ARMORED PLATE

DE602017085657T2Active Publication Date: 2024-10-23ROSSIQUET GILLES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602017085657
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-07-11
Filing Date
2017-07-07
Publication Date
2024-10-23
Estimated Expiration
2037-07-07

AI Technical Summary

Technical Problem

Current armor technologies face challenges in achieving multi-impact resistance with low mass density, particularly for large ceramic shielding surfaces, as they tend to fragment after initial shots and are heavy, making them unsuitable for vehicles and installations without excessive weight.

Method used

A monolithic ceramic armor plate with a surface area greater than 150 cm², thickness greater than 12 mm, and apparent density less than 3.5 g/cm³, featuring grains of ceramic material with Vickers hardness greater than 15 GPa, a silicon nitride or silicon oxynitride matrix, and a rear energy dissipation coating, optimized for low porosity and silicon content, to enhance ballistic performance.

Benefits of technology

The solution provides improved resistance to fragmentation and perforation from successive armor-piercing projectiles while maintaining a low mass-to-surface ratio, equivalent to steel-based plates but with reduced weight, adhering to STANAG 4569 and AEP 55 standards for protection levels 4 and 5.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to products with anti-ballistic properties, that is to say whose hardness is sufficiently high to justify their use in armor or shielding elements.

[0002] The invention finds its application in particular as an element of armor or shielding allowing the protection of vehicles (land, sea or air) or fixed installations (building, perimeter wall, guard post in particular).

[0003] In particular, with regard to armored vehicles protected from projectiles by such anti-ballistic products, the additional mass linked to the wearing of armor is a crucial element. Indeed, this additional mass can lead to excessive weighting and be an obstacle to rapid movement of the vehicle and limit its range of action.

[0004] Metals and alumina are commonly used as armor for vehicles. In particular, systems formed by the so-called "mosaic" assembly of ceramic pieces having a specific polygonal shape and individually resistant to the impact of a projectile are known. JP2005247622 describes, for example, an arrangement of such shapes 20 to 100 mm wide, for a thickness of a few mm.

[0005] This type of mosaic of parts has the advantage of resisting successive shots (so-called "multi-shot" or "multi-hit" protection in English). Even if the probability of two shots at the same part is low and generally not considered in the standards, it nevertheless proves to be a sensitive problem in view of the advances in current weaponry. The assembly of such "mosaic" structures is however long and expensive. In addition, it can be difficult to maintain a low overall tolerance of the whole because the tolerances of each part are added to constitute the assembly. This has an impact on the width of the residual spaces between the parts (joint planes) produced by the assembly. Furthermore, if it also has a curved shape, the spaces constitute a significant weak zone of this protection system when the projectile impacts these places.

[0006] There are other so-called monolithic systems, i.e. formed by a single piece or by a very limited number of large-surface pieces, each monolith having a surface area greater than 150 cm 2< , so as to reduce the number of joints. Thus, many materials have been proposed to constitute armor intended for people whose armor mass to protection surface ratio must remain low, typically less than 50 kg / m 2< , or non-personal armor intended for vehicles or fixed installations whose mass to protection surface ratio is typically greater than 60 kg / m 2< . This ratio on non-personal protections is necessary and considered to resist more energetic and / or more armor-piercing munitions or even larger calibers, for example calibers 12.7mm, 14.5mm or even 25mm, or even 30mm.

[0007] For example: for STANAG 4 type protection (ammunition: 14.5mm API B32), the mass ratio of the metal armor plate to the surface subjected to impact is typically around 180kg / m 2< , for STANAG 5 type protection (ammunition: 25mm caliber), the ratio is typically around 200 kg / m 2< , for STANAG 6 type protection (ammunition: 30mm caliber), the ratio is typically around 280kg / m 2< .

[0008] In particular, among the ceramic materials used in such an application are silicon carbide (SiC) products.

[0009] Publication WO 2013 / 186453 A1 describes such a product whose grain shape and chemical composition of the product are specified in order to constitute an armor or an armoring element.

[0010] Publication EP 1380809 A2 also discloses a system comprising two layers of material, the first denser layer A formed on the surface by a carbide and a metal, for example a silicon carbide SiC and metallic silicon Si, and a second more porous layer B formed by the carbide, for example silicon carbide.

[0011] Publication EP1710218A1 discloses a sintered material based on silicon nitride and tungsten carbide with the help of additives such as rare earths, tungsten added preferably in oxidized form.

[0012] Porous SiC products are also known from US4604249 or US4415632 which can be used for vehicle armoring, but this type of monolithic armoring thus formulated cannot withstand a second shot, the ceramic constituting the armoring being too fragmented after a first shot under standard conditions known to those skilled in the art such as according to the STANAG 4569 and AEP 55 standards (in particular protection level 4 where the maximum distance between the first two successive shots is 10cm with a 14.5mm API B32 projectile). This standard represents a challenge in terms of multi-impact resistance for those skilled in the art.

