ENERGY-EFFICIENT PRODUCTION OF A FERRITIC WARM BAND IN A DILLING-ROLLING COMPOSITE PLANT
Patent Information
- Application Number
- DE502020009491
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-15
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-12-15
AI Technical Summary
The energy-intensive process of producing ferritic hot strips in composite casting-rolling plants results in high energy consumption due to the need for intensive heating and cooling, compromising energy efficiency while maintaining good metallurgical properties and surface quality.
The process involves using inductive surface heating modules to heat the broad sides of the intermediate strip to a surface temperature of ≥1000 °C with alternating current frequencies ≥20 kHz, followed by descaling and finish rolling without additional cooling, allowing the last rolling pass to occur in the ferritic temperature range, thereby reducing energy input and maintaining high surface quality.
This method significantly reduces energy consumption by only heating the surface layers of the intermediate strip, ensuring thorough descaling and maintaining good metallurgical properties and surface quality, while achieving a high coiling temperature without additional heating or cooling.
Description
field of technology
[0001] The present invention relates to the technical field of steel metallurgy, specifically to the particularly energy-efficient production of a ferritic hot strip in a combined casting and rolling plant.
[0002] On the one hand, the invention relates to a method for producing a ferritic hot strip in a combined casting and rolling plant, comprising the steps of: continuously casting a liquid steel into a strand with a slab or thin slab cross-section in a continuous casting plant; pre-rolling the strand into an intermediate strip in a multi-stand roughing train; descaling the broad sides of the heated intermediate strip in a descaling device; finish rolling the descaled intermediate strip into the hot strip in a multi-stand finishing train, wherein at least the last rolling pass in the finishing train takes place in the ferritic temperature range of the steel; adjusting the hot strip to coiling temperature; and coiling the hot strip in a coiling system.
[0003] On the other hand, the invention relates to the use of a combined casting and rolling plant which is particularly well suited for producing a ferritic hot strip, comprising: a continuous casting plant for continuously casting a liquid steel into a strand with a slab or thin slab cross-section; a multi-stand roughing train for rough-rolling the strand into an intermediate strip; a descaling device for descaling the broad sides of the heated intermediate strip; a multi-stand finishing train for finish-rolling the descaled intermediate strip into the hot strip, wherein at least the last rolling pass in the finishing train takes place in the ferritic temperature range of the steel; a cooling section for adjusting the hot strip to coiling temperature; and a coiling system for winding the hot strip. State of the art
[0004] From the unpublished application PCT / EP2020 / 068520 it is known to produce a ferritic hot strip in a combined casting and rolling plant by the steps of continuously casting a strand with a slab or thin slab cross-section, pre-rolling the strand to an intermediate strip in a multi-stand roughing train, heating the intermediate strip to an average temperature ≥ 1070 °C, descaling the heated intermediate strip, finish rolling the descaled intermediate strip to a hot strip in a multi-stand finishing train, wherein at least the last rolling pass in the finishing train takes place in the ferritic temperature range, cooling the hot strip to coiling temperature, and winding the hot strip in a coiling system.Although the produced ferritic hot-rolled strip exhibits good metallurgical properties and a good surface quality, the process is energy-intensive because the average temperature of the intermediate strip is first raised to a high temperature of ≥ 1070 °C, the intermediate strip is then descaled, and then, in an intensive cooling step, the average temperature of the intermediate strip is cooled to < 900 °C. The document does not explain how the process can be modified so that the hot-rolled strip exhibits equally good metallurgical properties and a good surface quality, while significantly reducing energy consumption. Summary of the invention
[0005] The object of the invention is to modify a method for producing a ferritic hot strip in a combined casting and rolling plant such that the ferritic hot strip can be produced significantly more energy-efficiently while still exhibiting good metallurgical properties and a good surface quality. Furthermore, a particularly suitable combined casting and rolling plant is to be specified, which is used accordingly.
[0006] The procedural aspect of this problem is solved by a method according to claim 1. Advantageous further developments are the subject of the dependent claims.
