Compound, rubber compound containing the compound, vehicle tire incorporating the rubber compound in at least one component, method for producing the compound, and use of the compound as an anti-aging agent and / or antioxidant and / or oxidant and / or colorant

DE502021005755D1Active Publication Date: 2024-11-28CONTINENTAL REIFEN DEUTSCHLAND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005755
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-02
Filing Date
2021-09-29
Publication Date
2024-11-28
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing anti-aging agents for rubber materials, such as vehicle tires, have limitations in reactivity and protective effects against oxidation and ozone, leading to reduced longevity and performance over time, especially at higher temperatures.

Method used

A novel compound, N-(1,3-dimethylbutyl)-N'-p-hydroxyphenyl-p-phenylenediamine, with enhanced reactivity towards oxygen, ozone, and radicals due to a hydroxy group, is introduced, which can be used in rubber mixtures and vehicle tires to provide improved protective effects.

Benefits of technology

The compound offers increased longevity and ozone protection for rubber materials by capturing more radicals and providing better reactivity compared to existing anti-aging agents, leading to improved durability and performance in various rubber applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a compound, a rubber mixture containing the compound, a vehicle tire which has the rubber mixture in at least one component, a process for producing the compound and the use of the compound as an age inhibitor and / or antioxidant and / or antiozonant and / or dye.

[0002] It is known that polymeric materials, particularly rubber, are used in vehicle tires and technical rubber articles.

[0003] Natural rubber, synthetic polymers (such as IR, BR, SSBR, ESBR, etc.), as well as natural and synthetic oils, greases, and lubricants, are subject to oxidation reactions during extended storage, especially in their intended application, which often takes place at elevated temperatures. These oxidation reactions adversely affect the original desired properties. Depending on the type of polymer, the polymer chains are shortened, even leading to liquefaction, or the material subsequently hardens.

[0004] Anti-aging agents therefore contribute significantly to the longevity of vehicle tires and other technical rubber products.

[0005] Well-known anti-aging agents are aromatic amines, such as 6-PPD (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine), IPPD (N-isopropyl-N'-phenyl-p-phenylenediamine) or SPPD (N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine).

[0006] These molecules can react with oxygen or ozone or formed radicals, such as alkyl, alkoxy and alkylperoxy radicals, and thus capture them and protect the rubbers etc. from further oxidation reactions.

[0007] Anti-aging agents that react particularly with ozone and capture it are also called "ozone protectants" or "antiozonants".

[0008] EP 0 617 004 A1, for example, discloses a process for the preparation of N-substituted N'-phenyl-p-phenylenediamines, in particular for use as antioxidants or antiozonants.

[0009] The invention is based on the object of providing a novel compound which can be used in particular as an ageing inhibitor in vehicle tires or other technical rubber articles in order to achieve an improved protective effect of these articles on the basis of the prior art.

[0010] The object is achieved by the compound according to the invention according to claim 1, the rubber mixture according to the invention containing the compound, and the vehicle tire according to the invention, which has the rubber mixture according to the invention in at least one component. Furthermore, the object is achieved by the processes for producing the compound and the use of the compound as an anti-aging agent and / or antioxidant and / or antiozonant.

[0011] The compound according to claim 1 can also be used as a dye.

[0012] The compound according to claim 1 has the formula I):

[0013] The compound according to formula I) is therefore N-(1,3-dimethylbutyl)-N'-p-hydroxyphenyl-p-phenylenediamine.

[0014] The compound according to formula I) exhibits increased reactivity toward oxygen, ozone, or radicals (see above) compared to the known anti-aging agents 6PPD or IPPD, presumably due to the hydroxy group. This results in an improved protective effect, particularly in vehicle tires and other technical rubber articles, but also in oils and lubricants. However, the invention is not intended to be tied to a specific mechanism of action or a specific explanation.

[0015] DE1220124 discloses a compound according to formula S1):

[0016] Compared to the compound according to formula S1), the compound according to formula I) according to the invention has an additional hydrogen donor with the hydroxy group, whereby the compound according to formula I) can capture more radicals.

[0017] Combinations of different aging protection classes, e.g., phenols with aromatic amines, are also known from CN 105272892 and CN 107935867. However, the individual building blocks are not in direct conjugation, but are always isolated by an aliphatic spacer. Therefore, there is no direct influence or interaction between the groups. The compound according to the invention according to formula I) thus also exhibits improved reactivity and thus protective effect compared to the compounds from CN 105272892 and CN 107935867.

[0018] US 6770785B1 discloses the compounds according to formula S2 and S3.

[0019] Compared to the compound of formula S2), the compound of formula I) according to the invention has the advantage that its building blocks are in conjugation, resulting in a better protective effect. In formula S2), the conjugation is interrupted by the -CH 2 -NH group.

[0020] Compared to the compound according to formula S3), the compound according to the invention according to formula I) has the advantage that there is an aliphatic and not an aromatic group on the outer nitrogen atom, which results in a better protective effect against ozone.

[0021] Compounds or molecules which have only aliphatic or aromatic residues on the outer nitrogen atom instead of the 1,3-dimethylbutyl group and a hydrogen atom, i.e. no hydrogen atom, and are thus maximally substituted on the nitrogen atom, also have poorer protection against ozone compared to the compound according to the invention according to formula I), since this part of the molecule significantly influences the reactivity and the possibility of splitting off a hydrogen atom from the nitrogen atom contributes to the protective effect.

[0022] The compound according to the invention according to formula I) is particularly suitable as an ageing inhibitor and / or ozone protectant in vehicle tires and / or technical rubber articles, such as in particular an air spring, a bellows, conveyor belt, strap, belt, hose, rubber band, profile, a seal, a membrane, tactile sensors for medical applications or robot applications, or a shoe sole or parts thereof, and / or oils and / or lubricants.

