Flame-retardant adhesive
Patent Information
- Application Number
- DE502020009365
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-18
- Filing Date
- 2020-11-10
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-11-10
AI Technical Summary
Current pressure-sensitive adhesives face a challenge in balancing adhesive strength and shear strength with flame retardancy, often compromising on soot formation during fires, as flame retardants can significantly reduce adhesive performance.
A pressure-sensitive adhesive composition incorporating poly(meth)acrylate and aromatic organophosphorus compounds, with specific monomer ratios of (meth)acrylic acid esters and acrylic acid, along with rosin esters, to achieve a balanced adhesive profile and effective flame retardancy.
The solution provides enhanced adhesive strength, shear strength, and minimized soot formation during fires, meeting demanding flame retardancy requirements while maintaining adhesive performance.
Description
[0001] The invention relates to the technical field of pressure-sensitive adhesives, as they are used in a wide variety of technical fields for the temporary or permanent bonding of two substrates. More specifically, a pressure-sensitive adhesive with improved flame-retardant properties is proposed.
[0002] In many areas of technology, for example in construction, the automotive industry, and the aircraft industry, increasingly demanding requirements are being placed on the flame-retardant behavior of installed components. Various test methods have been developed to meet specific requirements. For example, components and accessories used in aircraft construction must pass a so-called vertical Bunsen burner test. This also applies to adhesive tapes used in aircraft construction, for example, for attaching insulation packages or floor coverings. Accordingly, flame-retardant pressure-sensitive adhesives are required for such adhesive tapes. However, as has been shown, formulating pressure-sensitive adhesives with good flame-retardant properties is not without its challenges. The flame retardants used often lead to massive losses in adhesive strength and / or a significant deterioration in shear strength.Many flame-retardant pressure-sensitive adhesive compositions also exhibit strong soot development in the event of a fire, which is also undesirable. Thus, there is usually a trade-off between the required adhesive performance of the pressure-sensitive adhesives on the one hand and the equally required flame-retardant properties on the other.
[0003] In the past, there has been no shortage of attempts to defuse this conflict of objectives. For example, US Pat. No. 7,501,169 B2 describes an adhesive film composite comprising a substrate free of antimony and halogens and an adhesive polymer coated with a non-halogenated, phosphate-based flame retardant.
[0004] JP 2011148863 A discloses a composition comprising an acrylate polymer having a monomer base of acrylic acid and (meth)acrylic acid esters having 1 to 8 carbon atoms in the alcohol component, a phosphazene flame retardant, a phosphoric acid ester flame retardant, a crosslinker and an adhesive resin, wherein the polymer and flame retardant as well as the flame retardants are present in certain ratios to one another.
[0005] JP 2013018944 A follows a similar approach, where the polymer is composed of butyl acrylate, a monomer with a reactive functional group and / or an alkyl (meth)acrylate.
[0006] JP 2012031422 A describes a flame-retardant pressure-sensitive adhesive containing an acrylate ester copolymer at 100 parts by weight, ammonium polyphosphate at 50 to 115 parts by weight, aluminum hydroxide at 40 to 85 parts by weight and aliphatic polyalcohols.
[0007] JP 2015067653 A discloses a substrate having applied thereto an adhesive composition containing an adhesive resin at 100 parts by weight, a phosphinate-based flame retardant at 52 to 150 parts by weight and a phosphate ester-based flame retardant, which is liquid at room temperature, at 10 to 50 parts by weight.
[0008] EP 3 362 531 A1 relates to a halogen-free, flame-retardant adhesive composition which comprises an adhesive and a flame retardant composition comprising a phosphoric acid ester compound and a flame retardant selected from melamine cyanurate, melamine pyrophosphate and phosphinate salt.
[0009] JP 2017132893 A aims to create a pressure-sensitive adhesive for construction applications with good adhesion to rough substrates and excellent flame-retardant properties. This is to be achieved by curing a composition comprising 100 parts by weight of a polymerizable (meth)acrylic acid alkyl ester monomer, 10 to 50 parts by weight of a (meth)acrylic acid ester polymer with a weight-average molecular weight of 800,000 to 3,000,000, and 5 to 65 parts by weight of a halogen-free phosphoric acid ester-based flame retardant, the latter based on the total weight of the other two components, with the proportion of unreacted monomer in the total of these monomers before curing being a maximum of 1.5% by weight. A similar approach is also pursued in JP 2017179329 A.
[0010] WO 20148 079853 A1 describes a pressure-sensitive adhesive layer comprising 100 parts by weight of a (meth)acrylate ester polymer and 1 to 60 parts by weight of a halogen-free phosphate ester flame retardant, wherein the proportion of residual monomers is not more than 0.5% by weight.
[0011] CN 108329857 A relates to a single-sided adhesive tape, the adhesive layer of which is made of polyacrylate, crosslinkers, a first and second flame retardant and a solvent, the first flame retardant being solid at room temperature and the second being liquid at room temperature.