[0007] Specifically, the solution is achieved by a method for producing a ferritic hot strip in a combined casting and rolling plant, comprising the steps of: continuously casting a liquid steel into a strand with a slab or thin slab cross-section in a continuous casting plant; pre-rolling the strand into an intermediate strip in a multi-stand roughing train; heating the broad sides of the intermediate strip by one or preferably more inductive surface heating modules to a surface temperature ≥ 1000 °C, preferably ≥ 1050 °C, wherein the surface heating module is operated with an alternating current with a first frequency f1 and the following applies to the first frequency f1: f1 ≥ 20 kHz, preferably f1 ≥ 50 kHz, particularly preferably f1 ≥ 100 kHz; descaling the broad sides of the heated intermediate strip in a descaling device;Finish rolling the descaled intermediate strip into the hot strip in a multi-stand finishing mill, wherein the descaled intermediate strip, after descaling, enters a first stand of the finishing mill without further cooling at an average temperature of 775-900 °C, and at least the last rolling pass in the finishing mill takes place in the ferritic temperature range of the steel; adjusting the hot strip to coiling temperature; and coiling the hot strip in a coiling system.
[0008] The mean temperature (also called average temperature) is the temperature corresponding to the average temperature of the various layers of the intermediate strip in the thickness direction. It is therefore generally not the temperature of the intermediate strip in the thickness direction in the middle (i.e., in the central region).
[0009] When adjusting the hot strip to coiling temperature, the hot strip is typically thermally insulated in the area between the last stand of the finishing train and the coiling system, so that the average temperature of the hot strip drops only slightly. This achieves a high coiling temperature without actively heating or reheating the hot strip. Alternatively, the hot strip can either be actively cooled or even heated by a heating device. A combination of a heating device after the last stand of the finishing train and a cooling section for actively cooling the hot strip before coiling is also conceivable and advantageous for certain steel grades.
[0010] According to the invention, the intermediate strip is heated to a surface temperature ≥ 1000 °C by at least one surface heating module. Since the surface heating module(s) are operated with an alternating current at a first frequency f1, and the following applies to the first frequency f1: f1 ≥ 20 kHz, only the layers of the broad sides close to the surface are heated, with the temperature of the core of the intermediate strip changing only slightly. In other words, the surface temperature on the broad sides of the intermediate strip is increased considerably more by the surface heating module(s) than the average temperature of the intermediate strip. The broad sides of the hot intermediate strip are then descaled, e.g. by a so-called pinch roll descaler.Immediately after descaling, i.e., without further cooling, the descaled intermediate strip enters the first stand of the finishing train at an average temperature of 775–900°C and is finish-rolled into hot strip in the multi-stand finishing train. For the direct production of ferritic hot strip in the combined casting and rolling mill, at least the last rolling pass in the finishing train takes place in the ferritic temperature range of the steel. The temperature of the ferritic hot strip is then adjusted to coiling temperature, and it is rolled into coils in the coiling system. coils, wound up.
[0011] This results in several differences compared to the state of the art: Firstly, the inductive surface heating modules only heat the layers of the broad sides closest to the surface and not all layers of the intermediate strip evenly. Since the broad sides have a surface temperature of ≥ 1000 °C before descaling, descaling is very thorough, which leads to a high surface quality of the hot strip. Secondly, the descaled intermediate strip enters the first stand of the finishing train directly at an average temperature of 775 - 900 °C, without being cooled down separately in an intensive cooling step after descaling. This saves energy, as only the layers of the broad sides of the intermediate strip closest to the surface need to be heated to a comparatively high temperature before descaling, and not the entire intermediate strip. Secondly, the average temperature of the intermediate strip before descaling can be very low (e.g.between 875 and 990°C), which in turn is very beneficial for the energy efficiency of the manufacturing process.
[0012] Preferably, the ratio between the thickness s of the intermediate strip and the penetration depth d into the heated intermediate strip is: s / d ≤ 6, preferably s / d ≤ 10, particularly preferably s / d ≤ 14 and most preferably s / d ≤ 16. The so-called penetration depth δ (also called current penetration dimension) is an area in the intermediate strip in which the current density has dropped to 37 percent compared to the outer edge of the broad sides. In the penetration depth area, 86 percent of the induced energy is converted into heat, with only 14 percent heating deeper areas. In concrete terms, this means that, for example, with an intermediate strip thickness of 24 mm, the penetration depth d may be a maximum of 4 mm at s / d ≤ 6. The penetration depth can be calculated using the formula δ = 1 πμ 0 μ r fκ where µ 0 is the magnetic field constant, µ r is the relative electromagnetic permeability of the steel, f is the frequency of the alternating current, and κ is the electrical conductivity. All of the above quantities are to be used in SI units. Since κ in particular, but also µ r, are strongly temperature-dependent, these values must be used at the actual temperature during heating.
