USE OF A STEEL POWDER FOR THE ADDITIVE MANUFACTURING OF A STEEL COMPONENT

DE502020009260D1Active Publication Date: 2024-10-02DEUT EDELSTAHLWERKE SPECIALTY STEEL GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009260
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-19
Publication Date
2024-10-02
Estimated Expiration
2040-11-19

AI Technical Summary

Technical Problem

In additive manufacturing of steel components, the rapid cooling of steel powders melted by electron or laser beams leads to high thermal stresses, causing cracks, especially in steels with higher carbon contents, due to the limitations of existing heating technologies that cannot maintain temperatures above 225 °C, which restricts the production of components with optimal hardenability and wear resistance.

Method used

A steel powder with a martensite starting temperature (Ms) of no more than 225 °C, composed of specific alloying elements like C, Si, Mn, Ni, Cr, Mo, W, and V, is used, allowing for controlled cooling and preventing the formation of hard martensitic phases, thereby reducing thermal stresses and enabling inductive surface hardening for enhanced wear resistance.

Benefits of technology

The use of this steel powder ensures the production of components with high wear resistance and crack hardness, avoiding microcracks and residual austenite, while maintaining the component temperature within the limitations of conventional additive manufacturing devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to the use of a steel powder for the additive manufacturing of a steel component, in which, in a repeatedly performed process, steel powder is applied to a heating plate to build up the component, the applied steel powder is melted into a molten portion by means of an electron or laser beam, and the respective molten portion is cooled to form a solid section of the steel component, wherein the component, which grows section by section in this way, is kept at a temperature during production by means of the heating plate that corresponds at least to a minimum heating temperature Tmin and is at most 225 °C.

[0002] Where "%" values ​​are given below for steel compositions, these refer to mass (specified in "mass"), unless explicitly stated otherwise.

[0003] The proportions of certain components in the structure of a steel material or a steel component are given in volume % ("Vol.-%") in this text, unless expressly stated otherwise.

[0004] Similarly, the proportions that the various particles occupy in the total volume of the powder used according to the invention are given in vol.%, unless otherwise expressly stated.

[0005] The hardness values ​​given here in HRC are the result of a Rockwell hardness test carried out in accordance with DIN EN ISO 6508-1: 2016-12.

[0006] The production of powders consisting of steel particles can be carried out in a known manner by atomization or by mechanical comminution, such as wet milling. Likewise, mechanical alloying of elemental powders is also possible in a known manner, provided that the powders are supplied in the necessary particle sizes and mixed together in the proportions corresponding to the alloying formula according to the invention.

[0007] Steel powders are used in various ways in the prior art for the manufacture of components.

[0008] A first example of this is the process described in WO 01 / 79575 A1, in which a nitrogen-alloyed steel with high wear resistance is produced by spray compaction. For this purpose, the steel has, in wt%, 0.8–2.5% C, 0.03–0.75% N, 0.15–1.8% Si, ≤ 1.0% Mn, ≤ 0.03% P, ≤ 0.05% S, 4.0–11.5% Cr, 0.5–6.0% Mo, ≤ 4.0% V, ≤ 4.0% Nb, ≤ 3.5% W, ≤ 0.005% O2, optionally further alloying elements, and the remainder being iron and usual impurities. The chemical composition is optimized in such a way that the carbide / carbonitride-forming elements meet a wear factor SV and the silicon-nitrogen ratio VSiN is maintained to minimize retained austenite content.

[0009] EP 2 662 462 A1 specifies broadly defined alloys for low-temperature hardenable steels with excellent machinability, whose only mandatory component is carbon in amounts of 0.15–3.0 wt.%. Optionally, the respective alloy may contain, for example, N, B, Cr, Ni, Si, Mn, Al, Mo, W, Ti, Ta, Zr, Hf, V, Nb, Cu, and Co within wide ranges. It is also mentioned that such broadly formulated steels are suitable for powder metallurgy applications.