[0012] EP 3 093 322 A1 discloses a pressure-sensitive adhesive comprising an acrylic polymer composed of 63 wt% 2-ethylhexyl acrylate, 25 wt% butyl acrylate and 12 wt% acrylic acid, and a terpene phenol resin.
[0013] JP 2013 199651 A discloses a flame-retardant pressure-sensitive adhesive composed of 30 parts by weight of an acrylic copolymer of butyl acrylate (84 wt%), 2-ethylhexyl acrylate (10 wt%), and acrylic acid (6 wt%) with a T g of -51°C, 30 parts by weight of a xylene-phenol novolak resin, and 40 parts by weight of a xylene novolak resin. 30 parts by weight of a phenoxy-substituted cyclophosphazene were also added to the pressure-sensitive adhesive as a flame retardant.
[0014] There is a continuing need for pressure-sensitive adhesives with good adhesive and flame-retardant properties. The object of the invention was to provide such a pressure-sensitive adhesive that exhibits particularly good bond strength and shear strength. Furthermore, the lowest possible soot formation in the event of a fire was desirable.
[0015] A first and general object of the invention with which this object is achieved is a pressure-sensitive adhesive which: contains at least one poly(meth)acrylate and at least one aromatic organophosphorus compound as flame retardant and is characterized in that the monomer composition on which the poly(meth)acrylate is based comprises at least one (meth)acrylic acid ester whose alcohol component contains more than 4 C atoms; at least one (meth)acrylic acid ester whose alcohol component contains a maximum of 4 C atoms; and acrylic acid and / or (meth)acrylic acid in a total of at least 5 wt.%; and the pressure-sensitive adhesive contains at least one rosin ester.
[0016] Such a pressure-sensitive adhesive shows a balanced adhesive profile and good flame-retardant properties.
[0017] For the purposes of the invention, a pressure-sensitive adhesive is understood, as is common parlance, to be a substance that is permanently tacky and adhesive, at least at room temperature. A characteristic of a pressure-sensitive adhesive is that it can be applied to a substrate by pressure and remains adhered there, whereby the pressure to be applied and the duration of this pressure are not defined in more detail. In general, however, depending on the exact type of pressure-sensitive adhesive and the substrate, the temperature, and the humidity, the application of short-term, minimal pressure, which does not go beyond a light touch for a brief moment, is sufficient to achieve the adhesion effect; in other cases, a longer exposure period of higher pressure may be necessary.
[0018] Pressure-sensitive adhesives have special, characteristic viscoelastic properties that lead to their permanent tack and adhesive strength. They are characterized by the fact that, when mechanically deformed, both viscous flow processes and the development of elastic restoring forces occur. The respective proportions of both processes are in a specific relationship to each other, depending on the precise composition, structure, and degree of crosslinking of the pressure-sensitive adhesive, as well as the speed and duration of the deformation and the temperature.
[0019] The viscous flow component is necessary to achieve adhesion. Only the viscous components, often caused by macromolecules with relatively high mobility, enable good wetting and flow onto the substrate to be bonded. A high proportion of viscous flow leads to high pressure-sensitive adhesion (also referred to as tack or surface stickiness) and thus often to high adhesion. Highly cross-linked systems, crystalline, or glass-like polymers, are generally not or at least only slightly pressure-sensitive due to the lack of flowable components.
[0020] The proportional elastic restoring forces are necessary to achieve cohesion. They are caused, for example, by very long-chain and highly entangled macromolecules, as well as by physically or chemically cross-linked macromolecules, and enable the transfer of forces acting on an adhesive bond. They ensure that an adhesive bond can sufficiently withstand continuous loading, for example, in the form of permanent shear stress, over an extended period of time.
[0021] For a more precise description and quantification of the degree of elastic and viscous components as well as the relationship between the components, the storage modulus (G') and loss modulus (G"), which can be determined using Dynamic Mechanical Analysis (DMA), are used. G' is a measure of the elastic component, G" a measure of the viscous component of a material. Both parameters depend on the deformation frequency and the temperature.
[0022] These parameters can be determined using a rheometer. The material under test is subjected to sinusoidal oscillating shear stress, for example, in a plate-on-plate arrangement. Shear stress-controlled devices measure the deformation as a function of time and the temporal offset of this deformation relative to the application of the shear stress. This temporal offset is referred to as the phase angle δ.
[0023] The storage modulus G' is defined as follows: G' - (τ / γ) • cos(δ) (τ = shear stress, γ = deformation, δ = phase angle = phase shift between shear stress and deformation vector). The definition of the loss modulus G" is: G" - (τ / γ) • sin(δ) (τ = shear stress, γ = deformation, δ = phase angle = phase shift between shear stress and deformation vector).