[0023] The compound according to the invention according to formula I) is particularly suitable for producing a rubber article, in particular an air spring, a bellows, conveyor belt, strap, belt, hose, rubber band, profile, a seal, a membrane, tactile sensors for medical applications or robot applications, or a shoe sole or parts thereof.

[0024] For use of the compound according to formula I) in the aforementioned articles or substances, it is used in a composition and mixed into it. In the case of vehicle tires or other technical rubber articles, this is particularly a rubber compound.

[0025] The invention further relates to the use of the compound according to formula I) in oils and lubricants, such as, in particular, fuels or operating fluids for engines. The compound according to the invention can thus be used in particular in engines.

[0026] The invention further relates to the use of the compound according to the invention according to formula I) as a dye in fibers and / or polymers and / or paper and / or in (coating) paints and varnishes.

[0027] A further subject of the invention is therefore a rubber mixture.

[0028] The rubber mixture according to the invention contains the compound according to formula I). ​​The rubber mixture according to the invention can, in principle, be any rubber mixture in which the novel compound according to the invention according to formula I) achieves improved properties, in particular increased durability through ageing protection and / or ozone protection.

[0029] The rubber mixture according to the invention contains at least one rubber.

[0030] The rubber mixture according to the invention preferably contains 0.1 to 10 phr, particularly preferably 0.1 to 5 phr, very particularly preferably 1 to 5 phr, of the compound according to formula I).

[0031] The term phr (parts per hundred parts of rubber by weight) used in this document is the standard quantity used in the rubber industry for compound formulations. The dosage of the parts by weight of the individual substances in this document is based on 100 parts by weight of the total mass of all high-molecular-weight (Mw greater than 20,000 g / mol) and therefore solid rubbers present in the compound.

[0032] According to advantageous embodiments of the invention, the rubber mixture according to the invention contains at least one diene rubber.

[0033] The rubber mixture can therefore contain a diene rubber or a mixture of two or more different diene rubbers.

[0034] Diene rubbers are rubbers that are produced by polymerization or copolymerization of dienes and / or cycloalkenes and thus have C=C double bonds either in the main chain or in the side groups.

[0035] The diene rubber is preferably selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, liquid rubbers with a molecular weight M w of greater than 20,000 g / mol, halobutyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, Polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile-butadiene rubber and hydrogenated styrene-butadiene rubber.

[0036] In particular, nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halobutyl rubber, and / or ethylene-propylene-diene rubber are used in the production of technical rubber articles, such as belts, straps, and hoses, and / or shoe soles. The preferred blend compositions for these rubbers—specific with regard to fillers, plasticizers, vulcanization systems, and additives—are known to those skilled in the art.

[0037] The natural and / or synthetic polyisoprene in all embodiments can be either cis-1,4-polyisoprene or 3,4-polyisoprene. However, the use of cis-1,4-polyisoprenes with a cis-1,4 content of > 90 wt.% is preferred. Such a polyisoprene can be obtained by stereospecific polymerization in solution with Ziegler-Natta catalysts or using finely divided lithium alkyls. Natural rubber (NR) is also a cis-1,4-polyisoprene in which the cis-1,4 content in the natural rubber is greater than 99 wt.%.

[0038] Furthermore, a mixture of one or more natural polyisoprenes with one or more synthetic polyisoprene(s) is also conceivable.

[0039] For the purposes of the present invention, the term "natural rubber" refers to naturally occurring rubber that can be obtained from Hevea rubber trees and non-Hevea sources. Non-Hevea sources include, for example, guayule shrubs and dandelions such as TKS (Taraxacum kok-saghyz; Russian dandelion).

[0040] If butadiene rubber (= BR, polybutadiene) is present in the rubber mixture according to the invention, it can be any type known to the person skilled in the art. These include, among others, the so-called high-cis and low-cis types, with polybutadiene with a cis content of greater than or equal to 90 wt. % being referred to as the high-cis type and polybutadiene with a cis content of less than 90 wt. % being referred to as the low-cis type. An example of a low-cis polybutadiene is Li-BR (lithium-catalyzed butadiene rubber) with a cis content of 20 to 50 wt. High-cis BR achieves particularly good properties and low hysteresis of the rubber mixture.

[0041] The polybutadiene(s) used can be end-group modified and / or functionalized along the polymer chains. The modifications can include hydroxyl groups, ethoxy groups, epoxy groups, siloxane groups, amino groups, aminosiloxane, carboxyl groups, phthalocyanine groups, and / or silane sulfide groups. However, other modifications known to the skilled person, also referred to as functionalizations, are also possible. Metal atoms can be a component of such functionalizations.

[0042] If at least one styrene-butadiene rubber (styrene-butadiene copolymer) is present in the rubber mixture, it can be either solution-polymerized styrene-butadiene rubber (SSBR) or emulsion-polymerized styrene-butadiene rubber (ESBR), although a mixture of at least one SSBR and at least one ESBR can also be used. The terms "styrene-butadiene rubber" and "styrene-butadiene copolymer" are used synonymously in the context of the present invention.

[0043] The styrene-butadiene copolymer used can be end-group modified with the modifications and functionalizations mentioned above for polybutadiene and / or functionalized along the polymer chains.

[0044] Preferably, the at least one diene rubber is selected from the group consisting of natural polyisoprene (NR, natural rubber), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halobutyl rubber.

[0045] According to a particularly preferred embodiment of the invention, the at least one diene rubber is selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR) and emulsion-polymerized styrene-butadiene rubber (ESBR).

[0046] According to a particularly advantageous embodiment of the invention, the rubber mixture contains at least one natural polyisoprene (NR), preferably in amounts of 5 to 55 phr, and according to a particularly advantageous embodiment of the invention, 5 to 25 phr, most preferably 5 to 20 phr. Such a rubber mixture exhibits good processability and reversion stability as well as optimized tear properties and optimal rolling resistance behavior.