[0010] EP 0 754 942 A1 describes a process in which a powder, for example consisting of steel 1.2842, is formed into a hardness comparison plate by hot isostatic pressing. For this purpose, the steel powder is filled into a steel capsule. The capsule is then evacuated, sealed, and the powder contained within is pressed into the respective plate under a pressure of 100–4000 bar at a temperature at which no liquid phase occurs during pressing.

[0011] The term "additive manufacturing processes" encompasses all manufacturing processes in which material is added to create a component. This addition typically occurs layer by layer. Additive manufacturing processes, often also referred to as "generative processes" or more generally as "3D printing," contrast with traditional subtractive manufacturing processes, such as machining (e.g., milling, drilling, and turning), in which material is removed to give the component its shape.

[0012] The additive manufacturing principle makes it possible to produce geometrically complex structures that cannot be realized, or can only be realized with considerable effort, using conventional manufacturing processes such as the aforementioned machining processes or primary and secondary forming processes (casting, forging) (see VDI Status Report "Additive Manufacturing Processes", September 2014, published by the Association of German Engineers, Department of Production Engineering and Manufacturing Processes, www.vdi.de / statusadditiv).

[0013] More detailed definitions of the processes that are summarized under the general term "additive processes" can be found, for example, in the VDI guidelines 3404 and 3405.

[0014] The processing of steel powders in additive manufacturing is now fundamentally possible. Steels considered weldable are typically used to produce the particles of suitable steel powders. These are steels with carbon contents below 0.30 wt%, preferably below 0.20 wt%, with steels with minimized carbon contents below 0.05 wt%, within the impurity range, proving particularly suitable.

[0015] A general problem with processing steel powders in additive manufacturing is that the powder portion captured by the electron or laser beam, typically under vacuum, melts very quickly, and the resulting small volume of melt is then rapidly cooled as it bonds to the previously solidified section of the component. This rapid cooling, inherent to the process and resulting in a high cooling rate, leads to high thermal stresses, which can cause cracks in the component, especially in steels with higher carbon content.

[0016] To minimize the risk of stress cracking, it is advisable to use powders made of steels for additive manufacturing that, despite the unavoidable rapid cooling, form the softest possible microstructure. Soft martensitic materials or materials characterized by so-called "lancet martensite" are suitable for this purpose. Examples of such steels are those known as "maraging steels," whose alloys are standardized under material numbers such as 1.2709, 1.6315, 1.4545, and 1.4542.

[0017] These steels achieve their mechanical properties through a martensitic transformation (without forced dissolution of carbon to carbon-free nickel or soft martensite) and subsequent precipitation hardening. The resulting precipitates and intermetallic phases contribute to the increased hardness. Due to the minimized carbon content, carbides are formed only to a minimal extent. For maraging steels to achieve the required mechanical properties despite their low carbon content, they must be alloyed with high concentrations of expensive alloying elements such as molybdenum, cobalt, or nickel. However, components made of maraging steels cannot be inductively surface hardened due to the lack of carbon.

[0018] The term "process for inductive hardening of a surface layer" refers to processes in which the surface layer of the steel material adjacent to the surface to be hardened, from which the component supporting the surface is made, is heated to hardening temperature by means of an electromagnetic field induced in the component, and in which the heated section of the surface layer is then cooled sufficiently quickly by applying a suitable quenching medium in order to create hardened structures in the relevant surface section.

[0019] The technical and physical background of inductive surface hardening is explained in the information sheet 236, "Heat treatment of steel - Surface hardening", edition 2009, which is published by the German Steel Federation, Sohnstraße 65, 40237 Düsseldorf, and is available for download at the URL https: / / www.stahl-online.de / index.php / service / publikationen / stahlanwendung-dokumentationen / 2 / , accessed on November 15, 2020.

[0020] A well-known method for preventing the transformation of the molten steel produced during additive manufacturing into hard martensite, particularly with higher carbon contents, is the use of a heated bed. However, industrially available additive manufacturing equipment either lacks this option or is equipped with heated beds capable of heating the component to a maximum temperature of 225 °C. Heating temperatures of up to 200 °C are typical. This limit stems from the poor thermal conductivity of the steel powder used in additive manufacturing, which means that higher heating temperatures, especially for small build heights typically less than 200 mm, lead to improved results.Furthermore, excessive heating can lead to undesirable reactions of the steel powder due to the intense heat input, such as burning with heavy smoke development. Devices with heating plates capable of maintaining heating temperatures of 500 °C and above are therefore the exception in practice.

