SAFETY ELEMENT AND METHOD FOR ITS MANUFACTURING
Patent Information
- Application Number
- DE502022001965
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-19
- Filing Date
- 2022-01-12
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2042-01-12
AI Technical Summary
Existing heat-sealing adhesives used in security elements for valuable documents can be overly reactive, leading to unintentional curing during physical drying, resulting in inadequate adhesion or insufficient stability, especially when exposed to high temperatures, which affects the security and durability of the documents.
Incorporating a radiation-crosslinkable component and a reactive diluent into the heat-sealing adhesive, along with plasticizers and photoinitiators, to reduce sealing temperature, improve wetting properties, and enhance adhesion, while maintaining stability and resistance to hot water.
The solution achieves a tack-free system at room temperature, allowing for easier processing and storage, with improved adhesion and internal strength, and high stability, including resistance to hot water, ensuring the security element's integrity and durability.
Description
[0001] The invention relates to a security element for valuables or the like, coated with a heat-sealable adhesive suitable for applying the security element to a valuables document substrate, which is non-sticky at room temperature. The invention further relates to a method for manufacturing such a security element. In addition, the invention relates to a valuables document with such a security element and a method for manufacturing the valuables document provided with the security element.
[0002] Valuables, especially banknotes, are often equipped with security features that allow verification of the document's authenticity and simultaneously serve as protection against unauthorized reproduction. Valuables within the meaning of the present invention include, in particular, banknotes, shares, identity cards, credit cards, bonds, certificates, vouchers, checks, high-value tickets, but also other documents susceptible to forgery, such as passports and other identification documents, as well as product security features such as labels, seals, packaging, and the like. The term "value document" in the following also includes the preliminary stage of a valuable document, in particular security paper, even if it is not yet ready for circulation.
[0003] It is known to secure valuable documents, such as banknotes, with a security element in the form of a security thread, a security strip or a patch or label.
[0004] In almost all security and banknote papers today, a security thread coated with heat-seal adhesive, especially heat-seal varnish, is embedded into the paper on the paper machine. The heat-seal varnish serves to improve the anchoring of the thread in the paper. Heat-seal varnishes are also used in banknote production for the application of holograms and holographic strips.
[0005] When applying security features using heat-seal lacquers, at least one of the substrates to be bonded is coated with a solvent-based polymer solution or an aqueous solution or dispersion. After physical drying by heating, a non-sticky surface is present at room temperature. Upon exposure to heat, the sealable compound melts and acts as an adhesive.
[0006] From EP 1 776 240 B1, the use of a heat-seal adhesive that is non-sticky at room temperature for applying a security element to a document substrate by a heat-sealing process under increased pressure and temperature is known. The heat-seal adhesive also contains a component that can be crosslinked by high-energy radiation. The presence of this component within the heat-seal adhesive allows crosslinking by irradiation to be carried out when the security element is applied to the document substrate. This creates a high-melting-point to infusible system, resulting in high stability and, in particular, pronounced hot water resistance. Hot water resistance can be verified, for example, using a washing machine. A suitable hot water test is performed, in particular, under the conditions of 100°C for 30 minutes or 60°C for 1.5 hours.
[0007] The heat-sealable adhesive known from EP 1 776 240 B1 can be applied to the security element to be applied in the form of a solution, an emulsion, or a dispersion. The radiation-curable coating applied in this form melts at low temperatures and penetrates the document substrate, resulting in easy processing. Ideally, the security elements coated in this way, before they are cured, can be stored without a change in their melting point. For example, films coated with this non-sticky coating at room temperature can be wound up and stored for extended periods without any change in their melting point.
[0008] When applying the heat-seal adhesive known from EP 1 776 240 B1, in the form of a solution, emulsion, or dispersion, to the security element to be applied, physical drying is required, for example, by slightly increasing the temperature to 80°C. This drives off any solvent and / or water that may be present in the radiation-curable dispersion, solution, or emulsion. Physical drying may require such a high heat exposure that, in the case of highly reactive adhesive systems, unintended curing can occur. In the case of a less reactive adhesive system, an insufficient thermal exposure time during the application of the heat-seal adhesive-coated security element to a document substrate would lead to inadequate curing and thus to poor adhesion of the security element to the document substrate.
[0009] The present invention is based on the objective of providing a safety element that overcomes the disadvantages of the prior art.
[0010] This problem is solved by the combination of features defined in the main claim. Further developments of the invention are the subject of the dependent claims.
[0011] Detailed description of the invention: Instead of the formulation "a heat-seal adhesive that is not tacky at room temperature", the formulation "a heat-seal adhesive that is tack-free at room temperature" or the formulation "a heat-seal adhesive that is essentially tack-free at room temperature" is also used herein. The term "room temperature" is understood to mean a temperature of 23°C.
[0012] The term "heat sealant" is also used here instead of "heat sealant adhesive".
[0013] The safety element according to the invention is equipped with a heat-seal adhesive that is non-sticky at room temperature. The heat-seal adhesive also comprises a radiation-crosslinkable component and a reactive diluent. The invention is based on the heat-seal adhesive known from EP 1 776 240 B1. The invention is based on the finding that a reduction in the sealing temperature and simultaneously improved wetting properties of the melt can be achieved by adding a reactive diluent to the heat-seal adhesive composition. Particularly advantageous effects can be achieved in aqueous formulations when a reactive diluent is present in addition to the actual dispersed urethane acrylate component. While not definitively conclusive, it can be assumed that the reactive diluents migrate into the dispersion particles in the first step and are found to a lesser extent in the aqueous phase.After physical drying, they act as coalescing agents, thus promoting film formation. Depending on the formulation, complete tack-free behavior, i.e., non-sticky, can be ensured. An example of a dispersion that already contains reactive diluents in its supplied form is Alberdingk Lux 481. This contains less than 10% DPHA and 3% to 5% TMP(EO) x TA. The abbreviation "TMP(EO)TA" stands for trimethylolpropane(ethoxy)triacrylate, and the abbreviation DPHA for dipentaerythritol hexaacrylate. Particularly good heat-sealable dispersions can also be achieved with a TMP(EO) x TA content of less than 15% alone. In the formula TMP(EO) x TA, x is preferably selected in the range of 1 to 9, more preferably in the range of 3 to 9, with x being particularly preferably 3.
[0014] The heat-seal lacquer formulations according to the invention are preferably aqueous dispersions and in particular those which contain either from the outset or after addition 5% to 25%, preferably 9% to 16% of a low molecular weight compound (M<1000g / mol).
[0015] The advantages of reactive diluents are the general reduction of the sealing temperature and the improved wetting properties of the melt. A disadvantage is the reduction in blocking strength. The use of multifunctional reactive diluents leads to a high-molecular-weight system after crosslinking, which may no longer be meltable. This property, while not detrimental, is not desirable as long as the melting point is only so high that melting is no longer possible for the non-destructive removal of a safety element.
