METHOD FOR MANUFACTURING A WATCH GLASS WITH AT LEAST ONE RECESS AND TOOL FOR SUCH A METHOD
Patent Information
- Application Number
- DE502020009408
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-16
- Filing Date
- 2020-04-22
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-04-22
AI Technical Summary
Current methods for producing watch glasses with recesses face challenges such as precise positioning difficulties, high rejection rates due to size and shape deviations, rough inner surfaces, and inability to create angular recesses, leading to suboptimal optical effects and increased production time.
A method involving a starting glass with greater original thickness than the desired watch glass, heated to a temperature below its melting point to allow precise pressing of recesses without deformation, using a tool with a circumferential projection and inner projections to form the recesses and shape the glass to the desired thickness, ensuring precise dimensions and smooth surfaces.
This method enables the production of watch glasses with recesses that meet quality requirements, allowing for precise placement of decorative elements, reducing rejection rates, and enabling various shapes and lighting effects, while maintaining the glass's optical clarity and precision.
Description
[0001] The invention relates to a method for producing a watch crystal with at least one recess, as well as a tool used in such a method. Watch crystals with recesses for accommodating gemstones, indices, or other (decorative) elements are known from the prior art. Such a watch crystal is described, for example, in DE 10 2015 204613.
[0002] WO2013081119 A1 teaches a method for pressing a cover glass with indentations, which can be polished after pressing. The pressing die comprises an at least partially circumferential projection and smaller projections within this circumferential projection. US5049177 A discloses a tool for pressing glass comprising a base body with a circumferential projection and further projections within the circumferential projection.
[0003] Typically, the recesses are drilled into the watch crystal using a mechanical drill, an ultrasound device, a laser beam, or a water jet. However, these methods have some disadvantages.
[0004] Drilling a recess or hole requires very precise positioning of the tool, which can be laborious and / or difficult using the methods described. This then results in the recess not being placed in the exact location intended, which means the watch crystal can no longer be used for quality reasons.
[0005] If a recess in a watch crystal with multiple or multiple recesses exhibits deviations in size and / or shape, or generally fails to meet the expected manufacturing requirements, this renders the entire crystal worthless. For example, in a watch crystal with twelve recesses, a 5% defect rate in the recesses would result in more than 50% of the watch crystals being rejected. A deviation from a perfect recess can occur, for example, due to a chip in the crystal.
[0006] In addition, the recesses are roughened on the inside after drilling, regardless of the drilling method used. If a decorative element is to be inserted into the recess, the roughness of the inner surface of the recesses will impair the optical effect of the watch crystal.
[0007] To eliminate this problem and achieve a highly polished recess, the recess must be polished in a second step using polishing paste and a flexible polishing burr. However, the internal dimensions of the recess may no longer have an absolutely precise shape after this step.
[0008] Especially when using mechanical drills such as diamond drills, it is impossible to achieve square recesses. Furthermore, mechanical drilling can cause the edge of the recess to chip on the glass surface. It should also be noted that drilling itself is generally a very time-consuming process, which may require water cooling.
[0009] Due to all these disadvantages, a 100% fit of an element, especially a gemstone, into an optically fully transparent and polished recess is very difficult to achieve using the means described.
[0010] It is therefore an object of the invention to propose a method for producing a watch crystal with at least one recess, which overcomes the disadvantages described above and, in particular, enables the production of a watch crystal with a more precise recess. It is also an object of the invention to provide a tool that can be used in the production of such a watch crystal.
[0011] The first object is achieved by a method for producing a watch glass with at least one recess according to claim 1.
