COLOR MIRROR

DE602019061469T2Active Publication Date: 2024-11-06SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602019061469
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-28
Filing Date
2019-03-27
Publication Date
2024-11-06
Estimated Expiration
2039-03-27

AI Technical Summary

Technical Problem

Specular mirrors with a silver reflective layer lack options for achieving a bronze or golden tint, and existing solutions do not provide adequate corrosion protection and optical opacity simultaneously.

Method used

A specular mirror is created using a glass substrate coated with a stack of thin layers, including a reflective silver layer and a paint layer, where the stack comprises silicon nitride and metal layers, optimized by magnetic field-assisted cathode sputtering, to achieve the desired tint and corrosion resistance.

Benefits of technology

The solution provides mirrors with a bronze or golden tint while ensuring excellent corrosion resistance and opacity, with specific colorimetric coordinates and high light reflection, effectively addressing the limitations of existing mirror technologies.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to the field of mirrors. More particularly, it concerns specular mirrors, in which a user can see their reflection. Such mirrors are, for example, placed inside dwellings, such as in bathrooms, or are used as elements of furniture (closet doors, etc.) or decoration. These mirrors generally comprise a glass substrate coated on face 2 (the face opposite the one facing the user) with a reflective silver layer, which is itself coated with a layer of paint. The paint has an optical function: to prevent any visibility through the mirror by blocking the passage of light rays transmitted through the silver layer. The paint also serves to protect the silver layer against corrosion. Document WO 2015 / 177474 A1 describes a specular mirror having a pink or pinkish tint in reflection.

[0002] The aim of the invention is to provide a mirror that reflects a bronze or gold tint.

[0003] For this purpose, the invention relates to a specular mirror according to claim 1.

[0004] The invention also relates to a method for obtaining the aforementioned mirror, according to claim

[0005] The term "coated" means that the layer coating the substrate or another layer is deposited on top of said substrate or that other layer, but not necessarily in contact with them. When a first layer is placed "on top" of a second layer, it means that the first layer is further from the substrate than the second layer.

[0006] The term "based on" generally means that the layer comprises at least 50% by weight of the compound in question, in particular at least 60%, and even 70%, 80%, or 90% by weight of the compound in question. A silicon nitride-based layer advantageously comprises at least 80%, or even 90%, silicon nitride. When deposited by magnetically assisted sputtering, it advantageously includes a small amount of aluminum, since doping a silicon target with aluminum accelerates layer deposition. The stoichiometry of the silicon nitride layer is not specified here. The metallic layer is preferably made of the aforementioned metal or alloy.

[0007] Preferably, the stack of thin films is in contact with the glass substrate and the reflective silver layer. The mirror then preferably consists of the glass substrate, the stack of thin films, the reflective silver layer, and the paint layer. The paint layer is normally in contact with the reflective silver layer.

[0008] The concept of contact does not, however, preclude the presence of surface treatments commonly used in the silver plating process, when the silver layer is deposited using this method. In this latter case, it is advantageous to treat the surface onto which the silver will be deposited with a solution containing tin and palladium chlorides. These treatments can form extremely thin layers detectable only by advanced analytical techniques.

[0009] The thin-film stack preferably comprises only one metallic layer. The thin-film stack preferably comprises a single silicon nitride-based layer disposed above the metallic layer, or a single silicon nitride-based layer disposed below the metallic layer, or two silicon nitride-based layers disposed on either side of the metallic layer.

[0010] The glass substrate is preferably a flat substrate. The thickness of the glass substrate is preferably in the range of 1 to 19 mm, in particular 2 to 12 mm and even 3 to 9 mm.

[0011] The glass is preferably a soda-lime silicate glass, but other types of glass such as borosilicates or aluminosilicates may be used. The glass is preferably obtained by flotation. The glass is preferably colorless. It preferably comprises an iron content by weight, expressed as Fe₂O₃, of between 0.01 and 0.20%, in particular between 0.04 and 0.12%.

[0012] The reflective silver layer is deposited by silvering. Silvering refers to the process classically used for the manufacture of mirrors, and which includes the liquid deposition of a silver salt and a reducing agent.