[0016] It is advantageous to add triphenyl phosphate, pentaerythritol tetrabenzoate, cyclohexanedimethanol dibenzoate, and / or sucrose benzoate as a soluble component to the heat-seal lacquer formulation according to the invention. These are plasticizers with a preferred melting point in the range of 50°C to 120°C. It is preferred that the plasticizer be added in a weight fraction of 1% to 30%, preferably 2% to 10% (based on the solid content). These substances, which are solid at room temperature, are less critical with regard to blocking behavior than liquid substances. Due to their solubility in reactive diluents, they can also be incorporated into the overall formulation.
[0017] Alternatively, if one does not assume an aqueous dispersion, but rather a UV system, such as is available as a dual-cure system, in particular a solvent-based formulation, where preferably butyl acetate can be used as the solvent, the aforementioned plasticizers can also be dissolved directly, whereby they are solid again after physical drying and have little influence on the blocking.
[0018] The heat-seal lacquer formulation according to the invention comprises at least one solvent which is present in a preferred weight fraction in a range of 30% to 90%, particularly preferably in a range of 40% to 75%, wherein the solvent is preferably selected from the group consisting of butyl acetate, propyl acetate, ethyl acetate and a mixture of two or more of the aforementioned substances.
[0019] It is preferred to additionally add a prepolymer that is tack-free at room temperature after physical drying, contains on average at least two reactive groups, and has a molecular weight of at least 600 g / mol. The prepolymer is preferably present in the heat-seal lacquer formulation in a weight fraction in the range of 8% to 65%.
[0020] To increase reactivity, an A-min synergist can be added to the heat sealant formulation.
[0021] In the case of electron beam curing, no photoinitiator is required. Particularly in the case of aqueous formulations, the photoinitiators TPO-L, Omnirad 500, and Omnirad 819 DW are advantageous. The preferred weight fraction is 1% to 8% based on the respective solid. Additionally, especially when using photoinitiators from the BAPO series, a sensitizer, for example from the ITX family, can be advantageous for higher reactivity. The abbreviation "BAPO" stands for phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and the abbreviation "ITX" stands for isopropylthioxanthone.
[0022] In some cases, the heat-seal lacquer does not adhere directly to the security element to be bonded. In these cases, it is advisable to modify the security element, e.g., by using a pressure-pretreated film, or to pretreat it using known methods such as plasma or corona treatment, or to apply a primer.
[0023] When selecting suitable primers, it has become apparent that the potential of UV crosslinking of the heat-seal lacquer can be fully utilized, especially with reactive primer systems. These include, for example, 2K-PU systems, which are particularly often applied in multiple layers. It is especially advantageous if at least one layer contains an aliphatic isocyanate.
[0024] The reactive diluents mentioned in relation to aqueous systems and the soluble, low-molecular-weight components or plasticizers specifically mentioned in relation to solvent systems are capable of migration. This means that, if stored properly, they can disperse throughout the entire structure, leading to a loss of adhesion to the substrate and a deterioration of the sealing properties.
[0025] In the field of PVC films, the use of barrier layers to prevent the migration of plasticizers is common. Solvent-based coatings of relatively high molecular weight acrylates are used in this area. Typical substances for this purpose are available under the brand names Degalan and Elvacite.
[0026] According to a special variant, a radiation-curable heat-sealable lacquer can be applied in several layers, with the first layer being pre-cured. If the first layer of the heat-sealable lacquer is radiation-cured on a primer after physical drying, the first layer itself can also serve as a barrier layer against migratory components of the subsequent heat-sealable lacquer layers. Furthermore, it prevents any spacers used, such as waxes, from sinking into the heat-sealable lacquer or primer layer.
[0027] The crosslinking of the heat-seal lacquer can take place directly after sealing, preferably while still utilizing the elevated temperature of the sealing process. At this stage, the raw materials have not yet had the opportunity to crystallize, resulting in better mobility of the reactive groups and thus improved crosslinking. This is particularly advantageous when crosslinking with medium-pressure mercury lamps, which themselves generate a significant amount of heat, and with LED lamps, which have low heat output. If the heating provided by the lamps is insufficient, a heating roller is useful for controlling the temperature before and during crosslinking.
[0028] If UV crosslinking is not possible in the application machine, it can also be performed in a separate step. A step in which UV crosslinking is already planned is preferred. A typical example is crosslinking on a screen printing machine, which, with appropriate equipment, can irradiate a substrate from both sides. If the security element to be bonded is a patch, usually only a portion of it has an opaque layer, which makes crosslinking more difficult. The edge area is typically transparent. Therefore, the edge area can be easily crosslinked by exposure from above, while the areas beneath the opaque coating are preferably exposed from below, through the substrate.The opaque coating is often a metallization that reflects the corresponding light, thus enabling better utilization of the light transmitted through the substrate.
[0029] Heat-seal varnishes in their uncrosslinked state have the property of softening when exposed to heat. In intaglio printing, elevated temperatures and high pressure are present. By using a thick layer of heat-seal varnish, a deep embossing can be achieved. When crosslinking occurs subsequently, the embossing can be permanently fixed. This is particularly advantageous for substrates that can be plastically deformed in intaglio printing.
[0030] Radiation-cured heat-sealable lacquers, besides having the advantage of high resistance, have the disadvantage that the so-called ribbing, i.e., poor flatness, is particularly pronounced after cross-linking, since it is a system that shrinks during curing and a cross-linked, non-flowable system after curing, and stress reduction is hardly possible later.
[0031] This can be achieved, on the one hand, by adding the plasticizers described above, which allow limited deformability even after crosslinking, and on the other hand, by adding so-called chain carriers. These can be, for example, thiols. Chain carriers shift the gel point to a later stage during the crosslinking reaction, thereby reducing the build-up of stress.
[0032] The top layer of the security element, which comes into contact with the heat-seal lacquer, can be, for example, a standard, untreated polyester film, or it can be a co-extruded film with a layer exhibiting lower adhesion to the heat-seal lacquer. Since, for example, a patch may also use a double film as a carrier, any film with lower adhesion to the adhesive can be laminated on top. A siliconized polyester film is also possible. A standard polyester film can also be additionally coated with a layer that is less prone to clogging. This layer can also incorporate larger spacers.
[0033] The photoinitiator used in UV curing can be a small, defined molecule with a fixed melting point. If this melting point falls within the appropriate temperature range, it can promote the melting process.
[0034] While the use of UV absorbers or stabilizers is common in aqueous dispersions for outdoor applications, the use of stabilizers is only common in hot melts to enable longer temperature stability in the melt in the extruder or application device.