[0024] A composition is considered to be a pressure-sensitive adhesive and is defined as such within the meaning of the invention in particular if, at 23 °C, in the deformation frequency range from 10 0< to 10 1< rad / sec, both G` and G" are at least partly in the range from 10 3< to 10 7< Pa. "Partly" means that at least a section of the G' curve lies within the window spanned by the deformation frequency range from 10 0< to 10 1< rad / sec (abscissa) and the range of G' values from 10 3< to 10 7< Pa (ordinate), and if at least a section of the G" curve also lies within the corresponding window.
[0025] A "poly(meth)acrylate" is understood to mean a polymer obtainable by radical polymerization of acrylic and / or methacrylic monomers and, optionally, other copolymerizable monomers. In particular, a "poly(meth)acrylate" is understood to mean a polymer whose monomer base consists of at least 50 wt.% acrylic acid, methacrylic acid, acrylic esters, and / or methacrylic esters, with acrylic esters and / or methacrylic esters being present at least in part, preferably at least 30 wt.%, based on the total monomer base of the polymer in question.
[0026] The pressure-sensitive adhesive of the invention preferably contains poly(meth)acrylate in a total amount of 30 to 70 wt. %, more preferably in a total amount of 35 to 65 wt. %, in particular in a total amount of 40 to 60 wt. %, such as, for example, in a total amount of 45 to 60 wt. %, based in each case on the total weight of the pressure-sensitive adhesive. It may contain a (single) poly(meth)acrylate or several poly(meth)acrylates; the plural term "poly(meth)acrylates" thus includes—also in the continuation of the present description—in its meaning, just like the term "total," both the presence of a single poly(meth)acrylate and the presence of several poly(meth)acrylates.
[0027] The glass transition temperature of the poly(meth)acrylate of the pressure-sensitive adhesive of the invention is preferably <0°C, more preferably between -20 and -50°C, in particular between -25 and -40°C, such as, for example, between -28 and -35°C. The glass transition temperature of polymers or of polymer blocks in block copolymers is determined in the present application by means of dynamic scanning calorimetry (DSC). For this purpose, approximately 5 mg of an untreated polymer sample is weighed into an aluminum crucible (volume 25 µl) and sealed with a perforated lid. A DSC 204 F1 from Netzsch is used for the measurement. The measurement is carried out under nitrogen for inerting purposes. The sample is first cooled to -150°C, then heated at a heating rate of 10 K / min to +150°C and cooled again to -150°C. The subsequent second heating curve is again run at 10 K / min and the change in heat capacity is recorded.Glass transitions are detected as steps in the thermogram (test method A).
[0028] According to the invention, the monomer composition underlying the poly(meth)acrylate comprises at least one (meth)acrylic acid ester whose alcohol component contains more than 4 carbon atoms. Preferably, the (meth)acrylic acid ester whose alcohol component contains more than 4 carbon atoms is selected from the group consisting of isooctyl acrylate, isooctyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, 2-propylheptyl acrylate, and 2-propylheptyl methacrylate. Particularly preferred is the (meth)acrylic acid ester whose alcohol component contains more than 4 carbon atoms, 2-ethylhexyl acrylate.
[0029] (Meth)acrylic acid esters whose alcohol component contains more than 4 carbon atoms are present in the monomer composition underlying the poly(meth)acrylate of the pressure-sensitive adhesive of the invention, preferably in a total amount of 50 to 90 wt. %, particularly preferably in a total amount of 60 to 80 wt. %, and in particular in a total amount of 65 to 75 wt. One or more (meth)acrylic acid esters whose alcohol component contains more than 4 carbon atoms may be present in the monomer composition; the term "total" encompasses both variants.
[0030] According to the invention, the monomer composition underlying the poly(meth)acrylate further comprises at least one (meth)acrylic acid ester whose alcohol component contains a maximum of 4 carbon atoms. Preferably, the (meth)acrylic acid ester whose alcohol component contains a maximum of 4 carbon atoms is selected from the group consisting of n-butyl acrylate, n-butyl methacrylate, and methyl acrylate; in particular, the (meth)acrylic acid ester is methyl acrylate.
[0031] (Meth)acrylic acid esters whose alcohol component contains a maximum of 4 carbon atoms are present in the monomer composition underlying the poly(meth)acrylate of the pressure-sensitive adhesive of the invention, preferably in a total amount of 10 to 40 wt. %, particularly preferably in a total amount of 15 to 30 wt. %, and in particular in a total amount of 20 to 25 wt. One or more (meth)acrylic acid esters whose alcohol component contains a maximum of 4 carbon atoms may be present in the monomer composition; the term "total" encompasses both variants. In a particularly preferred embodiment, the monomer composition underlying the poly(meth)acrylate of the pressure-sensitive adhesive of the invention contains more than 15 wt. %, preferably more than 17 wt. %, such as, for example, 20 to 30 wt. %, of methyl acrylate.