[0047] According to a particularly advantageous embodiment of the invention, the rubber mixture contains at least one polybutadiene (BR, butadiene rubber), preferably in amounts of 10 to 80 phr, particularly preferably 10 to 50 phr, and according to a particularly advantageous embodiment of the invention 15 to 40 phr. This achieves particularly good tear and abrasion properties of the rubber mixture according to the invention and optimal braking behavior.

[0048] According to a particularly advantageous embodiment of the invention, the rubber mixture contains at least one solution-polymerized styrene-butadiene rubber (SSBR), preferably in amounts of 10 to 80 phr, more preferably 30 to 80 phr, and according to a particularly advantageous embodiment of the invention, 50 to 70 phr. This achieves particularly good rolling resistance properties of the rubber mixture according to the invention. According to particularly advantageous embodiments of the invention, SSBR is used in combination with at least one other rubber to achieve an optimal and balanced property profile.

[0049] The rubber mixture preferably contains at least one filler, preferably in amounts of 30 to 500 phr, particularly preferably 50 to 400 phr, again preferably 80 to 300 phr.

[0050] According to advantageous embodiments of the invention, the filler is a reinforcing filler, which is preferably selected from the group consisting of carbon blacks and silicas.

[0051] According to particularly advantageous embodiments of the invention, the rubber mixture contains at least one silica as a filler, preferably in amounts of 30 to 500 phr, particularly preferably 50 to 400 phr, again preferably 80 to 300 phr. In these amounts, silica is present in particular as the sole or main filler (more than 50 wt.% based on the total filler amount).

[0052] According to further advantageous embodiments of the invention, the rubber mixture contains at least one silica as a further filler, preferably in amounts of 5 to 100 phr, particularly preferably 5 to 80 phr, again preferably 10 to 60 phr.

[0053] In these amounts, silica is included in particular as an additional filler in addition to another main filler, such as in particular a carbon black.

[0054] The silica can be the types of silica known to the person skilled in the art that are suitable as fillers for tire rubber compounds. However, it is particularly preferred to use a finely divided, precipitated silica which has a nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) of 35 to 400 m² / g, preferably of 35 to 350 m² / g, particularly preferably of 85 to 320 m² / g and very particularly preferably of 120 to 235 m² / g, and a CTAB surface area (according to ASTM D 3765) of 30 to 400 m² / g, preferably of 30 to 330 m² / g, particularly preferably of 80 to 300 m² / g and very particularly preferably of 115 to 200 m² / g. Such silicas lead, for example, to particularly good physical properties of the vulcanizates in rubber mixtures for tire treads.Furthermore, this can result in advantages in compound processing due to a reduction in mixing time while maintaining consistent product properties, leading to improved productivity. Silicas that can be used include, for example, Ultrasil®< VN3 (trade name) from Evonik as well as highly dispersible silicas, so-called HD silicas (e.g., Zeosil®< 1165 MP from Solvay).

[0055] In the event that at least two different silicas, which differ, for example, in their BET surface area, are contained in the rubber mixture according to the invention, the stated quantities refer to the total amount of all silicas contained.

[0056] The terms "silicic acid" and "silica" are used synonymously in the present invention.

[0057] The rubber mixture may also contain other fillers, such as carbon blacks, in particular industrial carbon blacks or pyrolysis carbon blacks, or other fillers which may or may not have a reinforcing effect.

[0058] Other (non-reinforcing) fillers within the scope of the present invention include aluminosilicates, kaolin, chalk, starch, magnesium oxide, titanium dioxide or rubber gels as well as fibers (such as aramid fibers, glass fibers, carbon fibers, cellulose fibers).

[0059] Other potentially reinforcing fillers include carbon nanotubes (CNTs) including discrete CNTs, so-called hollow carbon fibers (HCFs) and modified CNTs containing one or more functional groups, such as hydroxyl, carboxy and carbonyl groups), graphite and graphene and so-called "carbon-silica dual-phase fillers".

[0060] Zinc oxide is not considered a filler in the context of the present invention.

[0061] According to particularly advantageous embodiments of the invention, the rubber mixture according to the invention contains 0.1 to 60 phr, preferably 3 to 40 phr, more preferably 5 to 30 phr, most preferably 5 to 15 phr, of at least one carbon black. In these amounts, carbon black is present in particular as a further filler in addition to a main filler, such as, in particular, silica.

[0062] According to further advantageous embodiments of the invention, the rubber mixture according to the invention contains 30 to 300 phr, preferably 30 to 200 phr, particularly preferably 40 to 100 phr of at least one carbon black. In these amounts, carbon black is present as the sole or main filler, optionally in combination with silica in the above-mentioned smaller amounts.

[0063] All types of soot known to the expert person can be considered as soot.

[0064] In one embodiment, the carbon black has an iodine number, according to ASTM D 1510, which is also referred to as iodine adsorption number, between 30 and 250 g / kg, preferably 30 to 180 g / kg, more preferably 40 to 180 g / kg, and most preferably 80 to 150 g / kg, and a DBP number according to ASTM D 2414 of 30 to 200 ml / 100 g, preferably 70 to 200 ml / 100 g, more preferably 90 to 200 ml / 100 g.

[0065] The DBP number according to ASTM D 2414 determines the specific absorption volume of a carbon black or a light filler using dibutyl phthalate.

[0066] The use of such a type of carbon black in the rubber compound, especially for vehicle tires, ensures the best possible compromise between abrasion resistance and heat build-up, which in turn influences the ecologically relevant rolling resistance.

