding claims, wherein the resulting surface modification is further modified by covalent bonding of water-soluble substances to the hydroxy (-OH) groups present there by means of an ester, acetal, urethane or ether bond.

10. The method according to any of the preceding claims, wherein the foam particles are made of polyurethane or of expandable thermoplastics on the basis of polyether block amide (ePEBA), on the basis of polylactate (PLA), on the basis of polyamide (ePA), on the basis of polybutylene terephthalate (ePBT), on the basis of polyester-ether-elastomer (eTPEE), on the basis of polyethylene terephthalate (ePET), or are made of expandable polyethylene (ePE), expandable polypropylene (ePP) or expandable polystyrene (ePS).