[0013] Preferably, an inductive surface heating module heats the intermediate strip using transverse field heating. However, it is also possible for the heating to occur using longitudinal field heating. With transverse field heating, it is advantageous for a first inductor to heat the upper broad side of the intermediate strip and a second inductor to heat the lower broad side of the intermediate strip.
[0014] It is advantageous to adjust or maintain the so-called coupling gap, the vertical distance between an upper inductor and the upper broad side of the intermediate strip, depending on the intermediate strip thickness. This adjustment is achieved, for example, by a linear motor.
[0015] For thorough descaling of the intermediate strip in the width direction, it is advantageous for each wide side of the intermediate strip to be descaled by at least one row of several spray nozzles each. The spray nozzles in a row are arranged either stationary or on rotating rotors.
[0016] A good descaling effect is achieved when descaling is carried out using a liquid descaling agent, e.g. water, with the descaling agent being applied to the spray nozzles at a pressure of 450 bar > p > 100 bar.
[0017] In order to keep the descaling agent in the descaling device, it is advantageous if a pair of driver rollers (engl. pinch roll ) is arranged.
[0018] Depending on the steel grade, operating mode (continuous, semi-continuous, or batch operation), or casting speed, it may be advantageous to increase the average temperature of the intermediate strip in an induction furnace using several inductive soaking modules before heating the broad sides. The soaking module(s) increase the average temperature of the intermediate strip by approximately the same amount as the surface temperature. It is advantageous to operate the inductive surface heating modules at a first frequency f1 and the inductive soaking modules at a second frequency f2, where f1 > f2, preferably f1 ≥ 2*f2, particularly preferably f1 ≥ 5*f2.
[0019] To adjust the inlet temperature of the descaled intermediate strip into the finishing train, it is advantageous if the surface temperature T actual of the partially finish-rolled intermediate strip between the first and the second or between the second and the third finishing stand of the finishing train is measured by a pyrometer, a temperature controller taking into account T actual as a function of a target surface temperature T actual outputs a control variable to at least one, preferably to several, inductive soaking modules, and the soaking modules heat the intermediate strip to such an extent that the measured surface temperature T actual corresponds as closely as possible to the target surface temperature T actual.
[0020] This process is based on the realization that the temperature of the heated and descaled intermediate strip before the finishing train can only be measured imprecisely, and that temperature measurement in one of the inter-stand areas of the first three stands is significantly more accurate. The inductive soaking modules are controlled by a temperature controller based on the measured actual temperature, taking the target temperature into account, so that the actual temperature corresponds as closely as possible to the target temperature.
[0021] The object is also achieved by the use of a combined casting and rolling plant according to claim 13. Advantageous further developments are the subject of the dependent claims.
[0022] Specifically, the solution is achieved by using a combined casting and rolling plant for producing a ferritic hot strip in a process according to one of the preceding claims, comprising: a continuous casting plant for continuously casting liquid steel into a strand with a slab or thin slab cross-section; a multi-stand roughing train for pre-rolling the strand into an intermediate strip; one or more inductive surface heating modules for heating the broad sides of the intermediate strip to a surface temperature ≥ 1000 °C, wherein a surface heating module is operated with an alternating current at a first frequency f1 and the following applies to the first frequency f1: f1 ≥ 20 kHz, preferably f1 ≥ 50 kHz, particularly preferably f1 ≥ 100 kHz; a descaling device for descaling the broad sides of the heated intermediate strip;a multi-stand finishing mill for finish-rolling the descaled intermediate strip into the hot strip, wherein the descaled intermediate strip enters a first stand of the finishing mill after descaling without further cooling at an average temperature of 775-900 °C, and at least the last rolling pass in the finishing mill takes place in the ferritic temperature range of the steel; a cooling section for adjusting the hot strip to coiling temperature; and a coiling system for winding the hot strip.