[0013] US6389594B1 proposes an outer shell of the monolithic ceramic armor that is subjected to compressive stress. This shell is made of a polymer material based on aramid or other antiballistic materials, particularly based on glass fibers. This outer shell does not prevent the fracturing of the monolithic block and if the latter has a size greater than 100 cm 2 and / or if the projectile is of large caliber, due to the significant energy to be dissipated, the "blocking" effect is too weak, the decohesion of the monolithic block is strong and the resistance to multiple shots remains too weak.

[0014] More recently, WO2008 / 130451 (EP2095055A1) proposed an approach consisting of reducing the propagation of the stress wave linked to the impact of the projectile by using an envelope formed this time by a permeable media, typically a layer of organic fibers (for example aramid) fixed on the ceramic part then impregnated by a hyper elastic polymer in order to absorb the energy linked to the impact of the projectile and reduce the propagation of cracks and the multifracturing of the ceramic. This system is only of interest for ceramic parts also of small dimensions and the tested example is made from an assembly of 9 ceramic parts of dimension 100mm*100mm*8mm. The energy absorbed by this new envelope cannot prevent the decohesion of a ceramic block with a surface greater than 150cm 2< .

[0015] Patent application WO2014 / 096846 describes materials having high mechanical strength, consisting of a silicon carbide phase, a SiAlON phase and an intergranular binder phase comprising at least one rare earth. The binder phase according to the present invention is a silicon nitride or silicon oxynitride phase and does not comprise such a binder phase comprising at least one rare earth.

[0016] There is therefore a continual need to improve the products used as armor, this improvement being measured in particular by their ballistic performance. The object of the present invention is therefore to propose a new product, different from the products currently used in the field, and whose performance is improved, in particular so as to be able to resist perforation, even under the successive impact of two projectiles in the same region of the armor.

[0017] In particular, there is currently a need for a monolithic ceramic armor with a surface area greater than 150 cm 2< , preferably greater than 200 cm 2< , or even greater than 500 cm 2< or even greater than 1000 cm 2< , capable of resisting fragmentation after at least two successive shots of armor-piercing projectiles with a diameter greater than or equal to 12.7 mm in the same region of the armor, but which nevertheless has a low apparent density, typically less than 3.5 g / cm 3< , or even less than 3.3 g / cm 3< , in order to protect vehicles (land, sea or even air) or fixed installations, such as buildings, without weighing them down too much.

[0018] According to a first general aspect, the present invention relates to an anti-ballistic armor plate comprising a ceramic body made of a hard material, provided on its inner face with a rear energy dissipation coating, preferably made of a material of lower hardness than that of the material constituting the ceramic body.

[0019] In a plate according to the invention: said ceramic body is monolithic and has a surface area greater than 150 cm 2< , a thickness greater than 12 mm and an apparent density less than 3.5 g / cm 3< , the material constituting the ceramic body comprises grains of ceramic material with a Vickers hardness greater than 15 GPa and a matrix binding said grains, said matrix being essentially constituted by a silicon nitride phase and / or a silicon oxynitride phase or a SiMON phase where M is a metal chosen from Ca, Mg, Sr, Ba, said matrix representing between 5 and 40% by weight, preferably between 15 and 35% by weight, of said material constituting the ceramic body, said grains of ceramic material have a maximum equivalent diameter less than or equal to 800 micrometers, preferably less than or equal to 500 micrometers or even less than or equal to 300 micrometers.said material constituting the ceramic body has an open porosity greater than 5% and less than 14%, the mass content of silicon in metallic form in said material, expressed per mm of thickness of said body, is less than 0.5%.

