VPO catalytic converter with improved selectivity and stability, and method for its manufacture.

DE502023000320D1Active Publication Date: 2024-12-05CLARIANT INT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502023000320
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-21
Filing Date
2023-10-19
Publication Date
2024-12-05
Estimated Expiration
2043-10-19

AI Technical Summary

Technical Problem

VPO catalysts used for the oxidation of butane to maleic anhydride have low intrinsic activity and high costs due to expensive starting materials, requiring large amounts and needing improvements in activity, selectivity, and mechanical stability.

Method used

A VPO catalyst in the form of a shaped body with 0.05% to 7.0% Zn, primarily as ZnO, exhibiting specific infrared and X-ray diffraction characteristics, and having enhanced mechanical strength through the addition of ZnO, which stabilizes the catalyst particles and improves catalytic performance.

Benefits of technology

The VPO catalyst with ZnO content shows increased mechanical strength and catalytic performance, including improved selectivity and stability, addressing the limitations of existing VPO catalysts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a VPO catalyst in the form of a shaped body for the oxidation of hydrocarbons with molecular oxygen, in particular for the oxidation of butane to maleic anhydride with molecular oxygen, wherein the VPO catalyst contains between 0.05 wt.% and 7.0 wt.%.-% Zn, which is partially present as ZnO and, when infrared spectroscopy is performed in transmission, exhibits a first absorption band with a maximum between 790 cm⁻¹ and 810 cm⁻¹ and optionally a second absorption band with a maximum between 820 cm⁻¹ and 840 cm⁻¹, characterized in that only the first absorption band is present or the strength of the first absorption band is greater than the strength of the second absorption band, and that the VPO catalyst, when examined by powder X-ray diffraction, exhibits reflections at 31.7° to 31.9°, 34.3° to 34.5°, and 36.2° to 36.4°, when measured with a Bruker AXS D4 Endeavor with Cu-Kα radiation and a Lynxeye detector, wherein the diffractrograms are measured in an angular range 2θ from 5° to 50° with a step size of 0.02° at a recording time of 1.5 s per step with a fixed divergence aperture of 0.3°.

[0002] The strength of the absorption bands is determined by first drawing a straight line that touches the spectrum tangentially to the left and right below the band in question. A second straight line is then drawn from the band's maximum in the direction of constant wavelength and decreasing absorption, and the intersection of the two lines is determined. The strength of the absorption band is defined as the length between the maximum and the intersection point. Lateral compressive strength is measured using a Zwick Z0.5 instrument according to ASTM D4179 at a constant force rate of 20.0 N / s. One hundred tablets are individually placed with the cylinder axis parallel to the measuring jaw surface and measured to determine an average breaking force, which represents the lateral compressive strength.

[0003] The invention also relates to a method for producing a VPO catalyst according to the invention, comprising the steps: a) Production of a catalyst precursor containing vanadyl hydrogen phosphate, b) Forming the catalyst precursor into shaped bodies, c) Activating the shaped bodies to form a VPO phase, characterized in that, after step a), ZnO is mixed with the catalyst precursor.

[0004] Maleic anhydride is a chemical intermediate of great economic importance. It is used, for example, in the production of alkyd and polyester resins, either alone or in combination with other acids. Furthermore, it is a versatile intermediate for chemical synthesis, for instance, in the synthesis of γ-butyrolactone, tetrahydrofuran, and 1,4-butanediol, which in turn can be used as solvents or further processed into polymers such as polytetrahydrofuran or polyvinylpyrrolidone.

[0005] Maleic anhydride is typically produced by the partial oxidation of n-butane in the gas phase with molecular oxygen or with a gas containing molecular oxygen in the presence of a vanadium phosphorus oxide (VPO) catalyst containing vanadyl pyrophosphate (VPP). In its pure form, vanadyl pyrophosphate has a vanadium oxidation state of +4 and is particularly suitable for the production of maleic anhydride from unbranched saturated or unsaturated hydrocarbons with at least four carbon atoms. Both fixed-bed and fluidized-bed reactors are used.

[0006] VPO catalysts exhibit only low intrinsic activity in the reaction of n-butane to maleic anhydride. Therefore, a large amount of catalyst is required for sufficient conversion. Furthermore, VPO catalysts are among the most expensive non-precious metal catalysts, primarily due to the high cost of their starting materials. Consequently, the challenge lies in improving the catalytic performance (activity and selectivity), as well as the lifetime and mechanical stability of such catalysts. It is known from the prior art that the performance of VPO catalysts can be improved by adding foreign elements to the vanadium phosphorus oxide phase (VPO phase), such as molybdenum (Mo promoter or Mo doping).

[0007] US 5,929,256 discloses the synthesis of an active molybdenum-modified vanadium-phosphorus catalyst for the production of maleic anhydride. In this process, a compound containing substantial amounts of pentavalent vanadium is reacted with a compound containing pentavalent phosphorus in an alcoholic medium suitable for reducing the vanadium to an oxidation state below 5. Molybdenum is incorporated into the reaction product, forming a solid, molybdenum-modified precursor composition. The alcohol is removed to obtain a dried, solid, molybdenum-modified precursor composition. Molds containing the dried, solid, molybdenum-modified precursor compound are formed. The dried and formed molybdenum-modified precursor compositions are activated to convert them into the active catalyst.

[0008] US 5,070,060 discloses an improvement of an oxidation catalyst used for the partial oxidation of n-butane containing vanadium and phosphorus, zinc, and lithium mixed oxides, comprising the addition of a molybdenum compound modifying agent in an amount of about 0.005 to 0.025 / 1 Mo / V to the catalyst during the reaction of the reduced vanadium compound with concentrated phosphoric acid. The addition of Mo produces a catalyst that is very stable, a more active system, and has a longer shelf life than the unmodified catalyst.

[0009] US 3,980,585 discloses a catalyst complex suitable for the gas-phase conversion of ordinary C4 hydrocarbons to maleic anhydride, comprising the components vanadium, phosphorus and copper, as well as one of the elements selected from the group Te, Zr, Ni, Ce, W, Pd, Ag, Mn, Cr, Zn, Mo, Re, Sm, La, Hf, Ta, Th, Co, U and Sn, preferably with an alkali metal or an alkaline earth metal.

[0010] US 4,056,487 discloses a composition suitable for the partial oxidation of alkanes to the corresponding anhydrides, for example, of ordinary C4 hydrocarbons which are converted to maleic anhydride in the gas phase, comprising the components vanadium, phosphorus and oxygen, Nb, Cu, Mo, Ni, Co and Cr. Compositions containing one or more elements from Ce, Nd, Ba, Hf, U, Ru, Re, Li or Mg are preferred.

[0011] US 4,515,904 discloses a process for the production of a phosphorus-vanadium catalyst and a phosphorus-vanadium-co-metal catalyst for use in the production of maleic anhydride from butane, the process comprising reacting a vanadium compound in an organic ether solvent having about 2 to about 10 carbon atoms with a phosphorus halide at a temperature of about 0 °C to about 200 °C in the presence of water or an aliphatic alcohol having about 1 to about 8 carbon atoms; removing the solvent; and activating the catalyst by adding butane or another hydrocarbon starting material and a phosphorus compound at a temperature of about 300 °C to about 500 °C.

[0012] US 5,158,923 discloses an improvement of an oxidation catalyst used for the partial oxidation of n-butane containing vanadium and phosphorus, zinc, and lithium mixed oxides, comprising the addition of a molybdenum compound modifying agent in an amount of about 0.005 to 0.025 Mo / V to the catalyst during the digestion of the reduced vanadium compound by concentrated phosphoric acid. The addition of Mo produces a catalyst that is very stable, a more active system, and has a longer shelf life than the unmodified catalyst.