[0023] Preferably, an induction furnace with several inductive soaking modules is arranged in the material flow direction between the roughing train and the inductive surface heating modules, wherein the induction furnace increases the average temperature of the intermediate strip.
[0024] It is further preferred that a pyrometer for measuring the surface temperature T actual of the partially finish-rolled intermediate strip is arranged between the first and the second or between the second and the third finishing stand of the finishing train, the pyrometer is signal-connected to a temperature controller and the temperature controller is signal-connected to at least one inductive soaking module, the temperature controller can output a control variable to at least one inductive soaking module taking into account T actual as a function of a target surface temperature T actual, wherein the soaking modules can heat the intermediate strip to such an extent that the measured surface temperature T actual corresponds as closely as possible to the target surface temperature T actual.
[0025] The above-described properties, features, and advantages of this invention, as well as the manner in which they are achieved, will become clearer and more readily understood in connection with the following description of an embodiment, which is explained in more detail in conjunction with the drawings. Fig. 1 shows a schematic representation of a combined casting and rolling plant according to the invention for carrying out the method according to the invention, Fig. 2 shows a temperature profile for the method according to the invention, and Fig. 3 shows a thickness profile for the method according to the invention. Description of the embodiments
[0026] In the combined casting and rolling plant 1 of the Fig. 1 In the continuous casting plant 2, liquid steel with the following chemical composition is produced Table 1: Chemical composition of the steel element Weight% C <0,004 Mn < 0,2 P < 0,01 Ti+Nb 0,03 Fe rest continuously cast into a strand 3 with a slab cross-section. Strand 3 leaves the continuous caster 2 with a thickness of 90 mm and a speed of 6 m / min. Preferably, the partially solidified strand 3 is subjected to soft core or liquid core reduction (LCR) in the curved strand guide. This reduces the thickness of the strand and improves its internal quality. Strand 3 enters the three-stand roughing mill 5 uncut, where it is reduced to an intermediate strip 4 with a thickness of 12.4 mm. The last rolling pass in stand R3 of roughing mill 5 takes place in the austenitic temperature range at a final rolling temperature of 1050°C. The average temperature of the intermediate strip 4 is then increased from 900°C to 950°C by six soaking modules of an induction furnace IH. Subsequently, the surface temperature of the broad sides of the heated intermediate strip 4 is heated to 1070°C by two surface heating modules 7.The surface heating modules operate at a frequency of 50 kHz and heat the intermediate strip through transverse field heating. Heating the broad sides causes the average temperature of the intermediate strip to rise to 960°C. After heating, the broad sides of the intermediate strip 4 are descaled in a descaling device D, specifically a so-called descaling unit. pinch roll descaler, descaled. The average temperature of the intermediate strip drops to 850 °C. After descaling, the descaled intermediate strip 3 enters the five-stand finishing train 8 and is finish-rolled there in 5 passes to form a hot strip 6 with a thickness of 1.7 mm. Since the last pass in stand F5 takes place at an average temperature of 760 °C, the hot strip has a ferritic structure after the last pass at the latest. Preferably, the last three passes in stands F3, F4 and F5 (particularly preferably all passes) of finishing train 8 are carried out using roll gap lubrication. In this case, a mineral oil is sprayed between the work rolls of the finishing stand and the rolled stock, which reduces the coefficient of friction in the roll gap to a value µ < 0.15. This prevents the formation of shear bands in the finished hot-rolled strip, which could lead to the development of an undesirable GOSS texture.The hot strip 6 leaves the finishing train 8 with a surface temperature of 760°C. To achieve a high coiling temperature, the hot strip is not actively cooled in the area of the cooling section 9 shown in dashed lines, but is thermally insulated by insulation panels 14. The coiling temperature is 700°C. Shortly before the coil has reached its target weight, the endless hot strip is cut transversely by the shears 10 and the. Winding on another (in Fig. 1 not shown) winding device, whereby the ferrite in the hot strip 6 at least partially forms a {1 1 1} texture. The average temperatures for the individual units of the combined casting-rolling plant 1 result either from Fig. 2 or the following table: Table 2: Temperature control Temperature [°C] CCM Out 1200 R1 1150 R2 1100 R3 1050 Your In 900 IH Out 950 SHM In 950 SHM Out 1070 D 850 F1 840 F2 820 F3 800 F4 780 F5 760 DC 700
[0027] The reduction rates in the individual stands R1... R3 and F1... F5 as well as the thicknesses of the thin slab 2, the intermediate strip 4 and the hot strip 6 are determined either from Fig. 3 or the following table: Table 3: Thicknesses and reduction rates Thickness [mm] Reduction rates [%] CCM Out 90,0 R1 In 90,0 50 R1 Out 45,0 R2 In 45,0 50 R2 Out 22,5 R3 In 22,5 45 R3 Out 12,4 Your In 12,4 IH Out 12,4 SHM In 12,4 SHM Out 12,4 D 12,4 F1 In 12,4 45 F1 Out 6,8 F2 In 6,8 40 F2 Out 4,1 F3 In 4,1 35 F3 Out 2,7 F4 In 2,7 25 F4 Out 2,0 F5 In 2,0 15 F5 Out 1,7 DC 1,7
[0028] In order to ensure the continuous operation of the combined casting and rolling plant 1, the hot strip 6 is cut directly in front of the winding devices and wound alternately by at least two DC winding devices.
