High-temperature-resistant vehicle-mounted OCA optical adhesive and preparation method thereof

Through the combination of modified polyester and thermal stabilizer, the problem of unstable performance of OCA optical adhesive in high temperature environment is solved, and its high temperature resistance and adhesion are significantly improved, ensuring the stability under long-term high temperature exposure and sunlight. Security.

CN118978880APending Publication Date: 2024-11-19JIANGSU TOPFLY NEW MATERIALS CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411022245.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing OCA optical glue has unstable performance in high temperature environments and is prone to yellowing, bubbles and falling off, affecting the display effect and safety of use.

Method used

High-temperature resistant OCA optical glue is prepared through esterification and polycondensation reaction to improve its high-temperature resistance, and the adhesion and adhesion force are improved through uniform dissolution and mixing of ethyl acetate.

Benefits of technology

It significantly improves the high temperature resistance and adhesion of OCA optical glue, reduces the appearance of bubbles at high temperatures, and enhances its stability under long-term high temperature exposure.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of optical cement materials, and particularly discloses a high-temperature-resistant vehicle-mounted OCA optical cement and a preparation method thereof. The high-temperature-resistant vehicle-mounted OCA optical adhesive is prepared from the following raw material components in parts by weight: 70 to 90 parts of polyacrylate, 5 to 10 parts of modified polyester, 0.1 to 1 part of a cross-linking agent, 0.01 to 0.1 part of a coupling agent, 0.1 to 1.2 parts of a photoinitiator, 1 to 3 parts of a heat stabilizer and 0.1 to 0.5 part of a synergist, the modified polyester comprises the following raw materials: aromatic diol, aromatic dicarboxylic acid, inorganic nanoparticles and a catalyst. A preparation method of the high-temperature-resistant vehicle-mounted OCA optical adhesive comprises the following steps: dissolving the modified polyester by using the ethyl acetate to obtain a mixed solution, then adding the mixed solution into the polyacrylate, finally adding the heat stabilizer, the synergist, the cross-linking agent, the coupling agent and the photoinitiator, and uniformly stirring and mixing to obtain the OCA optical adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of optical adhesives, and in particular to a high temperature resistant vehicle-mounted OCA optical adhesive and a preparation method thereof. Background Art

[0002] With the continuous development of in-vehicle display technology, the performance requirements for OCA optical adhesives are getting higher and higher. Although the commonly used OCA optical adhesives can meet the general transparency and bonding strength requirements, their performance stability in high temperature environments still needs to be improved. Especially under long-term high temperature exposure, the adhesive layer is prone to yellowing, bubbles, or even falling off, which seriously affects the display effect and safety of use. Summary of the invention

[0003] In order to improve the high temperature resistance of OCA optical adhesive, the present application provides a high temperature resistant vehicle-mounted OCA optical adhesive and a preparation method thereof.

[0004] In the first aspect, the present application provides a high temperature resistant vehicle-mounted OCA optical adhesive, which adopts the following technical solution: A high-temperature resistant vehicle-mounted OCA optical adhesive, the raw materials of which include the following components in parts by weight: 70-90 parts of polyacrylate, 5-10 parts of modified polyester, 0.1-1 part of cross-linking agent, 0.01-0.1 part of coupling agent, 0.1-1.2 parts of photoinitiator, 1-3 parts of thermal stabilizer, and 0.1-0.5 part of synergist; the raw materials of the modified polyester include aromatic diol, aromatic dicarboxylic acid, inorganic nanoparticles, and a catalyst.

[0005] By adopting the above technical scheme, under the action of a catalyst, aromatic diols and aromatic dicarboxylic acids are synthesized into modified polyesters. Aromatic diols, as the flexible part of the polyester molecular chain, can improve the high temperature resistance of the polyester while maintaining its flexibility; aromatic dicarboxylic acids have a rigid benzene ring structure, which can increase the rigidity of the polyester molecular chain, thereby improving its high temperature resistance; inorganic nanoparticles themselves have high high temperature resistance, which can further improve the high temperature resistance of polyester. Therefore, the addition of modified polyester, combined with heat stabilizers and synergists, improves the high temperature resistance of the obtained OCA optical adhesive.

[0006] In a specific embodiment, the preparation method of the modified polyester comprises the following steps: Aromatic dicarboxylic acid, inorganic nanoparticles and catalyst are added to aromatic diol, stirred and mixed evenly, firstly esterification reaction is carried out at 200-300°C, and then polycondensation reaction is carried out at 250-300°C to obtain modified polyester.