[0013] US 5,262,548 discloses an improvement of an oxidation catalyst used for the partial oxidation of n-butane containing vanadium and phosphorus, zinc, and lithium mixed oxides, comprising the addition of a molybdenum compound modifying agent in an amount of about 0.005 to 0.025 Mo / V to the catalyst during the digestion of the reduced vanadium compound by concentrated phosphoric acid. The addition of Mo produces a catalyst that is a very stable active system and has a longer lifetime than the unmodified catalyst.

[0014] WO 2013062919 A1 discloses a process for producing a promoted VPO catalyst, wherein the catalyst comprises the mixed oxides of vanadium and phosphorus and wherein the catalyst is promoted with at least one of niobium, cobalt, iron, zinc, molybdenum or titanium, the process comprising the steps of: (i) producing a VPO catalyst comprising vanadyl pyrophosphate as the main component and containing less than 5 wt% vanadyl phosphate, (ii) contacting the VPO catalyst with a solution comprising a compound as a metal source with at least one metal selected from the group consisting of niobium, cobalt, iron, zinc, molybdenum or titanium to form a metal-impregnated VPO catalyst, and (iii) drying the metal-impregnated VPO catalyst to form the promoted VPO catalyst. In one embodiment, a niobium-activated VPO catalyst is produced.

[0015] US 6,407,030 B1 discloses a process for the preparation of a catalyst that can be used for the synthesis of maleic anhydride by the oxidation of saturated and / or unsaturated C4 hydrocarbons. A vanadium(V) compound is reacted with a mixture of phosphonic and phosphoric acid in a specific ratio in a solvent mixture comprising a structure-forming agent and an energizing agent, wherein the water of reaction is distilled off together with the energizing agent and the resulting precursor is subjected to calcination.

[0016] US 4,132,670 A discloses the preparation of a crystalline vanadium(IV) phosphate composition with an intrinsic surface area of ​​more than 10 m² / g by the reaction of orthophosphoric acid with a vanadium(IV) oxide compound. The vanadium compound is suspended in a suitable organic medium containing hydroxyl groups, for example, isobutanol, and brought into contact with the acid at a temperature in the range of 20 °C to 210 °C until the conversion is complete.

[0017] US 4,382,876 discloses a process for the preparation of catalysts for the gas-phase oxidation of saturated or unsaturated hydrocarbons to maleic anhydride, comprising the steps of: (a) mixing a vanadium compound containing pentavalent vanadium with orthophosphoric acid in an alcohol from the series of monovalent lower aliphatic alcohols having 2 to 8 carbon atoms, optionally in the presence of promoters and a reducing agent combination of H₃PO₃ and alcohol, wherein the sum of H₃PO₃ and H₃PO₄ is controlled such that a P to V atom ratio of 1.0 to 1.2 is achieved, and wherein the H₃PO₃ is used in such substoichiometric amounts as are sufficient to reduce the vanadium to an oxidation state of only 4.2 to 4.4, and wherein the reducing agent combination is subsequently used to further reduce the vanadium to an oxidation state between 3.9 and 4.0. reduce(a) Any water present is distilled off by heating as an azeotrope with the alcohol; (b) Addition of titanium dioxide obtained by high-temperature pyrolysis of titanium tetrahalide and optionally additional promoters Ni, Fe, Li, Mg; (c) Formation of a precipitated catalyst in a known manner; and (d) Activation of the catalyst in an oxidation reactor at temperatures of about 450 °C to 510 °C for about 12 to 72 hours in the presence of an air-hydrocarbon stream.

[0018] WO 9529006 A1 discloses a process for the production of oxidation catalysts containing vanadium-phosphorus mixed oxides, comprising contacting a phosphorus compound with a vanadium compound in an organic solvent under conditions that allow the production, recovery and drying of the precursor and the calcination of the precursor under an atmosphere containing air, steam or inert gas or a mixture thereof at a temperature between 350 °C and 550 °C during the time required to obtain active catalysts, and using the catalysts for the production of maleic anhydride by oxidation of aliphatic hydrocarbons.

[0019] US 5,185,455 discloses the improvement of a process for the production of maleic anhydride by catalytic oxidation of n-butane in the presence of trimethyl phosphate over a fixed-bed catalyst of vanadium phosphorus oxide in a tubular reactor.The trimethyl phosphate content of the gas entering the reactor is in a range between approximately 0.9 N and approximately 1.1 N, where N is a normative concentration of trimethyl phosphate in ppm, determined by the following relationship: N = 5 × C₄ + 6 × (H₂O - 2.4) + 0.75 × - (CONV - c) + (SV / (25 × P in )), where: C₄ is the mole percent of n-butane in the gas entering the reactor; H₂O is the mole percent of moisture in the gas entering the reactor; CONV = percent butane conversion in the reactor; SV = hourly gas head velocity of the gas at the reactor inlet, reduced to a pressure of one atmosphere and 60 °F; P in = the pressure at the reactor inlet (psig); and c = 84 × 0.05 [(SV × C₄) / P in ]; Regardless of the calculation of N, the trimethyl phosphate content is at least approximately one ppm.

[0020] US 5,280,003 discloses an improvement of an oxidation catalyst used for the partial oxidation of n-butane, containing mixed oxides of vanadium and phosphorus, zinc, lithium, and molybdenum, comprising its preparation by carrying out the crystallization step under static conditions, which allow for more uniform conditions for crystal growth. The static conditions are maintained by heating the solvent under reflux during the crystallization period.

[0021] US 4,251,390 discloses an improvement of an oxidation catalyst used for the partial oxidation of n-butane, containing vanadium and mixed oxides of phosphorus, characterized in that a zinc compound in an amount of 0.15 to 0.001 Zn / V is added to the catalyst during the reaction of the reduced vanadium portion with concentrated phosphoric acid. The addition of zinc produces a catalyst that is more readily activated and very stable against heating of the reaction system. Small amounts of lithium and silicon compounds also have additional desirable catalytic effects without diminishing the advantage of the zinc compound.

[0022] DE 10 2014 004786 A1 relates to a catalyst containing a vanadium phosphorus oxide and an alkali metal, wherein the weight fraction of alkali metal in the vanadium phosphorus oxide is in the range of 10 to 400 ppm, based on the total weight of the vanadium phosphorus oxide, a process for its production and the use of the catalyst for the gas-phase oxidation of hydrocarbons, in particular for the production of maleic anhydride.

[0023] To produce VPO catalysts containing a VPP phase, a reduction of vanadium pentoxide (V₂O₅) is typically carried out in the simultaneous presence of phosphoric acid in an organic alcoholic solvent with benzyl alcohol as the reducing agent, yielding vanadyl hydrogen phosphate (VHP) in addition to benzaldehyde. The resulting redox reaction (the "reduction"), in which vanadium with oxidation state V (V(V)) reacts to form the VHP phase, in which vanadyl species (VO₂⁺) are present with vanadium in oxidation state IV (V(IV)), is: (1) V₂O₅ + 2H₃PO₄ + Ph-CH₂-OH → 2VOHPO₄ * ½H₂O + Ph-CHO + 2H₂O

[0024] In a subsequent activation step, the VHP phase is converted to the vanadyl pyrophosphate phase by the action of heat, with the elimination of water. (2) 2VOHPO₄ * ½H₂O → (VO)₂P₂O₇ + ½H₂O

[0025] In the catalytic conversion of butane to maleic anhydride using VPO catalysts, a challenge arises from the fact that the process must be operated in a pore diffusion-limited regime. Here, the porosity directly influences the catalytic yield. Therefore, care must be taken to ensure that the pore structure is not negatively affected during the shaping process (e.g., by tableting). This, however, results in a reduction in the mechanical stability of the tablets. This stability must be sufficient to allow the tablets to survive the filling process (falling into an approximately 6-meter-long reaction tube) intact. Otherwise, the smaller fragments would cause excessive back pressure in the process, leading to high compressor costs and / or reduced throughput. A key technical challenge, therefore, is to increase the mechanical strength of the tablets without negatively impacting their pore structure.At the same time, there is a need for VPO catalysts with improved performance, i.e., improved activity, selectivity and stability.