[0020] Various preferred embodiments of the present invention are described below, which can of course, if necessary, be combined with each other: said grains of ceramic material have a maximum equivalent diameter greater than 5 micrometers, preferably greater than 10 micrometers or even greater than 50 micrometers, the material constituting the ceramic body comprises grains of a metal carbide or boride, more preferably grains of silicon carbide or boron or a mixture of these two carbides and preferably comprises only grains of silicon carbide, said material constituting the ceramic body has an open porosity greater than 6%, more preferably greater than 7% or even greater than 8%, said material constituting the ceramic body has an open porosity less than 13%, more preferably greater than 12%, the material constituting the ceramic body comprises grains of ceramic material with a Vickers hardness greater than 20 GPa, said ceramic body has a surface area greater than 500 cm 2 < , more preferably greater than 1000 cm 2 < ,said ceramic body has a thickness greater than 15 mm, more preferably greater than 20 mm, said ceramic body has an apparent density of less than 3.2 g / cm 3< , preferably an apparent density of less than 3.0 g / cm 3< , the mass content of silicon in metallic form in said material is less than 0.4% per mm of thickness of said body, more preferably less than 0.2% per mm of thickness of said body, or very preferably less than 0.1% per mm of thickness of said body, the mass content of silicon in metallic form in said material is greater than 0.005% per mm of thickness of said body, more preferably greater than 0.01% per mm of thickness of said body, the matrix representing between 5 and 40% by weight of said material constituting the ceramic body,silicon in metallic form is present in said material constituting the ceramic body according to a concentration gradient from the external edges to the core of said body, according to its thickness, said phase in the matrix is ​​chosen from Si 3 N 4 , Si 2 ON 2 or SiMON where M is a metal chosen from Ca, Mg, Sr, Ba, the plate has a mass to surface ratio, measured in kg / m 2 < , greater than 60 and preferably less than 200, the total sum of rare earths in the material constituting the ceramic body is less than 0.05% by weight, more preferably is less than 0.01% by weight, the grains constituting the ceramic material consist essentially of SiC, preferably in alpha form, the grains, in particular of SiC, in the material constituting the ceramic body have a maximum equivalent diameter of between 10 micrometers and 500 micrometers, preferably an average equivalent diameter of between 50 and 300 micrometers,or even between 100 and 200 micrometers, the material constituting the ceramic body does not contain any element from the rare earth group, the material constituting the ceramic body does not contain yttrium, the material constituting the ceramic body does not contain lanthanum, the material constituting the ceramic body does not contain any element from the actinide group, the grains constituting the ceramic material have an average equivalent diameter greater than 5 micrometers and less than 300 micrometers, preferably between 50 and 200 micrometers, the total content of silicon in metallic form is less than 10% of the total weight of the material constituting the ceramic body, preferably is less than 5%, or even less than 1%, of the total weight of the material constituting the ceramic body, the nitrogen content in the material constituting the ceramic body is greater than 4% by weight, the binding matrix is ​​essentially made of silicon nitride,in particular of formulation Si 3 N 4 and / or silicon oxynitride Si 2 ON 2 , preferably consists essentially of silicon nitride in particular of formulation Si 3 N 4 , the total content of aluminum in metallic form is less than 1% of the total weight of the material constituting the ceramic body, preferably is less than 0.5% of the total weight of the material constituting the ceramic body, alternatively, the binder matrix comprises or consists essentially of a SiMON phase where M is a metal chosen from Ca, Mg, Sr, Ba, preferably where M is Mg, the material constituting the back coating is chosen from polyethylenes PE, in particular ultra high density polyethylenes (UHMPE), glass or carbon fibers, aramids, metals such as aluminum, titanium or their alloys or steel, the ceramic body-back coating assembly is surrounded by an envelope of a containment material,the material constituting the envelope is chosen from PE polyethylenes, in particular ultra high density polyethylenes (UHMPE), glass or carbon fibers, aramids, metals such as aluminum or steel.

[0021] The invention also relates to the ceramic body whose characteristics have just been described previously, and in particular to a monolithic ceramic body in the form of a plate, having a surface area greater than 150 cm 2 and a thickness greater than 12 mm, an apparent density less than 3.5 g / cm 3, made of a material comprising: grains of ceramic material with a Vickers hardness greater than 15 GPa, preferably a metal carbide or boride, more preferably a silicon or boron carbide or a mixture of these two carbides, said grains having a maximum equivalent diameter less than or equal to 500 micrometers, and a matrix binding said grains, said matrix essentially consisting of a silicon nitride phase and / or a silicon oxynitride phase or a SiMON phase where M is a metal chosen from Ca, Mg, Sr, Ba, said matrix representing between 5 and 40% by weight of said material constituting the ceramic body, said ceramic material having an open porosity greater than 5% and less than 14% and a mass content of silicon in metallic form in said material, expressed per mm of thickness of said body, less than 0.5%.

[0022] Without it being necessary here to repeat, for the sake of brevity, all of the technical characteristics already described previously in relation to the shielding range, a ceramic body according to the invention of course covers all of the same preferred modes.

[0023] The following indications and definitions are given, in relation to the preceding description of the present invention: By equivalent grain diameter is meant the half-sum of the greatest length of the grain and the greatest width of the grain, measured in a direction perpendicular to said greatest length.

[0024] Hard material means a material whose hardness is high enough to justify its use in armor or shielding elements.

[0025] The maximum and average equivalent diameters are conventionally determined from the observation of the microstructure of the sintered material constituting the ceramic body, conventionally using images taken by SEM (scanning electron microscopy) on a section of the sintered product. It has been verified in the examples which follow that said microstructure is substantially identical, whatever the orientation of the section.