[0007] By adopting the above technical scheme, aromatic dicarboxylic acid, inorganic nanoparticles and catalyst are first added to aromatic diol, stirred, and then esterification reaction is carried out under the action of the catalyst, and then polycondensation reaction is carried out to obtain modified polyester with good high temperature resistance.

[0008] In a specific embodiment, the weight ratio of the aromatic diol, the aromatic dicarboxylic acid, the inorganic nanoparticles, and the catalyst is 1: (1.0-1.2): (0.02-0.04): (0.0002-0.0004).

[0009] By adopting the above technical solution, the ratio of aromatic diol, aromatic dicarboxylic acid, inorganic nanoparticles and catalyst in the raw materials is further limited, so that the modified polyester can be better synthesized and its performance can be improved.

[0010] In a specific embodiment, the aromatic diol includes a mixture of one or more of ethylene glycol, propylene glycol, and butanediol.

[0011] In a specific embodiment, the aromatic dicarboxylic acid includes a mixture of one or more of terephthalic acid, isophthalic acid, and phthalic acid.

[0012] In a specific embodiment, the inorganic nanoparticles include a mixture of one or more of nano-silicon dioxide, nano-aluminum oxide, and nano-zinc oxide.

[0013] By adopting the above technical solution, nano silicon dioxide, nano aluminum oxide and nano zinc oxide are resistant to high temperatures, thereby improving the high temperature resistance of the prepared modified polyester.

[0014] In a specific embodiment, the catalyst includes a mixture of one or more of an organic tin compound, a titanate compound, and a germanium compound.

[0015] In a specific embodiment, the heat stabilizer includes a mixture of one or more of calcium soap, zinc soap and barium soap.

[0016] By adopting the above technical solution, metal soap compounds such as calcium soap, zinc soap and barium soap can react with unstable groups in polymer materials, thereby improving the thermal stability of the materials.

[0017] In a specific embodiment, the synergist includes a mixture of one or more of epoxidized soybean oil, epoxidized fatty acid methyl ester, triphenyl phosphite, and triethyl phosphite.

[0018] By adopting the above technical scheme, epoxidized soybean oil and epoxy fatty acid methyl ester can react with the active groups in the polymer material, and triphenyl phosphite and triethyl phosphite can capture the free radicals generated during the processing of the polymer material, both of which can prevent the degradation of the material, thereby improving the stability of the material.

[0019] In the second aspect, the present application provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, which adopts the following technical solution: A method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive comprises the following steps: First, the modified polyester is dissolved in ethyl acetate to obtain a mixed solution, which is then added to the polyacrylate, and finally a heat stabilizer, a synergist, a cross-linking agent, a coupling agent, and a photoinitiator are added, and the mixture is stirred and mixed to obtain an OCA optical adhesive.

[0020] By adopting the above technical scheme, the modified polyester is first dissolved with ethyl acetate and then added to the polyacrylate, followed by adding a heat stabilizer, a synergist, a cross-linking agent, a coupling agent, and a photoinitiator, and stirring and mixing them evenly to obtain an OCA optical adhesive with good high temperature resistance; and the addition of ethyl acetate can also improve the adhesion and bonding strength of the optical adhesive.

[0021] In summary, the present application includes at least one of the following beneficial technical effects: 1. In the present application, under the action of a catalyst, aromatic diols and aromatic dicarboxylic acids are synthesized into modified polyesters. Aromatic diols, as the flexible part of the polyester molecular chain, can maintain the flexibility of the polyester while improving the high temperature resistance of the polyester; aromatic dicarboxylic acids have a rigid benzene ring structure, which can increase the rigidity of the polyester molecular chain, thereby improving its high temperature resistance; inorganic nanoparticles themselves have high high temperature resistance, which can further improve the high temperature resistance of polyester, so the addition of modified polyester, combined with thermal stabilizers and synergists, improves the high temperature resistance of the prepared OCA optical adhesive; 2. In the present application, epoxidized soybean oil and epoxy fatty acid methyl ester can react with active groups in polymer materials, and triphenyl phosphite and triethyl phosphite can capture free radicals generated during the processing of polymer materials, which can prevent the degradation of materials, thereby improving the stability of materials; 3. The method in the present application first uses ethyl acetate to dissolve the modified polyester, then adds it to the polyacrylate, and then adds a heat stabilizer, a synergist, a cross-linking agent, a coupling agent, and a photoinitiator, and stirs and mixes evenly to obtain an OCA optical adhesive with good high temperature resistance; and the addition of ethyl acetate can also improve the adhesion and bonding strength of the optical adhesive. DETAILED DESCRIPTION

[0022] The present application is further described in detail below with reference to the embodiments.

