METHOD FOR DESCALING A STEEL STRIP AND APPARATUS FOR DESCALING A STEEL STRIP

DE502021005772D1Active Publication Date: 2024-11-28THYSSENKRUPP STEEL EUROPE AG PATENTE PATENT DEPARTMENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005772
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-09
Filing Date
2021-01-27
Publication Date
2024-11-28
Estimated Expiration
2041-01-27

AI Technical Summary

Technical Problem

Existing methods for descaling steel strips during the production process either lead to excessive pickling of grain boundaries, incomplete removal of scale, or structural damage due to improper treatment time, resulting in high costs and effort.

Method used

A method involving continuous cathodic polarization of steel strips in an acidic solution with a controlled belt speed and treatment duration, using a treatment line with multiple stages and monitoring the belt speed to prevent excessive treatment time, ensuring complete scale removal without damaging the steel.

Benefits of technology

This approach effectively removes scale without excessive pickling of grain boundaries, allowing for efficient processing and reducing the risk of structural damage, thereby minimizing costs and maintaining the integrity of the steel strip.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for descaling a steel strip and to a system for descaling a steel strip.

[0002] During the production process of steel strips, so-called scale inevitably forms. The term "scale" encompasses oxides of the iron contained in the steel, as well as other alloying elements present. Scale forms particularly during hot rolling of steel through the reaction of oxygen, primarily atmospheric oxygen, with these elements. Scale typically contains FeO, Fe₂O₃, Fe₃O₄, and oxides of other alloying elements present in the steel, such as MnO, SiO₂, and others. Scale layers are typically up to several micrometers thick.

[0003] Methods for removing scale layers are known to those skilled in the art.

[0004] DE 10 2005 055 768 A1 discloses a process for descaling steel strips, wherein the respective steel strip is anodically polarized with a current density of 0.3 to 20 A / dm² and a mixture of hydrochloric acid, sulfuric acid, pickling inhibitors and surfactants is used as a pickling solution.

[0005] EP 0 763 609 A1 discloses a method for the electrolytic pickling of steel strips comprising the treatment of the steel strips in an alkaline electrolyte with alternating anodic and cathodic strip polarization.

[0006] The JP H05 247699 A and the JP H04 351221 A reveal an electrolytic treatment of a steel strip.

[0007] The CN 109 594 086 A is an acid pickling plant for a strip of stainless steel.

[0008] With methods known from the prior art, the existing scale can be removed essentially completely. However, this can lead to excessive pickling of the grain boundaries, which can negatively affect subsequent process steps, particularly the application of a corrosion-protective coating. Another disadvantage of the known methods is that the scale present on the surface is not completely removed, which can also lead to problems in subsequent process steps. A further disadvantage of the aforementioned methods is that while the scale is not sufficiently removed if the treatment time of the steel strips is too short, even a slightly longer treatment time can structurally damage the steel strip itself, as undesirable chemical reactions occur between the treatment fluid and the steel strip.As a result, the treatment time of the steel strip must be precisely set and closely monitored to avoid or at least detect any deviations in treatment time, including unintentional ones. Each of the aforementioned disadvantages leads to significant effort and, consequently, high costs.

[0009] Given the aforementioned disadvantages, the task arises to provide improved methods for descaling steel strip.

[0010] The problem is solved by a method having the features of claim 1 and by a descaling system having the features of claim 10.

[0011] A process is provided that serves the purpose of descaling a steel strip.

[0012] To achieve the goal, the procedure stipulates that at least the following steps must be carried out: A) Introducing the scale-bearing steel strip into a treatment line. The treatment line is a treatment bath or a series of treatment baths arranged sequentially in the direction of steel strip transport. The treatment bath(s) is / are an acidic solution. B) Transporting the steel strip through the treatment line at a predetermined strip speed. The predetermined strip speed corresponds to a planned treatment duration. The treatment duration refers to the period during which a position of the steel strip, i.e., a position along its length, is exposed to acid. A planned treatment duration is therefore the period that is scheduled for acid contact at a given position of the steel strip.The specified belt speed is preferably constant, but it is also possible for the specified belt speed to vary over time.

[0013] This results from the fact that, given a specific length of the treatment line, the length of the treatment process can be adjusted by specifying the belt speed for a particular position or section of the belt. This determines how long that specific position of the belt is subjected to treatment, i.e., how long it remains in the treatment bath or baths. The treatment duration is therefore the total time during which, under a predetermined process, a specific location along the belt—that is, a specific point or section of the belt—is subjected to acid treatment. In the standard case of a constant belt speed, the treatment duration is the same for every point on the steel belt. The crucial point is that the steel belt is treated for a duration specified by the operator.