[0035] If required, benzotriazole-based UV absorbers such as Tinuvin 9945 DW and / or triazines such as Tinuvin 477 DW can be added as additives. The quantity added should be such that the blocking resistance is not impaired. For the absorbers to be effective, they should be compatible with the aqueous dispersion film. Ideally, the absorbers should be liquid or have a low melting point at room temperature. Therefore, the addition of these absorbers is expected to improve not only weathering resistance but also sealing properties. In the long-wave UV range, i.e., at the boundary with the visible range, typically LED 395 nm, crosslinking should not be affected.
[0036] In the case of a security strip to be applied to a document substrate, in particular a paper substrate, especially a transfer element to be removed from a temporary carrier film, the exposure can take place after the security strip has been applied from the side of the security strip through the carrier film, or after the carrier film has been removed, or from the side of the document substrate, depending on the transparency of the various elements.
[0037] In the case of a security strip with a permanent carrier film to be applied to a valuable document substrate, the exposure after application of the security strip can take place from the side of the security strip through the carrier film, or from the side of the valuable document substrate, depending on the transparency of the various elements.
[0038] When applying a patch or label to a document substrate, certain limitations arise. To save on backing film and produce more cost-effective patch elements, the patch elements are often more densely packed on the backing film than on the final document substrate. Therefore, exposure can either occur only after the backing film has been removed, or with the aid of a mask that can, for example, rotate so that only the already applied patch is exposed and not the patch elements still on the backing film. Alternatively, in the case of an LED light source, the light source can be controlled so that it only illuminates at the precise moment required for patch exposure and is then effectively switched off again. This aspect of patch exposure through rapid switching of the light source is advantageous because a significant problem with LED lights is their temperature. At high temperatures, they lose performance and their lifespan is reduced.If the patch area to be irradiated only makes up about 1 / 3 of the total area, the heat generation is reduced by 2 / 3, which means that the radiant can potentially even be operated at a higher power than its continuous power output, and cooling power is saved.
[0039] If necessary, it is advisable to print a primer beneath the security element to be applied to the document substrate. The primer can be based on a similar formula to the heat-seal varnish to be used. Printing a primer that first undergoes physical drying usually results in better adhesion than conventional heat sealing. If the primer and the heat-seal varnish have a similar base, they bond optimally during heat sealing and can permanently polymerize together upon subsequent irradiation. However, there is a potential problem that the primer may also melt during the sealing process, leading to contamination of the calender or counter roller. Therefore, it is advisable to test a primer print that is narrower than the security element to be sealed.
[0040] The heat-seal varnish according to the invention leads to an advantageous reduction in the required sealing temperature. If a system is present that, for example, has an additional primer or an additional ink-receptive layer, but is not optimized for a low melting point, it can also be printed over a larger area and still does not adhere to rollers during the sealing process. The process window can be extended by applying a non-stick coating to the corresponding roller.
[0041] Consequently, the use of systems with different sealing properties as a pre-coating is conceivable, at least in a partial area of the substrate, as is their use as a heat-seal varnish.
[0042] The coating according to the invention can be applied in the form of a solution, an emulsion, or a dispersion. The radiation-crosslinkable coating applied in this form melts at low temperatures and penetrates the substrate, resulting in easy processability. The safety element according to the invention is therefore equipped with a low-melting-point system that is essentially tack-free at room temperature. The presence of a radiation-crosslinkable component in the coating allows crosslinking by irradiation to be carried out after application of the coating. This creates a high-melting-point to infusible system, resulting in high stability and, in particular, sufficient hot water resistance, e.g., in washing machine tests. A suitable hot water test is performed, in particular, at 100°C for 30 minutes or 60°C for 1.5 hours.
[0043] During crosslinking, adhesion to the substrate, e.g., a pressure-pretreated film, improves, and the internal strength of the coating increases. The temperature of the coating immediately before, during, and immediately after curing is an important parameter determining the achievable degree of crosslinking. Higher temperatures allow for a higher degree of crosslinking because the mobility of the reactive groups is greater.
[0044] Conventional UV coatings are liquid before crosslinking and generate considerable heat of reaction due to the high density of reactive groups. In contrast, the radiation-curable, and especially UV-curable, coatings according to the present invention consist of molecules with a relatively high molecular weight and are solid at room temperature. The lower number of reactive groups per unit volume / mass results in less heat of reaction. Consequently, external heat input plays a more significant role in the crosslinking process. The temperature during curing can therefore be used to control the mechanical properties of the coating.
[0045] The safety elements coated in this way, but not yet cross-linked, can be stored without a change in melting point. For example, films with this coating, which is essentially tack-free at room temperature, can be wound up and stored for extended periods without any change in melting point.
[0046] According to an advantageous embodiment of the invention, the coating, which is essentially tack-free at room temperature, is at least physically dried. By slightly increasing the temperature to, for example, 80°C, any solvent and / or water present are driven off from the radiation-curable dispersion, solution, or emulsion. This physical drying results in the coating being essentially tack-free at room temperature.
[0047] In the context of this description, the term "essentially tack-free" also means essentially non-adhesive, in the sense of a smooth, essentially non-sticky surface. This can be verified by the following test: Coated film pieces of approximately 100 cm² are stacked, loaded with a weight of 10 kg, and stored for 72 hours at 40°C. If the film pieces can then be easily separated from each other without damaging the coating, the coating is considered essentially tack-free.
[0048] The substrate of the security element according to the invention can, in principle, be in any desired form. For example, the security element according to the invention can consist of fibers coated with a coating that is essentially tack-free at room temperature. According to an advantageous embodiment of the invention, however, the substrate is planar with two opposing main surfaces. Preferably, only one main surface of the substrate is provided with a coating that is essentially tack-free at room temperature.
[0049] Generally, it is sufficient if a major surface of the substrate is partially coated with the essentially tack-free coating at room temperature. However, for optimal embedding of the security element in security paper or a valuable document, it is advisable for the main surface(s) of the substrate to be fully coated with the essentially tack-free coating at room temperature. Depending on the size of the security element, it may also be sufficient for only a portion of the substrate to be coated with the essentially tack-free coating at room temperature.
[0050] If the security element is completely embedded in the security paper, it has proven particularly advantageous if both main surfaces of the substrate are coated with a coating that is essentially tack-free at room temperature. This variant is especially useful when the security element is embedded in security paper or a valuable document, similar to a window security thread. The main surfaces can be coated with either the same or different coatings.
[0051] According to a further preferred embodiment of the present invention, the security element has a thickness of 1 µm to 100 µm, preferably a thickness of 2 µm to 50 µm. These are thicknesses of the security elements that are easy to handle when equipping valuable documents and security papers with security elements.
[0052] Preferably, the substrate of the security element according to the invention is designed to be multilayered and / or flexible. The advantages associated with the multilayered nature of the security element are described in more detail below. The flexibility of the security element is often desirable, since the valuable documents equipped with the security element, such as banknotes or certificates, are also usually flexible.