[0023] All raw materials in the embodiment can be obtained commercially. Aromatic diols include but are not limited to mixtures of one or more of ethylene glycol, propylene glycol, and butanediol, and ethylene glycol is preferred in this application; aromatic dicarboxylic acids include but are not limited to mixtures of one or more of terephthalic acid, isophthalic acid, and phthalic acid, and terephthalic acid is preferred in this application; inorganic nanoparticles include but are not limited to mixtures of one or more of nano-silicon dioxide, nano-alumina, and nano-zinc oxide, and nano-silicon dioxide is preferred in this application; catalysts include but are not limited to mixtures of one or more of organic tin compounds, titanate compounds, and germanium compounds, and dibutyltin diisooctanoate is preferred in this application; heat stabilizers include but are not limited to mixtures of one or more of calcium soaps, zinc soaps, and barium soaps, and stearic acid is preferred in this application; synergists include but are not limited to mixtures of one or more of epoxy soybean oil, epoxy fatty acid methyl ester, triphenyl phosphite, and triethyl phosphite, and epoxy fatty acid methyl ester is preferred in this application.

[0024] Preparation Example Preparation Example 1 Preparation Example 1 provides a method for preparing a modified polyester, comprising the following steps: Aromatic dicarboxylic acid, inorganic nanoparticles and catalyst are added to aromatic diol, stirred and mixed evenly, and made into slurry. Esterification reaction is first carried out at 200°C and relative pressure of 0.1MPa for 1.5 hours, and then polycondensation reaction is carried out at 250°C and absolute pressure of 75Pa for 5 hours to obtain modified polyester; wherein the aromatic dicarboxylic acid is terephthalic acid; the inorganic nanoparticles are nano-silicon dioxide; the catalyst is dibutyltin diisooctanoate; the aromatic diol is ethylene glycol; the weight ratio of aromatic diol, aromatic dicarboxylic acid, inorganic nanoparticles and catalyst is 1:0.9:0.01:0.0001.

[0025] Preparation Example 2 Preparation Example 2 provides a method for preparing a modified polyester, comprising the following steps: Aromatic dicarboxylic acid, inorganic nanoparticles and catalyst are added to aromatic diol, stirred and mixed evenly, and made into slurry. Esterification reaction is first carried out at 250°C and relative pressure of 0.1MPa for 1.5 hours, and then polycondensation reaction is carried out at 275°C and absolute pressure of 75Pa for 5 hours to obtain modified polyester; wherein the aromatic dicarboxylic acid is terephthalic acid; the inorganic nanoparticles are nano-silicon dioxide; the catalyst is dibutyltin diisooctanoate; the aromatic diol is ethylene glycol; the weight ratio of aromatic diol, aromatic dicarboxylic acid, inorganic nanoparticles and catalyst is 1:0.9:0.01:0.0001.

[0026] Preparation Example 3 Preparation Example 3 provides a method for preparing a modified polyester, comprising the following steps: Aromatic dicarboxylic acid, inorganic nanoparticles and catalyst are added to aromatic diol, stirred and mixed evenly, and made into slurry. First, esterification reaction is carried out at 300°C and relative pressure of 0.1MPa for 1.5 hours, and then polycondensation reaction is carried out at 300°C and absolute pressure of 75Pa for 5 hours to obtain modified polyester; wherein the aromatic dicarboxylic acid is terephthalic acid; the inorganic nanoparticles are nano-silicon dioxide; the catalyst is dibutyltin diisooctanoate; the aromatic diol is ethylene glycol; the weight ratio of aromatic diol, aromatic dicarboxylic acid, inorganic nanoparticles and catalyst is 1:0.9:0.01:0.0001.

[0027] Preparation Example 4 The difference between Preparation Example 4 and Preparation Example 2 is that the weight ratio of the aromatic diol, the aromatic dicarboxylic acid, the inorganic nanoparticles, and the catalyst is 1:1:0.02:0.0002; the remaining steps are consistent with Preparation Example 2.

[0028] Preparation Example 5 The difference between Preparation Example 5 and Preparation Example 2 is that the weight ratio of the aromatic diol, the aromatic dicarboxylic acid, the inorganic nanoparticles, and the catalyst is 1:1.1:0.03:0.0003; the remaining steps are consistent with Preparation Example 2.

[0029] Preparation Example 6 The difference between Preparation Example 6 and Preparation Example 2 is that the weight ratio of the aromatic diol, the aromatic dicarboxylic acid, the inorganic nanoparticles, and the catalyst is 1:1.2:0.04:0.0004; the remaining steps are consistent with Preparation Example 2.