[0014] In a special case of the process and the system described below, the treatment line is a treatment bath located in a tub, whereby the treatment bath is divided into a sequence of treatment stages by means of separation cells. For example, it can be provided that acid with different periods of prior use can be used in the different separation cells, thereby increasing the overall efficiency of use, as the acid can be used for a longer period overall.

[0015] Within the scope of the present invention, "acidic solution" means that it has a pH value of less than 7, preferably 0.01 to 4. According to the invention, an aqueous solution is used, that is, a water-based solution. For example, an aqueous solution containing at least HCl and preferably at least one salt, an aqueous solution containing at least H₂SO₄ and preferably at least one salt, or an aqueous solution containing at least H₂SO₄ and H₃PO₄ is used as the acidic solution. It can further be provided, for example, that the salts originating from the steel strip to be treated and / or from the scale to be removed are also used, or almost completely used, such as iron salts, chromium salts, and manganese salts, wherein sulfate, chloride, hydroxide, etc., can be present as counterions.

[0016] In a preferred embodiment of the process according to the invention, a solution containing at least one iron salt is used. Preferably, iron salts are used in which the iron cation has an oxidation state of +2. Particularly preferred iron salts are selected from the group consisting of FeSO₄, FeCl₂, and mixtures thereof.

[0017] According to the invention, the steel strip is placed in a cathodically polarized state during the treatment period, that is, during the intended treatment period and also during any additional treatment period that may occur. In a preferred embodiment, this means that a given position, i.e., along its length, of the steel strip is cathodically polarized for the entire treatment period. Particularly preferred is that the entire steel strip is passed through the treatment line exclusively in a cathodically polarized state, that is, that after completing the treatment line, the entire steel strip has undergone treatment in the acid bath(s) and has been continuously, i.e., without interruption, polarized during this time.

[0018] According to the invention, direct current is used. This can be generated using any device known to those skilled in the art, for example, by means of a corrosion protection rectifier that is contacted with the strip and by means of which the strip is set as the cathode. Preferably, the counter pole is formed by a suitable electrode, for example, a graphite or platinum electrode, which is immersed in the acidic solution. A dimensionally stable electrode is particularly preferred.

[0019] As a further process step according to the invention, C) the belt speed is monitored. This can mean that the speed of the belt is monitored directly, for example using optical methods. Alternatively or additionally, it can also be provided that the speed of the belt is determined indirectly, for example by controlling the rotational speed of one or more transport rollers used to transport the belt.

[0020] According to the invention, if monitoring reveals a drop in the belt speed below the predetermined speed, the additional treatment time resulting from this drop in belt speed is determined, particularly while maintaining the cathodically polarized state of the steel belt. In the simplest example, where the drop in belt speed results in a belt standstill for a determined standstill period, this standstill period is calculated as the additional treatment time.

[0021] According to the invention, it is also provided that if the intended treatment duration plus the additional treatment duration does not exceed a maximum treatment duration, the steel strip is subjected to regular further processing, and otherwise the steel strip is processed further as scrap.

[0022] In the simplest case, regular further processing can involve coiling immediately after descaling to make the steel strip available for distribution, but further steps can also be included, such as coating, for example with a corrosion protection layer, preferably a zinc-containing corrosion protection layer.

[0023] The further processing of the steel strip as scrap means that the steel strip, for which the maximum treatment time has been exceeded, is considered defective or potentially defective and, as a precaution, is not given for further processing or distribution, but is alternatively, for example, recycled.

[0024] According to the invention, the maximum treatment duration is 900 seconds or longer.

[0025] In other words, this means that the steel strip is monitored, and in the event of a deviation in the strip transport from the predetermined sequence – which typically occurs unintentionally, for example, due to a strip standstill – the steel strip is processed normally under certain predetermined conditions. According to the invention, the certain condition is that in all cases, an unintentional remaining period of up to 900 seconds of the cathodically polarized steel strip, preferably a continuously cathodically polarized steel strip, or more precisely, a section of the steel strip, in the treatment bath has no negative consequences for further processing. Only if a defined maximum treatment duration is exceeded, for example, if a maximum treatment duration of 900 seconds is exceeded, is the steel strip considered scrap.

[0026] The innovation is based on two fundamental insights which the developers of the innovation described above noticed during experiments and which they utilize for the described process variants as well as for the system explained below.