[0032] The monomer composition preferably comprises acrylic acid and / or (meth)acrylic acid in a total amount of at least 6 wt.%, in particular in a total amount of at least 6.5 wt.%. Particularly preferably, the monomer composition comprises acrylic acid in a total amount of at least 6 wt.%, more preferably in a total amount of at least 6.5 wt.%.
[0033] The poly(meth)acrylates are preferably produced by conventional radical polymerizations or controlled radical polymerizations. The poly(meth)acrylates can be produced by copolymerization of the monomers using conventional polymerization initiators and, if appropriate, regulators. Polymerization takes place at conventional temperatures in bulk, in emulsion, for example, in water or liquid hydrocarbons, or in solution.
[0034] The poly(meth)acrylates are preferably prepared by copolymerizing the monomers in solvents, particularly preferably in solvents having a boiling range of 50 to 150 °C, in particular of 60 to 120 °C, using 0.01 to 5 wt.%, in particular 0.1 to 2 wt.%, in each case based on the total weight of the monomers, of polymerization initiators.
[0035] In principle, all conventional initiators are suitable. Examples of radical sources include peroxides, hydroperoxides, and azo compounds, for example, dibenzoyl peroxide, cumene hydroperoxide, cyclohexanone peroxide, di-t-butyl peroxide, cyclohexylsulfonylacetyl peroxide, diisopropyl percarbonate, t-butyl peroctoate, and benzpinacol. Preferred radical initiators are 2,2'-azobis(2-methylbutyronitrile) (Vazo ®< 67 ™< from DuPont), 2,2'-azobis(2-methylpropionitrile) (2,2'-azobisisobutyronitrile; AIBN; Vazo ®< 64 ™< from DuPont), and bis(4-tert-butylcyclohexanyl) peroxydicarbonate.
[0036] Preferred solvents for the preparation of the poly(meth)acrylates are alcohols such as methanol, ethanol, n- and isopropanol, n- and isobutanol, especially isopropanol and / or isobutanol; hydrocarbons such as toluene and especially gasolines with a boiling range of 60 to 120 °C; ketones, especially acetone, methyl ethyl ketone, and methyl isobutyl ketone; esters such as ethyl acetate, and mixtures of the aforementioned solvents. Particularly preferred solvents are mixtures containing isopropanol in amounts of 2 to 15 wt. %, especially 3 to 10 wt. %, based in each case on the solvent mixture used.
[0037] The poly(meth)acrylate(s) of the pressure-sensitive adhesive composition of the invention are preferably crosslinked by linking reactions—particularly in the sense of addition or substitution reactions, or even coordination reactions—of the carboxylic acid functions contained therein with special compounds—so-called crosslinkers. The positions within the crosslinker molecules from which the macromolecules are attacked are also referred to as "reactive centers." Crosslinker molecules contain two or more reactive centers and are therefore capable of linking two or more macromolecules together. Undesirable side reactions occasionally occur in which the reactive centers of one and the same crosslinker molecule react with only one macromolecule.
[0038] Basically, two types of networkers can be distinguished: 1) Covalent crosslinkers, whose reactive centers covalently attack the poly(meth)acrylate macromolecules, thus forming a covalent bond between the reactive center of the crosslinker and the attacked carboxylic acid group of the macromolecule. In principle, all reaction types leading to the formation of covalent bonds are possible. 2) Coordinative crosslinkers, whose reactive centers coordinately attack the poly(meth)acrylate macromolecules, thus forming a coordinative bond between the reactive center of the crosslinker and the attacked carboxylic acid group of the macromolecule. In principle, all reaction types leading to the formation of coordinative bonds are possible.
[0039] In one embodiment, the poly(meth)acrylate of the pressure-sensitive adhesive according to the invention is at least covalently crosslinked with one or more crosslinkers selected from the group consisting of glycidylamines, multifunctional epoxides, multifunctional aziridines and multifunctional isocyanates. Particularly preferably, the poly(meth)acrylate of the pressure-sensitive adhesive according to the invention is at least covalently bonded to one or more crosslinkers selected from the group consisting of N,N,N',N'-tetrakis(2,3-epoxypropyl)cyclohexyl-1,3-dimethylamine, N,N,N',N'-tetrakis(2,3-epoxypropyl)-m-xylyl-α,α'-diamine, (3,4-epoxycyclohexyl)methyl-3,4-epoxycyclohexylcarboxylate, trimethylolpropane tris(2-methyl-1-aziridinepropionate), tolylene diisocyanate (TDI), 2,4-tolylene diisocyanate dimer, naphthylene-1,5-diisocyanate (NDI), o-tolylene diisocyanate (TODI), diphenylmethane diisocyanate (MDI), triphenylmethane triisocyanate, tris-(p-isocyanatophenyl)thiophosphate and Polymethylene polyphenyl isocyanate crosslinked.
[0040] The poly(meth)acrylates of the pressure-sensitive adhesive according to the invention can be crosslinked with one or more covalent crosslinkers, one or more coordinative crosslinkers or with a mixture of one or more covalent and coordinative crosslinkers.
