Sintered powder containing a thermoplastic polyurethane, a flow agent and an organic additive

DE502021005263D1Active Publication Date: 2024-10-10BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005263
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-03
Filing Date
2021-07-27
Publication Date
2024-10-10
Estimated Expiration
2041-07-27

AI Technical Summary

Technical Problem

Existing sintering powders for rapid prototyping, particularly those made from thermoplastic polyurethane, face challenges with low flowability and coalescence, leading to defects and poor mechanical properties in produced moldings, especially when using inorganic flow agents that can hinder sintering and cause issues like curling and distortion.

Method used

A sinter powder composition containing 59.5 to 99.85% thermoplastic polyurethane, 0.05 to 0.5% flow agent, 0.1 to 5% organic additive such as polypropylene waxes grafted with maleic acid or maleic anhydride, and 0 to 30% reinforcing agent, which improves flowability and coalescence without compromising mechanical properties.

Benefits of technology

The sinter powder exhibits enhanced flowability and coalescence, resulting in high tensile strength and elongation at break, with improved processing efficiency and reduced clogging during comminution steps, leading to higher quality moldings with better economic efficiency and process stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a sintering powder (SP) which contains 59.5 to 99.85% by weight of at least one thermoplastic polyurethane (A), 0.05 to 0.5% by weight of at least one flow agent (B), 0.1 to 5% by weight of at least one organic additive (C), 0 to 5% by weight of at least one further additive (D) and 0 to 30% by weight of at least one reinforcing agent (E), in each case based on the sum of the percentages by weight (A), (B), (C), (D) and (E), wherein the at least one organic additive (C) is selected from the group consisting of polypropylene waxes grafted with maleic acid and / or maleic anhydride and amide waxes.Furthermore, the present invention relates to a process for producing a shaped body by sintering the sinter powder (SP), to a shaped body obtainable by the process according to the invention, and to the use of at least one flow agent (B) and at least one organic additive (C) in a sinter powder (SP) to improve the flowability and coalescence of the sinter powder (SP). Furthermore, the present invention relates to the use of the sinter powder (SP) in a sintering process and to a process for producing the sinter powder (SP).

[0002] The rapid provision of prototypes has become a frequently encountered task in recent times. One process particularly suitable for this so-called "rapid prototyping" is selective laser sintering (SLS). In this process, a plastic powder is selectively exposed to a laser beam in a chamber. The powder melts, the molten particles merge, and then solidify again. Repeated application of plastic powder and subsequent exposure to a laser enables the modeling of three-dimensional molded bodies.

[0003] The process of selective laser sintering for producing shaped bodies from powdered polymers is described in detail in the patents US 6,136,948 and WO 96 / 06881.

[0004] A further development of selective laser sintering is high-speed sintering (HSS), described in EP 1 648 686, or HP's Multijet Fusion technology (MJF). High-speed sintering involves spraying an infrared-absorbing ink onto the component cross-section to be sintered and subsequently exposing it to an infrared lamp. This achieves a higher processing speed compared to selective laser sintering.

[0005] Another variant of sintering is the selective heat sintering process (SHS), which uses the printing unit of a conventional thermal printer to selectively melt the plastic powder.

[0006] Of particular importance in the above-mentioned sintering processes is the flowability of the plastic powder. This should be as high as possible to ensure easy processing. High flowability enables the flawless formation of the powder layers and improves the sintering behavior of the plastic powder, resulting in a molded article of high quality, i.e., a good surface finish and high component density.

[0007] In contrast, plastic powders with low flowability are difficult to process in sintering processes, and molded articles produced with them often exhibit defects and lower component density, which is often reflected in the mechanical properties. In addition, poor flowability can lead to problems with powder dosing and, in the worst case, to the interruption of the printing process. As described in the article "An experimental study into the effects of bulk and flow behavior of laser sintering polymer powders on resulting part properties" by S. Ziegelmeier et al. (Journal of Materials Processing Technology, 2015, 215, 239), plastic powders made of elastic or soft materials, such as thermoplastic polyurethane (TPU), in particular, exhibit reduced flowability.

[0008] To improve flowability, so-called flow agents, also known as flow aids, are typically used. Flow agents are usually inorganic additives such as silicates, metal oxides, and minerals.

[0009] US Pat. No. 6,110,411, for example, describes a sintering powder containing a polyether ester elastomer and 0.02 to 5 wt.%, based on the total weight of the sintering powder, of a flow agent. Fumed silica, for example, is used as the flow agent.

[0010] US 2004 / 0204531 describes a composition containing 88 to 99.99 wt.% of a polymer selected from the group consisting of polyamides, polyamide derivatives, or mixtures thereof, and 0.05 to 0.25 wt.% of a flow aid. The flow aid is selected from inorganic pigments and silicas.

[0011] However, the use of these flow agents is disadvantageous. As described, for example, in the article "Laser sintering of polyamides and other polymers" by RD Goodridge et al. (Progress in Materials Science, 2012, 57, 229), excessively high flow agent content leads to impaired mechanical properties of the printed molded articles. This is primarily due to the fact that high contents of inorganic additives prevent the melting of the plastic powder during the sintering process. Furthermore, the inorganic additives can act as nucleation nuclei and accelerate crystallization, which can cause problems such as curling and warping during the sintering process.

[0012] In addition to flowability, the coalescence of the plastic powder during the melting process also has a significant impact on processability and, in particular, the mechanical properties of the resulting molded article. Plastic powders, such as elastic plastic powders such as TPU, which exhibit poor coalescence behavior, can exhibit poor processability even despite excellent flowability, resulting in porous molded articles with poor mechanical properties. The occurrence of surface defects and cracks is particularly pronounced in the production of molded articles with a complex structure or geometry.

[0013] EP 3 157 737 B1 discloses a thermoplastic powdered agent containing 0.02 to 0.5 wt.%, based on the total amount of agent, flow agent and powdered thermoplastic polyurethane for producing articles in powder-based additive manufacturing processes.

[0014] DE 10 2017 124047 A1 discloses a composition comprising at least one polymer system and at least one anti-agglomeration agent. The polymer system may comprise a thermoplastic polyurethane. In Example 1, Aerosil R 812 (Evonik) is used as the anti-agglomeration agent, and in Example 2, HDK H2O (Wacker) is used.

[0015] The object underlying the present invention is therefore to provide a sintering powder that, in a process for producing molded articles by sintering, does not exhibit, or only to a limited extent, the aforementioned disadvantages of the sintering powders and processes described in the prior art. The sintering powder and the process should be as simple and cost-effective to produce and implement as possible.

[0016] This task is solved by a sintering powder (SP) containing the components 59.5 to 99.85 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one thermoplastic polyurethane (A), 0.05 to 0.5 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one flow agent (B), 0.1 to 5 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one organic additive (C), 0 to 5 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one further additive (D) and 0 to 30 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one reinforcing agent (E), wherein the at least one organic additive (C) is selected from the group consisting of polypropylene waxes and amide waxes grafted with maleic acid and / or maleic anhydride.

[0017] It has surprisingly been found that the simultaneous use of at least one flow agent and at least one organic additive, in particular an organic additive selected from the group consisting of polyethylene waxes, polypropylene waxes, polypropylene waxes grafted with maleic acid and / or maleic anhydride, amide waxes, fatty acid esters, and glycerol fatty acid esters, significantly improves both the flowability and the coalescence of the sinter powder during the sintering process, without the use of the at least one flow agent and the at least one organic additive having a negative effect on the mechanical properties of the molded body produced. The molded bodies produced from the sinter powder according to the invention have both high tensile strength and high elongation at break.

[0018] Furthermore, the use of at least one superplasticizer and at least one organic additive also optimizes the production of the sinter powder itself. The improved flowability accelerates comminution steps such as grinding and / or sieving, as clogging of the sieve is avoided. This leads to improved cost-effectiveness and process stability. Sinter powder (SP)

[0019] According to the invention, the sintering powder (SP) contains as component (A) 59.5 to 99.85 wt. % of at least one thermoplastic polyurethane, as component (B) 0.05 to 0.5 wt. % of at least one flow agent, as component (C) 0.1 to 5 wt. % of at least one organic additive (C), as component (D) 0 to 5 wt. % of at least one further additive (D) and as component (E) 0 to 30 wt. % of at least one reinforcing agent (E), in each case based on the sum of the percentages by weight (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0020] The weight percentages of components (A), (B), (C), (D) and (E) usually add up to 100 wt.%.

[0021] In the context of the present invention, the terms "component (A)" and "at least one thermoplastic polyurethane" are used synonymously and therefore have the same meaning.

[0022] The same applies to the terms "component (B)" and "at least one flow agent." These terms are also used synonymously within the scope of the present invention and therefore have the same meaning.

[0023] Accordingly, the terms "component (C)" and "at least one organic additive" are used synonymously and have the same meaning.

[0024] The terms "component (D)" and "at least one further additive" as well as "component (E)" and "at least one reinforcing agent" are also used synonymously within the scope of the present invention and therefore have the same meaning.

[0025] The sintering powder (SP) preferably contains in the range from 74.15 to 99.7 wt.% of component (A), in the range from 0.1 to 0.35 wt.% of component (B), in the range from 0.2 to 3 wt.% of component (C), in the range from 0 to 2.5 wt.% of component (D) and in the range from 0 to 20 wt.% of component (E), in each case based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0026] Most preferably, the sinter powder (SP) contains in the range of 76.12 to 99.42 wt.% of component (A), in the range of 0.18 to 0.28 wt.% of component (B), in the range of 0.4 to 1.1 wt.% of component (C), in the range of 0 to 2.5 wt.% of component (D) and in the range of 0 to 20 wt.% of component (E), in each case based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sinter powder (SP).

[0027] If the sintering powder (SP) contains component (D), it can contain, for example, in the range from 0.1 to 5% by weight of component (D), preferably in the range from 0.2 to 2.5% by weight of component (D), based on the sum of the percentages by weight of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0028] If the sintering powder (SP) contains component (E), it can contain, for example, in the range of 5 to 30 wt.% of component (E), preferably in the range of 10 to 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0029] If the sintering powder (SP) contains component (D) and / or component (E), the percentages by weight of the at least one thermoplastic polyurethane (A) contained in the sintering powder (SP) are usually reduced accordingly, so that the sum of the percentages by weight of the at least one thermoplastic polyurethane (A), component (B), component (C) and component (D) and / or component (E) amounts to 100% by weight.