[0026] By apparent density of a product, we mean, for the purposes of the present invention, the ratio equal to the mass of the product divided by the volume occupied by said product. It is conventionally determined by the Archimedes method. The ISO 5017 standard, for example, specifies the conditions for such a measurement. This standard also makes it possible to measure open porosity for the purposes of the present invention.

[0027] By "matrix" of the ceramic body is meant a crystallized or non-crystallized phase, ensuring a substantially continuous structure between the grains and obtained, during sintering, from the constituents of the starting charge and possibly from the constituents of the gaseous environment of this starting charge. A matrix substantially surrounds the grains of the granular fraction, that is to say coats them.

[0028] In a sintered ceramic body according to the invention, the ceramic grains are bound by the matrix. During sintering, they substantially retain the shape and chemical nature they had in the initial charge. In the sintered ceramic body, the matrix and the grains together represent 100% of the mass of the product.

[0029] A matrix obtained by reactive sintering has particular characteristics. In particular, during reactive sintering, nitriding of the precursor metals of the nitrogenous crystallized phases occurs. The resulting increase in volume, typically 1 to 30%, advantageously fills the pores of the matrix and / or compensates for the shrinkage caused by sintering of the grains. Reactive sintering thus improves the mechanical strength of the sintered product. Reactively sintered products thus have a significantly lower closed porosity than that(s) of other sintered products under similar temperature and pressure conditions. Upon firing, reactively sintered products show substantially no shrinkage.

[0030] The phase composition of the material constituting the monolithic ceramic body is normally obtained by X-ray diffraction and Rietveld analysis.

[0031] Elemental nitrogen (N) contents in the sintered products were measured using LECO analyzers (LECO TC 436DR; LECO CS 300). Values ​​are provided as mass percentages.

[0032] The crystallized phases, especially the nitrogenous crystallized phases, were measured by X-ray diffraction and quantified according to the Rietveld method.

[0033] Residual silicon in metallic form in the sintered material or after firing is normally measured according to the method known to those skilled in the art and referenced under ANSI B74-151992 (R2000).

[0034] In the ceramic material according to the invention, the residual silicon content is generally maximum at the heart of the ceramic body, that is to say substantially in the middle of its thickness.

[0035] It was also determined by the applicant company that the residual silicon content strongly influences the antiballistic properties of the ceramic material. Residual aluminum in metallic form in the sintered material or after firing can be measured by X-ray diffraction and quantified using the Rietveld method.

[0036] The Vickers hardness of ceramic grains can be measured using a standardized pyramidal diamond point with a square base and an apex angle between faces equal to 136°. The imprint made on the grain therefore has the shape of a square; the two diagonals d1 and d2 of this square are measured using an optical device. The hardness is calculated from the force applied to the diamond point and the average d value of d 1 and d 2 according to the following formula: <menclose notation="box"> H V = 0,189 ⋅ F d 2 avec H V = Dureté Vickers F = Force appliquée N d = Moyenne des diagonales de l ′ empreinte mm < / menclose>

[0037] The force and duration of the support are also standardized. The reference standard is ASTM C1327: Standard Test Method for VICKERS Indentation Hardness of Advanced Ceramics.

[0038] “Containing a”, “comprising a” or “comprising a” means “comprising at least one”, unless otherwise indicated.

[0039] Unless otherwise indicated, in this description all percentages are mass percentages.

[0040] The product according to the invention provides protection against any type of projectile, for example a bullet, a shell, a mine or an element projected during the detonation of explosives, such as bolts, nails (or IED for "Improvised Explosive Device") and normally constitutes an element of armor for vehicles, generally in the form of modules such as plates.

[0041] According to the invention, the protective plate conventionally comprises at least two layers: a first ceramic part as described previously associated with another less hard and preferably ductile material, on the rear face, conventionally called "backing", such as polyethylene fibers (e.g.: Tensylon ™< , Dyneema ®< , Spectra ™< ), aramid (e.g.: Twaron ™< , Kevlar ®< ), glass fibers, or metals such as for example steel or aluminum alloys, in the form of plates. Adhesives, for example based on polyurethane or epoxy polymers, are used to bond the different elements constituting the armor plate.

[0042] Under the impact of the projectiles, the ceramic material fragments and its main role is to break the cores of the projectiles. The role of the rear face, associated with the ceramic material constituting the ceramic body, is to consume the kinetic energy of the debris and to maintain a certain level of confinement on the ceramic plate, further optimized by the confinement envelope.

[0043] The applicant company has thus developed a new armour element comprising an armour element including a ceramic plate capable of resisting at least two successive shots according to the STANAG 4569 and AEP 55 standards, considering protection level 4, or even 5 and 6.

[0044] Such armor intended for the applications mentioned above may have a mass to armor surface ratio typically greater than 60 kg / m 2 < but minimized compared to currently available plates, for the same anti-ballistic performance. This results in a reduction in the weight of the armor, for identical protection.