[0067] It is preferred if only one type of carbon black is used in the respective rubber mixture, but different types of carbon black can also be mixed into the rubber mixture.

[0068] According to a particularly advantageous embodiment of the invention, the rubber mixture contains 5 to 60 phr, particularly preferably 5 to 40 phr, of at least one carbon black and 50 to 300 phr, preferably 80 to 200 phr of at least one silica.

[0069] Furthermore, the rubber mixture may contain conventional additives in the usual parts by weight, which are preferably added in at least one basic mixing stage during its production. These additives include a) ageing inhibitors known in the prior art, such as diamines, such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N`-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), or dihydroquinolines, such as 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) activators, such as B. zinc oxide and fatty acids (e.g. stearic acid) and / or other activators, such as zinc complexes such as zinc ethylhexanoate, c) activators and / or agents for the binding of fillers, in particular carbon black or silica, such as S-(3-aminopropyl)thiosulphuric acid and / or its metal salts (binding to carbon black) and silane coupling agents (binding to silica), d) ozone protection waxes, e) resins, in particular adhesive resins for inner tire components, f) mastication aids, such as2,2'-dibenzamidodiphenyl disulfide (DBD) and g) processing aids, such as in particular fatty acid esters and metal soaps, such as zinc soaps and / or calcium soaps h) plasticizers, such as in particular aromatic, naphthenic or paraffinic mineral oil plasticizers, such as MES (mild extraction solvate) or RAE (residual aromatic extract) or TDAE (treated distillate aromatic extract), or rubber-to-liquid oils (RTL) or biomass-to-liquid oils (BTL), preferably with a polycyclic aromatics content of less than 3% by weight according to method IP 346 or triglycerides, such as e.g. B. rapeseed oil, or factitious substances or hydrocarbon resins or liquid polymers whose average molecular weight (determined by GPC = gel permeation chromatography, based on BS ISO 11344:2004) is between 500 and 20,000 g / mol.

[0070] When using mineral oil, this is preferably selected from the group consisting of DAE (Distilled Aromatic Extracts) and / or RAE (Residual Aromatic Extract) and / or TDAE (Treated Distilled Aromatic Extracts) and / or MES (Mild Extracted Solvents) and / or naphthenic oils.

[0071] According to particularly advantageous embodiments, the rubber mixture according to the invention contains no further ageing inhibitors from the group of p-phenylenediamines in addition to those according to formula I), see list a) above. In particular, according to a particularly preferred embodiment, the rubber mixture according to the invention contains 0 to 0.1 phr, in particular 0 phr, of further ageing inhibitors based on diamines, which are selected from the group containing, preferably consisting of, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N`-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD).

[0072] With the preferably very small amounts of 0 to 0 phr, or particularly preferably 0 phr, of the aforementioned diamines and the compound according to formula I) contained according to the invention, it is possible to achieve an improved protective effect. The compound according to formula I) according to the invention replaces the aforementioned phenylenediamines known in the prior art.

[0073] According to further advantageous embodiments of the invention, at least one further of the aforementioned diamine anti-aging agents is also present, so that the compound according to the invention only partially replaces the diamines known in the prior art. This also achieves the advantage of the invention, but not to an optimal extent.

[0074] According to advantageous embodiments, anti-aging agents based on dihydroquinoline, such as TMQ, are present in the rubber mixture in addition to the compound according to the invention according to formula I). ​​The amount of dihydroquinolines present, such as in particular TMQ, is preferably 0.1 to 3, in particular 0.5 to 1.5 phr.

[0075] According to further advantageous embodiments, the rubber mixture according to the invention contains no further ageing inhibitors, ie 0 phr of further ageing inhibitors apart from the compound according to the invention according to formula I).

[0076] The silane coupling agents can be any type known to the person skilled in the art.

[0077] Furthermore, one or more different silane coupling agents can be used in combination. The rubber compound can thus contain a mixture of different silanes.

[0078] The silane coupling agents react with the surface silanol groups of the silica or other polar groups during the mixing of the rubber or rubber compound (in situ) or even before the addition of the filler to the rubber in the sense of a pretreatment (premodification).

[0079] Coupling agents known from the prior art are bifunctional organosilanes that possess at least one alkoxy, cycloalkoxy, or phenoxy group as a leaving group on the silicon atom and that have, as another functionality, a group that, optionally after cleavage, can enter into a chemical reaction with the double bonds of the polymer. The latter group can be, for example, the following chemical groups: -SCN, -SH, -NH 2 , or -S x - (where x = 2 to 8).

[0080] For example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane, or 3,3'-bis(triethoxysilylpropyl)polysulfides with 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide (TESPD), or mixtures of sulfides with 1 to 8 sulfur atoms with varying contents of the various sulfides, can be used as silane coupling agents. TESPT can also be added, for example, as a mixture with carbon black (trade name X50S ®< from Evonik).

[0081] Blocked mercaptosilanes, such as those known from WO 99 / 09036, can also be used as silane coupling agents. Silanes such as those described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1, and WO 2008 / 083244 A1 can also be used. Examples of suitable silanes include those marketed under the name NXT in various versions by Momentive, USA, or those marketed under the name VP Si 363 ® by Evonik Industries.

[0082] The proportion of the total amount of further additives is preferably 3 to 150 phr, particularly preferably 3 to 100 phr and most preferably 5 to 80 phr.

[0083] The total amount of other additives may contain zinc oxide (ZnO) in the amounts stated above.

[0084] This can be any type of zinc oxide known to those skilled in the art, such as ZnO granules or powder. The conventionally used zinc oxide generally has a BET surface area of ​​less than 10 m 2 / g. However, a zinc oxide with a BET surface area of ​​10 to 100 m 2 / g, such as so-called "nano-zinc oxides," can also be used.