[0021] In light of the prior art described above, the object of the invention was to to specify a steel powder suitable for the production of components optimized in terms of their hardenability and wear resistance using an additive manufacturing process P can be used.

[0022] To solve this problem, the invention proposes the use specified in claim 1.

[0023] Advantageous embodiments of the invention are specified in the dependent claims and, like the general concept of the invention, are explained in detail below.

[0024] A steel powder used according to the invention for the additive manufacturing of a steel component is therefore formed by steel particles produced from a steel having a martensite start temperature Ms of at most 225 °C and, in mass %, consisting of C: 0,80 - 1,20 %, Yes: 0,1 - 1,0 %, Mn: 0,1 - 4,0 %, Ni: ≤ 2,0 %, Cr: ≤ 6,00 %, Mon: ≤ 3,0 %, W: ≤ 6,0 %, S: ≤ 0,05 %, AI: 0,004 - 0,035 %, V: 0,02 - 0,20 %, Ti: ≤ 0,10 %, Note: ≤ 0,40 %, B: ≤ 0,0030 %, and consists as a remainder of iron and steel-typical impurities, which in total amount to a maximum of 0.55 wt.% and include up to 0.05% P and up to 0.12% N, where the respective Mn content %Mn, the respective Ni content %Ni, the respective Si content %Si, the respective er content %Cr, the respective N content %N and the respective B content %B of the steel, each used as a % value, is as follows: %Mn + %Ni < 5 % and

[0025] In an additive manufacturing process using steel powder according to the invention, steel powder is applied to a heating plate in a repeated process to build up the component in accordance with the prior art described above. The steel powder is melted into a molten portion by means of an electron or laser beam. Each molten portion is then cooled to form a solid section of the steel component. During production, the component, which grows in sections in this way, is maintained at a temperature THeiz by means of the heating plate. This temperature must be at least Tmin and at most 225 °C (Tmin ≤ THeiz ≤ 225 °C).

[0026] According to the invention, in such a process a steel powder produced in the manner mentioned above and explained in detail below is used, wherein the minimum heating temperature Tmin of the heating plate is determined according to the following formula: where %Mn denotes the respective Mn content, %Si the respective Si content, %Cr the respective Cr content, %Ni the respective Ni content, %N the respective N content and %B the respective B content of the steel, and the respective content fractions are inserted as simple % values ​​into the formula for calculating Tmin.

[0027] By ensuring that more than 90% by mass, and in particular more than 95% by mass, of the steel particles in a steel powder according to the invention have a particle diameter of 10–65 µm, it can be guaranteed that components can be reliably produced using such steel powder with conventional devices of the type described above by additive manufacturing. The selection of suitably sized steel particles can usually be carried out by sieving and classifying. Typically, up to 2% by mass of particles with diameters above the range specified for particle diameters according to the invention and up to 5% by mass of particles with diameters below the particle diameter range specified according to the invention are permitted.

[0028] The invention thus selects a steel for the steel particles of a steel powder intended for additive manufacturing that has a carbon content ("C") of at least 0.8 wt%. This C content is adjusted such that the martensite start temperature ("Ms temperature") of the steel is not significantly above 200 °C and in no case exceeds 225 °C.

[0029] Preferably, the composition of the steel is adjusted by adding further alloy contents so that its martensite start temperature is at most 200 °C.

[0030] By first ensuring a low Ms temperature through sufficiently high C content, the formation of hard martensitic phases during the layer-by-layer construction of the component is avoided.