[0045] A ceramic body according to the invention may in particular be obtained by a sintering process, in particular a reactive sintering process comprising the following steps: a) preparing a starting charge comprising: at least one powder of silicon carbide particles, a powder comprising metallic silicon, optionally a powder of a solid-phase sintering additive, b) shaping the starting charge in the form of a preform, c) demolding after hardening or drying, d) optionally, drying the preform, preferably until the residual moisture is between 0 and 0.5% by weight, e) firing and sintering the preform under a nitrogen atmosphere, or under a non-oxidizing atmosphere if nitrogen is present in the starting charge, preferably at a temperature between 1300 and 1600°C, so as to obtain the sintered product.

[0046] In such a method, at least one initial silicon carbide powder is used, the median particle diameter of which is between 10 micrometers and 500 micrometers, and preferably between 50 and 300 micrometers. In certain advantageous embodiments, a second silicon carbide powder is used with a median size at least twice smaller than the first and preferably with an average diameter of between 1 and 5 micrometers.

[0047] In step b), the preform can be obtained by casting or pressing the filler or mixture into a mold, with or without vibration.

[0048] During firing in step e), the nitrogen in the firing furnace reacts (“reactive sintering”) with some of the constituents of the preform, in particular with metallic silicon or even with metallic aluminum if this is present alone or in the form of an alloy with silicon, also with calcined alumina or an aluminum silicate, for example clay, if these additions are present, to form a matrix and thus bind the grains of the ceramic body.

[0049] In the ceramic body according to the invention, the ceramic grains, preferably grains of silicon carbide and / or boron, may be bonded by a matrix comprising or consisting essentially of a silicon nitride or silicon oxynitride phase without the addition of rare earth compounds and without resorting to a high sintering temperature, i.e. at a temperature above 1650°C. In particular, the firing of a preform may be carried out under a nitrogen atmosphere between 1360 and 1500°C for a sufficiently long period (for example of at least 4 hours) to obtain a sintered ceramic body having a mass content of metallic Al and Si of less than 1%.

[0050] The median particle diameter (or median “size”) of the particles constituting a powder is given, for the purposes of the present invention, by a particle size distribution characterization. A laser particle size analyzer allows the measurement of sizes less than or equal to 3 mm.

[0051] The particle size distribution characterization is conventionally carried out with a laser particle size analyzer in accordance with ISO 13320-1. The laser particle size analyzer can be, for example, a Partica LA-950 from HORIBA. For the purposes of this description and unless otherwise stated, the median particle diameter refers to the particle diameter below which 50% by mass of the population is found.

[0052] The "median diameter" or "median size" of a set of particles, in particular of a powder, is called the percentile D 50 , that is to say the size dividing the particles into first and second populations equal in volume, these first and second populations comprising only particles having a size greater than, or less than, respectively, the median size.

[0053] The initial mixture may also include a fraction of an alumina powder with a median diameter of between 1 and 10 micrometers, serving as a sintering agent.

[0054] The ceramic body according to the invention is in particular obtained by a process as described above, preferably in the presence of a sintering additive chosen from carbon, boron, titanium, zirconium carbides or zirconium, titanium borides, alone or as a mixture.

[0055] In a particularly preferred embodiment, the product is obtained by a process as described above in which the sintering additive comprises or consists of boron carbide B 4 C.

[0056] By sintering additive, often more simply called “additive” in the present description, is meant a compound usually known to enable and / or accelerate the kinetics of the sintering reaction.

[0057] In one embodiment, the feedstock contains a binder and / or a lubricant and / or a surfactant. In one embodiment, the feedstock does not contain a binder.

[0058] The mixing is carried out in such a way as to obtain a good homogeneity of distribution of the different elements, the mixing time being able to be adapted to achieve this result.

[0059] Preferably, the initial reagents are mixed in a jar mill, with a mixing time of more than 15 hours. A mixing time of 24 hours is suitable. Once the mixture is obtained, it can be atomized or granulated, for example by "freeze granulation", in order to obtain granules which will be shaped, for example by pressing in order to obtain a ceramic preform. Other shaping techniques can be used, such as injection, slip casting. After shaping, the preform can be machined.

[0060] The preform is then sintered. Sintering is carried out in a nitrogen atmosphere.

[0061] Preferably, the silicon carbide powder has an oxygen element content of less than 2%, preferably less than 1.6%, preferably less than 1.4%, preferably less than 1.2%, preferably less than 1%, or even less than 0.7%, or even less than 0.5%, or even less than 0.3% by weight. In one embodiment, the oxygen element content of the silicon carbide powder may be reduced before use by any technique known to those skilled in the art, such as, for example, acid washing.