[0029] By applying the method according to the invention in the combined casting and rolling plant 1, the coiled hot strip 6 has good deep drawability without the hot strip 6 having to be cold rolled or annealed after hot rolling.
[0030] Although the invention has been illustrated and described in detail by the preferred embodiments, the invention is not limited by the disclosed examples and other variations can be derived by those skilled in the art within the scope of the claims without departing from the scope of the invention. List of reference symbols
[0031] 1Combined casting and rolling plant 2Continuous casting plant 3Strand 4Intermediate strip 5Roughing mill 6Hot strip or finished strip 7Surface heating module 8Finishing mill 9Cooling section 10Shear 14Insulation panel 15, DC coiler DEscaling device F1... F5First to fifth stands of the finishing train IHInduction furnace InInput of a unit OutOutput of a unit R1... R3First to third stands of the roughing train T lst Actual surface temperature T Soll Target surface temperature
Claims
1. Process for producing a ferritic hot-rolled strip (6) in an integrated casting-rolling plant (1), comprising the steps: continuous casting of a liquid steel to give a strip (3) having a slab or thin slab cross section in a continuous casting plant (2, CCM); prerolling of the strip (3) to give an intermediate strip (4) in a multipart roughing stand (5); heating of the broad sides of the intermediate strip (4) by one or preferably more inductive surface heating modules (7) to a surface temperature of ≥ 1000°C, preferably ≥ 1050°C, where a surface heating module (7) is operated using an alternating current having a first frequency f1 and the first frequency f1 obeys: f1 ≥ 20 kHz, preferably f1 ≥ 50 kHz, particularly preferably f1 ≥ 100 kHz; descaling of the broad sides of the heated intermediate strip (4) in a descaling apparatus (D); final rolling of the descaled intermediate strip (4) to give the hot-rolled strip (6) in a multipart finishing stand (8), where the descaled intermediate strip (4) after descaling and without further cooling enters a first set (F1) of the finishing stand (8) with an average temperature of 775-900°C and at least the last rolling pass (F5) in the finishing stand takes place in the ferritic temperature range of the steel; setting of the hot-rolled strip (6) to coiler temperature; and winding-up of the hot-rolled strip (6) in a coiler (15, DC).
2. Process according to Claim 1, characterized in that the ratio of the thickness s of the intermediate strip (4) and the penetration depth d into the heated intermediate strip (4) obeys: s / d □ 6, preferably s / d □ 10, particularly preferably s / d □ 14 and very particularly preferably s / d □ 16, where the penetration depth d refers to a region in the intermediate strip (4) in which the current density has dropped to 37% relative to the outer edge of the broad sides, so that in the region of the penetration depth d, 86% of the induced energy is converted into heat while only 14% heats the regions deeper down.
3. Process according to Claim 1 or 2, characterized in that an inductive surface heating module (7) heats the intermediate strip (4) by transverse field heating.
4. Process according to Claim 3, characterized in that a first inductor heats the upper broad side of the intermediate strip (4) and a second inductor heats the lower broad side of the intermediate strip (4).
5. Process according to Claim 4, characterized in that the vertical distance between the first inductor and the upper broad side is kept constant as a function of the intermediate strip thickness.