[0041] The pressure-sensitive adhesive according to the invention preferably contains covalent crosslinkers in a total amount of 0.015 to 0.1% by weight, particularly preferably in a total amount of 0.02 to 0.075% by weight, in each case based on the total weight of the poly(meth)acrylates.
[0042] The pressure-sensitive adhesive of the invention further comprises at least one aromatic organophosphorus compound as a flame retardant. The organophosphorus compound is preferably halogen-free. The organophosphorus compound is preferably selected from the group consisting of phosphoric acid esters and iminophosphoranes.
[0043] The organophosphorus compound is particularly preferably an aromatic organophosphorus compound, in particular an aromatic phosphoric acid ester. "Aromatic" means that the compound in question has at least one aromatic structural unit, e.g., an aromatic substituent. The organophosphorus compound is most preferably selected from the group consisting of triphenyl phosphate, resorcinol bis(diphenyl phosphate), and bisphenol A bis(diphenyl phosphate). For example, the organophosphorus compound is selected from resorcinol bis(diphenyl phosphate) and bisphenol A bis(diphenyl phosphate), in particular it is bisphenol A bis(diphenyl phosphate).
[0044] The pressure-sensitive adhesive may contain one or more organophosphorus compounds. The pressure-sensitive adhesive of the invention preferably contains organophosphorus compounds in a total amount of at least 15% by weight, more preferably at least 18% by weight.
[0045] The pressure-sensitive adhesive of the invention may contain further components beyond those listed above. The pressure-sensitive adhesive of the invention contains at least one rosin ester as an adhesive resin, also referred to as an adhesion promoter or tackifier. According to the general understanding of those skilled in the art, a "tackifier" is understood to mean an oligomeric or polymeric resin that increases the autohesion (tack, inherent stickiness) of the pressure-sensitive adhesive compared to an otherwise identical pressure-sensitive adhesive that does not contain a tackifier.
[0046] In principle, all known adhesive resins compatible with poly(meth)acrylates are suitable. The pressure-sensitive adhesive preferably comprises at least one adhesive resin selected from terpene-phenolic resins and rosin esters, with the pressure-sensitive adhesive according to the invention containing at least one rosin ester. The rosin ester is, in particular, a pentaerythritol rosin ester. As has been shown, this allows for further improvement of the flame retardancy, which is reflected in particular in minimized burning distances and further reduced soot formation.
[0047] The pressure-sensitive adhesive composition according to the invention preferably contains 18 to 28% by weight of adhesive resin, in particular 21 to 24% by weight.
[0048] Furthermore, the pressure-sensitive adhesive according to the invention may contain further additives, for example Plasticizers, e.g. low molecular weight poly(meth)acrylates, phthalates, water-soluble plasticizers; functional additives, e.g. initiators and accelerators; electrically conductive materials, e.g. conjugated polymers, doped conjugated polymers, metal pigments, metal particles, metal salts, metal-coated particles, e.g. silver-coated spheres; graphite, conductive carbon black, carbon fibers, ferromagnetic additives; foaming agents, blowing agents, expandable hollow spheres; the latter, however, only in an amount which does not negatively affect the flame-retardant effect; compounding agents, nucleating agents; ageing inhibitors, e.g. primary and secondary antioxidants; light stabilizers, ozone protectants; powdered and granular fillers, dyes and pigments, e.g. E.g. fibers, carbon blacks, zinc oxides, titanium dioxide, chalks, silicas, silicates, solid or hollow glass spheres, solid or hollow polymer spheres, ceramic solid or hollow spheres, microspheres made of other materials; and organic fillers..
[0049] In one embodiment, the pressure-sensitive adhesive contains at least one iminophosphorane and / or at least one amine. Preferred iminophosphoranes are cyclophosphazenes. More preferably, the pressure-sensitive adhesive contains at least one phenoxy-substituted cyclophosphazene and / or at least one sterically hindered N-alkoxyamine. In particular, the pressure-sensitive adhesive contains at least one sterically hindered N-alkoxyamine, e.g., a reaction product of N,N"-1,2-ethanediylbis(1,3-propanediamine) with cyclohexane and peroxidized N-butyl-2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine (CAS No. 191680-81-6).
[0050] As has been shown, such additives can be used to further optimize the flame retardant performance of the pressure-sensitive adhesive.
[0051] The pressure-sensitive adhesive of the invention preferably contains 15 to 35% by weight, preferably 20 to 30% by weight, of flame retardants. The term "flame retardant" encompasses, in particular, organophosphorus compounds, iminophosphoranes, and amines, without this being understood as limiting.
[0052] The pressure-sensitive adhesive of the invention is preferably prepared from a dispersion or solution by sequentially mixing the components, then forming the dispersion or solution into a sheet, and subsequently removing the solvent used. Preferred solvents are those already described for the preparation of the poly(meth)acrylates.