[0012] In particular, the method comprises the steps of providing a starting glass which has a greater original thickness than a predetermined thickness of the watch glass, heating the starting glass to a predetermined temperature below the melting temperature of the starting glass, pressing at least one recess into the starting glass and machining the starting glass with the at least one recess pressed therein, such that the thickness of the starting glass is reduced to the predetermined thickness of the watch glass for shaping / forming the watch glass. The heating of the starting glass serves to soften the starting glass so that the recess can be pressed in. The predetermined temperature is in particular selected such that the starting glass becomes so soft orhas a viscosity such that the recess can be pressed into the starting glass without the glass melting during pressing in or the glass deforming after the corresponding tool for pressing in the recess has been removed. Advantageously, the predetermined temperature is greater than or equal to 90% of the melting temperature and less than the melting temperature of the starting glass. The proposed method produces a watch glass with at least one recess, wherein the recess meets the desired quality requirements with regard to its dimensions, shape and surface properties. Due to the greater original thickness of the starting glass than the predetermined thickness of the watch glass, deformation of the region of the starting glass which is ultimately intended to correspond to the watch glass and to have the recess (recess region) is avoided when pressing in the at least one recess.This also prevents any deformation of the at least one recess that would otherwise result. In this regard, the starting glass advantageously has a stabilizing region with an original thickness corresponding to the difference between the original thickness of the starting glass and the predetermined thickness of the watch glass. In particular, the proposed method can prevent deformation as described above, since the starting glass can be stabilized in place via the stabilizing region during the pressing-in of the at least one recess. Thus, a visually high-quality appearance of the watch glass can be achieved if a decorative element, such as a gemstone, is inserted into the recess.Furthermore, the proposed method makes it possible to produce recesses of different shapes / cross-sections, for example, square recesses, and thus also to use elements, especially gemstones, of different shapes in the watch glass. This offers a wide variety of appearances for the watch glass, particularly due to the different lighting effects achieved by combining recesses and the elements inserted therein.
[0013] Within the scope of the invention, the term "watch glass" refers specifically to the end product (finished product). In other words, the watch glass is the glass after the proposed manufacturing process has been completed. Accordingly, within the scope of the invention, the starting glass is understood specifically as the glass that is or must be processed to ultimately produce the watch glass. In other words, within the scope of the invention, the term "starting glass" refers to the glass in every step of the proposed process until the watch glass is obtained.
[0014] In this context, within the scope of the invention, the term "original" with reference to the thickness of the starting glass or the stabilization region of the starting glass means in particular that the starting glass and thus also the stabilization region are those before any step of the proposed method where processing of the starting block takes place.
[0015] In particular, the starting glass has the form of a glass block, a glass plate, a glass rod or the like before its processing begins.
[0016] In particular, the at least one recess further comprises a base. This applies both to the recess in the initial glass and to the finished watch glass. In other words, the recess is advantageously not a continuous recess.
[0017] However, it is also possible that the recess in the original crystal (i.e., the recess immediately after the pressing process) is continuous. Alternatively, it is possible that the pressing process does not create a continuous recess, but that it then becomes a continuous recess in the finished watch crystal, especially if the underside of the original crystal is ground back during further processing.
[0018] Furthermore, a pressing direction, ie a direction in which the recess extends, is preferred, parallel to the direction of the thickness of the starting glass.
[0019] Preferably, a plurality of recesses, in particular identical recesses, are pressed into the starting glass.
[0020] Preferably, the at least one recess is pressed into the watch glass to a depth greater than a predetermined depth of the recess. In other words, the recess is formed deeper than the recess in the watch glass in a first step. The step of processing the starting glass with the at least one recess pressed into it, such that the thickness of the starting glass is reduced to the predetermined thickness of the watch glass for forming the watch glass, also comprises reducing the depth of the recess to the predetermined depth of the recess in the watch glass. The initially greater depth of the recess can ensure that any dimensional and / or shape deviation, which could possibly be caused by the pressing process in the region of an edge of the recess, will only be present in the starting glass and not in the finished watch glass.This can have a direct, positive impact on the manufacturing precision of at least one recess. The depth of the press-fit is also referred to as the offset.
[0021] According to the invention, the starting glass is reshaped so that a first region with a first cross-section and a second region with a second cross-section are formed in the starting glass. The first region has at least one recess, the first cross-section being smaller than the second cross-section. Particularly preferably, the first cross-section corresponds to a predetermined cross-section of the watch glass.
[0022] In particular, the starting glass is pressed to form the first region and the second region. For this purpose, the starting glass is pressed to a depth that is less than the thickness or original thickness of the starting glass. In this case, the pressing preferably corresponds to the forming of the starting glass. The pressing to form the first region and the second region can preferably be carried out in one step. The direction of pressing of the starting glass is referred to as the pressing direction in the context of the present invention.
[0023] In particular, the first cross section and the second cross section are substantially perpendicular to the press-in direction.
[0024] Preferably, the starting glass is formed such that the first region has a first thickness and the second region has a second thickness. The first thickness is preferably smaller than the second thickness. The sum of the first thickness and the second thickness is, in particular, greater than the predetermined thickness of the watch glass.