[0030] Preparation Example 7 The difference between Preparation Example 7 and Preparation Example 2 is that the weight ratio of the aromatic diol, the aromatic dicarboxylic acid, the inorganic nanoparticles, and the catalyst is 1:1.3:0.05:0.0005; the remaining steps are consistent with Preparation Example 2.

[0031] Preparation Example 8 Preparation Example 8 provides a method for preparing a modified polyester, comprising the following steps: Add aromatic dicarboxylic acid and catalyst to aromatic diol, stir and mix evenly, make into slurry, first carry out esterification reaction at 200°C and relative pressure of 0.1MPa for 1.5h, then carry out polycondensation reaction at 250°C and absolute pressure of 75Pa for 5h to obtain modified polyester; wherein the aromatic dicarboxylic acid is terephthalic acid; the catalyst is dibutyltin diisooctanoate; the aromatic diol is ethylene glycol; the weight ratio of aromatic diol, aromatic dicarboxylic acid and catalyst is 1:0.9:0.0001. Example

[0032] Example 1 Embodiment 1 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 1, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0033] Example 2 Embodiment 2 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 2, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0034] Example 3 Embodiment 3 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 3, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0035] Example 4 Embodiment 4 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 4, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0036] Example 5 Embodiment 5 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 5, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0037] Example 6 Embodiment 6 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 6, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0038] Example 7 Embodiment 7 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 7, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0039] Example 8 Embodiment 8 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 8 kg of the modified polyester in Preparation Example 5, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 80 kg of polyacrylate, and finally add 2 kg of heat stabilizer, 0.3 kg of enhancer, 0.5 kg of cross-linker, 0.05 kg of coupling agent, and 0.6 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; the photoinitiator is 2,4,6-trimethylbenzoyl.

[0040] Example 9 Embodiment 9 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 10 kg of the modified polyester in Preparation Example 5, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 90 kg of polyacrylate, and finally add 3 kg of heat stabilizer, 0.5 kg of enhancer, 1 kg of cross-linker, 0.1 kg of coupling agent, and 1.2 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0041] Comparative Example Comparative Example 1 Comparative Example 1 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add 0.1 kg of crosslinking agent, 0.01 kg of coupling agent and 0.1 kg of photoinitiator to 71.1 kg of polyacrylate, stir and mix evenly to obtain OCA optical adhesive; wherein the crosslinking agent is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0042] Comparative Example 2 Comparative Example 2 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add ethyl acetate to 5 kg of the modified polyester in Preparation Example 8, stir to dissolve the modified polyester to obtain a mixed solution, then add it to 70 kg of polyacrylate, and finally add 1 kg of heat stabilizer, 0.1 kg of enhancer, 0.1 kg of cross-linker, 0.01 kg of coupling agent, and 0.1 kg of photoinitiator, stir and mix evenly to obtain OCA optical glue; wherein the heat stabilizer is stearic acid; the enhancer is epoxy fatty acid methyl ester; the cross-linker is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0043] Comparative Example 3 Comparative Example 3 provides a method for preparing a high temperature resistant vehicle-mounted OCA optical adhesive, comprising the following steps: Add 1kg of heat stabilizer, 0.1kg of synergist, 0.1kg of cross-linking agent, 0.01kg of coupling agent and 0.1kg of photoinitiator to 75kg of polyacrylate, stir and mix evenly to obtain OCA optical glue; the heat stabilizer is stearic acid; the synergist is epoxy fatty acid methyl ester; the cross-linking agent is aluminum acetylacetonate; the coupling agent is 3-(2,3-epoxypropoxy)propyltriethoxysilane; and the photoinitiator is 2,4,6-trimethylbenzoyl.

[0044] Performance testing High temperature resistance: evenly coat the OCA optical adhesive on a heavy release film with a thickness of 75μm to a coating thickness of 175μm, then bake at 120°C for 3min, adhere a light release film with a thickness of 50μm to the adhesive surface, and then mature at 70°C for 24h to obtain the OCA optical adhesive film; tear off the light release film, adhere it to the mobile phone cover glass, then tear off the heavy release film, and adhere it to another mobile phone cover glass. After degassing and UV treatment, let it stand for 1 day, and then place it at 150°C, 0.2Mpa, and 90% humidity for 14 days, and then observe the number of bubbles in the sample, which are no bubbles, very few bubbles, a small amount of bubbles, and more bubbles. The fewer the bubbles, the better the high temperature resistance of the optical adhesive.