[0053] The coating, which is essentially tack-free at room temperature, is preferably applied to the substrate as a solution, emulsion, or dispersion and then physically dried. An aqueous dispersion is particularly preferred.
[0054] Such an aqueous dispersion can be applied directly to a substrate, to a suitably pressure-pretreated or primed film (e.g., Hostaphan RNK 2600, Mitsubishi Polyester Film), or, in cases where there are additional layers between the substrate and the coating, which is essentially tack-free at room temperature, to these layers. The resulting film can be wound up, transported, and stored. By applying pressure and temperature (approximately 100°C to 160°C), the film can be applied to paper, another film, or a polymer.
[0055] According to a further preferred embodiment of the present invention, the dispersion is selected from the group consisting of aliphatic polyurethane dispersions, aromatic polyurethane dispersions, acrylates, anionic acrylate-modified polyurethane dispersions, polyurethane polyether acrylates and mixtures thereof.
[0056] Acrylated polyurethane dispersions are particularly well-suited. Examples of such acrylated polyurethane dispersions include DW7770, DW7773, DW7825, DW7772, DW7849 (UCB, Surface Specialties) and Actilane 340 Epoxynovolacacrylate in butoxyethyl acetate (Akzo).
[0057] Weitere strahlenhärtbare Dispersionen sind beispielsweise NeoRad R-440 (NeoResins), NeoRad R-441 (NeoResins), NeoRad R-445 (NeoResins), Laromer LR 8949 (BASF), Laromer LR 8983 (BASF), Laromer LR 9005 (BASF), LUX 101 UV-Dispersion (Alberdingk), LUX 241 UV-Dispersion (Alberdingk), LUX 308 UV-Dispersion (Alberdingk), LUX 352 UV-Dispersion (Alberdingk), LUX 370 UV-Dispersion (Alberdingk), LUX 390 UV-Dispersion (Alberdingk), LUX 399 UV-Dispersion (Alberdingk), LUX 331 UV-Dispersion (Alberdingk), LUX 338 UV-Dispersion (Alberdingk), Halwedrol UV 95 / 92 W (Hüttenes-Albertus), Halwedrol UV 14 / 40 W (Hüttenes-Albertus), Halwedrol UV-TN 6711 / 40 W (Hüttenes-Albertus), Halwedrol UV 65 / 40 W (Hüttenes-Albertus), Halwedrol UV-TN 7561-3 / 40 W (Hüttenes-Albertus), Halwedrol UV-TN 7157 / 40 W (Hüttenes-Albertus) and Bayhydrol UV VP LS 2280 (Bayer).
[0058] The dispersions mentioned include anionic and non-ionic dispersions. Most of these dispersions are aliphatic polyurethane dispersions (e.g., aliphatic polyester polyurethanes), but there are also aromatic polyurethane dispersions and copolymers (e.g., dispersions based on aliphatic polyurethane and acrylic acid ester copolymers), acrylates (acrylic acid ester copolymers), as well as anionic acrylate-modified UV-curing polyurethane dispersions or polyurethane polyether acrylates.
[0059] Preferably, the solids content of the dispersion is between 30 wt.% and 60 wt.%, more preferably between 35 wt.% and 50 wt.%. However, the solids content can be adjusted as required by dilution.
[0060] Commercially available dispersions have a solids content between 38 wt.% and 51 wt.%. Due to their easy availability, such dispersions are preferred within the scope of the present invention.
[0061] The radiation-crosslinkable component contained in the coating can preferably be crosslinked by ultraviolet radiation or electron beam radiation. Iron-doped emitters are particularly well-suited in terms of their spectral range. Alternatively, undoped mercury or gallium-doped emitters can be used. However, mercury emitters exhibit a somewhat less favorable spectral range when cured through the applied elements, while gallium emitters result in poorer surface hardening.
[0062] According to a preferred embodiment, the coating, which is essentially tack-free at room temperature, contains a photoinitiator. Crosslinking can be initiated and controlled in a particularly simple manner using a photoinitiator. Preferred examples of such photoinitiators are Darocur 4265 (Ciba), Darocur 1173 (Ciba), Irgacure 500 (Ciba), Irgacure 184 (Ciba), Esacure KIP 100 F (Lamberti), and Irgacure 2959 (Ciba).
[0063] Preferably, the photoinitiator is a water-soluble photoinitiator, a water-dispersible photoinitiator, or a photoinitiator soluble in water using water-compatible solvents. Irgacure 2959 (Ciba) is an example of a water-soluble initiator. Irgacure 819 DW (Ciba) is an example of a water-dispersible (or pre-dispersed) initiator. Lucirin TPO (BASF) is an example of an initiator soluble using other water-compatible solvents.
[0064] In the case of water-miscible solvents, a higher VOC content may have to be accepted during processing, as the finished dispersion should contain a solvent component that prevents the precipitation of the photoinitiators used. If this is not possible, rheology additives (anti-settlement additives) must be used.
[0065] This prevents the dispersion from having to be stirred again before each use.
[0066] According to a further preferred embodiment of the present invention, the coating, which is essentially tack-free at room temperature, is a cationic radiation-curing resin. Epoxy-modified vinyl copolymers are particularly suitable. UCAR VERR-40 (The Dow Chemical Company) is an example of such an epoxy-modified vinyl copolymer.
[0067] The radiation-crosslinkable component contained in the tack-free coating can preferably be crosslinked by short-wave radiation, such as ultraviolet radiation or short-wave visible radiation, or by electron beam radiation. Standard UV lamps (doped or undoped) or UV LEDs are particularly preferred as the radiation source.
[0068] The tack-free coating comprising the cationic radiation-curing resin preferably contains a photoinitiator suitable for cationic radiation curing. This facilitates the initiation of crosslinking in a particularly simple manner. Optionally, the cationic radiation-curing resin can also be combined with other resins. Furthermore, the coating comprising the cationic resin can also be crosslinked purely thermally. In this case, the use of a photoinitiator is unnecessary.
[0069] Preferably, the security element comprises, in addition to the coating which is essentially tack-free at room temperature, at least one further layer, wherein this further layer is at least pre-crosslinked by radiation. This layer is preferably applied between the substrate and the coating which is essentially tack-free at room temperature. By means of radiation, this layer can be crosslinked to such an extent that subsequent melting, which is associated with the risk of loss of adhesion due to dewetting, is prevented, while still maintaining good overprintability. To produce a security element according to the invention, the additional layer, at least pre-crosslinked by radiation, is overlaid with the coating according to the invention, in particular with a UV-curable dispersion. This further layer is then only physically dried to achieve tack-free properties and simultaneously maintain meltability.
[0070] To increase counterfeit protection, the security element preferably also includes at least one additional security feature that can be visually and / or mechanically verified.