[0031] At the same time, steels of the type selected according to the invention exhibit a steadily decreasing hardness when heated from room temperature (= 20 °C) to 750 °C after quenching from the austenite. Unlike steels that form deformation-induced precipitates between 300 °C and 600 °C during cooling, the alloy of a steel selected according to the invention is chosen such that no mobile dislocations form during cooling. Such dislocations could represent nucleation sites for carbides or nitrides, which would block the movement of the dislocations, with the consequence that the material could crack in the area of ​​the respective blockage.

[0032] In contrast, a steel alloyed according to the invention, for example, exhibits a monotonous decrease in hardness / strength with increasing temperature when tempered at temperatures ranging from room temperature to 750 °C. This helps to reliably avoid thermal stresses in components produced from steel powder according to the invention by additive manufacturing.

[0033] The Ms temperature of the steel material selected according to the invention for the steel powder can be determined experimentally in a known manner by systematically creating cooling curves ("TTT diagram") or taken from TTT diagrams available for the respective steel.

[0034] A particular advantage of a steel powder used according to the invention is that it allows the production of components in which high wear resistance can be achieved through inductive surface hardening. For this purpose, the steel selected for the particles of the steel powder used according to the invention is alloyed such that it exhibits a high so-called "initial hardness," i.e., a hardness present during inductive surface hardening after inductive heating and quenching, but before a final tempering treatment, of over 55 HRC. This is ensured by the carbon contents of at least 0.80 wt% provided according to the invention, with carbon contents of at least 0.85 wt% being particularly advantageous.The high carbon content of the steel selected for the steel particles of the steel powder used according to the invention not only lowers the melting point temperature to the desired values, but also creates the conditions for the formation of high hardness and the development of wear-inhibiting carbides in the additively manufactured components made from the steel powder used according to the invention. Limiting the carbon content to values ​​of up to 1.2 wt%, and in particular to a maximum of 1.0 wt%, has proven particularly advantageous with regard to avoiding retained austenite at room temperature in additively manufactured components made from the steel powder used according to the invention.

[0035] Silicon ("Si") contributes to the quenchability and strength of the steel selected according to the invention. For this purpose, Si contents of 0.1 wt% to 1 wt% are provided. To reliably prevent negative effects of the presence of Si, such as a reduction in toughness, the Si content can be limited to a maximum of 0.7 wt%, in particular a maximum of 0.4 wt%.

[0036] Manganese ("Mn") is provided in the steel selected according to the invention in contents of 0.1 wt% to 4.0 wt%. Mn contributes to the desired reduction of the Ms temperature and increases the through-hardenability of the component additively manufactured from steel powder used according to the invention. Optimal effects of the presence of Mn in the steel selected according to the invention can be achieved at Mn contents of at least 1.0 wt%, in particular at least 1.6 wt% or at least 1.7 wt%. The positive effects achieved by the addition of Mn can be utilized particularly effectively at contents of up to 3 wt%, in particular up to 2.5 wt% or up to 2.1 wt%.

[0037] Nickel ("Ni") can be added to the steel selected according to the invention in amounts of up to 2.0 wt% to lower the melting point temperature. An effect of Ni is achieved at amounts of ≥ 0.3 wt%. Preferably, however, Ni is omitted as an effective alloying element or limited to a maximum of 0.5 wt%, and in particular < 0.3 wt%, in order to minimize the alloying costs of the steel powder used according to the invention. Ni contents of < 0.3 wt% can enter the steel used according to the invention as impurities that are ineffective with respect to its properties if it is produced using scrap. Preferably, in embodiments of the invention where no effective Ni content is to be present in the selected steel, the Ni content is nevertheless limited to less than 0.1 wt%.

[0038] The sum %Mn + %Ni of the contents %Mn of Mn and %Ni of Ni is limited to less than 5 mass-% in a steel selected according to the invention, in order to ensure that the steel undergoes a predominantly martensitic transformation during the cooling process occurring in the additive manufacturing process and that only minimal retained austenite content is present in the microstructure of the component obtained (%Mn + %Ni < 5 mass-%).