[0025] In particular, when the starting glass is pressed to form the first region and the second region, the depth to which the starting glass is pressed corresponds to the first thickness of the first region.
[0026] In other words, the thickness of the starting glass after forming or pressing the starting glass to form the first region and the second region is preferably smaller than the original thickness of the starting glass and larger than the predetermined thickness of the watch glass.
[0027] In this case, the difference between the thickness of the starting glass after the forming or pressing of the starting glass to form the first region and the second region preferably corresponds to the thickness of the stabilization region in this state of the process.
[0028] The second region can preferably be part of the stabilization region. In this case, the second region and a part of the first region preferably correspond to the stabilization region. The thickness of the stabilization region in this state of the starting glass is advantageously smaller than the original thickness of the stabilization region due to the pressing process. The first thickness of the first region is advantageously greater than the predetermined thickness of the watch glass. The second thickness of the second region is smaller than the original thickness of the stabilization region.
[0029] Preferably, a ratio of the original thickness of the starting glass and the predetermined thickness of the watch glass is in a range between "2 to 1" and "4 to 1", particularly preferably between "4 to 1" and "6 to 1".
[0030] In particular, a ratio of the thickness of the starting glass after forming or pressing the starting glass, whereby the first region and the second region are formed, and the predetermined thickness of the watch glass is in a range between "2 to 1" and "4 to 1", particularly preferably between "4 to 1" and "6 to 1".
[0031] According to a preferred embodiment of the invention, the finished watch crystal has a thickness between 1.4 mm and 1.8 mm, in particular 1.7 mm. The upper region preferably has a thickness that is (approximately) 0.5 mm greater than the thickness of the finished watch crystal. The second region is in particular (approximately) 6 mm thick.
[0032] This means that after the forming or pressing of the starting glass, the starting glass according to this preferred embodiment of the invention has a thickness between 7.9 mm and 8.3, in particular equal to 8.2 mm.
[0033] Preferably, the first region and the second region are formed in one step with the pressing-in of the recess. In other words, the additional forming of the starting glass to form the first region with a first cross-section and the second region with a second cross-section in the starting glass preferably takes place simultaneously with the pressing-in of the recess. This accelerates the entire process.
[0034] Advantageously, a direction of pressing the starting glass to form the first region and the second region is parallel to the pressing direction of the recess.
[0035] Preferably, the starting glass is cooled after pressing in the recess or forming the first region and the second region, and before machining the starting glass to reduce its thickness to the predetermined thickness of the watch glass for forming the watch glass. In particular, the starting glass is cooled to a temperature at which the starting glass is hard and no longer bendable.
[0036] Particularly preferably, the starting glass is cooled according to a predetermined cooling curve. This relaxes the starting glass, which relieves the buildup of stresses in the glass.
[0037] Furthermore, at least the second region is preferably ground. "At least" means that either only the second region or the second region and part of the first region can be ground. Thus, the starting glass takes on the final outer shape (outer contour) of the watch glass, and a top and bottom of the starting glass are formed parallel to each other after this step.
[0038] After the grinding process, the starting glass advantageously corresponds to the first region if only the second region is ground, or to the remaining part of the first region if the second region and part of the first region are ground. Preferably, after grinding at least the second region, an underside of the starting glass is polished.
[0039] In particular, a bottom surface of the starting glass is polished so that after polishing, a thickness of the starting glass corresponds to a sum of the predetermined thickness of the watch glass and a difference between the offset and the predetermined depth of the recess.
[0040] Furthermore, an upper surface of the starting glass is preferably ground and / or polished. In particular, an upper surface of the starting glass is ground and / or polished by the difference between the offset depth and the predetermined depth of the recess for forming the watch glass.
[0041] According to a preferred embodiment of the invention, the grinding and polishing of the upper side of the starting glass take place before the grinding of at least the second region. Alternatively, the grinding of at least the second region and the polishing of the underside of the starting glass can preferably take place before the grinding and / or polishing of the upper side of the starting glass.
[0042] The steps of cooling, grinding, and / or polishing the underside of the starting glass, and grinding and / or polishing the top side of the starting glass can advantageously be performed when producing many glasses at once. For example, the glass coins can be applied to grinding discs in quantities of 40 to 100 and ground together in a single operation. In particular, the top side of the starting glass is located in front of the underside of the starting glass in the pressing direction and / or the pressing direction. In other words, the top side is, in particular, the side into which the at least one recess is pressed and / or onto which the starting glass is pressed.