[0071] According to a preferred embodiment, the visually and / or machine-verifiable security feature can comprise an optically variable effect, in particular a diffraction pattern, a hologram, a color-shifting effect, or other interference effects. According to another preferred embodiment, the security feature is provided with a printed image, in particular with positive or negative patterns or positive or negative characters. The security feature can also include fluorescent substances, phosphorescent substances, and / or magnetic substances, which may be present in the substrate, as a further security feature. It is obvious that combinations of such security features are also possible.
[0072] Preferably, a transparent plastic film is used as the substrate for the safety element according to the invention. Such films have the advantage that irradiation with UV light can be carried out through the film. For example, a PET film is transparent in the UV range up to approximately 310 nm, starting from the visible spectrum. Therefore, commercially available UV lamps can be used for irradiation. Alternatively, the substrate can also comprise a paper layer, optionally in addition to the paper layer.
[0073] Particularly preferably, the safety element comprises, in addition to the substrate and the coating which is essentially tack-free at room temperature, at least one further layer, wherein the layer is at least partially reflective.
[0074] Also preferred are embodiments in which the security element, in addition to the substrate and the coating which is essentially tack-free at room temperature, comprises at least one further layer, wherein a diffraction structure in the form of a relief is embossed into it. The diffraction structure is preferably provided with a reflective layer, at least in some areas.
[0075] The coating, which is essentially tack-free at room temperature, can also be used as an embossing varnish. Conventional thermoplastic embossing varnishes either require high temperatures and pressures during embossing or become cloudy or matte when the hologram is applied to a substrate, as the embossed structures soften and deform under application conditions. With conventional, usually liquid, UV varnish systems, only complete curing of the embossed layer is possible, which makes a sharp, crisp cut-out during patch production impossible or only partially possible.
[0076] If a security element according to the invention is used with a coating that is essentially tack-free at room temperature on a substrate, in particular a plastic film, which may optionally be provided with a release layer (e.g., waxes), a low-melting-point thermoplastic embossing lacquer is initially present. A motif, in particular a diffraction pattern in the form of a relief, can be embossed into this lacquer layer. During or after this process (with a block-free setting and a corresponding glass transition temperature of the dispersion, this is also possible after winding), the dispersion is hardened by mask exposure. That is, the areas to be transferred later (patches) are exposed, while the intermediate areas are not. The intermediate areas therefore remain soft and meltable, which later enables sharp-edged melting, while the exposed areas remain hard even during the transfer process and retain their embossed structures.The coatings, which are essentially tack-free at room temperature according to the present invention, can therefore be cross-linked during the embossing process and are thus dimensionally stable and brilliant even at high pressures and temperatures.
[0077] According to a preferred embodiment of the present invention, the safety element therefore comprises, in addition to the substrate, a coating that is essentially tack-free at room temperature, wherein a diffraction structure in the form of a relief is embossed into the coating that is essentially tack-free at room temperature. Advantageously, the coating that is essentially tack-free at room temperature is in a partially hardened form. The coating that is essentially tack-free at room temperature is preferably provided with the diffraction structure only in the hardened areas.
[0078] Advantageously, at least the areas of the hardened layer provided with the diffraction pattern are at least partially equipped with a reflective layer. The reflective layer is preferably in the form of positive or negative patterns.
[0079] Security elements that are prepared on a separate layer, such as a plastic film, in the reverse order of their final placement on the security paper, and then transferred to the security paper in the desired outline shapes using an adhesive or varnish layer, are called transfer elements. The separate layer can be peeled away from the security element's layered structure after the transfer. To facilitate removal of the separate layer after the security element's transfer, a release liner can be provided between this layer and the part of the security element being removed.
[0080] According to a further preferred embodiment, the safety element therefore comprises, in addition to the substrate and the coating which is essentially tack-free at room temperature, at least one further layer, wherein the latter is a separating layer. It is particularly preferred if the separating layer is arranged between the substrate and the coating which is essentially tack-free at room temperature.
[0081] According to a further preferred embodiment, the coating of the security element, which is essentially tack-free at room temperature, is printed with ink and cross-linked by radiation. In particular, coatings on paper should be dirt-repellent, offer good ink adhesion, and not act as a barrier between the paper and ink during resistance tests. By applying a defined temperature at which the cross-linking reaction of the essentially tack-free coating occurs, the degree of cross-linking can be controlled, thus adjusting the balance between ink adhesion and dirt repellency.
[0082] Printing can alternatively take place either after the tack-free coating has fully cured or before curing. If printing occurs before curing, the coating, which is essentially tack-free at room temperature, is printed upon, resulting in a kind of dissolution of the coating by the printing ink. The printing ink bonds with the coating, further improving adhesion. To prevent problems caused by the coating being lifted or excessively absorbed by the paper during application, rheology additives (especially thickeners) can be used.
[0083] In another advantageous variant, the tack-free coating is pre-cured before printing with ink. However, complete curing still only occurs after printing.
[0084] In preferred embodiments, the security element is designed in the form of a security tape, a security strip, a patch or other planar security element.
[0085] The substrate of the safety element can also be in the form of fibers, with the fibers being surrounded by a coating that is essentially tack-free at room temperature.
[0086] Particular advantages arise when the security element is positioned above a window present in security paper or a valuable item. This window is preferably manufactured using papermaking techniques or die-cut.
[0087] The present invention also includes a security paper for the production of security or valuable documents, such as banknotes, checks, identification cards, certificates, or the like, which is equipped with a security element described above. Advantageously, the security paper has, in addition to the security element according to the invention, at least one additional carrier substrate. Paper is preferred as the carrier substrate. The present invention also includes a valuable item, branded goods, valuable document, or the like, equipped with such a security element.
[0088] Preferably, the security element can be attached to or embedded in the security paper or document. Alternatively, the security element can be embedded in the security paper or document in the manner of a window security thread and be visible on the surface of the security paper or document in window areas. The security element can also form a pendulum security thread that appears alternately on opposite surfaces of the security paper or document.
[0089] In the process for manufacturing one of the security elements described above, a coating that is essentially tack-free at room temperature is at least partially applied to a substrate. The coating, which is essentially tack-free at room temperature, is then preferably dried, at least physically.
[0090] According to a particularly preferred method variant, the coating, which is essentially tack-free at room temperature, is applied as an aqueous dispersion.
[0091] According to another preferred method variant, a cationic radiation-curing resin is applied as a coating that is essentially tack-free at room temperature.
[0092] In a preferred embodiment of the method, at least one further layer is applied to the substrate, at least partially, before the application of the coating, which is essentially tack-free at room temperature. This further layer can be a radiation-crosslinkable layer, which is at least pre-crosslinked by radiation before the tack-free coating is applied. This pre-crosslinking minimizes subsequent melting, which is associated with the risk of loss of adhesion to the substrate.