[0039] Chromium ("Cr") in contents of up to 6 wt%, in particular up to 5 wt% or up to 4 wt%, molybdenum in contents of up to 3.0 wt%, in particular up to 2 wt% or up to 1.5 wt%, tungsten ("W") in contents of up to 6 wt%, in particular up to 4 wt% or up to 3 wt%, and boron ("B") in contents of up to 0.0030 wt%, in particular up to 0.0020 wt%, may each optionally be present in the steel selected according to the invention to improve the through-hardenability.

[0040] Tungsten ("W") is less effective than Mo with regard to temperability, but can be used as a substitute element for Mo with regard to alloying costs. The addition of effective contents of Mo of at least 0.5 wt% and / or W of at least 0.75 wt% can promote the formation of carbides, thereby increasing the wear resistance of a component additively manufactured from steel powder alloyed according to the invention. A sufficient effect of Mo and / or W for the purposes of the invention can be achieved by limiting the sum of the contents of Mo and / or W to a maximum of 0.7 wt%, whereby Mo and W can each be present individually up to this content limit.If the effects of Mo and W are to be avoided, the content of these elements is limited to values ​​that are in the impurity range, i.e. ≤ 0.10 wt%, in particular ≤ 0.05 wt%, whereby in this case the sum of the Mo and W contents should ideally not exceed these values.

[0041] Optionally added Cr in amounts of at least 0.1 wt% also contributes to increased hardness and improved wear resistance through carbide formation.

[0042] Aluminum ("Al") is present in the steel selected according to the invention in amounts of 0.004 wt% to 0.035 wt%, as it is used for deoxidation during the steel production process. Al is particularly effective when added in amounts of 0.015 to 0.030 wt%.

[0043] Vanadium ("V") is also present in the steel selected according to the invention in amounts of at least 0.02 wt% to increase wear resistance. However, to prevent the formation of a secondary hardening maximum, the V content is limited to 0.3%. Optimal effects of the presence of V are achieved at V contents of at least 0.05 wt%, and in particular at least 0.07 wt%.

[0044] Sulfur ("S") in contents of up to 0.05 wt% can improve the machinability of components additively manufactured from steel powder used according to the invention. This effect can be achieved with S contents of at least 0.008 wt%, and in particular at least 0.01 wt%. However, higher S contents can lead to red fracture. To reliably prevent this, the S content can be limited to a maximum of 0.03 wt%. S contents of less than 0.008 wt% are ineffective with regard to the properties of the steel selected according to the invention and are among the impurities that are unavoidable during production. They enter the steel during production and can be accepted even if S is not specifically intended to be used to improve machinability.

[0045] Titanium ("Ti") can be added to the steel selected according to the invention in contents of up to 0.1 wt% to improve the wear resistance of components additively manufactured from powder used according to the invention by means of carbide formation. This effect can be reliably achieved at Ti contents of at least 0.01 wt%. However, at Ti contents of more than 0.1 wt%, coarse carbides may form, which would reduce the toughness of the material. Optimized effects of the optional presence of Ti can be achieved at Ti contents of up to 0.2 wt%, and in particular at contents of less than 0.2 wt%.

[0046] Like titanium, niobium ("Nb") also forms carbides, which increase the wear resistance of components additively manufactured from powder used according to the invention. This effect can be reliably achieved with Nb contents of at least 0.01 wt%. The effects made possible by the optional presence of Nb in the steel used according to the invention can be utilized particularly effectively when the Nb content is limited to a maximum of 0.02 wt%, and in particular to less than 0.02 wt%.

[0047] The impurities unavoidable during the manufacturing process, the total concentration of which must not exceed 0.55% by mass, include all alloying elements that enter the steel during its smelting and further processing. However, these elements must be present in concentrations that have no effect on the properties of the steel selected according to the invention for the steel particles of the steel powder used here. These impurities include phosphorus ("P") concentrations of up to 0.05% by mass and nitrogen ("N") concentrations of up to 0.12% by mass, preferably not more than 0.10% by mass or not more than 0.05% by mass.