[0026] The object of the present invention was therefore to provide an improved VPO catalyst for the gas phase oxidation of hydrocarbons, in particular for the production of maleic anhydride, which, compared to previously used catalysts, has higher catalytic performance, in particular improved selectivity and at the same time significantly improved mechanical strength.

[0027] The problem is solved by a VPO catalyst in the form of a shaped body for the oxidation of hydrocarbons with molecular oxygen, in particular for the oxidation of butane to maleic anhydride with molecular oxygen, wherein the VPO catalyst is between 0.05 wt.% and 7.0 wt.%.-% Zn, which is partially present as ZnO and, when infrared spectroscopy is performed in transmission, exhibits a first absorption band with a maximum between 790 cm⁻¹ and 810 cm⁻¹ and optionally a second absorption band with a maximum between 820 cm⁻¹ and 840 cm⁻¹, characterized in that only the first absorption band is present or the strength of the first absorption band is greater than the strength of the second absorption band, and that the VPO catalyst, when examined by powder X-ray diffraction, exhibits reflections at 31.7° to 31.9°, 34.3° to 34.5° and 36.2° to 36.4°, when measured with a Bruker AXS D4 Endeavor with Cu-Kα radiation and a Lynxeye detector, wherein the diffractrograms are in an angular range 2θ of 5 ° to 50° with a step size of 0.02° at a recording time of 1.5 s per step with a fixed divergence aperture of 0.3°.

[0028] The strength of the absorption band is determined by first drawing a straight line that touches the spectrum tangentially to the left and right below the band in question, then drawing a second straight line from the band's maximum in the direction of constant wavelength and decreasing absorption, and determining the intersection point of the two lines. The strength of the absorption band is defined as the length between the maximum and the intersection point. Preferably, the ratio of the strength of the first absorption band to the strength of the second absorption band is greater than 1.1, and more preferably greater than 2.

[0029] The molded bodies according to the invention have a lateral compressive strength of more than 25 N, preferably between 25 N and 200 N, wherein the lateral compressive strength is measured with a Zwick Z0.5 device using the standard ASTM D4179 with a constant force rate of 20.0 N / s, wherein 100 tablets are each individually placed with the cylinder axis parallel to the measuring jaw surface and measured to determine an average breaking force which represents the lateral compressive strength.

[0030] The VPO catalyst according to the invention, when examined by powder X-ray diffractometry using Cu-Kα radiation, exhibits reflections at 31.7° to 31.9°, 34.3° to 34.5° and 36.2° to 36.4°.

[0031] The VPO catalyst according to the invention comprises the VPO phase, or consists of, or consists substantially of, the VPO phase. For example, the VPO catalyst according to the invention comprises the VPO phase with a content of more than 70 wt.%, preferably more than 80 wt.%, and more preferably more than 90 wt.%, based on the total weight of the VPO catalyst. Furthermore, the VPO catalyst can comprise VPP, dopants, and unreacted oxides of the starting materials, such as vanadium pentoxide or phosphorus oxide.

[0032] The VPO catalyst according to the invention can optionally contain, for example, between 0.1 wt.% and 1 wt.%, preferably between 0.4 wt.% and 0.7 wt.% Mo, based on the total weight of the VPO catalyst.

[0033] The VPO catalyst according to the invention can also contain alkali metals such as Na and K, preferably 80 to 300 ppm alkali metal. Furthermore, the VPO catalyst according to the invention can also contain carbon, e.g., in the form of graphite, e.g., in an amount of 3 wt.% to 5 wt.%, based on the total weight of the catalyst. The graphite present serves, e.g., as a tableting aid.

[0034] The VPO catalyst according to the invention contains ZnO, but may also contain other Zn compounds. The Zn content resulting from the presence of ZnO and any other Zn compounds must be between 0.05 wt.% and 7.0 wt.%, preferably between 0.1 wt.% and 6.0 wt.%, more preferably between 0.2 wt.% and 4.0 wt.%, and most preferably between 0.7 wt.% and 3.0 wt.% Zn in each case, based on the total weight of the catalyst.

[0035] The VPO catalyst preferably has the following elemental composition: 0.05 wt.% to 7 wt.% Zn, 0 wt.% to 0.7 wt.% Mo, 26 wt.% to 31 wt.% V, 17 wt.% to 21 wt.% P, 3 wt.% to 5 wt.% C, the remainder oxygen, each based on the total weight of the VPO catalyst.

[0036] The VPO catalyst according to the invention contains ZnO, and if the content of these two phases is sufficiently high, the catalyst exhibits reflections typical of the ZnO phase in an XRD powder diffractogram recorded using Cu-Kα radiation. In particular, sharp reflections are detected at 31.7° to 31.9°, 34.3° to 34.5°, and 36.2° to 36.4°.

[0037] According to the invention, the presence of ZnO stabilizes the catalyst particles, resulting in higher mechanical strength compared to their strength without ZnO. The presence of ZnO also improves the catalytic performance (i.e., activity, selectivity, and stability) of the catalyst particles, particularly increasing their selectivity.

[0038] The VPO catalyst according to the invention is in the form of a molded body. The shape of the molded body can be designed differently depending on the desired contact time, flow rate, and back pressure during the catalytic reaction. The term "VPO catalyst in the form of a molded body" refers to molded bodies produced by a molding step such as tableting. A plurality of the molded bodies according to the invention form a layer or a catalyst bed in the tube bundle reactor, through which the reactants butane, in particular n-butane, and air are passed.

[0039] According to the invention, the molded body should not fall below a minimum size, which results, for example, from the fact that the molded body must not fit into an imaginary cube of 3 mm × 3 mm × 3 mm without exceeding its boundaries at any point.

[0040] For example, the shaped body according to the invention can be in a conventional cylindrical shape. The cylinder then has a height (length along the cylinder axis) of 3 mm to 8 mm and a substantially round base with a diameter of 3 mm to 8 mm. Preferably, the cylinder has a central axial opening, which can, for example, have a diameter of 1 mm to 3 mm.

[0041] For example, the molded body according to the invention can have a height of 4.7 mm, an outer diameter of 4.7 mm, and a central axial opening with a diameter of 1.3 mm. This molded body then has a geometric surface area of ​​1.2 cm², a volume of 0.075 cm³, and a mass of 0.12 g. When a plurality of these molded bodies are filled into a 21 mm reactor, a filling density of 0.85 g / cm³ to 0.89 g / cm³ is obtained.

[0042] For example, the molded bodies according to the invention can have a height of 5.6 mm, an outer diameter of 5.5 mm, and a mean axial opening with a diameter of 2.3 mm. These molded bodies then have a geometric surface area of ​​1.77 cm², a volume of 0.111 cm³, and a mass of 0.18 g. When a plurality of these molded bodies are filled into a 21 mm reactor, a filling density of 0.72 g / cm³ to 0.76 g / cm³ is obtained.