[0093] In another advantageous variant, the coating, which is essentially tack-free at room temperature, is cross-linked by ultraviolet radiation or electron radiation.
[0094] The present invention also includes a method for producing a security paper or valuable item described above, wherein the security paper or valuable item is equipped with a security element described above.
[0095] According to a preferred method variant, the security element is applied to a substrate under elevated pressure and temperature, and the coating, which is essentially tack-free at room temperature, is then at least pre-crosslinked by radiation. If the security element is a transfer element, the coating, which is essentially tack-free at room temperature, can be fully crosslinked after removal of the substrate and, if present, the separating layer. According to another preferred method variant, the coating, which is essentially tack-free at room temperature, is irradiated with short-wave radiation, in particular short-wave visible radiation or UV radiation, from the direction of the coating immediately before the security element is applied to the security paper or the valuable item, and then applied to a substrate under elevated pressure and temperature.Exposure from the coating side is advantageous because it avoids or at least significantly reduces the exposure of the substrate to UV radiation and the material of the safety element to UV radiation.
[0096] The present invention can also include the use of one of the security elements described above for the production of foil-laminated banknotes and its use as packaging material. For example, sterilizable foil packaging with a security element according to the invention can be sealed and cross-linked. Upon successful UV sterilization, the seal is simultaneously cross-linked and becomes strong.
[0097] Further embodiments and advantages of the invention are explained below with reference to the figures. For clarity, the figures are not drawn to scale or with accurate proportions.
[0098] It shows Fig. 1 shows a schematic cross-sectional representation of a security element according to the invention with a coating that is essentially tack-free at room temperature; Fig. 2 shows a schematic cross-sectional representation of a security paper coated with the security element of Fig. 1 is equipped; Fig. 3 a schematic cross-sectional representation of a security element according to another embodiment of the invention; Fig. 4 a schematic cross-sectional representation of a security paper equipped with the security element of Fig. 3 is equipped; Fig. 5 a schematic cross-sectional representation of security paper according to another embodiment of the invention; Fig. 6 a schematic cross-sectional representation of the security paper of Fig. 5 after the substrate of the security element designed as a transfer element has been detached; Fig. 7 a schematic cross-sectional representation of a security element or security paper according to another embodiment of the invention; Fig. 8 a schematic cross-sectional representation of a security element or security paper according to another embodiment of the invention; Fig. 9 a schematic cross-sectional representation of a security element designed as a transfer element according to another embodiment of the invention; Fig. 10 a schematic representation of the security element of Fig. 9 after exposure to UV radiation in cross-section; Fig. 11 a schematic cross-sectional representation of a security paper according to another embodiment of the invention; Fig. 12 a schematic top-down representation of a security document; Fig. 13 a cross-section through the security document of Fig. 12 .
[0099] Fig. 1 Figure 1 shows a schematic representation of a security element according to the invention, comprising a substrate 1 and a coating 2 that is essentially tack-free at room temperature. To produce the security element, for example, a UV-curable dispersion (UV dispersion) is applied to the substrate 1, for example, a plastic film, in particular a PET or OPP film. The UV dispersion is dried (e.g., at 80°C), resulting in a coating 2 that is essentially tack-free at room temperature.
[0100] The security element and all security elements described below may be equipped with further security features not shown in the respective figures, such as a hologram or a printed design.
[0101] Fig. 2 The diagram shows a schematic cross-section of a security paper featuring the security element of Fig. 1 is equipped. The security element is used to manufacture the security paper. Fig. 1 The coating is transferred to a substrate 3, e.g., paper, by a heat-sealing process at increased pressure and temperature (e.g., 140°C). In this case, the coating, which is essentially tack-free at room temperature, thus functions as a heat-seal varnish.
[0102] Then the coating 2 of Fig. 1 cross-linked by the action of UV radiation (e.g. Hg and Fe emitters), so that finally a security paper with a radiation-cross-linked, infusible coating 2 and a covering substrate 1, e.g. a plastic film, is obtained.
[0103] Fig. 3 Figure 1 shows a schematic cross-sectional representation of a security element according to another embodiment of the invention. To produce the security element, a UV dispersion is applied to a substrate 1, for example, a plastic film. The plastic film is, for example, a PET or OPP film. The UV dispersion is dried (e.g., at 80°C) and cross-linked by exposure to UV radiation, resulting in an infusible coating 4. A further coating of UV dispersion is applied over this coating 4 and dried (e.g., at 80°C), resulting in a coating 2 that is essentially tack-free at room temperature. Forming such a two-layer coating has the advantage of ensuring good adhesion to the substrate 1 during the subsequent heat-sealing process.
[0104] Fig. 4 The diagram shows a schematic cross-section of a security paper featuring the security element of Fig. 3 is equipped. The security element is used to manufacture the security paper. Fig. 3 The coating is applied to a paper substrate 3 by a heat-sealing process under increased pressure and temperature (e.g., at 140°C). The coating 2 is then... Fig. 3 cross-linked by the action of UV radiation (e.g. Hg and Fe emitters), so that finally a security paper with a two-layer, radiation-cross-linked, infusible coating 2, 4 and a covering substrate 1, here a plastic film, is obtained.
[0105] The described security elements are characterized by excellent adhesion of the coatings 2 and 4 to the substrate 1. This adhesion is not lost even at the elevated temperatures of the heat-sealing process. Should adhesion problems nevertheless occur with one of the plastic films used, a pressure-pretreated film (e.g., Hostaphan RNK2600, Mitsubishi Polyester Film) can be used.
[0106] Fig. 5 Figure 1 shows a schematic cross-sectional representation of a security paper according to another embodiment of the invention. The security element, designed here as a transfer element, is used to manufacture the security paper. Fig. 5 To equip the security paper shown, an embossing varnish 6 is applied to a substrate 1, for example, a PET carrier film. Optionally, a release layer, e.g., of wax, can be applied between the PET carrier film and the embossing varnish layer 6. The embossing varnish 6 is then coated with a reflective layer 7, for example, a metal layer or a high-refractive-index layer. All metals and many metal alloys are suitable as reflective materials. Examples of suitable high-refractive-index materials are CaS, CrO₂, ZnS, TiO₂, or SiOₓ. The reflective layer 7 can also be applied in the form of patterns or characters, in particular positive or negative patterns.The embossing of the embossing lacquer 6, for example a diffraction structure in the form of a relief, which is not shown here for the sake of clarity and is located on the side of the embossing lacquer 6 facing away from the substrate 1, can be carried out before or after the application of the reflective layer 7.
[0107] A UV dispersion is applied over the reflective layer 7 and thermally dried (e.g., at 80°C), resulting in a coating 4 that is essentially tack-free at room temperature. This coating, which is essentially tack-free at room temperature, can therefore serve as a protective coating for the metallization. If required, a primer / adhesion promoter layer can also be applied between the reflective layer 7 and the coating 4.