[0048] According to the invention, the contents %Mn, %Si, %Cr, %Ni, %N and %B of Mn, Si, Cr, Ni, N and B are matched to each other such that the dimensionless term A = 200 − 30 × %Mn − 7 × %Si − 12 × %Cr − 16 × %Ni − 220 × %N + 34600 × %B the condition 0 < A < 225 This requirement is met if the relevant contents %Mn, %Si, %Cr, %Ni, %N and %B are used as simple percentage values. In this way, it is ensured that the Ms temperature of the steel intended for the steel particles of the steel powder according to the invention is significantly below 225 °C.

[0049] Such low Ms temperatures allow for the trouble-free additive processing of steel powder alloyed according to the invention using conventional devices equipped with a heating plate that can maintain the respective solidified part of the component at temperatures of up to 225 °C, in particular up to 200 °C. It has thus been experimentally demonstrated that it is reliably possible to additively manufacture components free of microcracks using steel powder according to the invention, and this is achieved with conventional devices in which the respective solidified section of the part to be produced has been maintained at low heating temperatures.

[0050] The method to which the use according to the invention is directed provides accordingly that the additive manufacturing of a component from steel powder produced according to the invention takes place on a heating plate whose heating temperature THeiz corresponds to at least a minimum heating temperature Tmin, which is calculated as a function of the respective Mn content %Mn, the respective Si content %Si, the respective Cr content %Cr, the respective Ni content %Ni, the respective N content %N and the respective B content %B of the steel according to the formula already given above for determining Tmin. For the heating temperature THeiz of the heating plate, Tmin ≤ THeiz ≤ 225 °C, in particular Tmin ≤ THeiz ≤ 220 °C.

[0051] Following this guideline, minimum heating temperatures Tmin of 150 °C, and in particular at least 175 °C, have proven effective in practice.

[0052] The invention will now be explained in more detail using exemplary embodiments.

[0053] Melts of aluminum-killed steels standardized under material numbers 1.2842 and 1.2510, conforming to the specifications of the invention, as well as of steel not falling under the invention with material number 1.6587, each having an aluminum content of 0.015 - 0.030 wt%, were atomized into steel particles in a conventional manner.

[0054] The detailed compositions of steels 1.2842, 1.2510, and 1.6587 used in the tests reported here are given in Table 1. The steels contained, at most, ineffective amounts of Ni, N, and B attributable to impurities.

[0055] Similarly, in Table 1, the value A of the term is given for each specific steel composition. A = 200 − 30 × %Mn − 7 × %Si − 12 × %Cr − 16 × %Ni − 220 × %N + 34600 × %B and those according to the formula Tmin ° C = 150 − 30 × %Mn − 7 × %Si − 12 × %Cr − 16 × %Ni − 220 × %N + 34600 × %B , The calculated minimum heating temperature Tmin and the experimentally determined Ms temperature are specified.

[0056] From the steel particles obtained, those with a particle diameter of 10 - 65 µm were selected by sieving and screening.

[0057] The steel particles selected in this way each formed three steel powders, with the steel particles of the first steel powder consisting of steel 1.2842, the steel particles of the second steel powder consisting of steel 1.2510 and the steel particles of the third steel powder consisting of steel 1.6587.

[0058] In three trials each, components E1_1 to E1_3, E2_1 to E2_3, and V_1 to V_3 were produced from steel powders using an additive manufacturing method, namely selective laser melting (SLM) with a laser power between 130 and 400 watts, layer thicknesses between 30 and 60 µm, and track spacing between 60 and 120 µm. The components were built on a heated plate maintained at a temperature THeiz. Accordingly, the solidified section of the component on the heated plate was maintained at this temperature.

[0059] The heating temperature THeiz was varied from experiment to experiment.

[0060] Micrographs were taken of the recovered components and examined for cracks under a light microscope at 500x magnification. Any cracks found were classified as "microscopic".

[0061] The results of the evaluation are entered in Table 2.

[0062] It was shown that when processing steel powders consisting of steels 1.2842 and 1.2510 corresponding to the specifications of the invention, and when adjusting the temperature THeiz according to the invention, it was possible to reliably produce components that were crack-free (rated "without cracks").

[0063] In contrast, setting heating temperatures THeiz that were too low, below the minimum heating temperature Tmin determined according to the invention, led to components that exhibited microscopic cracks.