[0013] The reflective silver layer preferably has a physical thickness ranging from 50 to 200 nm, especially from 50 to 100 nm.

[0014] The mirror is preferably "copper-free", in the sense that the reflective silver layer is not covered by a layer of copper.

[0015] In mirrors, the paint layer is generally obtained by drying a liquid paint applied to the substrate. Throughout this text, the term "paint" will be used to refer to paint in its dry state, while the term "liquid paint" will be used to refer to paint in its liquid state, intended to be applied to the substrate.

[0016] Liquid paint is preferably water-based or solvent-free. "Water-based" means that the liquid paint contains less than 10%, specifically 5% by weight, of organic solvent, or even contains no organic solvents at all.

[0017] The weight percentage of dry extract in liquid paint is preferably at least 50%, or even 60%, particularly 60 to 70% in the case of water-based liquid paints. It can be 100% in the case of solvent-free liquid paint.

[0018] The paint layer preferably comprises at least one resin and at least one mineral filler, including at least one pigment. At least one resin is preferably selected from acrylic resins, polyurethane resins, epoxy resins, and alkyd resins. At least one mineral filler is advantageously selected from zinc oxide, barium sulfate, zinc phosphates, particularly zinc orthophosphate, talc, calcium carbonate, mica, titanium dioxide, carbon black, and mixtures thereof. The mineral fillers improve the corrosion resistance of the silver layer and / or provide the desired opacity or tint. The paint layer preferably does not contain lead. The paint layer preferably comprises 20 to 50% by weight of resins and 30 to 80% by weight of mineral fillers. The paint layer may further include various additives, such as defoamers, biocides, or surfactants.The liquid paint layer is preferably applied with a curtain, by spraying or with a roller. It can be applied in several coats.

[0019] The drying stage is preferably carried out in an oven at a temperature between 50 and 250°C, particularly between 100 and 200°C. The drying time is preferably 2 to 60 minutes, particularly 5 to 30 minutes. The drying stage is preferably preceded by a pre-drying stage at a lower temperature, particularly between 30 and 60°C for 5 to 60 minutes.

[0020] The paint layer (after drying) preferably has a thickness between 40 and 350 µm, in particular between 70 and 300 µm, or even between 100 and 250 µm.

[0021] Thin film stacking is preferably deposited by magnetic field-assisted sputtering. However, other techniques are possible, for example chemical vapor deposition (CVD).

[0022] In one embodiment, the thin-film stack comprises only a single silicon nitride-based layer. This layer is, in particular, positioned above or below the single metallic layer of the stack, preferably in contact with this metallic layer.

[0023] According to another embodiment, the thin-film stack comprises only two silicon nitride-based layers. These are preferably arranged on either side of the single metallic layer of the stack, each preferably being in contact with this metallic layer.

[0024] The thin-film stack advantageously includes, in contact with the reflective silver layer, an adhesion layer. This layer, intended to improve the adhesion of the silver layer, is preferably made of a metal oxide, particularly titanium oxide. The titanium oxide adhesion layer is preferably deposited by magnetic field-assisted sputtering using a titanium oxide ceramic target, preferably without the addition of oxygen to the plasma or with only a small amount added. The adhesion layer preferably has a physical thickness ranging from 2 to 20 nm, particularly from 3 to 10 nm.

[0025] The stacking of thin films preferably consists of 2, 3, or 4 thin films, especially 3 or 4 thin films.

[0026] The stacking of thin films is for example made up, successively from the glass substrate, of a metallic layer (advantageously in contact with the glass substrate) - in particular in nickel and chromium alloy, then of a silicon nitride-based layer, then of an adhesion layer (advantageously in contact with the reflective silver layer).

[0027] According to another advantageous example, the stack of thin films consists, successively from the glass substrate, of a first layer based on silicon nitride (advantageously in contact with the glass substrate), then of a metallic layer - in particular in nickel and chromium alloy, then of a second layer based on silicon nitride, then of an adhesion layer (advantageously in contact with the reflective silver layer).

[0028] The order of the layers and their thickness influence the resulting reflective color. This allows for varying shades, from bronze to gold.