6. Process according to any of the preceding claims, characterized in that each broad side of the intermediate strip (4) is descaled by at least one row of in each case a plurality of spray nozzles in the descaling apparatus (D).
7. Process according to Claim 6, characterized in that the spray nozzles of a row are either stationary or arranged on rotating rotors.
8. Process according to Claim 6 or 7, characterized in that descaling is carried out using a liquid descaling agent, for example water, where the descaling agent has a pressure in the range 450 bar > p > 100 bar at the spray nozzles.
9. Process according to any of Claims 6 to 8, characterized in that a pair of pinch rolls next to the intermediate strip (4) is arranged, in the flow direction of the material, before the first row and after the last row of spray nozzles, so that the descaling agent cannot leave the descaling apparatus.
10. Process according to any of the preceding claims, characterized in that the average temperature of the intermediate strip is increased using a plurality of inductive volume-heating modules in an induction furnace (IH) before heating of the broad sides of the intermediate strip, where the average temperature is increased to about the same degree as the surface temperature of the intermediate strip.
11. Process according to Claim 10, characterized in that the inductive surface heating modules are operated at a first frequency f1 and the inductive volume-heating modules are operated at a second frequency f2, where: f1 > f2, preferably f1 ≥ 2*f2, particularly preferably f1 ≥ 5*f2.
12. Process according to Claim 10 or 11, characterized in that the surface temperature Tact of the partially finished intermediate strip (4) between the first finishing set (F1) and the second finishing set (F2) or between the second finishing set (F2) and the third finishing set (F3) of the finishing stand (8) is measured by a pyrometer, a temperature regulator transmits an actuating variable as a function of an intended surface temperature Tint and taking into account Tact to at least one, preferably a plurality of, inductive volume-heating modules, and the volume-heating modules heat the intermediate strip to such a degree that the measured surface temperature Tact corresponds closely to the intended surface temperature Tint.
13. Use of an integrated casting-rolling plant (1) for producing a ferritic hot-rolled strip (6) in a process according to any of the preceding claims, comprising: a continuous casting plant (2, CCM) for continuously casting a liquid steel to give a strip (3) having a slab or thin slab cross section; a multipart roughing stand (5) for prerolling the strip (3) to give an intermediate strip (4); one or more inductive surface heating modules (7) for heating the broad sides of the intermediate strip (4) to a surface temperature of ≥ 1000°C, where a surface heating module (7) is operated using an alternating current having a first frequency f1 and the first frequency f1 obeys: f1 ≥ 20 kHz, preferably f1 ≥ 50 kHz, particularly preferably f1 ≥ 100 kHz; a descaling apparatus (D) for descaling the broad sides of the heated intermediate strip (4); a multipart finishing stand (8) for final rolling of the descaled intermediate strip (4) to give the hot-rolled strip (6), where the descaled intermediate strip (4) after descaling and without further cooling enters a first set (F1) of the finishing stand (8) with an average temperature of 775-900°C and at least the last rolling pass (F5) in the finishing stand (8) takes place in the ferritic temperature range of the steel; a cooling section (9) for setting the hot-rolled strip (6) to coiler temperature; and a coiler (15, DC) for winding up the hot-rolled strip (6).
14. Integrated casting-rolling plant according to Claim 13, characterized in that an induction furnace (IH) having a plurality of inductive volume-heating modules is arranged, in the flow direction of the material, between the roughing stand (5) and the inductive surface heating modules (7), where the induction furnace (IH) increases the average temperature of the intermediate strip.
15. Integrated casting-rolling plant according to Claim 13 or 14, characterized in that a pyrometer for measuring the surface temperature Tact of the partially finished intermediate strip (4) is arranged between the first finishing set (F1) and the second finishing set (F2) or between the second finishing set (F2) and the third finishing set (F3) of the finishing stand (8), the pyrometer is connected so as to be able to transmit a signal to a temperature regulator and the temperature regulator is connected so as to be able to transmit a signal to at least one inductive volume-heating module, the temperature regulator can transmit an actuating variable as a function of an intended surface temperature Tint and taking into account Tact to at least one inductive volume-heating module, where the volume-heating modules can heat the intermediate strip to such a degree that the measured surface temperature Tact corresponds closely to the intended surface temperature Tint.