[0062] In one embodiment, the aluminum content of the feedstock is less than 1000 ppm, or even less than 500 ppm or even less than 300 ppm, based on the weight of the feedstock.

[0063] Cooking takes place in a controlled atmosphere, preferably under nitrogen to obtain the nitrided intergranular phase.

[0064] "Sintering" is a heat treatment by which the product forms a microstructure consisting of an aggregate or a granular fraction whose grains are held together by means of a matrix. A sintered product according to the invention comprises a matrix containing at least one silicon nitride or oxynitride phase, obtained by sintering in a non-oxidizing atmosphere if nitrogen is provided by at least one of the constituents of the starting charge or by sintering under nitrogen, preferably at a temperature between 1300 and 1600°C, the latter type of process, allowing reactive sintering under nitrogen, being well known to those skilled in the art.

[0065] “Sintering under nitrogen” means sintering in a gaseous environment comprising more than 90%, preferably more than 95% or, more preferably, substantially 100% nitrogen, by volume percentage. Such a gaseous environment is referred to as a “nitrogen environment”.

[0066] A constituent present in the starting charge and still present in the sintered product obtained from this starting charge is called “residual”.

[0067] Impurities are understood to mean unavoidable constituents, introduced unintentionally and necessarily with the raw materials or resulting from reactions with these constituents. Impurities are not necessary constituents, but only tolerated. Such an impurity is in particular constituted by silica, disadvantageously known to inhibit the sintering of SiC or even aluminum. Without departing from the scope of the invention, it is possible to limit the silica impurity by washing the SiC powders or even the sintering additive in a preliminary step and / or by adding carbon-containing additives to the initial mixture, to eliminate it during sintering.

[0068] The following examples are given for purely illustrative purposes and do not limit the scope of the present invention in any of the aspects described. Examples:

[0069] In all the following examples, a ceramic piece in the form of a 500mm×500mm×26mm plate was initially produced by casting a suspension in a plaster mold using the process described previously and the formulations described in Table 1 below.

[0070] The ceramic body thus obtained is used as a ceramic plate in an armor plate. More precisely, said ceramic body is bonded using an epoxy glue to a layer of fiberglass connecting it to a high-density polyethylene (UHMWPE) plate marketed by the company DSM Dyneema. The whole is wrapped in a layer of Kevlar also bonded using an epoxy resin. The initial formulation of the different mixtures and the exact conditions of the process for obtaining the armor plate are reported in Table 1.

[0071] Comparative example 4 was carried out according to the principles described in the application JP2005247622 cited above.

[0072] It aims to show the multi-impact resistance of a set of ceramic elements assembled in the form of a mosaic, each individual ceramic element of the ceramic being produced according to the same process and with the same material as example 1 according to the invention.

[0073] The tiles used in this mosaic set have an individual size of 3 cm by 3 cm and were assembled into a 50×50 cm plate according to the process described in Example 1 of JP2005247622.

[0074] Comparative example 5 consists of an essentially metallic anti-ballistic plate produced using conventional techniques from the combination of a 10 mm thick steel plate marketed by the Thyssen company under the reference Secure 500 ®< , and a 20 mm rear coating of styrofoam bonded with an epoxy adhesive, another 10 mm thick Secure 500 steel plate and a 15 mm coating of Twaron ®< (Teijin company) T750 aramid bonded. The whole is wrapped in a layer of Kevlar ®< from the Dupont company, also bonded with an epoxy resin.

[0075] For each achievement, the characteristics of the ceramic body and the composition of the different materials constituting it are gathered in table 2.

[0076] The ballistic properties of the final armor plate are summarized in Table 3. The ballistic performance of the different armor plates was evaluated using the AEP 55 and STANAG 4569 standards, considering ballistic protection level 4 (14.5mm API B32 projectile). Four shots were carried out on the different armor plates in a 'stand-alone' configuration and in compliance with the protocols and instructions described in the AEP 55 and STANAG 4569 standards (firing speed, distance between impacts, verification of perforation or not with the witness plate, etc.).

[0077] The results reported in Tables 1 to 3 below show the advantages linked to the implementation of a large monolithic armor plate according to the invention: Examples 1 to 3 according to the invention have improved perforation resistance so that they are capable of resisting successive projectile impacts. Their ballistic resistance thus appears substantially equivalent to steel-based plates as illustrated by Comparative Example 5. The mass / surface ratio of the plates according to the invention is however much lower than such steel-based plates, as illustrated in Table 3.

[0078] The comparative examples also show the influence of the parameters on the ballistic performances finally obtained for the armour plate: Comparative example 1 shows that the residual silicon content, i.e. the metallic silicon that has not reacted during firing with nitrogen, must be minimised right down to the core of the material constituting the ceramic body. In particular, when the heat treatment is not suitable and the residual metallic silicon content in the material is too high (0.5% residual silicon per mm of thickness of the ceramic body), particularly at the core of the ceramic body (i.e. approximately in the middle of the thickness of the ceramic plate), this results in lower resistance to perforation, as visible in the ballistic results reported in Table 3.