[0030] If the sintering powder (SP) contains component (D), it contains, for example, in the range from 59.5 to 99.75 wt.% of component (A), in the range from 0.05 to 0.5 wt.% of component (B), in the range from 0.1 to 5 wt.% of component (C), in the range from 0.1 to 5 wt.% of component (D) and in the range from 0 to 30 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0031] If the sintering powder (SP) contains component (D), it preferably contains in the range from 74.15 to 99.5 wt.% of component (A), in the range from 0.1 to 0.35 wt.% of component (B), in the range from 0.2 to 3 wt.% of component (C), in the range from 0.2 to 2.5 wt.% of component (D) and in the range from 0 to 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0032] If the sintering powder (SP) contains component (D), it more preferably contains in the range from 76.12 to 99.22 wt.% of component (A), in the range from 0.18 to 0.28 wt.% of component (B), in the range from 0.4 to 1.1 wt.% of component (C), in the range from 0.2 to 2.5 wt.% of component (D) and in the range from 0 to 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0033] If the sintering powder (SP) contains component (E), it contains, for example, in the range from 59.5 to 94.85 wt.% of component (A), in the range from 0.05 to 0.5 wt.% of component (B), in the range from 0.1 to 5 wt.% of component (C), in the range from 0 to 5 wt.% of component (D) and in the range from 5 to 30 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0034] If the sintering powder (SP) contains component (E), it preferably contains in the range from 74.15 to 89.7 wt.% of component (A), in the range from 0.1 to 0.35 wt.% of component (B), in the range from 0.2 to 3 wt.% of component (C), in the range from 0 to 2.5 wt.% of component (D) and in the range from 10 to 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0035] If the sintering powder (SP) contains component (E), it more preferably contains in the range from 76.12 to 89.42 wt.% of component (A), in the range from 0.18 to 0.28 wt.% of component (B), in the range from 0.4 to 1.1 wt.% of component (C), in the range from 0 to 2.5 wt.% of component (D) and in the range from 10 to 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0036] If the sintering powder (SP) contains components (D) and (E), it contains, for example, in the range from 59.5 to 94.75 wt.% of component (A), in the range from 0.05 to 0.5 wt.% of component (B), in the range from 0.1 to 5 wt.% of component (C), in the range from 0.1 to 5 wt.% of component (D) and in the range from 5 to 30 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0037] If the sintering powder (SP) contains components (D) and (E), it preferably contains in the range from 74.15 to 89.5 wt.% of component (A), in the range from 0.1 to 0.35 wt.% of component (B), in the range from 0.2 to 3 wt.% of component (C), in the range from 0.2 to 2.5 wt.% of component (D) and in the range from 10 to 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0038] If the sintering powder (SP) contains components (D) and (E), it more preferably contains in the range of 76.12 to 89.22 wt.% of component (A), in the range of 0.18 to 0.28 wt.% of component (B), in the range of 0.4 to 1.1 wt.% of component (C), in the range of 0.2 to 2.5 wt.% of component (D) and in the range of 10 to 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0039] The sintering powder (SP) typically comprises particles. These particles have, for example, a size (D50 value) in the range of 10 to 190 µm, preferably in the range of 15 to 150 µm, more preferably in the range of 20 to 110 µm, and particularly preferably in the range of 40 to 100 µm.

[0040] In the context of the present invention, the "D50 value" is understood to mean the particle size at which 50 vol.% of the particles, based on the total volume of the particles, are less than or equal to the D50 value and 50 vol.% of the particles, based on the total volume of the particles, are greater than the D50 value.

[0041] In the present invention, the D50 value is determined using laser diffraction according to ISO 13320 (Horiba LA-960, Retsch Technology, Germany) with dry dispersion at 1 bar. The evaluation is carried out using the Fraunhofer method.

[0042] The sintering powder (SP) typically has a melting temperature (TM(SP)) in the range of 80 to 220°C. Preferably, the melting temperature (TM(SP)) of the sintering powder (SP) is in the range of 100 to 190°C, and particularly preferably in the range of 120 to 170°C.

[0043] The melting temperature (TM(SP) ) is determined in the context of the present invention according to DIN EN ISO 11357 using dynamic differential scanning calorimetry (DSC; Discovery series DSC, TA Instruments). During the measurement, the sample is subjected to the following temperature cycle under a nitrogen atmosphere: 5 minutes at -80°C, then heating to at least 200°C at 20°C / min (1st heating run (H1)), then 5 minutes at at least 200°C, then cooling to -80°C at 20°C / min, then 5 minutes at -80°C, then heating to at least 200°C at 20°C / min (2nd heating run (H2)). A DSC diagram is generated as shown in Figure 1is shown by way of example. The terms "melt onset (TM onset< )" and "melt endset (TM endset< )" are known to those skilled in the art. They correspond to the beginning (onset) and the end (endset) of the melting peak, respectively. The melting temperature (TM(SP) ) is understood to be the temperature at which the melting peak of the first heating run (H1) of the DSC diagram has a maximum. If several local maxima occur in the range between TM onset< and TM endset<, the melting temperature (TM(SP) ) is understood to be the numerical mean of the respective local maxima.

[0044] The sintering powder (SP) also typically has a melt volume rate (MVR) in the range of 3 to 150 cm 3 / 10 min. Preferably, the melt volume rate of the sintering powder (SP) is in the range of 15 to 100 cm 3 / 10 min, more preferably in the range of 30 to 70 cm 3 / 10 min.

[0045] The melt volume rate is determined in accordance with DIN EN ISO 1133 (mi2.1, Göttfert, Germany) in the context of the present invention. For this purpose, the sinter powder (SP) is pre-dried for 2 hours at 110°C in nitrogen and then subjected to a load of 2.16 kg and at a temperature of ( T m(SP) + 40°C) measured.

[0046] The sinter powder (SP) also typically has a bulk density of ≥ 300 g / L, preferably ≥ 350 g / L and more preferably ≥ 400 g / L.

[0047] For the purposes of this invention, the bulk density is determined according to DIN EN ISO 60. It can be used as a measure of the flowability of the sinter powder (SP). The higher the bulk density, the higher the flowability of the sinter powder (SP).

[0048] The sinter powder (SP) can be produced by any method known to those skilled in the art. For example, the sinter powder is produced by grinding, precipitation, melt emulsification, or microgranulation.

[0049] If the sinter powder (SP) is produced by precipitation, component (A) is typically mixed with a solvent and, optionally with heating, dissolved in the solvent to obtain a solution. The TPU powder is then precipitated, for example, by cooling the solution, distilling the solvent from the solution, or adding a precipitant to the solution. Components (B), (C), and optionally (D), and (E) are typically mixed with the dry TPU powder to obtain the sinter powder (SP).

[0050] The grinding can be carried out by any method known to the person skilled in the art, for example the components (A), (B) and (C) and optionally (D) and (E) are placed in a mill and ground therein.

[0051] All mills known to those skilled in the art are suitable, for example, classifier mills, opposed jet mills, hammer mills, ball mills, vibrating mills, or rotor mills such as pin mills and eddy current mills. The grain size is typically adjusted by a screening machine arranged downstream of the mill. In a preferred embodiment, a long-mesh screen is used. By using a long-mesh screen, the proportion of the acceptable fraction can be increased. The mesh size of the screen should be selected so that the above-mentioned D50 value of the sinter powder (SP) can be adjusted.

[0052] Grinding in the mill can also be carried out using any method known to those skilled in the art. For example, grinding can take place under an inert gas atmosphere and / or with cooling with liquid nitrogen. Cooling with liquid nitrogen is preferred. The grinding temperature is arbitrary; preferably, grinding is carried out at liquid nitrogen temperatures, for example, at a temperature in the range of -210 to -195°C. The temperature of the components during grinding is then, for example, in the range of -60 to 0°C.

[0053] Preferably, at least component (A) is in the form of granules prior to grinding. The granules may, for example, be spherical, cylindrical, or elliptical.

[0054] The process for producing a sinter powder (SP) containing 59.5 to 99.85 wt.%, based on the total weight of the sinter powder (SP), of at least one thermoplastic polyurethane (A), 0.05 to 0.5 wt.%, based on the total weight of the sinter powder (SP), of at least one flow agent (B), 0.1 to 5 wt.%, based on the total weight of the sinter powder (SP), of at least one organic additive (C), 0 to 5 wt.%, based on the total weight of the sinter powder (SP), of at least one further additive (D) and 0 to 30 wt.%, based on the total weight of the sinter powder (SP), of at least one reinforcing agent (E), wherein the at least one organic additive (C) is selected from the group consisting of polypropylene waxes grafted with maleic acid and / or maleic anhydride and amide waxes, then comprises in one embodiment the step a) grinding the total amount, based on the total weight of the sinter powder (SP), of the component (A), wherein a first part (BT1) of the total amount,based on the total weight of the sinter powder (SP), of component (B) and / or a first part (CT1) of the total amount, based on the total weight of the sinter powder (SP), of component (C) before step a) is admixed to component (A) to obtain a powder (P) and the remaining part (BT2) of the total amount of component (B) and / or the remaining part (CT2) of the total amount of component (C) is admixed to the powder (P) after step a) to obtain the sinter powder (SP), wherein the first part (BT1) makes up 0 to 100 wt.% of the total amount, based on the total weight of the sinter powder (SP), of component (B) and wherein the first part (CT1) makes up 0 to 100 wt.% of the total amount, based on the total weight of the sinter powder (SP), of component (C), and wherein the remaining part (BT2) (100-BT1) wt.% of the total amount, based on the Total weight of the sinter powder (SP), component (B) and the remaining part (CT2) (100-CT1) wt% of the total,based on the total weight of the sinter powder (SP), which constitutes component (C), and wherein, if appropriate, the total amount, based on the total weight of the sinter powder (SP), of component (D) and / or the total amount, based on the total weight of the sinter powder (SP), of component (E) are admixed before step a) or after step a).

[0055] Preferably, the at least one organic additive (C) is added to component (A) before the grinding process. This can significantly increase the throughput during the grinding process.

[0056] Mixing methods are known per se to those skilled in the art. Components (B) and / or (C), and optionally components (D) and / or (E), are typically added to component (A) in a dry state. However, it is also possible for the mixing to take place via compounding in an extruder, particularly preferably in a twin-screw extruder. However, it is also possible for a combination of partial compounding and partial dry mixing to be used.

[0057] For the grinding in step a), the previously described explanations and preferences with regard to grinding apply accordingly.

[0058] In a preferred embodiment, the at least one thermoplastic polyurethane (A) is tempered before step a).

[0059] Preferably, the at least one thermoplastic polyurethane (A) is tempered at a temperature TT which is at most 100°C below the melting temperature (TM(A) ) of the at least one thermoplastic polyurethane (A), more preferably at a temperature TT which is at most 70°C below the melting temperature (TM(A) ) of the at least one thermoplastic polyurethane (A), and particularly preferably at a temperature TT which is at most 40°C below the melting temperature (TM(A) ) of the at least one thermoplastic polyurethane (A).

[0060] Furthermore, the at least one thermoplastic polyurethane (A) is preferably tempered at a temperature TT which is at least 5°C below the melting temperature (TM(A) ) of the at least one thermoplastic polyurethane (A), more preferably at a temperature TT which is at least 10°C below the melting temperature (TM(A) ) of the at least one thermoplastic polyurethane (A), and particularly preferably at a temperature TT which is at least 20°C below the melting temperature (TM(A) ) of the at least one thermoplastic polyurethane (A).

[0061] The at least one thermoplastic polyurethane (A) is preferably annealed for at least 10 hours, more preferably at least 24 hours, and particularly preferably at least 48 hours. The at least one thermoplastic polyurethane (A) is preferably annealed for 7 days. Annealing is preferably carried out in a paddle dryer (> 4 t) under vacuum or inert gas. Nitrogen, for example, is used as an inert gas.

[0062] A further subject of the present invention is therefore also the sinter powder (SP) obtainable by the process according to the invention. Component (A)

[0063] According to the invention, component (A) is at least one thermoplastic polyurethane.

[0064] In the context of the present invention, "at least one thermoplastic polyurethane" means both precisely one thermoplastic polyurethane (A) and a mixture of two or more thermoplastic polyurethanes (A). Furthermore, the term "at least one thermoplastic polyurethane" in the context of the present invention means a mixture of at least one thermoplastic polyurethane and at least one further polymer miscible with the at least one thermoplastic polyurethane. "At least one further polymer miscible with the thermoplastic polyurethane" in the context of the present invention means both precisely one further polymer miscible with the thermoplastic polyurethane and a mixture of two or more polymers miscible with the thermoplastic polyurethane.