[0043] Preferably, the pressing direction corresponds to the pressing direction.
[0044] The second object is achieved by a tool according to claim 10, which comprises a base body having a first, at least partially circumferential, projection for pressing a starting glass and at least one second projection for pressing at least one recess into the starting glass. The second projection is arranged in an inner region of the first projection.
[0045] In the context of the invention, the second projection is also referred to as a pin.
[0046] According to the invention, the first at least partially circumferential projection and the at least second projection extend in the same direction.
[0047] Particularly preferably, the first projection is formed completely circumferentially.
[0048] The first projection, which is at least partially circumferential, advantageously projects beyond the second projection.
[0049] The first projection, which at least partially surrounds the entire circumference, is preferably annular. However, other shapes are also possible.
[0050] Preferably, the second projection is made of highly polished stamping steel.
[0051] Preferably, the tool has a plurality of second projections.
[0052] In particular, all second projections are identical to one another, particularly in terms of shape and dimensions. However, it is also possible to provide different second projections in the tool.
[0053] Further details, advantages and features of the present invention will become apparent from the following description of a preferred embodiment with reference to the drawing.
[0054] It shows: Fig. 1 shows a first step of the method according to the preferred embodiment, Fig. 2 shows a second step of the method according to the preferred embodiment, Fig. 3 shows a third step of the method according to the preferred embodiment, Fig. 4a shows a fourth step of the method according to the preferred embodiment, Fig. 4b shows the product after the fourth step of Fig. 4a , Fig. 5 a fifth step of the method according to the preferred embodiment, Fig. 6 a sixth step of the method according to the preferred embodiment, and Fig. 7 the watch glass produced by the method.
[0055] The following is based on Figures 1 to 7 a method for producing a watch glass with at least one recess according to a preferred embodiment is described in detail.
[0056] The finished watch glass 10, which has a predetermined thickness d10, is in Figure 7 shown, where Figures 1 to 6show the steps of the preferred embodiment of the method. The method uses a tool 100 which is Figures 1 to 3 can be seen.
[0057] Figure 1 shows a first step of the process.
[0058] In this step, a starting glass 1 is provided which has a greater original thickness d1 than the predetermined thickness d10 of the watch glass 10. In particular, the ratio of the original thickness d1 of the starting glass 1 to the predetermined thickness d10 of the watch glass 10 is two to one, preferably three to one, particularly preferably 4 to 1. Due to the oversize of the starting glass 1, a more precise production of the watch glass and its recess(es) is possible. This will be explained in more detail later with reference to the further steps of the method.
[0059] The starting glass 1 is preferably designed in the form of a glass block. However, it is also possible for the starting glass 1 to be in the form of a glass rod, a glass plate, or the like.
[0060] Within the scope of the invention, the starting glass 1 is to be understood as the glass that is processed or must be further processed to ultimately produce the watch glass 10. In other words, within the scope of the invention, the term "starting glass" is used for the glass in every step of the proposed method up to the production of the watch glass 10.
[0061] In this context, within the scope of the invention, the term "original thickness" means the thickness of the starting glass 1 before any processing of the starting glass 1. This means that a thickness of the starting glass 1 in the further steps of the process differs from the original thickness d1.
[0062] As from Figure 1As can be seen, the tool 100 comprises a base body 103 which has a first circumferential projection 101 for pressing the starting glass 1 and at least one second projection 102 for pressing the at least one recess 2 into the starting glass 1.
[0063] In this case, the tool 100 is provided with two second projections 102, which are particularly identical in design. The second projections 102 are arranged in an inner region 104 of the first circumferential projection 101 and are configured to press two recesses into the starting glass.
[0064] The first circumferential projection 101 and the two second projections 102 extend in the same direction.
[0065] Furthermore, the first circumferential projection 101 projects beyond the second projections 102 in the press-in direction 150.
[0066] Figure 2 shows a second step of the process.
[0067] In this step, the starting glass 1 is heated to a predetermined temperature below the melting temperature of the starting glass 1, so that the starting glass 1 becomes soft and its further processing is thus facilitated. Two identical recesses 2 are then pressed into the starting glass 1 using the second projections 102 of the tool 100. For this purpose, the tool 100 is preferably lowered (arrows 151) until the recesses 2 are completely formed in the starting glass 1.