[0043] Preferred shaped bodies for use in the reactor concept according to the invention are those described in EP 2643086 A1. The preferred double alpha shape is characterized in particular in that each individual shaped body is designed as a cylinder with an outer base [1], a cylindrical surface [2], a cylindrical axis and at least one continuous opening [3] extending parallel to the cylindrical axis, and the outer base [1] of the cylinder has at least four lobes [4a, 4b, 4c, 4d], wherein a geometric base body enclosing the shaped bodies is a prism having a prism base with a length and a width, the length being greater than the width, and wherein the lobes [4a, 4b, 4c, 4d] are enclosed by prism vertices of the prism base ( Figure 9 ).

[0044] A preferred molded body is a double alpha shape with a height (length along the cylinder axis) of 3 mm to 8 mm, a length of 5 mm to 9 mm, a width of 4 mm to 8 mm, and an inner hole diameter of 1 mm to 4 mm. For example, preferred molded bodies are those with a double alpha shape, a height of 5.6 mm, a length of 6.7 mm, a width of 5.8 mm, and an inner hole diameter of 2.1 mm. These catalyst molded bodies have a geometric surface area of ​​2.37 cm², a volume of 0.154 cm³, and a mass of 0.24 g. When filled into a 21 mm reactor, a filling density of 0.60 g / cm³ to 0.62 g / cm³ is obtained.

[0045] The VPO catalyst or the molded body according to the invention preferably has a lateral pressure strength of more than 25 N, preferably between 25 N and 200 N. A lateral pressure strength of more than 30 N to 150 N is particularly preferred, and even more preferably more than 35 N to 100 N.

[0046] The VPO catalyst or the cylindrical body according to the invention has a lateral pressure resistance of more than 25 N, preferably between 25 N and 50 N. A lateral pressure resistance of more than 30 N to 45 N is particularly preferred, and even more preferably more than 35 N to 40 N.

[0047] The VPO catalyst or the molded body according to the invention in double alpha shape has a lateral compressive strength of more than 50 N, preferably between 50 N and 200 N. A lateral compressive strength of more than 100 N to 170 N is particularly preferred, and even more preferably more than 120 N to 150 N.

[0048] The invention further relates to a method for producing a VPO catalyst according to the invention, comprising the steps: a) Production of a catalyst precursor containing vanadyl hydrogen phosphate, b) Forming the catalyst precursor into shaped bodies, c) Activating the shaped bodies to form a VPO phase, characterized in that, after step a), ZnO is mixed with the catalyst precursor.

[0049] In process step a), a catalyst precursor containing vanadyl hydrogen phosphate is prepared in a generally known manner. Typically, in a reaction mixture, a V(V) compound in solution is reduced in a reduction step using a reducing agent in the presence of a P(V) compound, optionally a Mo compound. For example, the reaction mixture can consist of 45 wt% to 90 wt% solvent, 5 wt% to 15 wt% reducing agent, 5 wt% to 15 wt% V(V) compound, up to 1 wt% Mo compound, and between 5 wt% and 25 wt% P(V) compound. More specifically, for example, 60 wt.% to 70 wt.% isobutanol, 5 wt.% to 15 wt.% benzyl alcohol, 5 wt.% to 15 wt.% vanadium pentoxide, 0.05 wt.% to 0.2 wt.% (NH 4 ) 2 Mo 2 O 7 and 10 wt.% to 20 wt.% phosphoric acid, each based on the total weight of the reaction mixture, can be submitted as a reaction mixture.

[0050] The V(V) compound used as a starting material in the reaction mixture for the preparation of vanadyl hydrogen phosphate is a compound containing vanadium in the V oxidation state and is preferably V₂O₅. The P(V) compound used as a starting material in the reaction mixture for the preparation of vanadyl hydrogen phosphate is a compound containing phosphorus in the V oxidation state and is preferably phosphoric acid or a phosphate salt, such as Na₃PO₄. If phosphoric acid (H₃PO₄) is used, it is preferably anhydrous (100% phosphoric acid) or phosphoric acid containing only small amounts of water, i.e., phosphoric acid with a concentration of 98 to 100%, preferably 99 to 100% (the value refers to the percentage by weight of pure phosphoric acid in relation to the weight of the water-phosphoric acid mixture, as is usually stated).Alternatively, in the preparation of the reaction mixture for the production of vanadyl hydrogen phosphate, phosphoric acid with a concentration of more than 100% can be used, which reacts immediately with any water that may be present in the reaction mixture at the beginning to form phosphoric acid with a concentration of 98 to 100%, preferably 99 to 100%, preferably 100%, so that no phosphoric acid with a concentration of more than 100% is present in the reaction mixture and at the same time no more than 0.2 wt% water, based on the weight of the reaction mixture, remains in the reaction mixture.

[0051] The Mo compound, which can optionally be used as a starting material in the reaction mixture for the production of vanadyl hydrogen phosphate, is any compound containing molybdenum, for example molybdenum trioxide, ammonium heptamolybdate ((NH₄)₆Mo₇O₂₄)*4H₂O), ammonium paramolybdate ((NH₄)₆Mo₇O₂*4H₂O), metamolybdate, molybdic acid (H₂MoO₄), and their salts such as (NH₄)₂MoO₄, Na₂MoO₄, K₂MoO₄, or (NH₄)₂Mo₂O₇.

[0052] The reducing agent present in the reaction mixture for the preparation of vanadyl hydrogen phosphate can be any reducing agent capable of reducing the V(V) compound to yield at least some vanadyl hydrogen phosphate. Preferably, the reducing agent is an organic reducing agent, such as ethanol, isobutanol, or an aromatic alcohol, including in particular benzyl alcohol.

[0053] The solvent present in the reaction mixture for the preparation of the vanadyl hydrogen phosphate is preferably an alcohol, particularly preferably a high-boiling aliphatic alcohol, especially isobutanol, alternatively ethanol or isopropanol.

[0054] The starting materials are provided in a suitable reaction vessel to carry out the reduction step and obtain the vanadyl hydrogen phosphate catalyst precursor. The reaction mixture is heated above room temperature, for example, to a temperature of 100 °C. After the reduction is preferably carried out in a reflux step with stirring, the reaction vessel preferably includes a reflux condenser and a device for stirring the reaction mixture. Optionally, the reaction vessel is equipped with a device that allows the water produced during the reduction to be removed from the reaction mixture, i.e., a water separator, such as a Dean Stark trap.

[0055] The reduction to vanadyl hydrogen phosphate preferably takes place under reflux at atmospheric pressure, with the temperature being increased depending on the boiling point of the solvent used. Preferably, only a single reflux step is carried out in the process according to the invention. The catalyst precursor preferably contains vanadyl hydrogen phosphate as the main phase or can even consist essentially of a vanadyl hydrogen phosphate phase. The molybdenum that may also be present in the catalyst precursor can be present as a dopant of the vanadyl hydrogen phosphate phase, whereby molybdenum doping means that the molybdenum is either incorporated into the vanadyl hydrogen phosphate phase or is present on its surface. In addition to the vanadyl hydrogen phosphate phase, however, further vanadium-phosphorus mixed oxides can be formed during the reduction, in which vanadium has an oxidation state of IV or even III.The reduction need not be complete, so that some of the V(V) compound and the P(V) compound remain in the catalyst precursor. Typically, however, the catalyst precursor exhibits an average vanadium oxidation state of 3.8 to 4.2.