[0029] The physical thickness of the silicon nitride-based layer (in the case of a stack comprising only one such layer), or the sum of the physical thicknesses of each silicon nitride-based layer (in the case of a stack comprising several such layers), is, according to the invention, within a range of 10 to 200 nm, in particular from 10 to 100 nm, or even from 10 to 50 nm or from 10 to 30 nm. It has been observed that greater thicknesses produce more bronze-like hues.

[0030] The physical thickness of the metallic layer (in the case of a stack comprising only one such layer), or the sum of the physical thicknesses of each metallic layer (in the case of a stack comprising several such layers), is, according to the invention, within a range of 2 to 10 nm, in particular from 2 to 7 nm, or from 3 to 10 nm. Thicknesses greater than 10 nm produce very dark shades, while thicknesses less than 2 nm produce very light shades.

[0031] According to one embodiment of the invention, the silicon nitride-based layer or at least one layer has, at a wavelength of 550 nm, a refractive index n ranging from 2.2 to 2.6, in particular from 2.3 to 2.5, and an extinction coefficient k ranging from 0.02 to 0.6, in particular from 0.03 to 0.3. This gives rise to mirrors exhibiting a more intense tint, particularly in bronze.

[0032] The extinction coefficient corresponds to the imaginary part of the complex refractive index. These parameters can be measured using known methods by ellipsometry. Such values ​​can be obtained by depositing the silicon nitride-based layer by magnetically assisted reactive sputtering, through a judicious choice of the nitrogen proportion in the plasma, particularly by reducing the nitrogen proportion compared to the usual conditions for depositing silicon nitride-based layers. Under normal conditions, the nitrogen and argon flow rates are approximately equal, resulting in refractive indices on the order of 2.1 and extinction coefficients on the order of 0. By reducing the nitrogen flow rate, for example, to about three times lower than the argon flow rate, the aforementioned preferred ranges of values ​​can be obtained.

[0033] The mirror according to the invention preferably has the following colorimetric coordinates in reflection: L* ranging from 40 to 85, in particular from 50 to 85, or even from 60 to 80; a* ranging from 0 to 20, in particular from 1 to 12, or even from 1 to 10; b* ranging from 5 to 30, in particular from 10 to 25, or even from 12 to 18. Low values ​​of a* give rather golden hues, and higher values ​​of a* correspond to bronze hues. The colorimetric coordinates are calculated from a reflection spectrum between 380 and 780 nm, taking into account the D65 illuminant and the CIE-1964 reference observer (10°). The light reflection of the mirror (also taking into account the illuminant D65 and the CIE-1964 reference observer (10°)) is preferably at least 50%, and ideally 60%. Light transmission, however, is zero due to the presence of the opaque paint layer.

[0034] The mirror preferably exhibits good corrosion resistance. Typically, edge corrosion is at most 1.5 mm, or even 1.2 mm and 1.0 mm after a 120-hour CASS test according to ISO 9227:2012. The CASS test is a copper-acetic salt spray resistance test.

[0035] The invention is illustrated by the following non-limiting examples. Example 1

[0036] A clear glass substrate marketed by the Applicant under the trade name Planiclear was coated with a stack of thin films by magnetic field assisted sputtering (magnetron process).

[0037] The stacking consists successively of: a layer of nickel and chromium alloy, deposited directly on the surface of the glass, and having a physical thickness of 5 nm, then a layer of silicon nitride comprising 8% by weight of aluminium, and having a physical thickness of 10 nm, deposited using a silicon and aluminium target, under a flow of plasmagenic gas comprising 47% by volume of nitrogen and 53% by volume of argon, then, an adhesion layer of titanium oxide with a physical thickness of 5 nm, deposited using a substoichiometric titanium oxide ceramic target, in the absence of oxygen in the plasma.

[0038] The substrate with this stack was then coated with a reflective silver layer using a silver plating process. The silver layer is 70 nm thick. In a known manner, the silver layer was then coated with a layer of paint.

[0039] The values ​​of n and k at 550 nm of the silicon nitride layer are respectively 2.08 and 0.00.