[0068] Out of Figure 2 It can be seen that the recesses 2 are pressed to a depth t1 (pressing depth). The pressing depth t1 is greater than a predetermined depth t10 of the recesses 2 to be achieved in the watch glass 1 ( Figure 7 ). The depth t1 corresponds to a length of the second projections 102 (measured from the base body 103).
[0069] Simultaneously with the pressing of the recesses 2 into the starting glass 1, the starting glass 1 is reshaped, so that a first region 11 with a first cross-section Q1 and a second region 12 with a second cross-section Q2 are formed in the starting glass 1. The first region 11 has the recesses 2.
[0070] In particular, the starting glass 1 is pressed to form the first region 11 and the second region 12 using the first circumferential projection 101 of the tool 100. The pressing direction of the starting glass 1 corresponds to the press-in direction 150. The second projections 102 and the first circumferential projection 101 extend in the pressing direction or press-in direction 150 of the starting glass 1.
[0071] By pressing the starting glass 1, the first region 11 is created with a smaller first cross section Q1 than the second cross section Q2 of the second region 12. In particular, the first cross section Q1 corresponds to a predetermined cross section Q10 of the watch glass 10. For this purpose, the tool 100 is preferably designed such that an inner contour of the first circumferential projection 101 corresponds to an outer contour of the watch glass 10 to be achieved or is complementary to the outer contour of the watch glass 10 to be achieved.
[0072] Furthermore, the starting glass 1 is formed such that the first region 11 has a first thickness d3 and the second region 12 has a second thickness d4, wherein the first thickness d3 is smaller than the second thickness d4. Due to the pressing process, the sum of the first thickness d3 and the second thickness d4 is, in particular, smaller than the original thickness d1 of the starting glass 1 and greater than the predetermined, to-be-achieved thickness d10 of the watch glass 10. Furthermore, the first thickness d3 is greater than the predetermined thickness d10 of the watch glass 10.
[0073] The oversize of the starting glass 1 ensures that when the recesses 2 are pressed into the starting glass 1, the area of the starting glass 1 that will ultimately correspond to the watch glass 10 is not deformed. Thus, the recesses 2 can also be formed precisely in this area.
[0074] In particular, a ratio of the original thickness d1 of the starting glass 1 to the predetermined thickness d10 of the watch glass 10 is two to one, preferably three to one, particularly preferably four to one.
[0075] In a third step of the procedure according to Figure 3 After pressing the recesses 2 into the starting glass 1 and forming the first region 11 and the second region 12, the tool 100 is removed from the starting glass 1 (arrows 152). Furthermore, the starting glass 1 is cooled according to a predetermined cooling curve to relieve the stress on the starting glass 1.
[0076] Figure 4a illustrates a fourth step of the process, where Figure 4b the output glass 1 after the end of the fourth step.
[0077] In the fourth step, the second area 12 is ground together with a part of the first area 11. This is Figure 4aindicated by the dashed line 153. Through the grinding process, the starting glass 1 takes on the desired outer contour of the watch glass 10, whereby an upper side 3 and a lower side 4 of the starting glass 1 are formed parallel to each other ( Figure 4b ). In other words, a cross-section of the starting glass 1 after the fourth step corresponds to the predetermined cross-section Q10 of the watch glass 10.
[0078] Subsequently, in a fifth procedure according to Figure 5 the underside 4 of the starting glass 1 is polished. This is Figure 5 indicated by the dashed line 154. In particular, the underside 4 is polished such that after polishing, a thickness of the starting glass 1 corresponds to a sum of the predetermined thickness d10 of the watch glass 10 and a difference between the offset depth t1 and the predetermined depth t10 of the recesses 2.
[0079] Finally, in a sixth step, according to Figure 6the top side 3 of the starting glass 1 is ground and / or polished. This is Figure 6 indicated by the dashed line 155. In particular, the upper side 3 is ground and / or polished by the difference between the offset depth t1 and the predetermined depth t10 of the recesses 2 for forming the watch glass 10.
[0080] After the end of the sixth step, the watch glass 10 is obtained ( Figure 7 ).