[0027] Firstly, the developers found that treating a scale-bearing steel strip in an acidic solution with continuous cathodic polarization, provided a minimum treatment time is met, is entirely sufficient to completely remove the scale and achieve an excellent pickling result. It is only necessary to achieve a minimum treatment time of, for example, approximately 20 seconds, which, however, is practically unavoidable and is generally achieved anyway. Surprisingly, the developers found that exclusive, preferably continuous, cathodic polarization of the steel strip throughout its entire immersion in the treatment bath is not only sufficient to remove the scale, but also prevents the grain boundaries from being completely pickled, thus preserving grain boundary oxidation.

[0028] Secondly, the developers surprisingly discovered that even with comparatively very long immersion times of 1200 seconds and more in the acid bath – times not typically used in the actual production process for economic reasons – the steel strip, contrary to all expectations and observations gathered with previously known treatment methods, showed no over-pickling and no stagnation spots despite the prolonged exposure to acid in the continuously cathodically polarized state. A definitive explanation for this observation has not yet been found; it may be due to the establishment of an electrolytic equilibrium on the steel strip surface.The inventive method thus specifically utilizes the finding that, at least within certain limits—exceptionally broad in light of current knowledge—for the dwell time of the steel strip in acid, further use or processing of the steel strip is possible without any restrictions, at least under cathodic polarization. This fact is systematically exploited by measuring the standstill time when, for example, a strip stoppage is detected, and evaluating it in such a way that even during long standstills of over 15 or over 20 minutes, further processing of the steel strip still takes place, and only above certain limits, for example at 1400 seconds or 2400 seconds of standstill time, is the steel strip marked as scrap as a precautionary measure.

[0029] A preferred embodiment of the inventive method comprises the step of measuring the downtime until the resumption of strip transport upon detection of a strip standstill. If the intended treatment duration plus the additional treatment duration resulting from the standstill does not exceed the maximum treatment duration, the steel strip is fed to the regular further processing; otherwise, the steel strip is processed as scrap. In other words, upon detection of a strip standstill, a timer is started, which can, for example, be implemented in a control unit for a strip transport device used for strip transport, and which measures the elapsed time from the strip standstill until the resumption of strip transport. This approach has the advantage of being simple and requiring minimal resources.

[0030] Preferably, the treatment duration is between 20 and 600 seconds, particularly preferably between 25 and 300 seconds, and even more preferably between 25 and 240 seconds. It goes without saying that the shortest possible treatment duration, while still achieving a successful treatment outcome, is advantageous for economic reasons.

[0031] The current density at the steel strip can, for example, be set to a value between 5 and 150 A / dm², preferably between 20 and 120 A / dm².

[0032] According to an advantageous embodiment, the current density is automatically increased, preferably by at least 20 percent, at least during the period of sustained decrease in belt speed when a drop in belt speed is detected. For example, the increase in current density can be initiated automatically upon detection of a belt standstill, for instance, by the control unit, which is coupled to a system for carrying out the inventive method and, in particular, to both a transport device for conveying the steel belt and an electrotechnical device for cathodic polarization. The underlying principle of this approach is to increase the cathodic protection of the steel belt from adverse reactions with the acid when the belt stands still.

[0033] Preferably, the maximum treatment duration is at least 1200 seconds. Since no adverse effects on the surface, structure, and / or microstructure of the steel strip could be observed even after such a long immersion in the acid, it is advisable to set the maximum treatment duration at or above 1200 seconds to further expand the possible process windows. To facilitate the execution and, in particular, the practical implementation of the equipment, an upper limit for the specified maximum treatment duration of, for example, 1400 or 2400 seconds could be provided.

[0034] The steel strip is preferably a hot-rolled strip.

[0035] The treatment can take place at a temperature higher than room temperature, for example at a treatment bath temperature between 30 degrees Celsius and 70 degrees Celsius.

[0036] For example, a sulfuric acid or hydrochloric acid solution could be used as the acidic solution.

[0037] In a preferred embodiment, the inventive method uses as an acidic solution an aqueous solution containing at least HCl and preferably at least one salt, an aqueous solution containing at least H2SO4 and preferably at least one salt, or an aqueous solution containing at least H2SO4 and H3PO4.

[0038] According to the invention, the salts present can be any salts originating from the steel flat product to be treated or from the scale to be removed, for example, iron salts, chromium salts, manganese salts, etc. Sulfate, chloride, hydroxide, etc., can be present as counterions. According to the invention, the salts preferably present in the solution are not additionally added to the solution from the outside, but rather the salts enter the solution from the steel flat product or the scale during the process. The preferred concentrations of the salts mentioned are reached after a very short time.