[0085] The rubber mixture according to the invention is preferably used in vulcanized form, in particular in vehicle tires or other vulcanized technical rubber articles.

[0086] The vulcanization of the rubber mixture according to the invention is preferably carried out in the presence of sulfur and / or sulfur donors with the aid of vulcanization accelerators, whereby some vulcanization accelerators can also act as sulfur donors. The accelerator is selected from the group consisting of thiazole accelerators and / or mercapto accelerators and / or sulfenamide accelerators and / or thiocarbamate accelerators and / or thiuram accelerators and / or thiophosphate accelerators and / or thiourea accelerators and / or xanthate accelerators and / or guanidine accelerators.

[0087] Preference is given to using a sulfenamide accelerator selected from the group consisting of N-cyclohexyl-2-benzothiazolesufenamide (CBS) and / or N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or benzothiazyl-2-sulfenemorpholide (MBS) and / or N-tert-butyl-2-benzothiazylsulfenamide (TBBS) or a guanidine accelerator such as diphenylguanidine (DPG).

[0088] All sulfur-donating substances known to the person skilled in the art can be used as the sulfur-donating substance. If the rubber mixture contains a sulfur-donating substance, this is preferably selected from the group comprising, for example, thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD) and / or tetramethylthiuram disulfide (TMTD) and / or tetraethylthiuram disulfide (TETD), and / or thiuram tetrasulfides, such as dipentamethylenethiuram tetrasulfide (DPTT), and / or dithiophosphates, such as

[0089] DipDis (bis-(diisopropyl)thiophosphoryl disulfide) and / or bis(O,O-2-ethylhexyl-thiophosphoryl)polysulfide (e.g. Rhenocure SDT 50 ®< , Rheinchemie GmbH) and / or zinc dichloryldithiophosphate (e.g. Rhenocure ZDT / S ®< , Rheinchemie GmbH) and / or zinc alkyldithiophosphate, and / or 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane and / or diarylpolysulfides and / or dialkylpolysulfides.

[0090] Other network-forming systems, such as those available under the trade names Vulkuren®, Duralink®, or Perkaiink®, or network-forming systems as described in WO 2010 / 049216 A2, can also be used in the rubber compound. This system contains a vulcanizing agent that crosslinks with a functionality greater than four and at least one vulcanization accelerator.

[0091] The use of the accelerators TBBS and / or CBS and / or diphenylguanidine (DPG) is particularly preferred.

[0092] In addition, vulcanization retarders may be present in the rubber compound.

[0093] The terms "vulcanized" and "crosslinked" are used synonymously in the context of the present invention.

[0094] According to a preferred development of the invention, several accelerators are added in the final mixing stage during the production of the sulfur-crosslinkable rubber mixture.

[0095] The sulfur-crosslinkable rubber mixture according to the invention is produced according to the process customary in the rubber industry, in which a base mixture containing all components except the vulcanization system (sulfur and vulcanization-influencing substances) is first prepared in one or more mixing stages. The finished mixture is created by adding the vulcanization system in a final mixing stage. The finished mixture is further processed, for example, by an extrusion process or calendering, and formed into the appropriate shape. Further processing then takes place by vulcanization, whereby sulfur crosslinking occurs due to the vulcanization system added within the scope of the present invention.

[0096] The rubber mixture according to the invention described above is particularly suitable for use in vehicle tires, in particular pneumatic vehicle tires.

[0097] For use in vehicle tires, the mixture is preferably formed into a tread shape as a ready-mix before vulcanization and applied as usual during the production of the green vehicle tire.

[0098] The rubber mixture according to the invention for use as a sidewall or other body mixture in vehicle tires is produced as already described. The difference lies in the shaping after the extrusion process or calendering of the mixture. The resulting shapes of the still unvulcanized rubber mixture for one or more different body mixtures are then used to construct a green tire.

[0099] The body compound refers to the rubber compounds for the inner components of a tire, such as the squeegee, inner liner (inner layer), apex, belt, shoulder, belt tread, carcass, bead reinforcement, bead tread, flange tread, and bandage. The unvulcanized green tire is then vulcanized.

[0100] For use of the rubber mixture according to the invention in belts and straps, particularly conveyor belts, the extruded, still unvulcanized mixture is molded into the appropriate shape and, during or afterward, often provided with reinforcements, e.g., synthetic fibers or steel cords. This usually results in a multi-layer structure consisting of one or more layers of rubber mixture, one or more layers of the same and / or different reinforcements, and one or more additional layers of the same and / or a different rubber mixture.

[0101] A further subject of the present invention is a vehicle tire which comprises the rubber mixture according to the invention containing the compound according to the invention in at least one component.

[0102] The vulcanized vehicle tire comprises, in at least one component, a vulcanizate of at least one rubber mixture according to the invention. Those skilled in the art are aware that most substances, such as the rubbers contained therein, are or can be present in a chemically altered form, either immediately after mixing or only after vulcanization.

[0103] For the purposes of the present invention, vehicle tires are understood to mean pneumatic vehicle tires and solid rubber tires, including tires for industrial and construction vehicles, truck, car and two-wheel tires.

[0104] The vehicle tire according to the invention preferably comprises the rubber mixture according to the invention in at least one outer component, wherein the outer component is preferably a tread, a sidewall and / or a horn profile.

[0105] The vehicle tire according to the invention can thus also comprise the rubber mixture according to the invention containing the compound according to the invention according to formula I) in several components in an optionally adapted composition.