[0053] The invention further relates to the use of a pressure-sensitive adhesive according to the invention as a flame-retardant pressure-sensitive adhesive, in particular as a flame-retardant pressure-sensitive adhesive in the equipment of aircraft, trains, ships, vehicles and buildings.
[0054] In one embodiment, the pressure-sensitive adhesive according to the invention is used for producing permanent bonds in interior spaces, particularly preferably for fixing thermal insulation material, in particular between interior and exterior walls; for fixing non-textile flooring in damp rooms, e.g., in kitchens and toilets; for fixing floor coverings in general; as an adhesive for moisture barrier applications and / or in corrosion protection applications and / or for fixing mirrors and / or lights.
[0055] In a further embodiment, the pressure-sensitive adhesive of the invention is used to produce bonds, preferably permanent bonds, in electric vehicles. The pressure-sensitive adhesive is particularly preferably used to produce bonds in the battery, in particular for producing mounting bonds, for example for bonding fire-resistant materials between battery cells; for bonding flexible printed circuit boards; for bonding foams, in particular silicone foams; for producing bonds for the purpose of electrically insulating battery modules and / or components, in particular for electrically insulating battery cells (battery cell wrapping) and / or the heating / cooling plate. Examples Raw materials used:
[0056] Butyl acrylate: CAS number: 141-32-2 Ethylhexyl acrylate: CAS number: 103-11-7 Methyl acrylate: CAS number: 96-33-3 Acrylic acid: CAS number: 79-10-7 Vazo 67: 2,2'-Azodi(2-methylbutyronitrile), CAS number 13472-08-7, Akzo Nobel Perkadox 16: Bis-(4-tert-butylcyclohexanyl) peroxydicarbonate, CAS number 15520-11-3, Akzo Nobel Dertophene T 105: Terpene phenolic resin, softening point approx. 105 °C; MW ~ 850 g / mol; DRT Foral 105 E: hydrogenated pentaerythritol rosin ester, softening point approx. 100 °C; MW ~ 1,002 g / mol; Eastman Erisys GA 240 : N,N,N',N'-Tetrakis(2,3-epoxypropyl)-m-xylene-α,α'-diamine, Emerald Performance Materials GC-BDP: Bisphenol A bis(diphenyl phosphate), CAS number: 5945-33-5; GREENCHEMICALS SPA GC-TPP: triphenyl phosphate, CAS number 115-86-6; GREENCHEMICALS SPA NORTH MIN RDP: Tetraphenyl-m-phenylene bis(phosphate) (resorcinol bis(diphenyl phosphate)), CAS number 57583-54-7; Nordmann Rabitle FP 110: phenoxyphosphazene; Fushimi pharmaceutical CO., Ltd. Flamestab NOR 116 FF: CAS number: 191680-81-6; BASF SE Production of polyacrylates: Polyacrylate 1
[0057] A conventional 2 L glass reactor suitable for radical polymerizations under evaporative cooling was filled with 300 g of a monomer mixture of 201 g n-butyl acrylate, 90 g 2-ethylhexyl acrylate and 9 g acrylic acid as well as 200 g acetone:special boiling point spirit 60 / 95 (1:1). After 45 minutes of nitrogen gas being passed through the reactor with stirring, it was heated to 58 °C and 0.15 g of 2,2'-azodi(2-methylbutyronitrile) (Vazo 67 ®<, Akzo Nobel) dissolved in 6 g of acetone was added. The external heating bath was then heated to 75 °C and the reaction was carried out at a constant external temperature. After a reaction time of 1 h, another 0.15 g of Vazo 67 ®<, dissolved in 6 g of acetone, was added. After 3 hours, the mixture was diluted with 90 g of special boiling point spirit 60 / 95.
[0058] After a reaction time of 5 h 30 min, 0.45 g of bis(4-tert-butylcyclohexanyl) peroxydicarbonate (Perkadox 16 ®<, Akzo Nobel) dissolved in 9 g of acetone was added. After a reaction time of 7 hours, a further 0.45 g of bis(4-tert-butylcyclohexanyl) peroxydicarbonate (Perkadox 16 ®<, Akzo Nobel) dissolved in 9 g of acetone was added. After a reaction time of 10 hours, the mixture was diluted with 90 g of special-boiling-point spirit 60 / 95. The reaction was stopped after 24 h and cooled to room temperature.
[0059] The resulting polyacrylate 1 has a glass transition temperature (T g ) according to test method A of -46°C. Polyacrylate 2
[0060] A conventional 2 L glass reactor suitable for radical polymerizations under evaporative cooling was filled with 300 g of a monomer mixture of 219 g of 2-ethylhexyl acrylate, 60 g of methyl acrylate and 21 g of acrylic acid as well as 200 g of acetone: special boiling point spirit 60 / 95 (1:1). After 45 minutes of nitrogen gas being passed through the reactor with stirring, it was heated to 58 °C and 0.15 g of 2,2'-azodi(2-methylbutyronitrile) (Vazo 67 ®<, Akzo Nobel) dissolved in 6 g of acetone was added. The external heating bath was then heated to 75 °C and the reaction was carried out at a constant external temperature. After a reaction time of 1 h, another 0.15 g of Vazo 67 ®<, dissolved in 6 g of acetone, was added. After 3 hours, the mixture was diluted with 90 g of special boiling point spirit 60 / 95.