[0065] The at least one thermoplastic polyurethane (A) can be produced by any method known to the person skilled in the art.

[0066] In a preferred embodiment, the at least one thermoplastic polyurethane (A) is prepared by reacting the components a) at least one isocyanate, b) at least one isocyanate-reactive compound, and c) optionally at least one chain extender having a number-average molecular weight MN in the range from 50 to 499 g / mol, optionally in the presence of d) at least one catalyst, e) at least one additive and / or f) at least one reinforcing agent.

[0067] The number average molecular weight MN is determined in the present invention by means of gel permeation chromatography.

[0068] Component (A) preferably has a weight-average molecular weight MW of at least 100,000 g / mol, more preferably at least 400,000 g / mol, and particularly preferably at least 600,000 g / mol. Furthermore, component (A) preferably has a weight-average molecular weight MW of at most 800,000 g / mol.

[0069] The weight-average molecular weight MW is determined in the present invention by means of gel permeation chromatography.

[0070] The at least one thermoplastic polyurethane typically has a melting temperature (TM(A)) in the range of 80 to 220°C. Preferably, the melting temperature (TM(A)) of the at least one thermoplastic polyurethane is in the range of 100 to 190°C, more preferably in the range of 120 to 170°C, and particularly preferably in the range of 135 to 145°C.

[0071] The melting temperature (TM(A) ) is determined in the context of the present invention according to DIN EN ISO 11357 using dynamic differential scanning calorimetry (DSC; Discovery series DSC, TA Instruments). During the measurement, the sample is subjected to the following temperature cycle under a nitrogen atmosphere: 5 minutes at -80°C, then heating to at least 200°C at 20°C / min (1st heating run (H1)), then 5 minutes at at least 200°C, then cooling to -80°C at 20°C / min, then 5 minutes at -80°C, then heating to at least 200°C at 20°C / min (2nd heating run (H2)). A DSC diagram is generated as shown in Figure 1is shown by way of example. The terms "melt onset (TM onset< )" and "melt endset (TM endset< )" are known to those skilled in the art. They correspond to the beginning (onset) and the end (endset) of the melting peak, respectively. The melting temperature (TM(SP) ) is understood to be the temperature at which the melting peak of the first heating run (H1) of the DSC diagram has a maximum. If several local maxima occur in the range between TM onset< and TM endset<, the melting temperature (TM(SP) ) is understood to be the numerical mean of the respective local maxima. Component (a))

[0072] Component (a)) is at least one isocyanate.

[0073] In the context of the present invention, "at least one isocyanate" means both exactly one isocyanate and a mixture of two or more isocyanates.

[0074] The at least one isocyanate may be an aliphatic, cycloaliphatic, araliphatic and / or aromatic isocyanate.

[0075] Preferably, component (a)) is a diisocyanate, for example selected from the group consisting of trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate (HDI), heptamethylene diisocyanate, octamethylene diisocyanate, 2-methylpentamethylene diisocyanate-1,5, 2-ethylbutylene diisocyanate-1,4, pentamethylene diisocyanate-1,5, butylene diisocyanate-1,4, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4-bis(isocyanatomethyl)cyclohexane (1,4-HXDI), 1,3-bis(isocyanatomethyl)cyclohexane (1,3-HXDI), 2,4-paraphenylene diisocyanate (PPDI), 2,4-tetramethylenexylene diisocyanate (TMXDI), 4,4'-, 2,4'- and 2,2'-dicyclohexylmethane diisocyanate (H12 MDI), 1,4-cyclohexane diisocyanate, 1-methyl-2,4- and 1-methyl-2,6-cyclohexane diisocyanate, 2,2'-diphenylmethane diisocyanate (2,2'-MDI), 2,4'-diphenylmethane diisocyanate (2,4'-MDI) and 4,4'-diphenylmethane diisocyanate (4,4'-MDI), 1,5-naphthylene diisocyanate (NDI), 2,4-Toluene diisocyanate (2,4-TDI) and 2,6-toluene diisocyanate (2,6-TDI), diphenylmethane diisocyanate, 3,3'-dimethyldiphenyl diisocyanate, 1,2-diphenylethane diisocyanate and phenylene diisocyanate.

[0076] Particularly preferred component (a)) is 4,4'-diphenylmethane diisocyanate (4,4'-MDI). Component (b))

[0077] Component (b)) is at least one compound reactive towards isocyanate.

[0078] In the context of the present invention, "at least one isocyanate-reactive compound" means both precisely one isocyanate-reactive compound and a mixture of two or more isocyanate-reactive compounds.

[0079] Preferably, component (b)) has a number-average molecular weight MN in the range from 500 to 100,000 g / mol, more preferably in the range from 500 to 8,000 g / mol, particularly preferably in the range from 700 to 6,000 g / mol and in particular in the range from 800 to 4,000 g / mol.

[0080] The at least one isocyanate-reactive compound (b)) preferably has on average at least 1.8 and at most 3.0 Zerewitinoff-active hydrogen atoms.

[0081] For the purposes of the present invention, the number of Zerewitinoff-active hydrogen atoms refers to the functionality of the at least one isocyanate-reactive compound (b). It indicates the amount of the at least one isocyanate-reactive group of the molecule, theoretically calculated from a molar amount to a molecule.

[0082] In a preferred embodiment, the functionality is in the range of 1.8 to 2.6, and preferably in the range of 1.9 to 2.2. In particular, the functionality is 2.

[0083] The at least one isocyanate-reactive compound is preferably linear.

[0084] It is preferably used with a molar fraction of 1 equivalent mol% to 80 equivalent mol%, based on the isocyanate group content of the at least one isocyanate.

[0085] Preferably, the at least one isocyanate-reactive compound (component (b))) has a reactive group selected from the group consisting of hydroxyl group, amino group, mercapto group and carboxylic acid group, more preferably the at least one isocyanate-reactive compound (component (b))) has a hydroxyl group.

[0086] In a preferred embodiment within the scope of the present invention, the at least one isocyanate-reactive compound (component (b))) is selected from the group consisting of polyesterdiols, polyetherdiols, and polycarbonatediols. Preferably, the at least one isocyanate-reactive compound (component (b))) is a polyesterdiol such as polycaprolactone and / or a polyetherdiol, for example based on ethylene oxide, propylene oxide, and / or butylene oxide. A particularly preferred polyether is polytetrahydrofuran (PTHF).

[0087] Particularly preferred isocyanate-reactive compounds (component (b))) are compounds from the group consisting of copolyesters based on adipic acid, succinic acid, pentanedioic acid and / or sebacic acid and mixtures of 1,2-ethanediol and 1,4-butanediol, copolyesters based on adipic acid, succinic acid, pentanedioic acid and / or sebacic acid and mixtures of 1,4-butanediol and 1,6-hexanediol, and polyesters based on adipic acid, succinic acid, pentanedioic acid and / or sebacic acid and 3-methyl-pentanediol-1,5 and / or polytetramethylene glycol (polytetrahydrofuran, PTHF), preferably copolyesters based on adipic acid and mixtures of 1,2-ethanediol and 1,4-butanediol and polyesters based on adipic acid, succinic acid, pentanedioic acid and / or sebacic acid and polytetramethylene glycol (PTHF). Component (c))

[0088] Component (c)) is at least one chain extender having a number average molecular weight MN in the range from 50 to 499 g / mol.

[0089] "At least one chain extender having a number-average molecular weight MN in the range from 50 to 499 g / mol" means, in the context of the present invention, both precisely one chain extender having a number-average molecular weight MN in the range from 50 to 499 g / mol and a mixture of two or more chain extenders having a number-average molecular weight MN in the range from 50 to 499 g / mol.

[0090] Aliphatic, araliphatic, aromatic and / or cycloaliphatic compounds with a number-average molecular weight of 50 g / mol to 499 g / mol can be used as component (c).

[0091] Component (c)) preferably has two isocyanate-reactive groups.

[0092] Preferred chain extenders are therefore diamines and / or alkanediols. More preferred chain extenders are alkanediols with 2 to 10 carbon atoms, and particularly preferred chain extenders are alkanediols with 3 to 8 carbon atoms in the alkylene radical. Furthermore, it is preferred that the alkanediols contain only primary hydroxyl groups.

[0093] In a preferred embodiment, component (c)) is selected from the group consisting of di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and decaalkylene glycols, 1,4-cyclohexanediol, 1,4-dimethanolcyclohexane, neopentyl glycol and hydroquinone bis(beta-hydroxyethyl) ether (HQEE).

[0094] Suitable di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and deca-alkylene glycols are, for example, 1,2-ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, oligo- and polypropylene glycols.

[0095] In the context of the present invention, 1,2-ethylene glycol, 1,3-propanediol, 1,4-butanediol and 1,6-hexanediol, more preferably 1,2-ethylene glycol, 1,4-butanediol and 1,6-hexanediol, are preferably used as chain extenders (component (c)).

[0096] In the production of softer thermoplastic polyurethanes, the molar ratio of component (b)) (at least one isocyanate-reactive compound) to component (c)) (at least one chain extender having a number-average molecular weight MN in the range from 50 to 499 g / mol) is preferably in the range from 1:1 to 1:5, more preferably in the range from 1:1.5 to 1:4.5.

[0097] If components (b)) and (c)) are mixed in this case, the hydroxyl equivalent weight is preferably > 200, more preferably the hydroxyl equivalent weight is in the range of 230 to 450.

[0098] In the production of harder thermoplastic polyurethanes, for example thermoplastic polyurethanes with a Shore A hardness of > 98, preferably thermoplastic polyurethanes with a Shore D hardness in the range from 55 to 75, the molar ratio of component (b)) (at least one isocyanate-reactive compound) to component (c)) (at least one chain extender with a number-average molecular weight MN in the range from 50 to 499 g / mol) is preferably in the range from 1:5.5 to 1:15, more preferably in the range from 1:6 to 1:12.

[0099] When components (b)) and (c)) are mixed in this case, the hydroxyl equivalent weight is preferably in the range of 110 to 200, more preferably in the range of 120 to 180.

[0100] The equivalent ratio of the NCO groups of component (a)) (at least one isocyanate) to the sum of the OH groups of components (b)) and (c)) is preferably in the range from 0.95:1 to 1.10:1, more preferably in the range from 0.98:1 to 1.08:1 and particularly preferably in the range from 1:1 to 1.05:1. Component (d))

[0101] Component (d)) is at least one catalyst.

[0102] In the context of the present invention, "at least one catalyst (d))" means both exactly one catalyst (d)) and a mixture of two or more catalysts (d)).

[0103] Catalysts as such are known to the person skilled in the art. In the present invention, catalysts are preferably used that accelerate the reaction between the NCO groups of the isocyanates (component (a))) and the hydroxyl groups of the isocyanate-reactive compound (component (b))) and, if used, the chain extender (component (c))).

[0104] Suitable catalysts are, for example, tertiary amines, in particular triethylamine, dimethylcyclohexylamine, N-methylmorpholine, N,N'-dimethylpiperazine, 2-(dimethylaminoethoxy)ethanol and diazabicyclo-(2,2,2)-octane.