[0108] By applying UV radiation from the direction of the coating, i.e., from the side of the security paper that is essentially transparent to UV radiation, the UV dispersion is cross-linked, resulting in an infusible coating 4. A further coating of a UV-curable dispersion is then applied to this cross-linked UV dispersion layer and thermally dried (e.g., at 80°C). The drying of the UV dispersion results in a coating 2 that is essentially tack-free at room temperature.
[0109] This security element is subsequently applied to a paper substrate 3 by a heat-sealing process under increased pressure and temperature (e.g., at 140°C) to produce the illustrated security paper. The coating 2 can then be pre-crosslinked through the PET carrier film by exposure to UV radiation (e.g., mercury and iron lamps), although pre-crosslinking is not strictly necessary.
[0110] The PET carrier film and, if present, the release liner are then removed. However, the PET carrier film can also remain on the embossing varnish layer 6 as a protective layer. In this case, no release liner is used. Finally, the pre-crosslinked coating 2 is crosslinked through the reflective layer 7 by exposure to UV radiation (e.g., an undoped mercury lamp), so that the coating is ultimately formed in Fig. 6 The security paper shown schematically in cross-section has a paper substrate 3, a two-layer, radiation-crosslinked, infusible coating 2, 4, a reflective layer 7 and an embossed varnish layer 6.
[0111] Crosslinking through a metal layer using UV radiation does not pose a technical problem, as metallizations (especially aluminum) exhibit relatively high transparency, particularly in the UV range. For example, an aluminum metallization (optical density = 2.0) is 5% to 10% transparent to long-wave UV radiation. Furthermore, the embossing lacquer layer 6, in conjunction with the metal layer, provides excellent oxygen exclusion, leading to improved UV crosslinking of the coatings 2 and 4.
[0112] Fig. 7 Figure 1 shows a schematic cross-sectional representation of a security element or security paper according to another embodiment of the invention. To produce the security element or paper, a UV dispersion is applied over the entire surface of a paper substrate 21. The UV dispersion can also be applied to both sides of the substrate 21, so that the substrate 21 is completely enclosed by the coating 22, which is not shown here for clarity. If required, the UV dispersion can also contain rheology additives. The UV dispersion is dried (e.g., at 80°C), resulting in a coating 22 that is essentially tack-free at room temperature. The essentially tack-free coating 22 is then printed with a printing ink 9.
[0113] This causes the UV-curable coating 22 in the upper area 10, facing away from the paper substrate, to be "dissolved", i.e., the printing ink bonds with the coating 22. Then the coating 22 is cross-linked by the action of UV radiation (e.g., Hg and Fe emitters), so that a security element or paper according to the invention is obtained with a paper layer, a now radiation-cross-linked, infusible coating 22, which is printed with the printing ink 9.
[0114] Alternatively, the production of the in Fig. 8 In another embodiment of the invention, a UV dispersion is applied over the entire surface of a paper substrate 21, as shown schematically in cross-section. Here, too, the UV dispersion can be applied to both sides of the substrate 21. The UV dispersion is dried (e.g., at 80°C), resulting in a coating 22 that is essentially tack-free at room temperature. The coating 22 is then cross-linked by exposure to UV radiation (e.g., mercury and iron lamps), so that a security element or paper according to the invention with a radiation-cross-linked, infusible coating 22 is obtained. The radiation-cross-linked coating 22 can then be printed with printing ink 9, whereby the ink adhesion and the dirt-repellent properties can be adjusted by the degree of cross-linking of the coating 22.
[0115] Fig. 9 Figure 1 shows a schematic cross-sectional representation of a security element designed as a transfer element according to another embodiment of the invention. To produce the security element, a coating of UV dispersion is applied to a substrate 1, for example, a PET carrier film. The UV dispersion is thermally dried (e.g., at 80°C), resulting in a coating 2 that is essentially tack-free at room temperature. Optionally, a release layer 5 can be applied between the PET carrier film and the coating 2.
[0116] A diffraction pattern 11 can be embossed into coating 2. In this case, the UV-curable dispersion is used as an embossing lacquer. During or after this process, coating 2 is cured by exposure to UV radiation. The exposure is carried out through a mask. As shown in the Fig. 10 As can be seen, UV exposure is only carried out at the points 12 where a motif in the form of a diffraction structure 11 has previously been embossed. In this way, the patches to be transferred in a subsequent step are exposed, but the areas in between are not. The intermediate areas 13 therefore remain soft and meltable, enabling sharp-edged melting when transferring the security element to a substrate. The exposed areas 12, on the other hand, remain hard even during the transfer process, and their embossed structures are retained. Optionally, the coating 2, including the diffraction structures 11, or even just the areas with a diffraction structure, can be coated with a metal layer or a high-refractive-index layer, which is not shown here for the sake of clarity. The metal layer orFurthermore, the high-refractive-index layer can be applied in the form of patterns or symbols, in particular positive or negative patterns.
[0117] Fig. 11 The diagram shows a schematic cross-section of a security paper featuring the security element of Fig. 10 is equipped. After the in Fig. 10 The patch is applied to a carrier substrate 3 using a heat-seal adhesive 14. This cross-linking of the coating 2, caused by UV exposure at the points 12 of the coating 2 where a motif in the form of a diffraction structure 11 was previously embossed, is achieved by means of the illustration. This cross-linking is achieved by means of UV exposure. Due to the UV exposure being limited to the points 12, the intermediate areas 13 remain soft and meltable, thus enabling a sharp-edged melting process when the security element is transferred using a hot die. The exposed areas 12, on the other hand, remain hard even during the transfer process, and their embossed structures are preserved.
[0118] However, it is also possible to use a coating of UV-curable dispersion instead of the heat-seal adhesive. It should be noted, however, that the UV-curable dispersion is only transferred and cross-linked by UV radiation after the removal of the uncured intermediate areas 13.
[0119] Fig. 12 Figure 15 shows a security document 15, for example a banknote, which is equipped with a continuous opening 16. The opening 16 is preferably manufactured by papermaking or die-cut. The machine production of such window openings 16 is described in DE 101 63 381 A1.
[0120] Fig. 13 shows a cross-section of the in Fig. 12 The depicted security document 15 differs in that the opening 16 is closed by a security element according to the invention. The security element comprises a substrate 1 and a coating 2 that is essentially tack-free at room temperature.
[0121] The safety element is preferably arranged in a recess 17 surrounding the opening 16. The recess 17 can be created by subsequent calendering of the paper web, i.e., by compressing the paper fibers. Alternatively, the recess 17 can also be created by actually reducing the paper thickness in this area. This is most easily achieved directly during the production of the paper web by making the sheet formation in this area thinner through appropriate shaping of the wire.