[0039] In a preferred embodiment of the process according to the invention, a solution containing at least one iron salt is used. Preferably, iron salts are used in which the iron cation has an oxidation state of +2. Particularly preferred iron salts are selected from the group consisting of FeSO₄, FeCl₂, and mixtures thereof.

[0040] Preferably, the solutions contain an iron salt selected from the group consisting of FeSO4, FeCl2 and mixtures thereof.

[0041] If an aqueous solution containing at least H2SO4 is used, it preferably contains 100 to 400 g / L, particularly preferably 180 to 300 g / L, H2SO4.

[0042] If an aqueous solution containing at least HCl is used, it preferably contains 10 to 30 wt.%, particularly preferably 15 to 25 wt.%, HCl.

[0043] If an aqueous solution containing at least one iron salt is used, it preferably contains 10 to 50 g / L, particularly preferably 20 to 45 g / L, of the at least one iron salt.

[0044] If an aqueous solution containing HCl and at least one iron salt is used, it preferably contains 10 to 30 wt.%, particularly preferably 15 to 25 wt.%, HCl and 10 to 50 g / L, particularly preferably 20 to 40 g / L, of the at least one iron salt, in particular FeCl₂.

[0045] If an aqueous solution containing H2SO4 and at least one iron salt is used, it preferably contains 100 to 400 g / L, particularly preferably 180 to 300 g / L, H2SO4 and 10 to 50 g / L, particularly preferably 20 to 45 g / L, of the at least one iron salt, especially FeSO4.

[0046] If an aqueous solution containing at least H₂SO₄ and H₃PO₄ is used, it preferably contains 20 to 60 vol%, particularly preferably 30 to 50 vol%, most preferably 40 to 50 vol%, H₃PO₄ and 20 to 60 vol%, particularly preferably 30 to 50 vol%, most preferably 30 to 40 vol%, H₂SO₄.

[0047] The solutions mentioned may contain other components, such as surfactants.

[0048] The method using steel strips is particularly preferred. consists of a steel that is not stainless steel, or of a steel that is IF steel.

[0049] The process offers particular advantages for such steels because steels produced from them have shown a high susceptibility to stagnation stains in known pickling processes.

[0050] For example, a steel can be used, consisting of iron and unavoidable impurities (each in weight percent, abbreviated: wt.%): The steel strip preferably consists of a steel according to one of the five alloy specifications listed below: I: 0.16 to 0.18 C; 0.35 to 0.45 Si; 1.45 to 1.60 Mn; 0.00 to 0.02 P; 0.00 to 0.008 S; 0.02 to 0.045 Al; 0.00 to 0.08 Cr; 0.00 to 0.12 Cu; 0.00 to 0.03 Mo; 0.0035 to 0.0085 N; 0.00 to 0.10 Ni; 0.02 to 0.03 Nb; 0.01 to 0.02 Ti; 0.00 to 0.02 V; 0.00 to 0.0005 B; balance Fe and unavoidable impurities. II: 0.13 to 0.15 C; 0.15 to 0.25 Si; 1.55 to 1.70 Mn; 0.00 to 0.015 P; 0.00 to 0.003 S; 0.02 to 0.05 Al; 0.70 to 0.85 Cr; 0.00 to 0.10 Cu; 0.00 to 0.10 Mo; 0.00 to 0.008 N; 0.00 to 0.10 Ni; 0.00 to 0.005 Nb; 0.03 to 0.04 Ti; 0.00 to 0.01 V; 0.0008 to 0.0012 B; balance Fe and unavoidable impurities. III: 0.100 to 0.500 C; 0.01 to 1.50 Si; 0.50 to 2.00 Mn; 0.000 to 0.020 P; 0.000 to 0.005 S; 0.00 to 1.50 Al; 0.01 to 1.00 Cr; 0.00 to 0.10 Cu; 0.01 to 0.2 Mo; 0.000 to 0.001 N; 0.00 to 0.01 Ni; 0.0010 to 0.0100 B; balance Fe and unavoidable impurities.IV: 0 to 0.2 C; 0 to 2 Si; 0 to 1 Mn; 0.000 to 0.100 P; 0.000 to 0.030 S; 3 to 7 Al; 3 to 11 Cr; 0 to 3 Cu; 0 to 2 Mo; 0 to 0.1 N; 0 to 2 Ni; 0 to 1 Nb; 0.25 to 0.3 Ti; 0 to 1 V; 0.0000 to 0.1000 B; balance Fe and unavoidable impurities. V: 0.1 to 1 C; 0.6 to 1.8 Si; 15 to 26 Mn; 0 to 0.08 P; <0.001 to 0.03 S; 0.3 to 2 Al; 0 to 8 Cr; 0 to 5 Cu; 0 to 2 Mo; 0.003 to 0.1 N; 0.1 to 8 Ni; 0.1 to 0.3 Nb; 0 to 0.5 Ti; 0 to 0.5 V; 0 to 0.01 B; balance Fe and unavoidable impurities.