[0105] In the present invention, organic metal compounds are preferably used, for example titanic acid esters, iron compounds, tin compounds and bismuth salts.

[0106] A suitable iron compound is, for example, iron(III) acetylacetonate. Suitable tin compounds include tin dialkyl salts, tin diacetate, tin dioctoate, and tin dilaurate. Preferred tin compounds are dibutyltin diacetate and dibutyltin dilaurate. A suitable bismuth salt is, for example, bismuth decanoate.

[0107] Particularly preferred catalysts in the present invention are titanic acid esters, tin dioctoate and bismuth decanoate.

[0108] If a catalyst (d)) is used, it is preferably used in amounts of 0.0001 to 0.1 parts by weight per 100 parts by weight of the isocyanate-reactive compound (component (b))). Component (e))

[0109] Component (e)) is at least one additive.

[0110] "At least one additive (e))" in the context of the present invention means both exactly one additive (e)) and a mixture of two or more additives (e)).

[0111] The at least one additive (e)) can be the same as the at least one further additive (D) described below, but it can also be different from the at least one further additive (D) described below. Preferably, it is different from the at least one further additive (D) described below.

[0112] However, the at least one additive (e) and the at least one further additive (D) differ in the manner of their addition. While the at least one additive (e) is preferably added to the reaction mixture during the synthesis of component (A) and thus polymerized into the TPU or is added to component (A) directly after the synthesis of component (A), the at least one further additive (D) is only added to component (A) directly before, during, or after the production of the sinter powder (SP).

[0113] Preferably, the at least one additive (e)) is selected from the group consisting of surface-active substances, flame retardants, nucleating agents, oxidation stabilizers, slip and demolding aids, dyes and pigments, stabilizers against hydrolysis, light, heat or discoloration and plasticizers.

[0114] Examples of suitable stabilizers include primary and secondary antioxidants, hindered phenols, hindered amine light stabilizers (HALS), UV absorbers, hydrolysis inhibitors, quenchers, and flame retardants. Examples of commercial stabilizers are given in Plastics Additives Handbook, 5th Edition, H. Zweifel, ed., Hanser Publishers, Munich, 2001 ([1]), pp. 98-136.

[0115] Suitable UV absorbers preferably have a number-average molecular weight MN of at least 300 g / mol, more preferably of at least 390 g / mol. Furthermore, suitable UV absorbers preferably have a number-average molecular weight MN of at most 5,000 g / mol, more preferably of at most 2,000 g / mol.

[0116] Particularly suitable UV absorbers are those selected from the group consisting of cinnamates, oxanilides, and benzotriazoles; benzotriazoles are particularly preferred. Examples of particularly suitable benzotriazoles are Tinuvin®< 213, Tinuvin®< 234, Tinuvin®< 312, Tinuvin®< 571, as well as Tinuvin®< 384 and Eversorb®< 82.

[0117] The UV absorbers are usually added in amounts of 0.01 to 5 wt.%, based on the mass of component (a)), (b)) and (e)), preferably in amounts of 0.1 to 2.0 wt.%, in particular in amounts of 0.2 to 0.5 wt.%.

[0118] Suitable hindered amine light stabilizers preferably have a number-average molecular weight MN of at least 500 g / mol. Furthermore, suitable hindered amine light stabilizers preferably have a number-average molecular weight MN of at most 10,000 g / mol, more preferably of at most 5,000 g / mol.

[0119] Particularly preferred hindered amine light stabilizers (HALS) are bis-(1,2,2,6,6-penta-methylpiperidyl) sebacate (Tinuvin®< 765, Ciba Spezialitätenchemie AG) and the condensation product of 1-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxypiperidine and succinic acid (Tinuvin®< 622). The condensation product of 1-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxypiperidine and succinic acid (Tinuvin®< 622) is particularly preferred if the titanium content of the finished product is less than 150 ppm, preferably less than 50 ppm, in particular less than 10 ppm, based on components (a)) and (b)).

[0120] Typically, the HALS are added in amounts of 0.01 to 5 wt.%, based on the mass of component (a)), (b)) and (e)), preferably in amounts of 0.1 to 1.0 wt.%, in particular in amounts of 0.15 to 0.3 wt.%.

[0121] A particularly preferred stabilization contains a mixture of a phenolic stabilizer, a benzotriazole and a HALS compound in the preferred amounts described above. Component (f))

[0122] Component (f)) is at least one reinforcing agent.

[0123] "At least one reinforcing agent (f))" in the context of the present invention means both exactly one reinforcing agent (f)) and a mixture of two or more reinforcing agents (f)).

[0124] The at least one reinforcing agent (f)) may be the same as the at least one reinforcing agent (E) described below, but it may also be different from the at least one reinforcing agent (E) described below.

[0125] For example, the at least one reinforcing agent (f)) is selected from the group consisting of carbon nanotubes, carbon fibers, boron fibers, glass fibers, glass spheres, silica fibers, ceramic fibers, basalt fibers, aluminum silicates, aramid fibers and polyester fibers.

[0126] The at least one reinforcing agent (f)) can be added to the reaction mixture during the preparation of component (A), wherein it can be added dry or as a masterbatch.

[0127] However, it is also possible that no reinforcing agent (f)) is added during the preparation of component (A) of the reaction mixture. In this case, it is possible that at least one reinforcing agent (E), which is described further below, is added to components (A), (B), (C), and optionally (D) during the preparation of the sinter powder (SP).

[0128] It is of course also possible that during the preparation of component (A) at least one reinforcing agent (f)) is added to the reaction mixture and then during the preparation of the sinter powder (SP) at least one reinforcing agent (E) is added to components (A), (B), (C) and optionally (D). Production of component (A)

[0129] The at least one thermoplastic polymer (A) can be produced in a batch process or a continuous process. For example, the at least one thermoplastic polymer (A) is produced using reaction extruders or the belt process, using the one-shot or prepolymer process, preferably the one-shot process.

[0130] In the "one-shot" process, components (a)) and (b)) and optionally also components (c)), (d)) and / or (e)) are mixed together successively or simultaneously, with the polymerization reaction starting immediately.

[0131] In the extrusion process, components (a)) and (b)) and optionally also components (c)), (d)) and / or (e)) are introduced into the extruder individually or as a mixture and reacted, preferably at temperatures of 100 to 280°C, more preferably at temperatures of 140 to 250°C. The resulting polyurethane is extruded, cooled, and granulated. It is preferably in the form of granules or powder.

[0132] A twin-screw extruder is preferred because it uses forced feeding and thus allows more precise adjustment of the temperature and output quantity on the extruder.

[0133] Thermoplastic polyurethanes according to the invention are available, for example, under the trade name Elastollan ®< SP9415 from BASF (BASF Polyurethanes GmbH, Lemförde, Germany). Component (B)

[0134] According to the invention, component (B) is at least one flow agent.

[0135] In the context of the present invention, "at least one flow agent (B)" means both exactly one flow agent (B) and a mixture of two or more flow agents (B).

[0136] Flow agents as such are known to those skilled in the art. In the context of the present invention, the at least one flow agent (B) is preferably an inorganic compound.

[0137] The at least one flow agent (B) is selected, for example, from the group consisting of silicon dioxide (silica), silicates, silicic acids, metal oxides, minerals, borates, phosphates, sulfates and carbonates.

[0138] Examples of suitable silicon dioxides (silica compounds) are hydrated silicon dioxides, glassy silicon dioxides and fumed silicon dioxides.

[0139] Examples of suitable silicates are aluminosilicates, alkali silicates, alkaline earth silicates, alkali aluminosilicates, alkaline earth aluminosilicates, calcium silicates and magnesium silicates.

[0140] Examples of suitable silicas are hydrophobic pyrogenic silicas.

[0141] Examples of suitable metal oxides are aluminum oxide, titanium dioxide and glassy oxides.

[0142] Examples of suitable minerals are talc, mica, kaolin and attapulgite.

[0143] Examples of suitable borates and phosphates are glassy borates and glassy phosphates.

[0144] Examples of suitable sulfates are magnesium sulfate, calcium sulfate, and barium sulfate. Examples of suitable carbonates are magnesium carbonate, calcium carbonate, and barium carbonate.

[0145] Preferably, the at least one flow agent (B) is selected from the group consisting of hydrophobic pyrogenic silicas, talc, kaolin, magnesium sulfate, calcium sulfate, barium sulfate, magnesium carbonate, calcium carbonate and barium carbonate.

[0146] The at least one flow agent (B) typically comprises particles. These particles have, for example, a size (D90 value) ≤ 10 µm, preferably ≤ 2 µm.

[0147] In the context of the present invention, the "D90 value" is understood to mean the particle size at which 90 vol.% of the particles, based on the total volume of the particles, are less than or equal to the D90 value and 10 vol.% of the particles, based on the total volume of the particles, are greater than the D90 value.

[0148] In the present invention, the D90 value is determined using laser diffraction according to ISO 13320 (Horiba LA-960, Retsch Technology, Germany), whereby the sintering powder (SP) or the at least one superplasticizer (B) was previously dry-dispersed at 1 bar. The evaluation is carried out using the Fraunhofer method.

[0149] Preferably, the sintering powder (SP) contains at least 0.05 wt.%, more preferably at least 0.1 wt.%, and particularly preferably at least 0.18 wt.%, of component (B), based on the sum of the weight percentages of components (A), (B), (C), optionally (D) and optionally (E), preferably based on the total weight of the sintering powder (SP).

[0150] Furthermore, the sintering powder (SP) preferably contains at most 0.5 wt.%, more preferably at most 0.35 wt.%, and particularly preferably at most 0.28 wt.%, of component (B), based on the sum of the weight percentages of components (A), (B), (C), optionally (D) and optionally (E), preferably based on the total weight of the sintering powder (SP). Component (C)

[0151] According to the invention, component (C) is at least one organic additive.

[0152] In the context of the present invention, "at least one organic additive" means both exactly one organic additive and a mixture of two or more organic additives.

[0153] Component (C) is at least one organic additive selected from polypropylene waxes grafted with maleic acid and / or maleic anhydride and amide waxes. Component (C) is particularly preferably an N,N'-alkylene difatty acid amide. Component (C) is most preferably N,N'-ethylene distearamide.

[0154] Suitable organic additives are available from companies such as Clariant and Baerlocher. An example of a suitable polypropylene wax grafted with maleic acid and / or maleic anhydride is Licocene PP MA 6452 TP from Clariant.

[0155] "Grafted with maleic acid and / or maleic anhydride" in the context of the present invention means that the polypropylene waxes are branched, containing polypropylene in their main chain and maleic acid and / or maleic anhydride in their branched chain.

[0156] In a preferred embodiment of the present invention, the at least one organic additive (C) is selected such that the dropping point DP of the at least one organic additive (C) satisfies the following condition (Formula I) T M A − 25 ° C ≤ D P < T M A + 25 ° C where DP the dropping point of the at least one organic additive (C) and TM(A) the melting temperature of the at least one thermoplastic polyurethane (A).

[0157] In a more preferred embodiment of the present invention, the at least one organic additive (C) is selected such that the dropping point DPof the at least one organic additive (C) satisfies the following condition (Formula II) T M A − 20 ° C ≤ D P < T M A + 20 ° C

[0158] In a particularly preferred embodiment of the present invention, the at least one organic additive (C) is selected such that the dropping point DP of the at least one organic additive (C) satisfies the following condition (Formula III) T M A − 15 ° C ≤ D P < T M A + 15 ° C

[0159] Particularly preferably, the at least one organic additive (C) is selected so that the dropping point DP of the at least one organic additive (C) satisfies the following condition (Formula IV) T M A , Onset ≤ D P < T M A , Endset where TM(A) , Onset the beginning of the melting peak of the at least one thermoplastic polyurethane (A) and TM(A), Endset the end of the melting peak of the at least one thermoplastic polyurethane (A).