[0122] In another embodiment not shown, the security element consists of a substrate and a coating that is essentially tack-free at room temperature. To produce the security element, for example, a cationic radiation-curing resin, in particular an epoxy-modified vinyl copolymer (e.g., UCAR VERR-40, The Dow Chemical Company), which is provided with a photoinitiator suitable for cationic radiation curing, is applied to the substrate, for example, a plastic film, in particular a PET or OPP film. The cationic radiation-curing resin is dried (e.g., at 80°C), resulting in a coating that is essentially tack-free at room temperature.
[0123] To produce security paper equipped with the security element described above, the security element is transferred to a substrate, e.g., paper, by a heat-sealing process under increased pressure and temperature (e.g., at 140°C). This process initiates the thermal cross-linking. Subsequently, the cationically radiation-curable coating is cross-linked by exposure to UV radiation (e.g., mercury and iron lamps), resulting in a security paper with a radiation-cross-linked, infusible coating and a covering substrate, e.g., a plastic film.
[0124] Alternatively, the coating can also be cross-linked purely thermally. For this, the security element is transferred to a substrate, such as paper, using a heat-sealing process under increased pressure and temperature (e.g., 140°C to 160°C). The thermal cross-linking occurs during the heat-sealing process. It is obvious that this method eliminates the need for a photoinitiator.
[0125] Cationic radiation curing, unlike radical radiation curing, is a slower process that continues even after irradiation has ceased. While radicals are neutralized quickly, cationic radiation curing releases an acid that catalyzes the crosslinking reaction within the coating. Therefore, in another embodiment of the above example, the cationically radiation-curable coating can be exposed to short-wave radiation (UV or short-wave blue radiation) from the coating side immediately before the application of the safety element. Either conventional UV lamps (doped or undoped) or, preferably, UV LEDs can be used as the radiation source. In addition to positive safety-related aspects, UV LEDs also offer technical advantages, such as lower heat input and lower energy consumption.Exposure from the coating side is advantageous because it avoids UV radiation on the substrate, e.g., paper, and results in less UV exposure for the security element material. The exposure initiates the crosslinking reaction. At the time of application to the substrate, this reaction has not yet progressed to the point where melting of the coating would be hindered, due to the short timeframe. However, since the reaction continues spontaneously without further intervention, the security paper with the security element exhibits the required resistance properties.
Claims
1. Security element for documents of value or the like, having a substrate (1, 21) which has been coated with a heat-sealing adhesive (2, 22) that is non-tacky at room temperature and suitable for applying the security element to a substrate of a document of value, wherein the heat-sealing adhesive (2, 22) contains a radiation-crosslinkable component, characterized in that the heat-sealing adhesive contains a reactive diluent.
2. Security element according to Claim 1, wherein the reactive diluent is a low molecular weight compound having a molecular molar mass M < 1000 g / mol and preferably is selected from TMP(EO)xTA and DPHA.
3. Security element according to Claim 1 or 2, wherein the heat-sealing adhesive (2, 22) additionally contains a plasticizer, which preferably has a melting point in a range from 50°C to 120°C.
4. Security element according to Claim 3, wherein the plasticizer is selected from the group consisting of triphenyl phosphate, pentaerythritol tetrabenzoate, cyclohexanedimethanol dibenzoate, sucrose benzoate, and a mixture of two or more of the aforementioned elements.
5. Security element according to Claim 3 or 4, wherein the plasticizer is present in the heat-sealing adhesive (2, 22) in a proportion by weight in a range from 1% to 30%, preferably 2% to 10%, based on the solids.
6. Security element according to any of Claims 1 to 5, wherein the heat-sealing adhesive (2, 22) that is non-tacky at room temperature and suitable for applying the security element to a substrate of a document of value is present in an at least physically dried state.
7. Security element according to any of Claims 1 to 6, wherein the substrate (1, 21) is a flat substrate (1, 21) having two opposite main surfaces, wherein at least one main surface of the substrate (1, 21) is at least partly provided with the heat-sealing adhesive (2, 22) that is non-tacky at room temperature and suitable for applying the security element to a substrate of a document of value.
8. Security element according to at least one of Claims 1 to 7, wherein the heat-sealing adhesive (2, 22) that is non-tacky at room temperature and suitable for applying the security element to a substrate of a document of value is obtainable by means of application of a solution, emulsion or dispersion.
9. Security element according to Claim 8, wherein the heat-sealing adhesive (2, 22) that is non-tacky at room temperature and suitable for applying the security element to a substrate of a document of value is obtainable by means of application of an aqueous dispersion.
10. Security element according to Claim 8, wherein the heat-sealing adhesive (2, 22) that is non-tacky at room temperature and suitable for applying the security element to a substrate of a document of value is obtainable by means of application of a solution based on an organic solvent, the organic solvent preferably comprising at least butyl acetate, propyl acetate or ethyl acetate, more preferably in a proportion by weight in a range from 30% to 90%, especially preferably 40% to 75%.
11. Security element according to Claim 10, wherein the heat-sealing adhesive (2, 22) additionally comprises a prepolymer that is non-tacky at room temperature after physical drying, contains on average at least two reactive groups and has a molecular weight of at least 600 g / mol, preferably in a proportion by weight in a range from 8% to 65%.
12. Security element according to Claim 9, wherein the dispersion is selected from the group consisting of aliphatic polyurethane dispersions, aromatic polyurethane dispersions, acrylates, anionic acrylate-modified polyurethane dispersions, polyurethane-polyether acrylates, and mixtures of two or more of the aforementioned elements.
13. Security element according to any of Claims 1 to 12, wherein the heat-sealing adhesive (2, 22) comprises a cationically radiation-curing resin.
14. Security element according to any of Claims 1 to 13, wherein the radiation-crosslinkable component is crosslinkable by ultraviolet radiation or electron beam radiation.
15. Security element according to any of Claims 1 to 14, wherein the heat-sealing adhesive (2, 22) contains a photoinitiator.
16. Security element according to any of Claims 1 to 15, wherein the substrate (1, 21) is a transparent plastics film.
17. Document of value, in particular a banknote, comprising a security element according to any of Claims 1 to 16.
18. Method for producing a security element according to any of Claims 1 to 16, comprising the step of applying to a substrate (1, 21) a heat-sealing adhesive (2, 22) that is non-tacky at room temperature and suitable for applying the security element to a substrate of a document of value, wherein the heat-sealing adhesive (2, 22) contains a radiation-crosslinkable component and a reactive diluent.
19. Method for producing a document of value according to Claim 17, comprising the step of equipping the substrate of the document of value, in particular a paper substrate, with the security element according to any of Claims 1 to 16.
20. Method according to Claim 19, wherein the security element is applied to the substrate (3) of the document of value at elevated pressure and elevated temperature and the heat-sealing adhesive (2, 22) that is non-tacky at room temperature is then at least precrosslinked by means of radiation.