[0106] A further object of the present invention is a process for preparing the compound according to formula I), wherein the process comprises at least the following process steps: a) Provision of the substance according to formula A) b) Providing methyl isobutyl ketone (MIBK) and hydrogen or methyl isobutyl ketone (MIBK) and formic acid; c) Reacting the substance according to step a) with the substances according to step b), preferably in the presence of a hydrogenation catalyst, to give the substance according to formula C) d) providing a Lewis acid, such as in particular boron tribromide (BBr 3 ), aluminum trichloride (AlCl 3 ), aluminum tribromide (AlBr 3 ), boron trifluoride diethyl etherate (BF 3 *OEt 2 ) or tin tetrachloride (SnCl 4 ), or a Brønsted acid (Brønsted acid), such as in particular hydrogen iodide (HI) or hydrogen bromide (HBr); e) reacting the substance according to formula C) with the substance from step d) to give the substance according to formula I)

[0107] In step b), the alternative methyl isobutyl ketone (MIBK) and hydrogen is preferred over MIBK and formic acid.

[0108] Preferably, the substance according to formula C) contained in step c) is dissolved in an organic solvent, preferably an aprotic solvent, such as in particular dichloromethane (DCM) or chloroform (CHCl 3 ), and then reacted according to step e).

[0109] A further subject of the present invention is a further process for preparing the compound according to formula I), wherein the process comprises at least the following process steps: a1) Provision of the substance according to formula A) b1) Providing a Lewis acid, such as in particular boron tribromide (BBr 3 ), aluminum trichloride (AlCl 3 ), aluminum tribromide (AlBr 3 ), boron trifluoride diethyl etherate (BF 3 *OEt 2 ) or tin tetrachloride (SnCl 4 ), or a Brønsted acid (Brønsted acid), such as in particular hydrogen iodide (HI) or hydrogen bromide (HBr); c1) Reacting the substance according to step a1) with the substance from step b1) to give the substance according to formula C1) d1) Providing methyl isobutyl ketone (MIBK) and hydrogen; e1) Reacting the substance according to formula C1) with the substances from step d1), preferably in the presence of a hydrogenation catalyst, to give the substance according to formula I)

[0110] Preferably, in the process steps in which a reaction with hydrogen takes place, a suitable catalyst, referred to in the present invention as a "hydrogenation catalyst", is used.

[0111] The hydrogenation catalyst in the process (step c) or e1)) is preferably a noble metal catalyst, such as palladium (Pd) or platinum (Pt). The noble metal is preferably used on carbon (C), such as palladium on carbon (Pd / C).

[0112] Furthermore, other known catalysts such as Raney nickel or copper chromite can also be used.

[0113] Palladium on carbon (Pd / C) is preferably used as the hydrogenation catalyst in step c).

[0114] Preferably, palladium on carbon (Pd / C) is used as hydrogenation catalyst in step e1).

[0115] The hydrogen pressure in the respective process steps in which hydrogen is used is preferably 1 to 40 bar, particularly preferably 10 to 30 bar, most preferably 15 to 25 bar.

[0116] The hydrogenation reaction in step c) or e1) preferably takes place in an autoclave, in particular a stainless steel autoclave.

[0117] The temperature in process step c) and e1) is preferably from room temperature (RT, in particular 20 °C) to 100 °C, particularly preferably 40 to 80 °C, most preferably 40 to 70 °C.

[0118] If the temperature is too high, undesirable hydrogenation of the aromatic components occurs.

[0119] All process steps, in particular steps e) and c1), advantageously take place under a protective gas atmosphere.

[0120] Process steps e) and c1) preferably take place at a temperature of -78 (minus seventy-eight) °C to +20 °C, particularly preferably -10 °C to +10 °C, in particular at 0 °C.

[0121] The reactions in process steps e) and c1) each represent an ether cleavage. In principle, any substance with which the desired ether cleavage of substance C) or A) can be carried out is suitable. The substance with which the ether cleavage is carried out is also referred to as the "ether cleavage reagent" in the context of the present invention.

[0122] For this purpose, a Lewis acid, such as, in particular, boron tribromide (BBr 3 ), aluminum trichloride (AlCl 3 ), aluminum tribromide (AlBr 3 ), boron trifluoride diethyl etherate (BF 3 *OEt 2 ), or tin tetrachloride (SnCl 4 ), or a Brønsted acid, such as, in particular, hydrogen iodide (HI) or hydrogen bromide (HBr), can be used. Brønsted acids are known to the person skilled in the art and can be characterized by their pKa value, also known as the pKs value.

[0123] Strong Brönsted acids have a pKa value of -1.74 (minus one point seven four) to 4.5 (four point five) and very strong acids have a pKa value of less than -1.74, as can be seen from the Römpp Online Encyclopedia (URL: https: / / roempp.thieme.de / lexicon / RD-19-00110?searchterm=s%C3%A4ure) results.

[0124] In the context of the present invention, very strong Brönsted acids with a pKa value of less than -1.74 are preferred, such as in particular hydrogen iodide (HI) or hydrogen bromide (HBr).

[0125] According to particularly advantageous embodiments of the invention, a Lewis acid, in particular boron tribromide (BBr 3 ), is used in c1) and e).

[0126] The substance according to formula A), as well as boron tribromide (BBr3), and methyl isobutyl ketone (MIBK) are commercially available. The other alternatives to BBr3 mentioned above are also commercially available.

[0127] In the following, the invention will be explained in more detail using exemplary embodiments.

[0128] The compound according to formula I) was prepared in the following ways: X1): Synthesis of N-(L3-dimethylbutyl)-N'-p-methoxyphenyl-p-phenylenediamine (compound according to formula C)) according to step c):

[0129]

[0130] 5.00 g (23.3 mmol, 1 eq) of 4-(4-methoxyphenylamino)aniline, 2.00 g of Pd / C (palladium on carbon C) (5%) (0.2 g per 4.67 mmol of substrate), and 50.0 mL of methyl isobutyl ketone (MIBK) were weighed into a stainless steel autoclave fitted with a Teflon liner. The mixture was then pressurized with 20 bar of hydrogen (H2) and stirred at 60°C for 10 hours. After the reaction was complete, the excess hydrogen was vented, and the suspension was filtered through diatomaceous earth (Celite®) and rinsed with ethanol. The filtrate was evaporated to dryness and dried under reduced pressure. The residue was purified on silica gel (cyclohexane / ethyl acetate 100:0 → 80:20). Orange oil; Yield 5.6 g (80% of theory).