[0160] In case the dropping point DPof the at least one organic additive (C) cannot be determined, the at least one organic additive (C) is selected in a preferred embodiment of the present invention such that the melting temperature T M ( C ) of the at least one organic additive (C) satisfies the following condition (Formula V) T M A − 25 ° C ≤ T M C < T M A + 25 ° C where T M ( C ) the melting temperature of the at least one organic additive (C) and T M ( A ) is the melting temperature of the at least one thermoplastic polyurethane (A).

[0161] In a more preferred embodiment of the present invention, the at least one organic additive (C) is then selected such that the melting temperature T M ( C ) of the at least one organic additive (C) satisfies the following condition (Formula VI) T M A − 20 ° C ≤ T M C < T M A + 20 ° C

[0162] In a particularly preferred embodiment of the present invention, the at least one organic additive (C) is then selected such that the melting temperature T M ( C ) of the at least one organic additive (C) satisfies the following condition (Formula VII) T M A − 15 ° C ≤ T M C < T M A + 15 ° C

[0163] Particularly preferably, the at least one organic additive (C) is selected such that the melting temperature T M ( C ) of the at least one organic additive (C) satisfies the following condition (Formula VIII) T M A , Onset ≤ T M C < T M A , Endset where TM(A), Onset the beginning of the melting peak of the at least one thermoplastic polyurethane (A) and TM(A), Endset the end of the melting peak of the at least one thermoplastic polyurethane (A).

[0164] Furthermore, the at least one organic additive (C) is preferably selected so that the total interfacial energy γ Sof the sintering powder (SP) ≤ 25 mN·m -1< , preferably ≤ 15 mN·m -1< , and particularly preferably ≤ 10 mN·m -1< . The disperse portion of the interfacial energy γ S D should preferably be ≤ 20 mN·m -1< , preferably ≤ 11 mN·m -1< , and particularly preferably ≤ 7 mN·m -1< , and the polar part of the interfacial energy γ S P should preferably be ≤ 5 mN m-1, more preferably ≤ 4 mN·m -1< , and particularly preferably ≤ 3 mN·m -1< .

[0165] The calculation of the interfacial energy is carried out in the present invention using the Owens-Wendt model (Owens, DK; Wendt, RC; Jour. of Applied Polymer Science, 13, 1741, (1969)).

[0166] For this purpose, the powdered samples are applied to a self-made adhesive film (Acronal V215 on PET film). Excess material is removed with an air gun. Eight to ten drops of test liquids (ethylene glycol, formamide, water) are applied to each powder layer with a drop volume of approximately 1.5 µL. The contact angle θ is determined by drop shape analysis immediately after the first contact with the surface (5 s after drop deposition). The measurement is performed at 23 °C. A Drop Shape Analyzer DSA100 (Krüss GmbH, Germany) is used as the analysis device.

[0167] In Figure 2 are the contact angle θ, the interfacial energy of the test liquid γ L , the interfacial energy of the sintering powder (SP) γ S and the interfacial energy γ SLbetween test liquid and sintering powder (SP). For contact angle measurement, the test liquid (I) is applied to the sample (II).

[0168] Using the Owens-Wendt equation (Formula IX) and the measured contact angle θ The interfacial energy of the powder can be determined using linear regression γ S with the polar γ S P and dispersed fraction γ S P be determined: γ L 1 + cosθ 2 γ L D 1 2 = γ S P 1 2 γ L P 1 2 γ L D 1 2 + γ S D 1 2

[0169] The following relationships must be taken into account (Formula X and Formula XI): γ L = γ L D + γ L P γ S = γ S D + γ S P Meaning of the variables:

[0170] θ Contact angle γ L Interfacial energy of the test liquid γ L D disperse fraction of the interfacial energy of the test liquid γ L P polar component of the interfacial energy of the test liquid γ S Interfacial energy of the sintered powder (SP) γ S D disperse fraction of the interfacial energy of the sintering powder (SP) γ S P polar part of the interfacial energy of the sintering powder (SP)

[0171] Preferably, the sintering powder (SP) contains at least 0.1 wt.%, more preferably at least 0.2 wt.%, and particularly preferably at least 0.4 wt.%, of component (C), based on the sum of the weight percentages of components (A), (B), (C), optionally (D) and optionally (E), preferably based on the total weight of the sintering powder (SP).

[0172] Furthermore, the sintering powder (SP) preferably contains at most 5.0 wt.%, more preferably at most 3.0 wt.%, and particularly preferably at most 1.1 wt.%, of component (C), based on the sum of the weight percentages of components (A), (B), (C), optionally (D) and optionally (E), preferably based on the total weight of the sintering powder (SP). Component (D)

[0173] Component (D) is at least one further additive.

[0174] In the context of the present invention, "at least one further additive" means both exactly one further additive and a mixture of two or more further additives.

[0175] Additives as such are known to those skilled in the art. For example, the at least one further additive is selected from the group consisting of antinucleating agents, stabilizers, conductive additives, end-group functionalizers, dyes, antioxidants (preferably sterically hindered phenols), flame retardants, and color pigments.

[0176] A suitable antinucleating agent is lithium chloride, for example. Suitable stabilizers include phenols, phosphites, metal soaps, and copper stabilizers. Suitable conductive additives include carbon fibers, metals, stainless steel fibers, carbon nanotubes, and carbon black. Suitable end-group functionalizers include terephthalic acid, adipic acid, and propionic acid. Suitable dyes and color pigments include carbon black and iron chromium oxide. A suitable antioxidant is, for example, Irganox®< 245 from BASF SE.

[0177] Suitable metal soaps include metal stearates such as magnesium stearate, calcium stearate, zinc stearate and sodium stearate, metal alkyl sulfonates such as sodium laurylsulfonate, metal alkyl sulfates and metal alkyl phosphates.

[0178] If the sintering powder (SP) contains component (D), it preferably contains at least 0.1% by weight of component (D), more preferably at least 0.2% by weight of component (D), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP).

[0179] If the sintering powder (SP) contains component (D), it further preferably contains at most 5 wt.% of component (D), more preferably at most 2.5 wt.% of component (D), based on the sum of the weight percentages of components (A), (B), (C), (D) and (E), preferably based on the total weight of the sintering powder (SP). Component (E)

[0180] According to the invention, the optionally present component (E) is at least one reinforcing agent.

[0181] In the context of the present invention, "at least one reinforcing agent" means both exactly one reinforcing agent and a mixture of two or more reinforcing agents.

[0182] In the context of the present invention, a reinforcing agent is understood to mean a material which improves the mechanical properties of shaped bodies produced by the process according to the invention compared to shaped bodies which do not contain the reinforcing agent.

[0183] Reinforcing agents as such are known to those skilled in the art. Component (E) can, for example, be spherical, platelet-shaped, or fibrous.

[0184] Preferably, the at least one reinforcing agent is spherical or platelet-shaped.

[0185] In the context of the present invention, "platelet-shaped" means that the particles of the at least one reinforcing agent have a diameter to thickness ratio in the range from 4:1 to 10:1, determined by microscopy with image analysis after ashing.

[0186] Suitable reinforcing agents are known to the person skilled in the art and are selected, for example, from the group consisting of carbon nanotubes, glass spheres and aluminum silicates.

[0187] Preferably, the at least one reinforcing agent is selected from the group consisting of glass beads and aluminum silicates. These reinforcing agents can also be epoxy-functionalized.

[0188] Suitable aluminum silicates are known to those skilled in the art. Aluminum silicates are compounds containing Al 2 O 3 and SiO 2 . Structurally, aluminum silicates have in common that the silicon atoms are coordinated tetrahedrally by oxygen atoms, and the aluminum atoms are coordinated octahedrally by oxygen atoms. Aluminum silicates may also contain other elements.

[0189] Preferred aluminum silicates are phyllosilicates. Calcined aluminum silicates are particularly preferred, and calcined phyllosilicates are especially preferred. The aluminum silicate can also be epoxy-functionalized.

[0190] If at least one reinforcing agent is an aluminum silicate, the aluminum silicate can be used in any form. For example, it can be used as pure aluminum silicate, or it is also possible for the aluminum silicate to be used as a mineral. Aluminum silicate is preferably used as a mineral. Suitable aluminum silicates include feldspars, zeolites, sodalite, sillimanite, andalusite, and kaolin. Kaolin is preferred as an aluminum silicate.

[0191] Kaolin belongs to the clay rocks and essentially contains the mineral kaolinite. The molecular formula of kaolinite is Al 2 [(OH) 4 / Si 2 O 5 ]. Kaolinite is a phyllosilicate. In addition to kaolinite, kaolin typically contains other compounds such as titanium dioxide, sodium oxides, and iron oxides. Kaolin preferred according to the invention contains at least 98 wt.% kaolinite, based on the total weight of the kaolin.

[0192] It is clear to a person skilled in the art that component (E) is different from component (B). Component (E) typically has a larger particle diameter than component (B), i.e., it has a size (D90 value) > 10 µm, for example.

[0193] If the sinter powder contains component (E), it preferably contains at least 5% by weight of component (E), more preferably at least 10% by weight of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D), and (E), preferably based on the total weight of the sinter powder (SP).

[0194] If the sinter powder contains component (E), it further preferably contains at most 30 wt.% of component (E), more preferably at most 20 wt.% of component (E), based on the sum of the weight percentages of components (A), (B), (C), (D), and (E), preferably based on the total weight of the sinter powder (SP). Sintering process

[0195] Another object of the present invention is a process for producing a shaped body comprising the steps: i) providing a layer of sintering powder (SP), ii) exposing or heating the layer of sintering powder (SP) provided in step i).

[0196] In step ii), the layer of sintering powder (SP) provided in step i) is exposed to light or heated.

[0197] Upon exposure or heating, at least part of the sintering powder (SP) layer melts. The molten sintering powder (SP) flows into each other and forms a homogeneous melt. After exposure, the molten portion of the sintering powder (SP) layer cools down again, and the homogeneous melt solidifies again.

[0198] All methods known to the person skilled in the art are suitable for exposure. Exposure in step ii) is preferably carried out using a radiation source. The radiation source is preferably selected from the group consisting of infrared radiators and lasers. Near-infrared radiators are particularly preferred as infrared radiators.

[0199] The present invention therefore also relates to a process in which the exposure in step ii) is carried out with a radiation source selected from the group consisting of lasers and infrared radiators.

[0200] Suitable lasers are known to those skilled in the art and include, for example, fiber lasers, Nd:YAG lasers (neodymium-doped yttrium aluminum garnet lasers), or carbon dioxide lasers. The carbon dioxide laser typically has a wavelength of 10.6 µm.

[0201] If a laser is used as the radiation source during the exposure in step ii), the layer of sintering powder (SP) provided in step i) is typically exposed locally and briefly to the laser beam. Only those parts of the sintering powder (SP) exposed to the laser beam are selectively melted. If a laser is used in step ii), the process according to the invention is also referred to as selective laser sintering. Selective laser sintering is known as such to those skilled in the art.