[0081] It should be noted that, according to the above description, the grinding of the second region 12 and a part of the first region 11 as well as the polishing of the underside 4 of the starting glass 1 takes place before the grinding and / or polishing of the upper side 3 of the starting glass 1.
[0082] However, it is also possible for the grinding and / or polishing of the upper side 3 of the starting glass 1 to take place before the grinding of the second region 12 and one part of the first region 11.
[0083] In addition to the above written description of the invention, for its supplementary disclosure, reference is hereby explicitly made to the graphic representation of the invention in the Fig. 1 to 7 Reference is made. List of reference symbols
[0084] 1 Source glass 2 Recess 3 Top of the source glass 4 Bottom of the source glass 10 Watch glass 11 First area 12 Second area 100 Tool 101 First circumferential projection of the tool 102 Second projection of the tool 103 Base body of the tool 104 Inner area of the first circumferential projection 150 Press-in direction / Pressing direction 151 Arrows 152 Arrows 153 Dashed line 154 Dashed line 155 Dashed line d1 Original thickness of the source glass d3 First thickness of the first area d4 Second thickness of the second area d10 Predetermined thickness of the watch glass Q1 First cross-section of the first area Q2 Second cross-section of the second area t1 Depth / Press-in depth of the recess t10 Predetermined depth of the recess
Claims
1. A method for producing a watch glass (10) with at least one recess for a decorative element, in particular a gemstone, comprising the steps: - providing a starting glass (1), which has an original thickness (d1) greater than a predetermined thickness (d10) of the watch glass (10), - heating the starting glass (1) to a predetermined temperature below the melting temperature of the starting glass (1), so that the starting glass (1) becomes soft, so that a press-fitting of a recess into the starting glass (1) can be performed, - press-fitting at least one recess (2) for a decorative element, in particular a gemstone, into the starting glass (1), and - processing the starting glass (1) with the at least one recess (2) pressed therein, so that the thickness of the starting glass (1) is reduced to the predetermined thickness (d10) of the watch glass (10) to form the watch glass (10), wherein the at least one recess (2) is pressed into the watch glass (10) to a depth (t1) greater than a predetermined depth (t10) of the recess (2), and wherein the starting glass (1) is deformed, so that a first region (11) with a first cross-section (Q1) and a second region (12) with a second cross-section (Q2) are formed in the starting glass (1), wherein the first cross-section (Q1) is smaller than the second cross-section (Q2) and corresponds to a predetermined cross-section (Q10) of the watch glass (10), and the first region (11) comprises the at least one recess (2).
2. The method according to claim 1, wherein the starting glass (1) is deformed, such that the first region (11) has a first thickness (d3) and the second region (12) has a second thickness (d4), wherein the first thickness (d3) is smaller than the second thickness (d4).
3. The method according to claim 2, wherein a ratio of the original thickness (d1) of the starting glass (1) to the predetermined thickness (d10) of the watch glass (10) is at least two to one, preferably at least three to one, particularly preferably at least four to one.
4. The method according to one of claims 1 to 3, wherein the forming of the first region (11) and the second region (12) is performed in one step with the press-fitting of the recess (2).
5. The method according to one of the preceding claims, wherein the starting glass (1) is cooled after the press-fitting of the recess (2) or the forming of the first region (11) and the second region (12) and before the processing of the starting glass (1).
6. The method according to one of claims 1 to 5, wherein at least the second region (12) is ground.
7. The method according to claim 6, wherein an underside (4) of the starting glass (1) is polished after grinding at least the second region (12).
8. The method according to one of the preceding claims, wherein an upper side (3) of the starting glass (1) is ground and / or polished.
9. The method according to any one of claims 6 to 8, wherein: - the grinding and / or the polishing of the upper side (3) of the starting glass (1) is performed before the grinding of at least the second region (12), or - the grinding of at least the second region (12) and the polishing of the underside (4) of the starting glass (1) is performed before the grinding and / or polishing of the upper side (3) of the starting glass (1).
10. A tool (100), which is adapted to be used in a method according to any one of claims 1 to 9, comprising a base body (103), which comprises a first at least partially circumferential projection (101) for press-fitting a starting glass (1) and at least one second projection (102) for press-fitting at least one recess (2) for a decorative element, in particular a gemstone, into the starting glass (1), wherein the second projection (102) is arranged in an inner region (104) of the first projection (101), wherein the first at least partially circumferential projection (101) and the at least second projection (102) extend in the same direction.