[0131] 1< H-NMR ( English "nuclear magnetic resonance") (500 MHz, DMSO d6 ) δ = 8.09 (s, 1H), 6.94 (td, J = 7.6, 1.5 Hz, 1H), 6.88 (dd, J = 7.6, 1.4 Hz, 1H), 6.69 - 6.63 (m, 2H), 6.51 (d, J= 8.4 Hz, 1H), 6.27 (dd, J = 8.5, 2.5 Hz, 1H), 6.21 (d, J = 2.5 Hz, 1H), 4.82 (d, J = 8.9 Hz, 1H), 3.30 (dt, J = 8.6, 6.5 Hz, 1H), 1.70 (dp, J = 13.5, 6.7 Hz, 1H), 1.38 (dt, J = 13.9, 7.1 Hz, 1H), 1.16 (dt, J = 13.5, 6.8 Hz, 1H), 1.02 (d, J = 6.1 Hz, 3H), 0.87 (dd, J = 19.4, 6.6 Hz, 6H).

[0132] 13< C-NMR (126 MHz, DMSO- d6 ) δ = 151.8, 143.0, 140.0, 133.0, 120.7, 116.0, 114.5, 113.6, 55.2, 46.1, 45.9, 26.3, 24.5, 22.8, 22.6, 20.87 (46.1 and 45.9 is the resolution as a consequence of enantiomers).

[0133] ESI-MS (electrospray ionization mass spectrometry) [M+H] +< = 299. Synthesis of N-(1,3-dimethylbutyl)-N'-p-hydroxyphenyl-p-phenylenediamine (compound according to the invention according to formula I)) according to step e):

[0134]

[0135] Under argon, 5.70 g (19.1 mmol, 1 eq) of N-(1,3-dimethylbutyl)-N'-p-methoxyphenyl-p-phenylenediamine was dissolved in 20.0 mL of dry dichloromethane (DCM) and cooled to 0°C. Subsequently, 5.52 mL (57.3 mmol, 5 eq) of boron tribromide were dissolved in 15 mL of dry DCM and carefully added dropwise. The mixture was stirred overnight, and the reaction was quenched by adding saturated NaHCO 3 solution (sol.) under protective gas and ice cooling. An additional 50 mL of a 3:1 mixture of ethyl acetate / isopropanol was added. The organic phase was washed with saturated (saturated) NaHCO 3 solution and saturated NaCl solution and dried over MgSO 4. After filtration, the solvent was evaporated to dryness and dried in vacuo. A light violet to blue solid was obtained; yield: 4.8 g (88% of theory).

[0136] 1< H-NMR (500 MHz, DMSO- d6 ) δ = 8.63 (s, 1H), 6.95 (s, 1H), 6.76 (d, J = 8.7 Hz, 2H), 6.71 (d, J = 8.8 Hz, 2H), 6.59 (d, J= 8.7 Hz, 2H), 6.51 - 6.44 (m, 2H), 4.71 (d, J = 8.2 Hz, 1H), 3.40-3.31 (d, J = 6.9 Hz, 1H), 1.73 (dp, J = 13.4, 6.7 Hz, 1H), 1.49 - 1.37 (m, 1H), 1.23 - 1.15 (m, 1H), 1.05 (d, J = 6.1 Hz, 3H), 0.91 (d, J = 6.6 Hz, 3H), 0.87 (d, J = 6.6 Hz, 3H).

[0137] 13< C-NMR (126 MHz, DMSO- d6 ) δ = 149.8, 142.5, 138.1, 133.9, 119.9, 117.0, 115.6, 113.3, 46.1, 45.9, 26.3, 24.5, 22.8, 22.6, 20.8 (46.1 and 45.9 is the splitting as a result of isomers).

[0138] ESI-MS [M+H] +< = 285.

[0139] The intermediate compound according to formula C) was prepared in an alternative variant of the reaction according to step c) in the following manner: X2): Synthesis of N-(1,3-dimethylbutyl)-N'-p-methoxyphenyl-p-phenylenediamine:

[0140]

[0141] Under protective gas, 0.40 g of palladium on carbon (5%) was suspended in 20 mL of dry ethanol, and 1.00 g (4.67 mmol, 1 eq) of 4-(4-methoxyphenylamino)aniline, 0.88 mL (23.3 mmol, 5 eq) of formic acid (23.3 mmol, 5 eq), and 1.17 mL (9.33 mmol, 2 eq) of methyl isobutyl ketone were added successively. The mixture was heated under reflux for 4 hours, filtered to remove the solids, and the solvent was removed in vacuo. The residue was purified on silica gel (cyclohexane / ethyl acetate 100:0 → 80:20). An orange oil; yield 1.0 g (73% of theory).

[0142] The spectra are identical to the first run (X1).

[0143] The implementation of process step c) according to X1) is preferred over that according to X2) (formate as a by-product from the reaction of amine and formic acid) due to the better reproducibility and the resulting fewer by-products.

[0144] Furthermore, the compound of the invention was prepared by an alternative synthesis route as follows: Synthesis of Np-hydroxyphenyl-p-phenylenediamine (compound according to formula C1) according to step c1):

[0145]

[0146] Under protective gas, 20 mL of degassed acetic acid and 10 mL of hydrobromic acid were added, and 1 g (4.67 mmol, 1 eq) of 4-(4-methoxyphenylamino)aniline was dissolved therein. The mixture was stirred at 120°C for 24 hours. After the solution was brought to RT, it was neutralized with saturated NaHCO 3 solution and extracted with a 3:1 mixture of ethyl acetate / isopropanol. The solvent was removed, and the residue was purified on silica gel (cyclohexane / ethyl acetate 1:1). Brown solid; yield 0.7 g (75% of theory).