[0079] According to Comparative Example 2, the constituent grains of the material constituting the ceramic body are larger than according to the present invention, resulting in inferior ballistic performance. Thickening the ceramic plate according to Comparative Example 3 does not compensate for this deficiency.

[0080] Comparative example 4 further shows that a mosaic structure according to the prior art has greatly reduced ballistic performance compared to large plates according to the invention.

[0081] Of course, the present invention is not limited to the embodiments described and shown, provided as examples. In particular, combinations of the different embodiments described also fall within the scope of the invention, which is defined by the appended claims. The invention is also not limited by the shape or dimensions of the sintered silicon carbide product. Table 1 invention example 1 invention example 2 invention example 3 comparative example 1 comparative example 2 comparative example 3 comparative example 4 Composition of the initial mixture (% by mass) SiC powder 100µm-1100µm D 50 = 600µm 80,2 80,2 SiC powder 20-200 µm D 50 = 100 µm 39,5 SiC powder 10-150µm D 50 = 75 µm 39,5 39,5 39,5 39,5 SiC powder 0.1-5µm D 50 = 2.5 µm 37,5 37,5 37,5 37,5 37,5 Powder Si 0.5-50µm D 50 = 20µm 17 17 17 17 16,0 16,0 17 Calcined clay 3,0 3,0 Alumina Powder D 50 = 2.5 µm 5,0 5,0 5,0 5,0 5,0 Fe 2 O 3 2.5 µm 0,5 0,5 0,5 0,5 0,5 B 4 C 95% <45µm D 50 =18 µm 0,5 0,5 0,5 0,5 0,8 0,8 0,5 total minerals % 100 100 100 100 100 100 100 water added % 12,5 12,5 12,5 12,5 6 6 12,5 dispersant added 0,5 0,5 0,5 0,5 0,2 0,2 0,5 Formatting conditions Drying (T° / duration) 110°C / 24h 11 0°C / 24h 110°C / 24h 110°C / 24h 110°C / 24h 110°C / 24h 110°C / 24h Cooking (T° / duration / time) 1420°C / 8h / Nitrogen 1420°C / 4h / Nitrogen 1420°C / 8h / Nitrogen 1350°C / 4h / Nitrogen 1420°C / 8h / Nitrogen 1420°C / 8h / Nitrogen 1420°C / 8h / Nitrogen Table 2 invention example 1 invention example 2 invention example 3 comparative example 1 comparative example 2 comparative example 3 comparative example 4 Body features / ceramic material thickness (mm) 26 26,5 25,7 27 27 35 26 Plate shape monolithic monolithic monolithic monolithic monolithic monolithic mosaic surface area (cm 2< ) 50×50 50×50 50×50 50×50 50×50 50×50 3x3 Granular fraction (nature / relative weight) SiC / 75% SiC / 75% SiC / 77% SiC / 75% SiC / 75% SiC / 75% SiC / 75% Maximum equivalent diameter of SiC grains in the material 0.150mm 0.150mm 0.2mm 0.150mm 1.1mm 1.1mm 0.150mm Average equivalent diameter of SiC grains in the material 30 µm 30 µm 80 µm 30 µm 600 µm 600 µm 30 µm Matrix binding the grains (nature / relative weight) If 3 N 4 *< / 25% If 3 N 4 *< / 25% If 3 N 4 *< / 22% If 3 N 4 *< / 25% If 3 N 4 *< / 25% If 3 N 4 *< / 25% If 3 N 4 *< / 25% open porosity % 10 11,5 9 13 14 14 9,7 apparent density % 2,81 2,75 2,84 2,7 2,67 2,67 2,83 N content 10% 5% 9% 3,5% 10% 10% 10% % If residual (in the material) <0,5 9 0,7 13,5 <0,5 <0,5 <0,5 % Residual Si / mm thickness <0,02 0,35 0,03 0,50 <0,02 <0,02 <0,02 Back coating features Chemical nature Fiberglass + high density PE Fiberglass + high density PE Fiberglass + high density PE Fiberglass + high density PE Fiberglass + high density PE Fiberglass + high density PE Fiberglass + high density PE Thickness 21 mm 21mm 21mm 21mm 21mm 21mm 21mm Containment envelope characteristics Chemical nature Aramid fibers (Kevlar ®< ) Kevlar ®< Kevlar ®< Kevlar ®< Kevlar ®< Kevlar ®< Kevlar ®< *< 23% by weight of Si 3 N 4 , 2% by weight of Si 2 ON 2 Table 3 invention example 1 invention example 2 invention example 3 comparative example 1 comparative example 2 comparative example 3 comparative example 4 comparative example 5 Features of this armor plate mass / surface ratio 95 95 95 95 94 115 96 175 Ballistic tests Visual observation after the shots no perforation no perforation no perforation perforation perforation perforation perforation no perforation