[0056] The water produced during reduction can be removed from the reaction mixture. In the prior art, this removal is achieved either physically, e.g., using a water separator, or chemically by using compounds that bind the water, such as drying agents or anhydrides like phosphoric acid at a concentration greater than 100%. The reaction mixture may contain anhydrides that react with and bind water; in particular, the reaction mixture may contain phosphoric acid at a concentration greater than 100%.

[0057] The suspension obtained after the reduction step can be filtered, for example, in an inert gas atmosphere such as nitrogen or a noble gas. In this context, inert gas means any gas that, under the given conditions, does not react with the catalyst precursor during filtration, while simultaneously displacing oxygen from the air, thus minimizing the risk of explosion. Filtration is carried out using methods known to those skilled in the art, typically a filter press, a decanter, or a Büchner funnel. Filtration yields an uncalcined catalyst precursor, which is still moistened with solvent.

[0058] The catalyst precursor obtained by filtration (the solid residue of the filtration) can then be dried. This is typically done at a temperature above room temperature, e.g., up to 150 °C, under reduced pressure or vacuum, or under inert gas to obtain a dried catalyst precursor. In this context, inert gas means any gas that does not react with the catalyst precursor under the drying conditions, but which also displaces oxygen from the air, thus minimizing the risk of explosion; for example, nitrogen or a noble gas. Preferably, drying takes place under reduced pressure or vacuum between 50 °C and 150 °C, more preferably between 90 °C and 140 °C.

[0059] Alternatively or optionally, following drying, calcination can be carried out to obtain the catalyst precursor. Calcination takes place at elevated temperatures between 150 °C and 350 °C, preferably between 230 °C and 290 °C, under an inert gas atmosphere. In this context, inert gas means any gas that does not react with the catalyst precursor under the calcination conditions but displaces oxygen from the air, thus minimizing the risk of explosion; for example, nitrogen or a noble gas.

[0060] Optionally, graphite can be added to the dried catalyst precursor to facilitate shaping in process step b). The dried catalyst precursor can also be compacted and / or granulated to obtain a compacted or granulated dried catalyst precursor. For this purpose, the catalyst precursor can be compacted into plates using a roller compactor with a contact pressure of 190 bar, a gap width of 0.60 mm, and a roller speed of 7 rpm, and then granulated through a 1 mm sieve.

[0061] In process step b), the resulting catalyst precursor is formed into catalyst bodies, for example by tableting. Here, the granules are pressed into the desired tablet shape and size using a rotary tablet press.

[0062] In the following process step c), the resulting catalyst pellets are activated at a temperature above 200 °C. Activation typically takes place in a gas mixture consisting of air, an inert gas, and steam. Any gas that does not react with the catalyst pellet under the given activation conditions can serve as the inert gas; nitrogen or a noble gas is particularly preferred. Alternatively, activation can also be carried out in process gas, i.e., a gas mixture containing air and butane. Activation is performed at a temperature in the range of 300 °C to 500 °C, preferably in the range of 350 °C to 450 °C. The finished VPO catalyst is obtained as the product of the process after activation. The tableted VPO catalyst typically has a lateral compressive strength above 25 N, typically between 25 N and 200 N.

[0063] The manufacturing process according to the invention for the VPO catalyst in the form of molded bodies is characterized in that, after process step a), ZnO is added to or mixed with the catalyst precursor. The ZnO, i.e., zinc(II) oxide, is used here as a powdered solid agent. The addition of the ZnO to the catalyst precursor can also be carried out using a metering device and a mixer. Generally, sufficient ZnO is added to produce the catalyst according to the invention. For example, based on the weight of the dried catalyst precursor (without ZnO), 0.5 wt% to 7.0 wt%, preferably 1.0 wt% to 5.0 wt%, and more preferably 1.5 wt% to 3.5 wt% ZnO in solid form can be added.

[0064] The ZnO is added to the catalyst precursor, i.e., after its preparation in process step a), for example by a reduction step, but before the formation of the catalyst bodies in process step c). Preferably, the ZnO is added to the dried catalyst precursor, particularly preferably to the dried and calcined catalyst precursor.

[0065] In a further preferred embodiment, in addition to the ZnO, another solid metal compound, preferably a metal compound in powder form, is added. It is preferred that a solid Mg compound, for example MgO, is included in the binder.

[0066] The invention further relates to a process for the production of maleic anhydride by catalytic oxidation of n-butane, wherein a reactant gas comprising oxygen and n-butane is passed through a reactor tube in which a bed of VPO catalysts according to the invention is located.

[0067] The packed bed of VPO catalysts in the reactor tube consists of the VPO catalysts or shaped bodies according to the invention, which are introduced into the reactor tube and form a packed bed by resting on it. The reactor tube is preferably part of a plurality of reactor tubes of a tube bundle reactor, as known to those skilled in the art for the industrial production of maleic anhydride. During the reaction, the packed bed of VPO catalysts is located at a temperature between 300 °C and 420 °C. The reactant gas can, for example, contain between 0.2 and 10 vol% n-butane and between 5 and 50 vol% oxygen and is passed through the reactor tube at a space-time velocity of 1100 h⁻¹ to 2500 h⁻¹, preferably 1300 h⁻¹ to 2000 h⁻¹. Figure 1 IR spectra of the samples according to examples 1 to 7 and example 12. Figure 2 IR spectra of the samples according to Examples 1, 15 and 16. Figure 3IR spectra of the samples according to Example 5 and comparison examples 17 and 18. Figure 4 : Influence of the use of ZnO or ZnO / MgO solids in the synthesis on the stability of the VPO catalysts according to examples 1 to 7. Figure 5 : Change in lateral pressure resistance and selectivity of VPO catalysts with different amounts of Zn addition. Figure 6 XRD diffractograms of the VPO catalysts according to examples 1 to 5. Figure 7 XRD diffractograms of the VPO catalysts according to examples 5 and 8 to 10. Figure 8 XRD diffractograms of the VPO catalysts according to Example 11 and 12 compared to the VPO catalyst produced according to the invention according to Example 5. Figure 9 : Representations of the preferred catalyst particle, the "double alpha form", from four different perspectives.

[0068] The numbers in parentheses in the figures refer to the sample produced according to the corresponding example. Examples Example 1 (Comparison) Equipment used

[0069] A mantle heater is placed on a lab stand, and a 2-liter four-necked flask is positioned inside it. A half-moon stirrer with a matching stir bar is inserted into the center opening of the four-necked flask and connected to the stirrer via a stirrer coupling. A thermometer is located in the right opening, and a riser tube leading to the reflux condenser is in the left. The front center opening is used for filling with chemicals, after which the nitrogen purge is connected there. The entire apparatus can also be purged with nitrogen. For this, the nitrogen is first passed through a gas washing bottle and then into the apparatus, before being discharged from the top of the condenser through another gas washing bottle. Production of the catalyst precursor

[0070] First, 1069.5 g of isobutanol and 156.0 g of benzyl alcohol are added. While stirring, 150 g of V₂O₅ are added. After the V₂O₅ addition, 2.52 g of ammonium dimolybdate are added. Then, 232.50 g of phosphoric acid (100%, or anhydrous) are added to the suspension and heated under nitrogen reflux for 10 h. Filter

[0071] After cooling the suspension, which contains the catalyst precursor as a solid, it is transferred from the four-necked flask to a filter funnel and the liquid is extracted. The moist filter cake is then pressed dry overnight at 14 to 18 bar. Drying / Calcining

[0072] The pressed filter cake is placed in the evaporator flask of a rotary evaporator. Under water jet vacuum, the filter cake is dried overnight at 110 °C. The dried powder is then placed in a suitable calcining pot in an oven and calcined in a nitrogen atmosphere at temperatures of 200 to 300 °C for 9 hours. Compaction / Tabletting

[0073] Prior to compaction / tableting, 5 wt% graphite is added to the calcined, powdered catalyst precursor and homogeneously mixed using a Rhönrad mixer. This powder is then compacted into plates using a roller compactor with a contact pressure of 190 bar, a gap width of 0.60 mm, and a roller speed of 7 rpm, and subsequently granulated through a 1 mm sieve.