[0051] Another aspect of the invention relates to a system for descaling a steel strip using a method according to the process described above or one of its further developments. The system for descaling the steel strip comprises at least: A treatment line comprising a trough filled with an acidic solution as a treatment bath. For example, one of the acidic solutions mentioned in connection with the method above can be used. A transport device for introducing a steel strip into the treatment bath of the treatment line and for transporting the steel strip through the treatment bath. In particular, the transport device can have one or more transport rollers. An electrotechnical device for continuous cathodic polarization of the steel strip during transport, preferably throughout the entire transport, through the Treatment line. The electrotechnical device may in particular include a rectifier and an electrical contact between the negative pole of the rectifier and the steel strip.

[0052] The transport device is coupled with means for monitoring the belt speed. These means can, for example, directly determine the belt speed, such as by optically detecting the guided steel belt. Alternatively or additionally, the means for monitoring the belt speed can determine it indirectly; for example, the means can include a speed sensor attached to a transport roller to detect its rotational speed. The system also features a control device that is linked to the monitoring system and is configured to detect, based on the monitoring of the strip speed, when a maximum processing time for the steel strip has been exceeded and, if this maximum processing time is exceeded, to mark the steel strip as scrap. "Marking" as scrap means that it is verifiably documented that an affected steel strip is to be treated as scrap, whereby "marking" includes not only markings applied directly to the strip but also entries in a processing log and the like.

[0053] In an advantageous embodiment, the transport device comprises at least one transport roller, wherein the monitoring means are designed to monitor the roller speed of the transport roller, for example, as a speed sensor arranged on the transport roller. The control device is configured to determine a standstill time until the resumption of strip transport upon detection of a roller standstill and, if the maximum treatment time is exceeded by the standstill time plus a predetermined treatment time, to mark the steel strip as reject.

[0054] The maximum treatment duration is preferably at least 900 seconds, more preferably at least 1200 seconds. The maximum treatment duration is advantageously less than 2400 seconds.

[0055] The acidic solution is preferably sulfuric acid or hydrochloric acid.

[0056] According to further training, the control device is also coupled with the electrotechnical equipment and is configured to automatically increase the current density generated for cathodic polarization by means of the electrotechnical equipment when a reduction in transport speed or a standstill of the transport roller is detected.

[0057] Further details, features and advantages of the subject matter of the invention will become apparent from the following description in conjunction with the figure.

[0058] They show: Fig. 1 : a schematic representation of a system according to the invention; Examples

[0059] The invention will now be explained in more detail using exemplary embodiments.

[0060] Samples of the steel grades listed in Table 1, with dimensions of 20 x 30 x 4.3 mm (hot-rolled strip), are treated with the solutions listed in Table 1 under the corresponding test conditions with respect to electrolyte, current density, treatment duration, bath temperature, and turbulence. Steel grades 1, 2, 3, 4, and 5 have the compositions shown in Table 1 (all values ​​in wt.%). The samples are immersed in the electrolyte (temperature between 55°C and 70°C) and cathodically polarized. A rectifier serves as the current source, and a platinum mesh is used as the counter electrode. A new sample is used for each individual test. The following tests were carried out for each steel grade: cathodic polarization at 40 A / dm² for 180 seconds, at 60 A / dm² for 210 seconds, at 100 A / dm² for 180 seconds, at 60 A / dm² for 600 seconds, at 60 A / dm² for 1200 seconds.

[0061] The following electrolytes are used: Electrolyte 1 H 2 SO 4 (250 g / L), FeSO 4 x 7 H 2 O (40 g / L) in water. Electrolyte 2 HCl (20% wt.), FeCl 2 x 4 H 2 O (30 g / L) in water.

[0062] Subsequently, each of the pickled samples underwent a metallographic evaluation of the micrograph. It was found that the scale had been removed from every sample, but that the base material was not attacked in any sample; in particular, no grain boundary oxidation or over-pickling was observed, contrary to expectations, even with the longest pickling times.