[0045] Table 1 Test results of optical adhesive sample Number of bubbles Example 1 Very few bubbles Example 2 Very few bubbles Example 3 Very few bubbles Example 4 No bubbles Example 5 No bubbles Example 6 No bubbles Example 7 Very few bubbles Example 8 No bubbles Example 9 No bubbles Comparative Example 1 More bubbles Comparative Example 2 A small amount of bubbles Comparative Example 3 A small amount of bubbles Combining Example 1 and Comparative Examples 1-3, the high temperature resistance of the optical adhesive in Example 1 is the best. It can be seen that when preparing the optical adhesive, aromatic diols, aromatic dicarboxylic acids, modified polyester synthesized from inorganic nanoparticles, as well as heat stabilizers and enhancers are added to the raw materials. The combination of the three can improve the high temperature resistance of the optical adhesive.

[0046] In combination with Examples 1-3, the adhesive films formed by the optical adhesives in Examples 1-3 all have very few bubbles, which shows that when preparing the modified polyester, the synthesis conditions of the modified polyester in Preparation Examples 1-3 are better, so that the optical adhesive has better high temperature resistance.

[0047] In combination with Example 2 and Examples 4-7, the optical adhesive in Example 4-6 has better high temperature resistance. It can be seen that when preparing the modified polyester, the ratio of aromatic diol, aromatic dicarboxylic acid, inorganic nanoparticles, and catalyst is preferably 1: (1.0-1.2): (0.02-0.04): (0.0002-0.0004), and the obtained optical adhesive has better high temperature resistance.

[0048] In combination with Example 5, Example 8 and Example 9, the adhesive films formed by the optical adhesives in Example 5, Example 8 and Example 9 are free of bubbles. It can be seen that under the raw material ratios in Example 5, Example 8 and Example 9, the optical adhesives obtained have better high temperature resistance.

[0049] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high temperature resistant vehicle-mounted OCA optical adhesive, characterized by: The raw materials of the optical adhesive include the following components in parts by weight: 70-90 parts of polyacrylate, 5-10 parts of modified polyester, 0.1-1 parts of cross-linking agent, 0.01-0.1 parts of coupling agent, 0.1-1.2 parts of photoinitiator, 1-3 parts of thermal stabilizer, and 0.1-0.5 parts of synergist; the raw materials of the modified polyester include aromatic diols, aromatic dicarboxylic acids, inorganic nanoparticles, and catalysts.

2. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 1, characterized in that: The preparation method of the modified polyester comprises the following steps: Aromatic dicarboxylic acid, inorganic nanoparticles and catalyst are added to aromatic diol, stirred and mixed evenly, firstly esterification reaction is carried out at 200-300°C, and then polycondensation reaction is carried out at 250-300°C to obtain modified polyester.

3. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 2, characterized in that: The weight ratio of the aromatic diol, the aromatic dicarboxylic acid, the inorganic nanoparticles and the catalyst is 1: (1.0-1.2): (0.02-0.04): (0.0002-0.0004).

4. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 2, characterized in that: The aromatic diol includes a mixture of one or more of ethylene glycol, propylene glycol and butanediol.

5. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 2, characterized in that: The aromatic dicarboxylic acid includes a mixture of one or more of terephthalic acid, isophthalic acid and phthalic acid.

6. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 2, characterized in that: The inorganic nanoparticles include a mixture of one or more of nano-silicon dioxide, nano-aluminum oxide and nano-zinc oxide.

7. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 2, characterized in that: The catalyst comprises a mixture of one or more of an organic tin compound, a titanate compound and a germanium compound.

8. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 1, characterized in that: The heat stabilizer includes a mixture of one or more of calcium soap, zinc soap and barium soap.

9. The high temperature resistant vehicle-mounted OCA optical adhesive according to claim 1, characterized in that: The synergist comprises a mixture of one or more of epoxidized soybean oil, epoxidized fatty acid methyl ester, triphenyl phosphite and triethyl phosphite.

10. A method for preparing the high temperature resistant vehicle-mounted OCA optical adhesive according to any one of claims 1 to 9, characterized in that: The following steps are involved: First, the modified polyester is dissolved in ethyl acetate to obtain a mixed solution, which is then added to the polyacrylate, and finally a heat stabilizer, a synergist, a cross-linking agent, a coupling agent, and a photoinitiator are added, and the mixture is stirred and mixed to obtain an OCA optical adhesive.

Citation Information

Cited By

  • Vehicle-mounted OCA optical adhesive and preparation method thereof

    CN119931513A

  • Anti-dazzle and ultraviolet-blocking vehicle-mounted OCA optical adhesive and preparation method thereof

    CN120843019A

  • High-temperature-resistant and high-air-permeability vehicle-mounted OCA adhesive and preparation method thereof

    CN121699543A