[0074] The granules are pressed into the desired tablet shape, with appropriate height, e.g. 5.6 × 5.6 × 2.3 mm, and lateral pressure resistance, using a rotary tablet press. Activation to pyrophosphate

[0075] The activation process, which produces vanadyl pyrophosphate, is carried out under controlled conditions in a retort installed in a programmable oven. The calcined tablets are evenly loaded into the retort, which is then tightly sealed. The catalyst is then activated in a moist air-nitrogen mixture (50% absolute humidity), first at over 300 °C for 5 hours and subsequently at over 400 °C for 9 hours. Examples 2 to 7 (according to the invention)

[0076] The VPO catalysts according to the invention were produced analogously to Example 1, except that the calcined powder of the catalyst precursor was mixed per 100 g with 4.5 g (Example 2), 1.8 g (Example 3), 5.0 g (Example 4), 2.0 g (Example 5), 1.0 g (Example 6), 0.5 g (Example 7) ZnO powder (commercial ZnO particle size < 100 µm, impurity below 0.05 wt%) and 0.5 g (Example 2) and 0.2 g (Example 3) MgO powder and simultaneously with the graphite. This resulted in calcined precursor powders with 5.0 wt% ZnO / MgO (Example 2), 2.0 wt% ZnO / MgO (Example 3), 5.0 wt% ZnO (Example 4), 2.0 wt% ZnO (Example 5), 1.0 wt% ZnO (Example 6), 0.5 wt% ZnO (Example 7).

[0077] The VPO catalysts according to Examples 1 to 7 were tested for their fracture toughness both before and after activation. In addition, XRD diffractograms of the VPO catalysts were generated and their catalytic selectivity was tested.

[0078] The ones in Table 1 and in Figure 5 The results presented show that the addition of ZnO or ZnO / MgO after the calcination step does not result in a systematic increase in sidewall flexural strength (SDF) when measured directly after tableting. Surprisingly, however, this is the case after the subsequent activation step of the VPO catalyst tablets. Here, a systematic and very clear increase in the sidewall flexural strength of the particles is observed with the addition of ZnO or ZnO / MgO. Table 1 and Figure 5 They also show that under the chosen catalytic conditions (85% conversion), the addition of ZnO or ZnO / MgO leads to an increase in selectivity.

[0079] The VPO catalyst according to the invention is further characterized by infrared spectroscopic features. Conventional VPO catalysts without ZnO exhibit a maximum in the IR spectrum between 790 cm⁻¹ and 810 cm⁻¹ (first absorption band) and a second maximum between 820 cm⁻¹ and 840 cm⁻¹ (second absorption band), with the second absorption band being stronger than the first absorption band. Figure 1 , (1)). It was found that with the addition of ZnO or ZnO / MgO, there is a simultaneous increase in the strength of the band at 790 cm⁻¹ to 810 cm⁻¹ (first absorption band) and a decrease in the strength of the maximum between 820 cm⁻¹ to 840 cm⁻¹ (second absorption band), such that the first absorption band in the samples according to the invention is stronger than the strength of the second absorption band, or the strength of the second absorption band is even reduced to such an extent that it is no longer detectable ( Figure 1, (2) - (7)). In the latter case, the VPO catalysts according to the invention are characterized by the fact that they only have the first absorption band.

[0080] It also turns out that the VPO catalysts according to the invention have the following features, observable by XRD diffractometry ( Figure 6 ): 31.7 to 31.9° (sharp reflection, ZnO) 34.3 to 34.5° (sharp reflection, ZnO) 36.2 to 36.4° (sharp reflection, ZnO)

[0081] These characteristics become more intense with increasing ZnO content and correspond well with ZnO (in wurzite structure or as zincite). Comparative example 8, examples 9, 10

[0082] To determine the relationship between the presence of the stabilizing ZnO phase and the timing of the binder addition, XRD diffractograms were recorded after various addition times. While in Examples 2 to 7 ZnO was always added after calcination and before tableting, the ZnO was added during the preparation of the reaction mixture during process step a), i.e., together with the addition of V₂O₅ (Comparative Example 8), immediately after filtration following process step c) (Example 9), and during process step d), i.e., after vacuum drying and before calcination (Example 10). In each case, 5.2 g of ZnO was added, so that the finished catalysts nominally contained 2 wt% ZnO each.

[0083] Figure 7, shows that the XRD reflexes observed when ZnO is added after calcination and before tableting, especially at 31.7 to 31.9°, 34.3 to 34.5°, 36.2 to 36.4°, are not visible when the ZnO is added at the beginning of the reflux step. Figure 7 , Diffractogram (8). Comparative examples 11 and 12

[0084] The VPO catalysts according to comparative examples 11 and 12 were prepared analogously to the VPO catalyst according to example 1, whereby the activated tablets were impregnated with Zn(OAc)₂ solution. Two different concentrations were used to obtain a Zn / V ratio of 0.008 (= 0.29 wt% Zn based on the total catalyst weight) and 0.016 (corresponding to 0.58 wt% based on the total catalyst weight), respectively. After impregnation, the catalysts were first dried in air for 18 h at 100°C and then for a further 20 min at 350°C.

[0085] Figure 8Figure 1 shows the XRD diffractograms of the VPO catalysts according to Comparative Examples 11 and 12 (diffractograms (11) and (12)) in comparison to the VPO catalyst produced according to the invention according to Example 5 (diffractogram (5)). It is evident that the addition of the ZnO compound to the activated tablets results in no reflections, particularly at 31.7 to 31.9°, 34.3 to 34.5°, and 36.2 to 36.4°. Comparative examples 13 and 14

[0086] The VPO catalyst according to Comparative Example 13 was produced analogously to the VPO catalyst according to Example 2, wherein 10 wt% binder of type SECAR 71 and 4 wt% graphite were added to the calcined powder.

[0087] The stability of a VPO catalyst can be readily assessed by measuring its stability with respect to the byproduct water, since a significant amount of water vapor is present during the reaction due to the oxidation process, which can damage the catalyst. Therefore, the stability with respect to the byproduct water of the VPO catalyst according to Example 4, compared to a VPO catalyst produced with a conventional binder according to Comparative Example 13, was tested. For this purpose, the selectivity of the untreated samples was tested, and subsequently both samples were impregnated with water, and the selectivity test was repeated (Comparative Example 14). It was found that the catalyst according to the invention did not suffer any loss of selectivity due to water impregnation within the measurement tolerance. Examples 15 and 16

[0088] The VPO catalysts according to Examples 15 and 16 were prepared analogously to the VPO catalyst according to Example 1, but without the addition of ammonium dimolybdate, so that the VPO catalyst obtained was free of Mo.