[0063] Fig. 1 A system for descaling a steel strip 1 is shown. The system features: a tub 2 filled with an acidic solution 3 as a treatment bath 3, a transport device 4 for introducing the steel strip 1 into the treatment bath 3 and for transporting the steel strip 1 through the treatment bath, an electrotechnical device 5 for continuous cathodic polarization of the steel strip during transport, wherein the transport device is coupled with means 6 for monitoring a strip speed, a control device 7 coupled with the means 6 for monitoring, which is configured to detect, depending on the monitoring of the strip speed, the exceeding of a maximum treatment time of the steel strip and, if the maximum treatment time is exceeded, to mark the steel strip as reject.

Claims

1. Method for descaling a steel strip, wherein at least the following steps are carried out: A) introduction of the steel strip having the scale into a treatment line, wherein the treatment line includes an acidic solution, that is to say: an aqueous solution having a pH value lower than 7, B) belt transport of the steel strip through the treatment line at a predetermined belt speed corresponding to an intended treatment duration, wherein the steel strip is put into a cathodically polarised state, C) monitoring of the belt speed, wherein if monitoring detects a decrease in the belt speed below the specified belt speed, the additional treatment time necessitated by the decrease in the belt speed is determined, wherein if the intended treatment time plus the additional treatment time do not exceed a maximum treatment duration, the steel strip is forwarded to regular further processing, and otherwise the steel strip is processed further as scrap, wherein the maximum treatment duration is at least 900 seconds.

2. Method according to Claim 1, wherein when a belt standstill is detected, a standstill time until the belt transport resumes is measured, and if the intended treatment time plus the additional treatment time necessitated by the standstill time does not exceed the maximum treatment duration, the steel strip is advanced to regular further processing, and otherwise the steel strip is processed further as scrap.

3. Method according to any one of the preceding claims, wherein the intended treatment duration is between 20 seconds and 600 seconds.

4. Method according to any one of the preceding claims, wherein the steel strip is put into the cathodic state with a current density between 5 and 150 A / dm2.

5. Method according to Claim 4, wherein upon detection of the decrease in the belt speed the current density is increased automatically, at least during the period of the decrease in the belt speed.

6. Method according to any one of the preceding claims, wherein the maximum treatment duration is at least 1200 seconds.

7. Method according to Claim 6, wherein the maximum treatment duration is between 1200 and 2400 seconds.

8. Method according to any one of the preceding claims, wherein the acidic solution is a sulphuric acid or a hydrochloric acid.

9. Method according to any one of the preceding claims, wherein the steel strip consists of a steel that is not stainless steel, or consists of a steel that is an IF steel.

10. Installation for descaling a steel strip (1) by means of a method according to any one of Claims 1 to 9, including: - a treatment line having a tub (2) filled with an acidic solution as a treatment bath (3), - a transport apparatus (4) for introducing a steel strip (1) into the treatment line and for transporting the steel strip (1) through the treatment line, - an electrotechnical device (5) for the continuous cathodic polarisation of the steel strip (1) during the transport, preferably during the entire duration of the transport through the treatment line, wherein the transport apparatus (4) is coupled to means (6) for monitoring a belt speed, - a control apparatus (7) that is coupled to the means (6) for monitoring and is configured to detect when a maximum treatment duration of the steel strip (1) is exceeded based on the monitoring of the belt speed, and to mark the steel strip (1) as scrap when the maximum treatment duration is exceeded.

11. Installation according to Claim 10, wherein the transport apparatus (4) is equipped with at least one transport roller, wherein the means (6) for monitoring are designed as means for monitoring the roller speed of the transport roller, wherein the control apparatus (7) is configured so as to calculate a standstill time until the belt transport resumes upon detection of a standstill time, and to mark the steel strip (1) as scrap if the maximum treatment duration is exceeded due to the standstill plus an intended treatment time.

12. Installation according to Claim 10 or Claim 11, wherein the maximum treatment duration is at least 900 seconds.

13. Installation according to any one of Claims 10 to 12, wherein the acidic solution is a sulphuric acid or a hydrochloric acid.

14. Installation according to any one of claims 10 to 13, wherein the control apparatus (7) is also coupled to the electrotechnical device (5) and is configured to automatically initiate an increase in the current density generated for the cathodic polarisation by means of the electrotechnical device (5) upon detection of a decrease in the transport speed or a standstill of the transport roller.