[0202] If an infrared radiator, in particular a near-infrared radiator, is used as the radiation source during exposure in step ii), the wavelength at which the radiation source radiates is usually in the range from 780 nm to 1000 µm, preferably in the range from 780 nm to 50 µm and in particular in the range from 780 nm to 2.5 µm.

[0203] During exposure in step ii), the entire layer of sintering powder (SP) is typically exposed. To ensure that only the desired areas of the sintering powder (SP) melt during exposure, an infrared-absorbing ink (IR-absorbing ink) is typically applied to the areas to be melted.

[0204] The process for producing the shaped body then preferably comprises, between step i) and step ii), a step i-1), applying at least one IR-absorbing ink to at least part of the layer of sintering powder (SP) provided in step i).

[0205] A further subject of the present invention is therefore also a process for producing a shaped body, comprising the steps i) Providing a layer of a sintering powder (SP) which comprises the components 59.5 to 99.85 wt. %, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one thermoplastic polyurethane (A), 0.05 to 0.5 wt. %, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one flow agent (B), 0.1 to 5 wt. %, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one organic additive (C), 0 to 5 wt. %, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one further additive (D) and 0 to 30 wt.-%, based on the sum of the percentages by weight of (A), (B), (C), (D) and (E), of at least one reinforcing agent (E), wherein the at least one organic additive (C) is selected from the group consisting of polypropylene waxes grafted with maleic acid and / or maleic anhydride and amide waxes, i-1) applying at least one IR-absorbing ink to at least part of the layer of sintering powder (SP) provided in step i), ii) exposing the layer of sintering powder (SP) provided in step i).

[0206] All IR-absorbing inks known to the person skilled in the art are suitable as IR-absorbing inks, in particular IR-absorbing inks known to the person skilled in the art for high-speed sintering.

[0207] IR-absorbing inks typically contain at least one absorber that absorbs IR radiation, preferably NIR radiation (near-infrared radiation). Upon exposure of the sinter powder layer (SP) in step ii), the portion of the sinter powder layer (SP) to which the IR-absorbing ink has been applied is selectively heated by the absorption of the IR radiation, preferably the NIR radiation, by the IR absorber contained in the IR-absorbing ink.

[0208] In addition to the at least one absorber, the IR-absorbing ink may contain a carrier liquid. Suitable carrier liquids are known to those skilled in the art and include, for example, oils or water.

[0209] The at least one absorber can be dissolved or dispersed in the carrier liquid.

[0210] If the exposure in step ii) is carried out with a radiation source selected from infrared radiators and step i-1) is carried out, then the process according to the invention is also referred to as High-Speed ​​Sintering (HSS) or Multijet fusion process (MJF) These processes are known to the person skilled in the art. Multijet fusion process (MJF) A non-absorbing ink, a "detailing agent", is also usually used.

[0211] Following step ii), the layer of sintering powder (SP) is typically lowered by the thickness of the layer of sintering powder (SP) provided in step i), and another layer of sintering powder (SP) is applied. This layer is then exposed or heated again according to step ii).

[0212] As a result, the upper layer of the sintering powder (SP) bonds with the lower layer of the sintering powder (SP), and the particles of the sintering powder (SP) within the upper layer bond with each other by melting.

[0213] In the process according to the invention, steps i) and ii) and optionally i1) can therefore be repeated.

[0214] By repeating the lowering of the powder bed, the application of the sintering powder (SP), and the exposure or heating, thus melting the sintering powder (SP), three-dimensional molded bodies are produced. It is possible to produce molded bodies that, for example, also have cavities. Additional support material is not necessary, since the unmelted sintering powder (SP) itself acts as the support material.

[0215] A further subject of the present invention is therefore also a shaped body obtainable via a sintering process using a sintering powder (SP) according to the invention.

[0216] The sintering powder (SP) according to the invention is particularly suitable for use in a sintering process.

[0217] The present invention therefore also relates to the use of a sintering powder (SP) which contains the components 59.5 to 99.85 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one thermoplastic polyurethane (A), 0.05 to 0.5 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one flow agent (B), 0.1 to 5 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one organic additive (C), 0 to 5 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one further additive (D) and 0 to 30 wt.%, based on the sum of the weight percentages (A), (B), (C), (D) and (E), of at least one reinforcing agent (E), wherein the at least one organic additive (C) is selected from the group consisting of polypropylene waxes and amide waxes grafted with maleic acid and / or maleic anhydride, in a sintering process, preferably in a selective laser sintering process (SLS) or in a multi-jet fusion process (MJF).

[0218] However, it is also possible to use the sintering powder (SP) according to the invention for the production of shaped bodies in addition to the selective laser sintering process (SLS) or the multi-jet fusion process (MJF) in other powder-based 3D printing processes.

[0219] A further object of the present invention is the use of at least one flow agent (B) and at least one organic additive (C) in a sintering powder (SP) containing at least one thermoplastic polyurethane (A) to improve the flowability and coalescence of the sintering powder (SP), wherein the at least one organic additive (C) is selected from the group consisting of polypropylene waxes grafted with maleic acid and / or maleic anhydride and amide waxes. molded body

[0220] The process according to the invention produces a molded body. The molded body can be removed from the powder bed after cooling. Any adhering particles of the sinter powder that have not been melted can be mechanically removed from the surface using known methods. Processes for surface treatment of the molded body include, for example, vibratory grinding or slide machining, as well as sandblasting, glass bead blasting, or microblasting.

[0221] It is also possible to further process the resulting molded bodies or, for example, to treat the surface.

[0222] A further subject of the present invention is therefore a shaped body obtainable by the process according to the invention.

[0223] The resulting molded body preferably has a tensile strength of ≥ 5 MPa, more preferably ≥ 7 MPa, and particularly preferably ≥ 9 MPa. Furthermore, it preferably has an elongation at break of ≥ 100%, more preferably ≥ 200%, and particularly preferably ≥ 300%.

[0224] In the context of this invention, the tensile strength and elongation at break were determined using the tensile test according to DIN 53504. The S2 shoulder bar was used as the test geometry, and specimens were drawn at 200 mm / min (Z010, Zwick / Roell, Germany). For the measurements, specimens were always printed horizontally in the X-direction within the build space layout.

[0225] The moldings obtained usually contain 59.5 to 99.85 wt.% of component (A), 0.05 to 0.5 wt.% of component (B), 0.1 to 5 wt.% of component (C), 0 to 5 wt.% of component (D) and 0 to 30 wt.% of component (E), in each case based on the total weight of the molding.

[0226] The shaped body preferably contains in the range from 74.15 to 99.7 wt.% of component (A), in the range from 0.1 to 0.35 wt.% of component (B), in the range from 0.2 to 3 wt.% of component (C), in the range from 0 to 2.5 wt.% of component (D) and in the range from 0 to 20 wt.% of component (E), in each case based on the total weight of the shaped body.

[0227] Most preferably, the shaped body contains in the range of 76.12 to 99.42 wt.% of component (A), in the range of 0.18 to 0.28 wt.% of component (B), in the range of 0.4 to 1.1 wt.% of component (C), in the range of 0 to 2.5 wt.% of component (D) and in the range of 0 to 20 wt.% of component (E), in each case based on the total weight of the shaped body.

[0228] The weight percentages of components (A), (B), (C), (D) and (E) usually add up to 100 wt.%.

[0229] If the shaped body contains component (D), it can contain, for example, in the range from 0.1 to 5% by weight of component (D), preferably in the range from 0.2 to 2.5% by weight of component (D), based on the total weight of the shaped body.

[0230] If the shaped body contains component (E), it can contain, for example, in the range of 5 to 30 wt.% of component (E), preferably in the range of 10 to 20 wt.% of component (E), based on the total weight of the shaped body.

[0231] If the molded body contains component (D) and / or component (E), the percentages by weight of the at least one thermoplastic polyurethane (A) contained in the molded body are usually reduced accordingly, so that the sum of the percentages by weight of the at least one thermoplastic polyurethane (A), component (B), component (C) and component (D) and / or component (E) amounts to 100% by weight.

[0232] If the shaped body contains component (D), it contains, for example, in the range from 59.5 to 99.75 wt.% of component (A), in the range from 0.05 to 0.5 wt.% of component (B), in the range from 0.1 to 5 wt.% of component (C), in the range from 0.1 to 5 wt.% of component (D) and in the range from 0 to 30 wt.% of component (E), based on the total weight of the shaped body.

[0233] If the shaped body contains component (D), it preferably contains in the range from 74.15 to 99.5% by weight of component (A), in the range from 0.1 to 0.35% by weight of component (B), in the range from 0.2 to 3% by weight of component (C), in the range from 0.2 to 2.5% by weight of component (D) and in the range from 0 to 20% by weight of component (E), based on the total weight of the shaped body.

[0234] If the shaped body contains component (D), it thus more preferably contains in the range of 76.12 to 99.22 wt.% of component (A), in the range of 0.18 to 0.28 wt.% of component (B), in the range of 0.4 to 1.1 wt.% of component (C), in the range of 0.2 to 2.5 wt.% of component (D) and in the range of 0 to 20 wt.% of component (E), based on the total weight of the shaped body.

[0235] If the shaped body contains component (E), it contains, for example, in the range from 59.5 to 94.85 wt.% of component (A), in the range from 0.05 to 0.5 wt.% of component (B), in the range from 0.1 to 5 wt.% of component (C), in the range from 0 to 5 wt.% of component (D) and in the range from 5 to 30 wt.% of component (E), based on the total weight of the shaped body.

[0236] If the shaped body contains component (E), it preferably contains in the range from 74.15 to 89.7% by weight of component (A), in the range from 0.1 to 0.35% by weight of component (B), in the range from 0.2 to 3% by weight of component (C), in the range from 0 to 2.5% by weight of component (D) and in the range from 10 to 20% by weight of component (E), based on the total weight of the shaped body.

[0237] If the shaped body contains component (E), it thus more preferably contains in the range of 76.12 to 89.42 wt.% of component (A), in the range of 0.18 to 0.28 wt.% of component (B), in the range of 0.4 to 1.1 wt.% of component (C), in the range of 0 to 2.5 wt.% of component (D) and in the range of 10 to 20 wt.% of component (E), based on the total weight of the shaped body.

[0238] If the shaped body contains components (D) and (E), it contains, for example, in the range from 59.5 to 94.75 wt.% of component (A), in the range from 0.05 to 0.5 wt.% of component (B), in the range from 0.1 to 5 wt.% of component (C), in the range from 0.1 to 5 wt.% of component (D) and in the range from 5 to 30 wt.% of component (E), based on the total weight of the shaped body.

[0239] If the shaped body contains components (D) and (E), it preferably contains in the range from 74.15 to 89.5 wt.% of component (A), in the range from 0.1 to 0.35 wt.% of component (B), in the range from 0.2 to 3 wt.% of component (C), in the range from 0.2 to 2.5 wt.% of component (D) and in the range from 10 to 20 wt.% of component (E), based on the total weight of the shaped body.

[0240] If the shaped body contains components (D) and (E), it thus more preferably contains in the range of 76.12 to 89.22 wt.% of component (A), in the range of 0.18 to 0.28 wt.% of component (B), in the range of 0.4 to 1.1 wt.% of component (C), in the range of 0.2 to 2.5 wt.% of component (D) and in the range of 10 to 20 wt.% of component (E), based on the total weight of the shaped body.