[0089] Furthermore, after calcination and before tableting, 1 wt% (Example 15) or 2 wt% ZnO (Example 16), based on the total weight of the calcined powder, was added. As Table 1 shows, an increase in catalytic selectivity combined with an increase in lateral pressure resistance is also achieved with the Mo-free VPO catalysts. The in Figure 2 The IR spectra shown, performed in transmission, also show that for these two samples according to the invention, the intensity of the band at 790 cm -1< to 810 cm -1< (first absorption band) is stronger than the maximum between 820 cm -1< to 840 cm -1< . Examples 17 and 18 (comparison) Equipment used

[0090] The same apparatus was used as in Example 1. Production of the catalyst precursor

[0091] First, 150 g of V₂O₅ are placed in a four-necked flask. To this, 300 mL of benzyl alcohol and 1200 mL of isobutanol are added. After inerting with N₂, the suspension is heated to reflux for 10 h with stirring. After cooling to a maximum of 40°C with stirring, 7.51 g of ammonium dimolybdate, 6.60 g of iron(III) nitrate nonahydrate, 2.55 g of cerium(III) nitrate hexahydrate, and 4.5 g of niobium ammonium oxalate are added. After the addition of 138 mL of 85% phosphoric acid with stirring within 15 min and inerting with N₂, the suspension is heated to reflux again with stirring for 24 h. Filter:

[0092] After cooling the suspension containing the catalyst precursor, it is transferred from the four-necked flask to a filter funnel and the liquid is siphoned off. The moist filter cake is washed once with 100% ethanol and the liquid is again siphoned off in the filter funnel. The same procedure is then repeated with double-distilled water. Drying / Calcination:

[0093] The washed filter cake is placed in the evaporator flask of a rotary evaporator. Under water jet vacuum, the filter cake is dried overnight at 120 °C. The dried powder is then placed in a suitable calcining pot in an oven and calcined in a nitrogen atmosphere at temperatures of 200 to 300 °C for 9 hours. Compaction / tableting:

[0094] Prior to compaction / tableting, 2.1 wt% Zn₃(PO₄)₂ and then 4 wt% graphite are added to the calcined, powdered catalyst precursor and homogeneously mixed using a Rhönrad mixer. This powder is then compacted into plates using a roller compactor with a contact pressure of 190 bar, a gap width of 0.60 mm, and a roller speed of 7 rpm, and subsequently granulated through a 1 mm sieve.

[0095] The granules are pressed into the desired tablet shape, with appropriate height, e.g. 5.6 × 5.6 × 2.3 mm, and lateral pressure resistance, using a rotary tablet press. Temperature treatment

[0096] The following temperature treatment is carried out in a retort installed in a programmable oven under controlled conditions. The calcined tablets are evenly filled into the retort, which is then tightly sealed. The catalyst is then treated in an air stream at 120°C for 18 hours.

[0097] The VPO catalyst according to Example 18 was prepared analogously to the VPO catalyst according to Example 1, wherein 2.1 wt% Zn 3 (PO 4 ) 2 based on the total weight of the calcined powder was added to the calcined powder after calcination and before tableting.

[0098] As shown in Table 1, the non-inventive samples according to Examples 17 and 18 exhibit a significantly lower selectivity compared to the inventive samples. At the same time, the IR spectra performed in transmission show... Figure 3, that in these two non-inventive samples, the intensity of the band at 790 cm -1< to 810 cm -1< (first absorption band) is not stronger than the maximum between 820 cm -1< to 840 cm -1< (Example 17) or both bands are not present (Example 18). Results

[0099] Table 1: Example binder Amount of binder [wt.%] Side pressure resistance before activation [N] Lateral pressure resistance after activation [N] IR, XR D Fig. Selectivity 85% (MA) [%] 1 (Comparison) - 0,0 23,4 23,5 1,6 64,5 2 (Invention) 9ZnO / 1MgO* 5,0 24,1 35,5 1,6 61,1 3 (Invention) 9ZnO / 1MgO* 2,0 26,1 28,7 1,6 67,8 4 (Invention) ZnO 5,0 21,1 35,5 1,6 58,5 5 (Invention) ZnO 2,0 20,9 27,5 1, 6, 7, 8 68,2 6 (Invention) ZnO 1,0 20,2 26,1 1 66,8 7 (Invention) ZnO 0,5 22,8 24,6 1 66,8 8 (comparison) ZnO 2,0 24,0 22,2 7 - 9 (Invention) ZnO 2,0 - - 7 - 10 (Invention) ZnO 2,0 - - 7 - 11 (Comparison) Zn(OAc) 2 0,3 - - 8 64,8 12 (Comparison) Zn(OAc) 2 0,6 - - 8 59,9 13 (Comparison) SECAR 10 - - - 64,6 14 (Comparison) SECAR 10 - - - 58,0 15 (Invention) ZnO 1,0 17,6 23,3 2 66,9 16 (Invention) ZnO 2,0 15,7 27,5 2 - 17 (Comparison) Zn 3 (PO 4 ) 2 2,1 19,3 13,9 3 65,3 18 (Comparison) Zn 3 (PO 4 ) 2 2,1 24,0 14,3 3 62,5 methods Infrared spectroscopy (IR)

[0100] The catalysts were characterized by transmission infrared (IR) spectroscopy. This involves determining the wavelength-dependent intensity of infrared radiation from a source (I0) after passing through a sample (I). Absorption of the IR radiation, and thus excitation of vibrational modes in the material under investigation, leads to a wavelength-dependent attenuation of the infrared radiation. The spectrum plots the absorption, calculated as log(I0 / I0), against the wavenumber.

[0101] The measurements were performed on a Nicolet Nexus 470 FTIR spectrometer with a liquid nitrogen-cooled mercury-cadmium tellurium (MCT) detector, an Everglo IR source, and a HeNe laser for frequency calibration. Sample preparation involved finely grinding tablets of the respective catalysts and producing a thin pellet with a diameter of 11 mm using a hand-operated press, yielding approximately 10 mg of material. This pellet was mounted in a vacuum chamber with KBr windows and positioned in the beam path. The sample was then pretreated for 2 hours at 200°C and a pressure of 10⁻⁴ mbar to remove adsorbed water. For the measurements, the vacuum chamber containing the sample was cooled to 77 K using liquid nitrogen, and the spectrum was recorded at a pressure of 10⁻⁴ mbar with a step size of 2 cm⁻¹, an aperture of 72, and an optical velocity of 0.64. Determination of the IR absorption maximum

[0102] The strength of the two absorption bands, each with a maximum in the range between 790 cm⁻¹ and 810 cm⁻¹, and between 820 cm⁻¹ and 840 cm⁻¹, corresponds to the strength of absorption in the region of the band's maximum compared to the spectral background. To determine the strength of absorption in the region of the maximum, a first straight line was defined as the linear background such that it touches the spectrum, i.e., the background of the spectrum, directly to the left and right of the band in question (i.e., within the frequency range up to an adjacent absorption band). Subsequently, a line is drawn perpendicularly downwards from the band's maximum (S₀), i.e., in the direction of constant wavelength and decreasing absorption, and the intersection of this line with the linear background (S₁) is determined. The strength of the absorption band is defined as the length of the path from S₀ to S₁. Test of fracture strength

[0103] A Zwick Z0.5 instrument was used to measure the breaking strength of the molded parts and determine the force required for fracture. Measurements were performed according to ASTM D4179. To dry the molded parts prior to measurement, they were stored in a drying oven at 100°C for at least 3 hours, and the subsequent breaking strength measurement was performed within 1 hour of drying. The instrument was operated according to ASTM D4179 at a constant force rate of 20.0 N / s. For each sample, 100 tablets were sequentially placed with the cylinder axis parallel to the surface of the measuring jaws (referred to as the "radial crush" in ASTM D4179) and measured. The mean value of the 100 individual values ​​for the force required to fracture the molded part was then calculated, representing the average breaking force of the molded part.All information regarding lateral compressive strength in this application refers to lateral compressive strengths obtained by the method described herein. Powder X-ray diffraction (XRD)

[0104] The catalysts were characterized using X-ray powder diffraction (XRD). In this technique, X-rays are diffracted at various diffraction angles by the crystalline regions of the sample. The diffraction angle is measured and plotted in 2θ. Depending on the phase present, characteristic reflections occur, which vary with the diffraction angle. These diffraction patterns can then be correlated with the corresponding phases using a database.