[0064] Likewise, it was not possible to produce crack-free components with the steel powder produced from the steel 1.6587 selected in a manner not in accordance with the invention. Table 1 Steel %C %Si %Mn %Cr %Mo + %W %V Ms Tmin A [%] *) [°C] 1.2842 0,87 0,20 1.97 0,41 0,02 0,11 175 85 135 1.2510 0,96 0,32 1,12 0,60 0,58 0,20 205 107 157 1.6587 0,21 0,21 0,62 1,62 0,22 0,03 392 111 161 *) Values ​​in mass %, balance Fe and unavoidable impurities Table 2 Attempt Steel THeiz Cracks? Invention? E1_1 1.2842 RT **) Micro no E1_2 170 Without Yes E1_3 200 Without Yes E2_1 1.2510 100 Micro no E2_2 200 Without Yes E2_3 250 Without Yes V_1 1.6587 RT Micro no V_2 V_3 200 Micro no 300 Micro no **) RT = Room temperature

Claims

1. Use of a steel powder for additive manufacturing of a steel component, in which, in a work process which is repeated several times, steel powder is applied to a heating plate to build up the component, the applied steel powder is melted by means of an electron beam or laser beam to form a melt portion, and the melted melt portion is cooled to form a solid portion of the steel component, wherein the component growing in portions in this way, by means of the heating plate, is kept at a temperature which corresponds at least to a minimum heating temperature Tmin and is at most 225°C during production, and wherein the steel powder is formed of steel particles of a steel which has a martensite start temperature Ms of at most 225°C and, in % by mass, of C: 0.80 - 1.20%, Si: 0.1 - 1.0%, Mn: 0.1 - 4.0%, Ni: ≤ 2.0%, Cr: ≤ 6.00%, Mo: ≤ 3.0%, W: ≤ 6.0%, S: ≤ 0.05%, Al: 0.004 - 0.035%, V: 0.02 - 0.20%, Ti: ≤ 0.10%, Nb: ≤ 0.40%, B: ≤ 0.0030%, and the remainder consists of iron and steel-typical impurities, which in total do not exceed 0.55 wt. % and include up to 0.05% P and up to 0.12% N, wherein for the respective Mn content %Mn, the respective Ni content %Ni, the respective Si content %Si, the respective Cr content %Cr, the respective N content %N and the respective B content %B of the steel, each introduced as a % value, the following applies: %Mn + %Ni < 5% and 2. Use according to claim 1, characterized in that the C content of the steel is 0.85 - 1.0% by mass.

3. Use according to any of the preceding claims, characterized in that the Si content of the steel is at most 0.4% by mass.

4. Use according to any of the preceding claims, characterized in that the Mn content of the steel is 1.7 - 2.1% by mass.

5. Use according to any of the preceding claims, characterized in that the Cr content of the steel is at most 4% by mass.

6. Use according to claim 5, characterized in that the Cr content of the steel is at most 1% by mass.

7. Use according to any of the preceding claims, characterized in that the V content of the steel is at least 0.07% by mass.

8. Use according to any of the preceding claims, characterized in that the sum of the content of Mo and / or W of the steel is at most 0.7% by mass.

9. Use according to claim 8, characterized in that the Mo and W content of the steel is in total less than 0.05% by mass.

10. Use according to any of the preceding claims, characterized in that more than 90% of the steel particles have a particle diameter of 10 µm to 65 µm selected by sieving and sifting.

11. Use according to any of the preceding claims, characterized in that the minimum heating temperature Tmin of the heating plate is determined according to the following formula (3): wherein %Mn denotes the respective Mn content, %Si the respective Si content, %Cr the respective Cr content, %Ni the respective Ni content, %N the respective N content and %B the respective B content of the steel.

12. Use according to claim 11, characterized in that the temperature Tmin is at least 150°C.

13. Use according to claim 12, characterized in that the temperature Tmin is at least 175°C.

14. Use according to any of claims 11 to 13, characterized in that the temperature Tmin is at most 200°C.