[0241] In general, component (A) refers to the component (A) contained in the sintering powder (SP). Similarly, component (B) refers to the component (B) contained in the sintering powder (SP), component (C) refers to the component (C) contained in the sintering powder (SP), component (D) refers to the component (D) contained in the sintering powder (SP), and component (E) refers to the component (E) contained in the sintering powder (SP).

[0242] When step i-1) has been carried out, the molded body also usually contains residual components of the IR-absorbing ink.

[0243] It is clear to the person skilled in the art that exposure to light or heating of the sintering powder (SP) can cause components (A), (B), and (C), as well as optionally (D) and (E), to undergo chemical reactions and thus change. Such reactions are known to the person skilled in the art.

[0244] Preferably, the components (A), (B) and (C) and optionally (D) and (E) do not enter into a chemical reaction during exposure in step ii), but the sintering powder (SP) merely melts.

[0245] The invention is explained in more detail below using examples, without being limited thereto. Examples

[0246] The following Components used: Component (A): Thermoplastic polyurethane (TPU); Elastollan SP9415, BASF SE Component (B1): Hydrophobic fumed silica; Aerosil R 812, Evonik, Germany Component (B2): Hydrophobic fumed silica; HDK H20, Wacker Chemie Component (B3): Hydrophobic fumed silica; Aerosil R 972, Evonik, Germany Component (C): N,N'-Ethylendi(stearamid), Tropfpunkt DP = 142°C Measurement methods: Determination of the interfacial energy of the sintering powder (SP)

[0247] The interfacial energy of the sintering powder (SP) was calculated using the Owens-Wendt model (Owens, DK; Wendt, RC; Journal of Applied Polymer Science, 13, 1741, (1969)).

[0248] For this purpose, the powdered samples were applied to a self-made adhesive film (Acronal V215 on PET film). Excess material was removed with an air gun. Eight to ten drops of the test liquids listed in Table 1 were each applied to the powder layers with a drop volume of approximately 1.5 µL. The contact angle θ was determined by drop shape analysis immediately after initial contact with the surface (5 s after drop deposition). The measurement was performed at 23 °C. A Drop Shape Analyzer DSA100 (Krüss GmbH, Germany) was used as the analysis device.

[0249] In Figure 2are the contact angle θ, the interfacial energy of the test liquid γ L , the interfacial energy of the sintering powder (SP) γ S and the interfacial energy γ SL between test liquid and sintering powder (SP). For contact angle measurement, the test liquid (I) is applied to the sample (II). Table 1 Interfacial energy (mN m -1< ) Dispersed fraction ( γ L D ) Polar component ( γ L P ) Total ( γ L ) Ethylene glycol 26,4 21,3 47,7 Formamide 39,5 18,7 58,2 Water 21,8 51,0 72,8

[0250] Using the Owens-Wendt equation (Formula IX) and the measured contact angle θ The interfacial energy of the powder can be determined using linear regression γ S with the polar γ S P and dispersed fraction γ S P be determined: γ L 1 + cosθ 2 γ L D 1 2 = γ S P 1 2 γ L P 1 2 γ L D 1 2 + γ S D 1 2

[0251] The following relationships must be taken into account (Formula X and Formula XI): γ L = γ L D + γ L P γ S = γ S D + γ S P Meaning of the variables:

[0252] θ Contact angle γ LInterfacial energy of the test liquid γ L D disperse fraction of the interfacial energy of the test liquid γ L P polar component of the interfacial energy of the test liquid γ S Interfacial energy of the sintered powder (SP) γ S D disperse fraction of the interfacial energy of the sintering powder (SP) γ S P polar part of the interfacial energy of the sintering powder (SP) Determination of the D50 value of the sintering powder (SP) and the D90 value of at least one flow agent (component (B))

[0253] The particle sizes were determined using laser diffraction according to ISO 13320 (Horiba LA-960, Retsch Technology, Germany). The sintering powder (SP) or at least one superplasticizer (B) were previously dry-dispersed at 1 bar. The evaluation was performed using the Fraunhofer method. Determination of the dropping point ( D p ) of at least one organic additive (component (C))

[0254] The dropping point ( D p ) of the organic additives was measured according to ISO 2176 using a dropping point meter (AD0566-600, Scavini, Italy). Determination of the melting temperature (T M(SP) ) of the sinter powder (SP)

[0255] The melting temperature was determined using DSC (Differential Scanning Calorimetry, Discovery series DSC, TA Instruments) according to DIN EN ISO 11357.

[0256] For the DSC measurements, the sample was subjected to the following temperature cycle under a nitrogen atmosphere: 5 minutes at minus 80°C, followed by heating to at least 200°C at 20°C / minute (1st heating run (H1)), then 5 minutes at least 200°C, followed by cooling to minus 80°C at 20°C / minute, then 5 minutes at minus 80°C, followed by heating to at least 200°C at 20°C / minute (2nd heating run (H2)). The melting temperature (TM(SP) ) then corresponded to the temperature at the maximum of the melting peak of the heating run (H1). If several local maxima occur in the range between TM Onset< and TM Endset<, the melting temperature TM is understood to be the numerical mean of the respective local maxima. Determination of bulk density

[0257] The bulk density was determined according to DIN EN ISO 60. Determination of tensile strength and elongation at break

[0258] Tensile strength and elongation at break were determined using the tensile test according to DIN 53504. The S2 shoulder bar was used as the test geometry, and specimens were drawn at 200 mm / min (Z010, Zwick / Roell, Germany). For the measurements, specimens were always printed horizontally in the X-direction within the build space layout. Determination of the melt volume rate of the sintering powder (SP) (melt volume rate, MVR)

[0259] The melt volume rate was determined according to DIN EN ISO 1133 (mi2.1, Göttfert, Germany). For this purpose, the sinter powder (SP) was pre-dried for 2 hours at 110°C under nitrogen and then subjected to a load of 2.16 kg and at a temperature of ( TM(SP) + 40°C) measured. Production of sinter powder (SP) Inventive Example 1 (B1)

[0260] Component (A) was annealed for 48 hours at 100°C in a dry nitrogen atmosphere. Subsequently, 0.05 wt.% of component (B1) and 1 wt.% of component (C) were added, and the mixture was mechanically processed to powder under cryogenic conditions (cryogenic comminution) in a pin mill (GSM 250, Gotic, Germany). The mixture was then classified using a vibrating screen (0.1 x 0.3 mm long mesh). After grinding, another 0.15 wt.% of component (B1) was added (Thermomix TM5, Vorwerk; 5 minutes at 2000 rpm). Inventive Example 2 (B2)

[0261] For this example, a composition was prepared analogously to Example 1. After grinding, an additional 1 wt.% of component (C) was added ( N,N '-Ethylenedi(stearamide), dropping point 142 °C). Comparison example 3 (VB3)

[0262] Example 2 from DE 10 2017 124 047 A1 was reworked. Comparison example 4 (VB4)

[0263] For this comparative example, a composition analogous to Example 1 was prepared, whereby component (C) not was used. 0.55 wt.% instead of 0.15 wt.% of component (B1) was added after grinding. Comparison example 5 (VB5)

[0264] For this comparative example, a composition was prepared analogously to Example 1. After grinding, an additional 5 wt.% of component (C) was added. Comparison example 6 (VB6)

[0265] Example 1 from EP 3 157 737 B1 was reworked.

[0266] The above-mentioned amounts of components and the properties of the produced sinter powders (SP) are given in Table 2. Table 2 Example / Comparison example B1 B2 VB3 VB4 VB5 VB6 Component (A) (wt%) 98,8 97,8 99,8 99,4 93,8 - TPU, synthesized according to EP 3 157 737 B1 (wt%) - - - - - 99,8 Component (B) (= B1 + B2 + B3) (% by weight) 0,2 0,2 0,2 0,6 0,2 0,2 Component (C) (wt%) 1,0 2,0 - - 6,0 - Bulk density (g / L) 524 526 500 536 529 490 Contact angle water (°) 134,2 135,3 126,9 121,4 137,7 125,3 Contact angle ethylene glycol (°) 124,6 127,1 100,6 95,9 134,3 99,5 Contact angle formamide (°) 125,9 127,3 92,8 84,2 131,2 94,5 Disperse interfacial energy (mN / m) 2,6 2,5 27,7 33,6 1,0 28,6 Polar interfacial energy (mN / m) 0,2 0,2 2,1 2,0 0,4 2,0 Total interfacial energy (mN / m) 2,8 2,5 29,8 35,6 1,4 31,1 Particle size D50 (µm) 79 77 72 71 74 75 Melting point TM(SP) (°C) 140 140 140 140 140 130 Melt volume rate MVR (cm 3 < / 10 min) 49 53 46 47 54 28 Production throughput (grinding + sieving) (kg / h) 125 125 30 30 125 20 Production of the molded bodies

[0267] The identical installation space layout was used for production examples 1 to 6. The installation space layout used is shown in Figure 3 The following parts were included in the build envelope layout: 37 tension bars (I) (X and Z orientation), 9 curl crosses (II), and 41 other technical test parts such as hollow spheres (III), tubes (IV), discs (V), and other free-form bodies. The free-form bodies were primarily used to verify component quality. In total, the build envelope layout contains 87 test parts, dimensions 180 x 180 x 226 mm, and a packing density of 7.7%.

[0268] The identical installation space layout was also used for production examples 10 to 12. This was an adapted installation space layout. This is shown in Figure 4The following parts were included in the build space layout: 74 tension bars (I) (X and Z orientation), 18 curl crosses (II), 120 other technical test parts such as hollow spheres (III), tubes (IV), discs (V), lattice structures (VI), shoe soles (VII), and other free-form bodies. The free-form bodies were primarily used to verify component quality. In total, the build space layout contains 87 test parts, dimensions 380 x 284 x 371 mm, and a packing density of 7.3%. Manufacturing example 1 (F1B1)

[0269] The sinter powder (SP) from Example 1 (B1) according to the invention was processed into molded bodies using a commercially available laser sintering machine (Farsoon, HT251P, China). The processing parameters for laser sintering are listed in Table 3. Manufacturing example 2 (F1B2)

[0270] The sinter powder (SP) from inventive example 2 (B2) was processed into molded bodies using a commercially available laser sintering machine (Farsoon, HT251P, China). The processing parameters for laser sintering are listed in Table 3. Manufacturing example 3 (F1VB3)

[0271] The sinter powder (SP) from Comparative Example 3 (VB3) was processed into molded bodies using a commercially available laser sintering machine (Farsoon, HT251P, China). The processing parameters for laser sintering are listed in Table 3. Manufacturing example 4 (F1VB4)

[0272] The sinter powder (SP) from Comparative Example 4 (VB4) was processed into molded bodies using a commercially available laser sintering machine (Farsoon, HT251P, China). The processing parameters for laser sintering are listed in Table 3. Manufacturing example 5 (F1VB5)

[0273] The sinter powder (SP) from Comparative Example 5 (VB5) was processed into molded bodies using a commercially available laser sintering machine (Farsoon, HT251P, China). The processing parameters for laser sintering are listed in Table 3. Manufacturing example 6 (F1VB6)

[0274] The sinter powder (SP) from Comparative Example 6 (VB6) was processed into molded bodies using a commercially available laser sintering machine (Farsoon, HT251P, China). The processing parameters for laser sintering are listed in Table 3. Table 3 Manufacturing examples 1 to 6 (except 6) Manufacturing example 6 Laser energy (W) 50 40 Installation space temperature (°C) 108 95 Laser line spacing (mm) 0,10 0,2 Laser speed (m / s) 15 4 Powder layer thickness (mm) 0,1 0,15 Manufacturing example 10 (F2B1)

[0275] The sinter powder (SP) from inventive example 1 (B1) was processed into test specimens using a Multi Jet Fusion machine (HP, HP Jet Fusion 5210 3D Printer, USA). 'Ultrasint TPU01 - Balanced' was used as the parameter settings. Manufacturing example 11 (F2VB3)

[0276] The sinter powder (SP) from Comparative Example 3 (VB3) was processed into test specimens using a Multi Jet Fusion machine (HP, HP Jet Fusion 5210 3D Printer, USA). 'Ultrasint TPU01 - Balanced' was used as the parameter settings. Manufacturing example 12 (F2VB5)

[0277] The sinter powder (SP) from Comparative Example 5 (VB5) was processed into test specimens using a Multi Jet Fusion machine (HP, HP Jet Fusion 5210 3D Printer, USA). The parameter settings used were 'Ultrasint TPU01 - Balanced'. Reference 1 (R1)

[0278] The values ​​from Example 1 of US 8114334 B2 were entered as comparison values ​​in Table 4.