[0147] 1< H-NMR (500 MHz, DMSO- d6 ) δ = 8.64 (s, 1H), 6.94 (s, 1H), 6.73 - 6.68 (m, 4H), 6.59 (d, J = 8.8 Hz, 2H), 6.48 (d, J = 8.6 Hz, 2H), 4.56 (s, 2H). Synthesis of N-(1,3-dimethylbutyl)-N'-p-hydroxyphenyl-p-phenylenediamine (compound according to the invention according to formula I)) according to step e1):

[0148]

[0149] 0.31 g (1.55 mmol, 1 eq) of Np-hydroxyphenyl-p-phenylenediamine, 0.66 g of palladium on carbon (5%) (0.2 g per 4.67 mmol of substrate), and 20.0 mL of methyl isobutyl ketone were weighed into a stainless steel autoclave fitted with a Teflon liner. The mixture was then pressurized with 20 bar of hydrogen, and stirred at 60°C for 10 hours. After the reaction was complete, the excess hydrogen was vented, and the suspension was filtered through diatomaceous earth (Celite®) and rinsed with ethanol. The filtrate was evaporated to dryness and dried under vacuum. According to NMR analysis, the crude product contained 70% of the target molecule.

[0150] The compound according to formula I) exhibits increased reactivity compared to 6PPD. This was demonstrated, for example, by calculating bond dissociation energies (BDE) and the free activation enthalpy ΔRG ≠< or the free standard reaction enthalpy ΔRG° for the reaction with a methyl peroxide radical. The values ​​are given in Table 1. Fig.1a and 1b the splitting mechanisms to which the values ​​refer are shown. Table 1 molecule BDE [kJ / mol] ΔRG° [kJ / mol] ΔRG ≠< [kJ / mol] 6PPD 313 -25,6 19,1 Formula I) 305 -28,8 16,0

[0151] As Table 1 shows, the compound according to the invention according to formula I) results in a lower bond dissociation energy and lower free enthalpies.

[0152] With the compound according to formula I), an improved protective effect can be achieved in the applications mentioned.

[0153] For use in a rubber mixture for vehicle tires, the compound according to the invention according to formula I) is added, for example, instead of the anti-aging agents known in the prior art, such as 6PPD, 7PPD or IPPD, etc., in a manner known to the person skilled in the art in one of the mixing stages during the preparation of the rubber mixture.

Claims

1. Compound of formula I):

2. Rubber mixture containing the compound of formula I) according to Claim 1.

3. Rubber mixture according to Claim 2, characterized in that it contains at least one diene rubber.

4. Rubber mixture according to Claim 3, characterized in that it contains at least one diene rubber selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halobutyl rubber.

5. Vehicle tyre comprising the rubber mixture according to any of Claims 2 to 4 in at least one component.

6. Vehicle tyre according to Claim 5, characterized in that it comprises at least one rubber mixture according to any of Claims 2 to 4 in at least one outer component, wherein the outer component is preferably a tread, a sidewall and / or a flange profile.

7. Process for producing the compound of formula I) according to Claim 1 comprising at least the process steps of: a) providing the substance of formula A) b) providing methyl isobutyl ketone (MIBK) and hydrogen or methyl isobutyl ketone (MIBK) and formic acid; c) reacting the substance of step a) with the substances of step b) to afford the substance of formula C) d) providing a Lewis acid, such as especially boron tribromide (BBr3), aluminium trichloride (AlCl3), aluminium tribromide (AlBr3), boron trifluoride diethyl etherate (BF3*OEt2) or tin tetrachloride (SnCl4), or a Bronsted acid, such as especially hydrogen iodide (HI) or hydrogen bromide (HBr); e) reacting the substance of formula C) with the substance from step d) to afford the substance of formula I) 8. Process for producing the compound of formula I) according to Claim 1 comprising at least the process steps of: a1) providing the substance of formula A) b1) providing a Lewis acid, such as especially boron tribromide (BBr3), aluminium trichloride (AlCl3), aluminium tribromide (AlBr3), boron trifluoride diethyl etherate (BF3*OEt2) or tin tetrachloride (SnCl4), or a Bronsted acid, such as especially hydrogen iodide (HI) or hydrogen bromide (HBr); c1) reacting the substance of step a1) with the substance from step b1) to afford the substance of formula C1) d1) providing methyl isobutyl ketone (MIBK) and hydrogen; e1) reacting the substance of formula C1) with methyl isobutyl ketone (MIBK) from step d1) to afford the substance of formula I) 9. Use of the compound of formula I) according to Claim 1 as an ageing stabilizer and / or antiozonant in particular in vehicle tyres and / or technical rubber articles, such as in particular an air spring, bellows, conveyor belt, strap, drive belt, hose, rubber band, profile, a seal, a membrane, tactile sensors for medical applications or robotics applications, or a shoe sole or parts thereof and / or oils and / or lubricants.

10. Use of a compound of formula I) according to Claim 1 for producing a rubber article, in particular an air spring, bellows, conveyor belt, strap, drive belt, hose, rubber band, profile, a seal, a membrane, tactile sensors for medical applications or robotics applications, or a shoe sole or parts thereof.

11. Use of the compound of formula I) according to Claim 1 in oils, lubricants, such as especially fuels or fluids for engines.

12. Use of the compound of formula I) according to Claim 1 as a dye in fibres and / or polymers and / or paper and / or in (decorating) paints and coatings.