Claims

1. An antiballistic armor plate including a ceramic body consisting of a hard material, provided, on its inner face, with a back energy-dissipating coating, preferably consisting of a material having a hardness that is lower than that of the constituent material of the ceramic body, said plate being characterized in that: - said ceramic body being monolithic and having an area that is larger than 150 cm2, a thickness that is greater than 12 mm and a bulk density that is lower than 3.5 g / cm3; - the constituent material of the ceramic body comprising grains of ceramic material having a Vickers hardness that is higher than 15 GPa, and a matrix binding said grains, said matrix consisting essentially of a silicon nitride phase and / or a silicon oxynitride phase or of a SiMON phase, where M is a metal chosen from Ca, Mg, Sr, Ba, said matrix representing between 5 and 40% by weight of said constituent material of the ceramic body; - the maximum equivalent diameter of said grains of ceramic material being smaller than or equal to 800 micrometers; - said constituent material of the ceramic body having an open porosity that is higher than 5% and lower than 14%; - the metallic silicon content in said material, expressed per mm of thickness of said body, being lower than 0.5% by weight.

2. The armor plate as claimed in claim 1, wherein the constituent grains of the ceramic material consist essentially of SiC, preferably in the alpha form.

3. The armor plate as claimed in either of the preceding claims, wherein the metallic silicon is present in said constituent material of the ceramic body along a concentration gradient from the outer edges to the core of said body, in the direction of its thickness.

4. The armor plate as claimed in one of the preceding claims, which has a mass-to-area ratio, measured in kg / m2, that is higher than 60 and preferably lower than 200.

5. The armor plate as claimed in one of the preceding claims, wherein the total sum of rare-earth elements in the constituent material of the ceramic body is lower than 0.05% by weight.

6. The armor plate as claimed in one of the preceding claims, wherein the maximum equivalent diameter of the grains in said constituent material of the ceramic body is comprised between 10 micrometers and 500 micrometers.

7. The armor plate as claimed in one of the preceding claims, wherein the constituent material of the ceramic body contains no elements from the group of the rare-earth elements, preferably no yttrium, preferably no lanthanum and more preferably no elements from the group of the actinides.

8. The armor plate as claimed in one of the preceding claims, wherein the mean equivalent diameter of the constituent grains of the ceramic material is larger than 5 micrometers and smaller than 300 micrometers.

9. The armor plate as claimed in one of the preceding claims, wherein the metallic silicon content of the constituent material of the ceramic body is lower than 10% by weight.

10. The armor plate as claimed in one of the preceding claims, wherein the nitrogen content in the constituent material of the ceramic body is higher than 4% by weight.

11. The armor plate as claimed in one of the preceding claims, wherein the binding matrix essentially consists of silicon nitride Si3N4 and / or silicon oxynitride Si2ON2, and preferably essentially consists of silicon nitride Si3N4.

12. The armor plate as claimed in one of the preceding claims, wherein the constituent material of the back coating is chosen from the polyethenes PE, in particular ultra-high-molecular-weight polyethenes (UHMPEs), glass or carbon fibers, aramids, metals such as aluminum, titanium or their alloys, or steel.

13. The armor plate as claimed in one of the preceding claims, wherein the ceramic body-back coating assembly is surrounded by an envelope of a confining material.

14. The armor plate as claimed in the preceding claim, wherein the constituent material of the envelope is chosen from the polyethenes PE, in particular ultra-high-molecular-weight polyethenes (UHMPEs), glass or carbon fibers, aramids, metals such as aluminum or steel.

15. A monolithic ceramic body in the form of a plate and having an area that is larger than 150 cm2 and a thickness that is greater than 12 mm, and a bulk density that is lower than 3.5 g / cm3, consisting of a material comprising: - grains of ceramic material having a Vickers hardness that is higher than 15 GPa, preferably a metal carbide or boride, more preferably a silicon or boron carbide or a mixture of these two carbides, the maximum equivalent diameter of said grains being smaller than or equal to 500 micrometers; and - a matrix binding said grains, said matrix consisting essentially of a silicon nitride and / or silicon oxynitride phase or of a SiMON phase, where M is a metal chosen from Ca, Mg, Sr, Ba, said matrix representing between 5 and 40% by weight of said constituent material of the ceramic body; said ceramic material having an open porosity that is higher than 5% and lower than 14% and a metallic silicon content in said material, expressed per mm of thickness of said body, that is lower than 0.5% by weight.