[0061] After a reaction time of 5 h 30 min, 0.45 g of bis(4-tert-butylcyclohexanyl) peroxydicarbonate (Perkadox 16 ®<, Akzo Nobel) dissolved in 9 g of acetone was added. After a reaction time of 7 hours, a further 0.45 g of bis(4-tert-butylcyclohexanyl) peroxydicarbonate (Perkadox 16 ®<, Akzo Nobel) dissolved in 9 g of acetone was added. After a reaction time of 10 hours, the mixture was diluted with 90 g of special-boiling-point spirit 60 / 95. The reaction was stopped after 24 h and cooled to room temperature.
[0062] The resulting polyacrylate 2 has a glass transition temperature (T g ) according to test method A of about -34°C. Production of pressure-sensitive adhesives: Example 1
[0063] The terpene phenolic resin Dertophene T 105 was dissolved in the polyacrylate 1 solution in a weight ratio of 70:30, based on the polymer solids content. Bisphenol A diphenyl phosphate was added to this solution so that the solids content in the mixture was 30% by mass. It was then diluted with acetone to achieve a final solids content of 38%. The mixture was placed on a roller bench until a homogeneous solution was formed (approximately 12 hours). A crosslinker solution (3 wt.% Erysis GA 240 in acetone) was then added at a dosage of 0.075 parts by weight, based on 100 parts by weight of polymer, and the adhesive was coated onto a siliconized film using a doctor blade on a laboratory coating table. The coatings were then dried at 120 °C for 15 minutes. Examples 2-9
[0064] The procedure in Example 1 was followed. The composition of the adhesives is given in Table 1. Production of test samples:
[0065] For the tests, a 23 µm thick PET film etched with trichloroacetic acid was laminated onto the adhesive. A further 100 µm thick layer of adhesive was laminated onto the adhesive-free side of the film, creating a double-sided tape. Test methods: Adhesive strength
[0066] The CRES steel bond strength was determined at a test temperature of 23 °C + / - 1 °C and 50% + / - 5% relative humidity.
[0067] A 20 mm wide strip of the adhesive tape sample was applied to steel plates that had previously been washed twice with acetone and once with isopropanol, and then left to air for 5 minutes to allow the solvent to evaporate. The pressure-sensitive adhesive strip was pressed onto the substrate twice with a contact pressure equivalent to a weight of 2 kg. The adhesive tape was then immediately peeled off the substrate at a speed of 300 mm / min and at an angle of 90°. The measurement results are given in N / cm and are averaged from three measurements. Static shear test
[0068] The shear strength was determined at a test temperature of 23 °C + / - 1 °C and 50% + / - 5% relative humidity.
[0069] The test specimens were cut to a width of 13 ± 0.2 mm and stored in a controlled atmosphere for at least 16 hours. 50 x 25 mm ASTM steel plates, 2 mm thick and with a 20 mm marking line, were used for the test. These plates were intensively cleaned several times with acetone before bonding and then allowed to dry for 1-10 minutes. The bonded area was 13 x 20 ± 0.2 mm. The test strip was applied longitudinally to the center of the substrate by wiping it with a finger or a suitable wiper, avoiding air pockets, so that the upper edge of the test specimen was exactly aligned with the 20 mm marking line.
[0070] Since the tested samples were double-sided, the back was taped with aluminum foil. The free, protruding end was taped with paper or a sheet of card. The adhesive strip was then rolled back and forth twice using a 2 kg roller. After rolling, a belt loop (weight 5-7 g) was attached to the protruding end of the adhesive tape.
[0071] An adapter plate was then attached to the front of the shear test plate using a screw and nut. To ensure the adapter plate was firmly seated on the plate, the screw was firmly tightened by hand.
[0072] The prepared plate was attached to a counter clock using a hook on the adapter plate; a 1 kg weight was then smoothly hooked into the belt loop.
[0073] The application time between rolling and loading was 12 minutes. The time until bond failure was measured in minutes; the measurement results are the average of three measurements. 12s Vertical Bunsen Burner Test
[0074] The 12-s vertical Bunsen burner test is conducted according to FAR 25.853 (Appendix F Part I (a)(1)(II)): The sample is held in a vertical position, suspended freely (i.e., without being bonded to a substrate), in a U-frame, and a Bunsen burner flame is applied from below for 12 seconds. After the 12-s exposure time, the burner is removed, and the material is observed. The following parameters are recorded: a) Average afterburning time: time in s during which the sample burns after the burner flame has been removed; b) Average droplet burning time: time in s during which the burning material continues to burn after it has fallen from the sample; c) Average burning length: distance from the initial sample edge to the furthest point where the sample is damaged. At least 3 test specimens were tested.