[0105] The measurements were performed on a Bruker AXS D4 Endeavor using Cu-Kα radiation and a Lynxeye detector. Diffractrograms were recorded over an angular range 2θ from 5° to 50° with a step size of 0.02° and a recording time of 1.5 s per step, using a fixed divergence aperture of 0.3°. For measurement, the samples were finely ground and compressed in a sample holder. Tilting the sample allowed for variation of the diffraction angle within the apparatus. All XRD reflections mentioned in this application refer to XRD reflections obtained using this method.

[0106] To improve comparability of the diffractograms, each one was normalized. For this purpose, the data point with the lowest intensity value is first identified for each diffractogram. This value is then subtracted from all intensity values ​​in the respective diffractogram. Next, the maximum intensity of the (024) reflection (which occurs at a 2θ value of 28.4–28.5°) in the respective diffractogram is determined. All intensity values ​​in the respective diffractogram are then divided by this value. Catalytic test reaction

[0107] To determine catalyst performance, all catalysts were tested for their catalytic properties in a bench-scale reactor at 1.5 mol% butane in air in a dilute catalyst bed (1:9 mixture catalyst: ceramic inert rings) after complete preparation (reflux, filtration, vacuum drying, calcination, compaction, tableting, activation). Selectivity for maleic anhydride (MA) was determined at a reaction temperature of 410°C (salt bath) by interpolating the mass-related GHSV in the range of 1300 to 5500 l / kg / h to achieve a conversion of 85%.

Claims

1. VPO catalyst in the form of a molded body for oxidizing hydrocarbons with molecular oxygen, in particular for oxidizing butane to maleic anhydride with molecular oxygen, wherein the VPO catalyst contains between 0.05 wt.% and 7.0 wt.% of Zn, which is partly present as ZnO and, in transmission infrared spectroscopy, has a first absorption band with a maximum between 790 cm-1 and 810 cm-1 and possibly a second absorption band with a maximum between 820 cm-1 and 840 cm-1, characterized in that only the first absorption band is present or the strength of the first absorption band is greater than the strength of the second absorption band, the strength of the absorption bands being determined by in each case setting a first straight line tangentially touching the spectrum immediately to the left and right below the band concerned, then drawing a second straight line starting from the maximum of the band in the direction of constant wavelength and decreasing absorption and determining the point of intersection of the two straight lines, the strength of the absorption band is defined as the length between the maximum and the point of intersection, and that the VPO catalyst, when examined by powder X-ray diffraction, exhibits reflections at 31.7° to 31.9°, 34.3° to 34.5° and 36.2° to 36.4°, when measured with a D4 Endeavor by the company Bruker AXS with Cu-Kα radiation and a LYNXEYE detector, wherein the diffractograms are recorded in an angular range 2θ of 5° to 50° with a step size of 0.02° at a recording time of 1.5 s per step with a fixed divergence diaphragm of 0.3°.

2. VPO catalyst according to claim 1, characterized in that the ratio between the strength of the first absorption band and the strength of the second absorption band is above 1.1, preferably above 2.

3. VPO catalyst according to one of the preceding claims, characterized in that the VPO catalyst has an Mo content of between 0.1 wt.% and 1 wt.%, preferably between 0.4 wt.% and 0.7 wt.% of Mo, based in each case on the total weight of the VPO catalyst.

4. VPO catalyst according to one of the preceding claims, characterized in that the VPO catalyst contains between 0.1 wt.% and 6 wt.%, preferably between 0.2 wt.% and 4 wt.%, more preferably between 0.5 wt.% and 3.5 wt.%, based on the total weight of the VPO catalyst, of Zn.

5. VPO catalyst according to one of the preceding claims, characterized in that the VPO catalyst has the following elemental composition: - 0.5 wt.% to 7 wt.% Zn, - 0 wt.% to 0.7 wt.% Mo, - 26 wt.% to 31 wt.% V, - 17 to 21% by weight of P, - 3 to 5% by weight of C, the remainder being oxygen, based in each case on the total weight of the VPO catalyst.

6. VPO catalyst according to one of the preceding claims, characterized in that the shaped body has a side compression strength of more than 25 N, preferably between 25 N and 200 N, the side compression strength being measured using a Zwick Z0.5 device ASTM D4179 standard at a constant force rate of 20.0 N / s, wherein 100 tablets are each placed individually with the cylinder axis parallel to the measuring jaw surface and measured to determine an average breaking force representative of the side crushing strength.

7. A VPO catalyst according to any of the preceding claims, characterized in that the shaped body has a double-alpha shape, with a height of 3 mm to 8 mm, a length of 5 mm to 9 mm, a width of 4 mm to 8 mm and a hole inside diameter of 1 mm to 4 mm.

8. VPO catalyst according to one of claims 1 to 6, characterized in that the shaped body has a cylindrical shape, with a height of 3 mm to 8 mm, a substantially round base with a diameter of 3 mm to 8 mm and a central axial opening with a diameter of 1 mm to 3 mm.

9. a process for preparing a VPO catalyst according to any one of claims 1 to 8, comprising the steps of: a) preparing a catalyst precursor comprising vanadyl hydrogen phosphate, b) forming the catalyst precursor into shaped bodies, c) activating the shaped bodies to form a VPO phase, characterized in that after step a) ZnO is mixed with the catalyst precursor.

10. Process for preparing a VPO catalyst according to claim 9, characterized in that the preparation of the catalyst precursor comprising vanadyl hydrogen phosphate in step a) is carried out by reducing a V(V) compound in the presence of a P(V) compound by means of an organic reducing agent during a reflux step at atmospheric pressure in an organic solvent.

11. Process for preparing a VPO catalyst according to claim 9 or 10, characterized in that the catalyst intermediate obtained in step a) is filtered in a step a1) and dried and / or calcined at a temperature of at most 300°C in a step a2).

12. Process for preparing a VPO catalyst according to claim 11, characterized in that step a2) is carried out in two steps, where in a first step drying is carried out in vacuo at a temperature in the range of 90°C to 140°C C for a period of 1 h to 24 h and in a second step calcining is carried out in nitrogen at a temperature in the range of 230°C to 290°C for a period of 1 h to 24 h.

13. Process for preparing a VPO catalyst according to claims 9 to 12, characterized in that the activation step is carried out in a gas mixture consisting of air, inert gas and water vapour, at a temperature in the range of 300°C to 500°C, preferably in the range of 350°C to 450°C, for a period of 1 h to 24 h.

14. Process for preparing a VPO catalyst according to any one of claims 9 to 13, characterized in that after step a) the catalyst precursor is additionally mixed with a Mg compound, preferably MgO.

15. Process for preparing maleic anhydride by catalytic oxidation of n-butane, in which a starting gas comprising oxygen and n-butane is passed through a reactor tube which contains a bed of VPO catalysts according to one of Claims 1 to 8.

16. Process according to claim 15, characterized in that the packing of the VPO catalysts is present in the reactor tube at a temperature between 300°C and 420°C.

17. Process according to any one of claims 15 or 16, characterized in that the educt gas contains from 0.2 to 10% by volume of n-butane and from 5 to 50% by volume of oxygen and is passed through the reactor tube at a space-time velocity of 1100 h-1 to 2500 h-1, preferably 1300 h-1 to 1600 h-1.