[0279] The properties of the produced molded bodies are summarized in Tables 4 and 5. Table 4 F1 B1 F1 B2 F1 VB3 F1 VB4 F1 VB5 F1 VB6 R1 Sinter powder B1 B2 VB3 VB4 VB5 VB6 - Tensile strength (MPa) 9,1 8,5 8,1 7,2 6,8 16 2.7 Tensile elongation (%) 360 320 270 220 170 370 170 Process capability* 9,7 9,3 6,3 3,3 3,8 1,2 - Component quality* 9,8 9,2 6,8 4,5 4,9 0,7 - Building demolitions** 0 0 1 2 1 7 - Table 5 F2B1 F2VB3 F2VB5 Sinter powder B1 VB3 VB5 Tensile strength (MPa) 9,0 8,3 6,3 Tensile elongation (%) 310 280 180 Process capability* 10 5,7 4,7 Component quality* 9,9 6,4 6,1 Building demolitions** 0 2 2 * The Process capability was monitored by at least three different machine operators during 10 complete print runs. A complete print run means that the build space layout could be completely created. In addition, the Component quality The molded parts produced during the aforementioned printing processes were examined by the machine operators. The process capability and part quality were then rated by the machine operators on a scale of 0 to 10 (10 = best; 1 = worst). The values ​​in Tables 5 and 6 correspond to the numerical mean of at least three independent evaluations. A score of 0 represents the lowest rating. If so many defects were observed during construction that the score would fall below 0, the printing process is aborted (see Demolition **).

[0280] A printing test is repeated until the build space layout has been completely created.

[0281] The following defects lead to a deduction in the process capability assessment: Flowability problems during dosing / feeding of the powder formulation: -2 points. Problems (inhomogeneities) during the application of the powder layers, such as: Agglomeration of the powder in / on the powder bed: -1 point. Streaks in the powder bed: -0.5 points (1-3 streaks), -1 point (4-6 streaks), -2 points (> 6 streaks); streaks are defined as slight, not very deep furrows. Deep holes or furrows in the powder bed: -1 point (per hole or furrow). Tilting / wedging of the application tool (e.g., doctor blade, roller): -2 points. So-called short feeds (with a short feed, too little powder is applied as a powder layer): -2 points.

[0282] The following defects lead to a deduction in the assessment of component quality: Overmelting of parts due to strong local heat build-up in the parts: -1 point Warpage of manufactured components: -3 points Surface defects: -1 point (per 3 defects) Excessively rough surface on the parts: -1 point ** At a Demolition the further printing process is prevented because, for example, the powder application system (blade, roller) is blocked, parts have come up (due to a warp), parts are stuck on the powder application system and / or the powder dosing is / becomes blocked.

[0283] A construction abort results in the partially manufactured molded parts having to be discarded and reprinted. This leads to increased material loss and a longer construction time, resulting in a significant deterioration in economic efficiency. Therefore, the number of construction aborts that occurred during the execution of 10 complete construction processes (excluding demolition) is listed separately. Thus, the number of construction aborts is not included in the process capability assessment, as a construction abort represents a clearly failed process.

Claims

1. A sinter powder (SP) comprising the following components: 59.5% to 99.85% by weight, based on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), of at least one thermoplastic polyurethane (A), 0.05% to 0.5% by weight, based on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), of at least one flow agent (B), 0.1% to 5% by weight, based on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), of at least one organic additive (C), 0% to 5% by weight, based on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), of at least one further additive (D) and 0% to 30% by weight, based on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), of at least one reinforcer (E), wherein the at least one organic additive (C) is selected from the group consisting of maleic acid- and / or maleic anhydride-grafted polypropylene waxes and amide waxes.

2. The sinter powder (SP) according to claim 1, wherein the at least one flow agent (B) is selected from the group consisting of silicon dioxide, silicates, silicas, metal oxides, minerals, borates, phosphates, sulfates and carbonates, preferably from hydrophobic fumed silicas, talc, kaolin, magnesium sulfate, calcium sulfate, barium sulfate, magnesium carbonate, calcium carbonate and barium carbonate.

3. The sinter powder (SP) according to claim 1 or 2, wherein the sinter powder (SP) comprises i) 74.15% to 99.7% by weight, preferably 76.12% to 99.42% by weight, of component (A), based in each case on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), and / or ii) 0.1% to 0.35% by weight, preferably 0.18% to 0.28% by weight, of component (B), based in each case on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), and / or iii) 0.2% to 3% by weight, preferably 0.4% to 1.1% by weight, of component (C), based in each case on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), and / or iv) 0% to 2.5% by weight of component (D), based on the sum total of the percentages by weight of (A), (B), (C), (D) and (E), and / or v) 0% to 20% by weight of component (E), based on the sum total of the percentages by weight of components (A), (B), (C), (D) and (E).

4. The sinter powder (SP) according to any of claims 1 to 3, wherein the at least one organic additive (C) i) is an N,N'-alkylene fatty acid diamide, and / or ii) is selected in such a way that the dropping point of the at least one organic additive (C) satisfies the following condition (formula I): T M A − 25 ° C ≤ D P < T M A + 25 ° C where DP is the dropping point of the at least one organic additive (C) and TM(A) is the melting temperature of the at least one thermoplastic polyurethane (A), and / or iii) is selected such that the total interfacial energy γS of the sinter powder (SP) is ≤ 25 mN·m-1, preferably ≤ 15 mN·m-1, more preferably ≤ 10 mN·m-1, and / or iv) is selected such that the disperse component of the interfacial energy γ S D of the sinter powder (SP) is ≤ 20 mN·m-1, preferably ≤ 11 mN·m-1, more preferably ≤ 7 mN·m-1, and / or v) is selected such that the polar component of the interfacial energy γ S P of the sinter powder (SP) is ≤ 5 mN·m-1, preferably ≤ 4 mN·m-1, more preferably ≤ 3 mN·m-1.

5. The sinter powder (SP) according to any of claims 1 to 4, wherein the sinter powder (SP) has i) a median particle size (D50) in the range from 10 to 190 pm, preferably in the range from 15 to 150 pm, more preferably in the range from 20 to 110 pm, especially preferably in the range from 40 to 100 pm, and / or ii) a melting temperature (TM(SP)) in the range from 80 to 220°C, preferably in the range from 100 to 190°C, more preferably in the range from 120 to 170°C, and / or iii) a melt volume flow rate (MVR) in the range from 3 to 150 cm3 / 10min, preferably in the range from 15 to 100 cm3 / 10min, more preferably in the range from 30 to 70 cm3 / 10min, and / or iv) a bulk density of ≥ 300 g / L, preferably of ≥ 350 g / L and more preferably of ≥ 400 g / L.

6. The sinter powder (SP) according to any of claims 1 to 5, wherein the at least one flow agent (B) has a D90 of ≤ 10 pm, preferably ≤ 2 pm.

7. The sinter powder (SP) according to any of claims 1 to 6, wherein the at least one further additive (D) is selected from the group consisting of antinucleating agents, stabilizers, conductive additives, end group functionalizers, dyes, antioxidants, flame retardants and color pigments.

8. The sinter powder (SP) according to any of claims 1 to 7, wherein the at least one reinforcer (E) is selected from the group consisting of carbon nanotubes, glass beads and aluminum silicates, preferably from the group consisting of glass beads and aluminum silicates.

9. A method of producing a sinter powder (SP) comprising 59.5% to 99.85% by weight, based on the total weight of the sinter powder (SP), of at least one thermoplastic polyurethane (A), 0.05% to 0.5% by weight, based on the total weight of the sinter powder (SP), of at least one flow agent (B), 0.1% to 5% by weight, based on the total weight of the sinter powder (SP), of at least one organic additive (C), 0% to 5% by weight, based on the total weight of the sinter powder (SP), of at least one further additive (D) and 0% to 30% by weight, based on the total weight of the sinter powder (SP), of at least one reinforcer (E), comprising the step of a) grinding the total amount, based on the total weight of the sinter powder (SP), of component (A), wherein a first portion (BT1) of the total amount, based on the total weight of the sinter powder (SP), of component (B) and / or a first portion (CT1) of the total amount, based on the total weight of the sinter powder (SP), of component (C) are mixed into component (A) prior to step a) to obtain a powder (P), and the remaining portion (BT2) of the total amount of component (B) and / or the remaining portion (CT2) of the total amount of component (C) are mixed into the powder (P) after step a) to obtain the sinter powder (SP), wherein the first portion (BT1) accounts for 0% to 100% by weight of the total amount, based on the total weight of the sinter powder (SP), of component (B) and wherein the first portion (CT1) accounts for 0% to 100% by weight of the total amount, based on the total weight of the sinter powder (SP), of component (C), and wherein the remaining portion (BT2) accounts for (100 - BT1)% by weight of the total amount, based on the total weight of the sinter powder (SP), of component (B) and the remaining portion (CT2) accounts for (100 - CT1)% by weight of the total amount, based on the total weight of the sinter powder (SP), of component (C), and wherein optionally the total amount, based on the total weight of the sinter powder (SP), of component (D) and / or the total amount, based on the total weight of the sinter powder (SP), of component (E) is mixed in before step a) or after step a), wherein the at least one organic additive (C) is selected from the group consisting of maleic acid- and / or maleic anhydride-grafted polypropylene waxes and amide waxes.

10. A method of producing a shaped body, comprising the steps of: i) providing a layer of a sinter powder (SP) according to any of claims 1 to 8, and ii) exposing or heating the layer of the sinter powder (SP) provided in step i).

11. A shaped body obtainable by a method according to claim 10.

12. The use of at least one flow agent (B) and at least one organic additive (C) in a sinter powder (SP) comprising at least one thermoplastic polyurethane (A) for improving the flowability and coalescence of the sinter powder (SP), wherein the at least one organic additive (C) is selected from the group consisting of maleic acid- and / or maleic anhydride-grafted polypropylene waxes and amide waxes.

13. The use of a sinter powder (SP) according to any of claims 1 to 8 in a sintering method, preferably in a selective laser sintering (SLS) method or in a multi-jet fusion (MJF) method.

14. A shaped body obtainable via a sintering method using a sinter powder (SP) according to any of claims 1 to 8.