[0075] The samples are considered flame-retardant if the following requirements according to FAR 25.853 (Appendix F Part I (a)(1)(II)) have been met: Average afterburn time: < 15 s Average drop burning time: < 5 s Average burning length: < 203.2 mm.
[0076] The results of the tests are shown in Table 1. Table 1: Compositions of the examples and results Example No. Composition 1 (cf.) 2 (cf.) 3 4 5 6 7 8 9 Polyacrylate 1 49% Polyacrylate 2 49% 49% 49% 55,3% 55,3% 55,3% 55,3% 55,3% Dertophene T 105 21% 21% Foral 105-E 21% 21% 23,7% 23,7% 23,7% Foral 85-E 23,7% Foral AX 23,7% Bisphenol A bis(diphenyl phosphate) 30% 30% 30% 20% 20% 20% 20% Resorcinol bis(diphenyl) phosphate 20% Triphenyl phosphate 20% Rabitle FP 110 10% Flamestab NOR 116 FF 1% 1% 1% 1% 1% Erysis GA 240 0,04% 0,04% 0,04% 0,04% 0,04% 0,04% 0,04% 0,04% 0,04% Example No. 1 2 3 4 5 6 7 8 9 Adhesive strength 90° CRES [N / cm] 7,2 12,9 10,5 11,0 12,0 5,6 5,1 3 4,4 Shear life RT [min] 633 3312 2888 4595 7213 2140 1532 718 6878 Burning distance [mm] 213 175 165 78 25 75 200 28 62 Afterburn duration [s] 0 14 7 0 0 0 8,4 0 0 Afterburning time drops [s] 0 0 1 0 0 1 1 0 0 Soot formation Yes Yes No No No No No No No
Claims
1. Pressure-sensitive adhesive comprising: - at least one poly(meth)acrylate and - at least one aromatic organophosphorus compound as flame retardant; characterized in that the monomer composition forming the basis for the poly(meth)acrylate comprises - at least one (meth)acrylic ester whose alcohol component contains more than 4 carbon atoms; - at least one (meth)acrylic ester whose alcohol component contains not more than 4 carbon atoms; and - acrylic acid and / or methacrylic acid at a total of at least 5 wt%; and the pressure-sensitive adhesive comprises at least one rosin ester.
2. Pressure-sensitive adhesive according to Claim 1, characterized in that the glass transition temperature of the poly(meth)acrylate by test method A in the description is < 0°C, preferably between -20 and -50°C, more particularly between -25 and -40°C, such as, for example, between -28 and -35°C.
3. Pressure-sensitive adhesive according to either of the preceding claims, characterized in that the at least one (meth)acrylic ester whose alcohol component contains more than 4 carbon atoms is present in the monomer composition forming the basis for the poly (meth) acrylate at a total of 50 to 90 wt%, preferably at a total of 60 to 80 wt%, and more particularly at a total of 65 to 75 wt%.
4. Pressure-sensitive adhesive according to either of Claims 1 and 2, characterized in that the at least one (meth)acrylic ester whose alcohol component contains not more than 4 carbon atoms is present in the monomer composition forming the basis for the poly (meth) acrylate at a total of 10 to 40 wt%, preferably at a total of 15 to 30 wt%, and more particularly at a total of 20 to 25 wt%.
5. Pressure-sensitive adhesive according to any of the preceding claims, characterized in that the monomer composition forming the basis for the poly (meth) acrylate comprises methyl acrylate at more than 15 wt%, preferably more than 17%, such as, for example, 20 to 30 wt%.
6. Pressure-sensitive adhesive according to any of the preceding claims, characterized in that the pressure-sensitive adhesive comprises organophosphorus compounds at a total of at least 15 wt%, based on the total weight of the pressure-sensitive adhesive.
7. Pressure-sensitive adhesive according to any of the preceding claims, characterized in that the organophosphorus compound is bisphenol A bis(diphenyl phosphate).
8. Pressure-sensitive adhesive according to any of the preceding claims, characterized in that the rosin ester is a pentaerythritol rosin ester.
9. Pressure-sensitive adhesive according to any of the preceding claims, characterized in that the pressure-sensitive adhesive comprises at least one iminophosphorane, preferably at least one cyclophosphazene and more particularly at least one phenoxy-substituted cyclophosphazene.
10. Pressure-sensitive adhesive according to any of Claims 1 to 8, characterized in that the pressure-sensitive adhesive comprises at least one amine such as, for example, a sterically hindered N-alkoxyamine, and optionally additionally at least one iminophosphorane.
11. Use of a pressure-sensitive adhesive according to any of the preceding claims as a flame-retardant pressure-sensitive adhesive.