[0040] The colorimetric coordinates in reflection of the obtained mirror (illuminant D65 and reference observer CIE-1964) are as follows: L*=74.5, a*=1.43 and b*=15.40. The reflected tint is golden. Example 2

[0041] A clear glass substrate marketed by the Applicant under the trade name Planiclear was coated with a stack of thin films by magnetic field assisted sputtering (magnetron process).

[0042] The stacking consists successively of: a first layer of silicon nitride comprising 8% by weight of aluminum, and having a physical thickness of 50 nm, deposited using a silicon and aluminum target, under a plasma gas flow comprising 26% by volume of nitrogen and 74% by volume of argon, then, a layer of a nickel and chromium alloy, deposited directly on the surface of the glass, and having a physical thickness of 7 nm, then a second layer of silicon nitride comprising 8% by weight of aluminum, and having a physical thickness of 50 nm, deposited like the first layer of silicon nitride, then, an adhesion layer of titanium oxide with a physical thickness of 5 nm, deposited using a substoichiometric titanium oxide ceramic target, in the absence of oxygen in the plasma.

[0043] The substrate, with its stack, was then coated with a reflective layer of silver using a silver plating process. The silver layer is 70 nm thick. In a known manner, the silver layer was then coated with a layer of paint.

[0044] The values ​​of n and k at 550 nm of the silicon nitride layer are 2.42 and 0.09 respectively.

[0045] The colorimetric coordinates in reflection of the obtained mirror (illuminant D65 and reference observer CIE-1931) are as follows: L*=68.1, a*=6.17 and b*=13.88. The hue in reflection is bronze.

Claims

1. A specular mirror comprising a glass substrate coated on one of the faces thereof, successively starting from said glass substrate, with a stack of thin layers, with a reflective silver layer deposited by silvering then with a layer of paint, characterized in that said stack of thin layers comprises: - at least one metal layer based on a metal chosen from niobium and titanium or based on a nickel-chromium alloy wherein the physical thickness of the metal layer, or the sum of the physical thicknesses of each metal layer, is within a range from 2 to 10 nm, and - at least one layer based on silicon nitride wherein the physical thickness of the layer based on silicon nitride, or the sum of the physical thicknesses of each layer based on silicon nitride, is within a range from 10 to 200 nm.

2. The mirror as claimed in claim 1, wherein the stack of thin layers is in contact with the glass substrate and with the reflective silver layer.

3. The mirror as claimed in either of the preceding claims, wherein the layer of paint is in contact with the reflective silver layer.

4. The mirror as claimed in one of the preceding claims, wherein the metal layer is based on a nickel-chromium alloy.

5. The mirror as claimed in one of the preceding claims, wherein the stack of thin layers comprises only a single metal layer.

6. The mirror as claimed in the preceding claim, wherein the stack of thin layers comprises a single layer based on silicon nitride positioned on top of the metal layer, or a single layer based on silicon nitride positioned underneath the metal layer, or two layers based on silicon nitride positioned on either side of the metal layer.

7. The mirror as claimed in one of the preceding claims, wherein the reflective silver layer has a physical thickness ranging from 50 to 200 nm.

8. The mirror as claimed in one of the preceding claims, wherein the stack of thin layers comprises, in contact with the reflective silver layer, an adhesion layer made of metal oxide, in particular made of titanium oxide.

9. The mirror as claimed in one of the preceding claims, wherein the stack of thin layers consists of two, three or four thin layers.

10. The mirror as claimed in one of the preceding claims, wherein the or at least one layer based on silicon nitride has, at a wavelength of 550 nm, a refractive index n ranging from 2.2 to 2.6 and an extinction coefficient k ranging from 0.02 to 0.06.

11. The mirror as claimed in one of the preceding claims, which has the following colorimetric coordinates in reflection: L* ranging from 40 to 85, a* ranging from 0 to 20, b* ranging from 5 to 30.

12. A process for obtaining a mirror as claimed in one of the preceding claims, comprising a step of depositing the stack of thin layers on a glass substrate, then a step of depositing, by silvering, the reflective silver layer on said stack of thin layers, then a step of depositing a layer of liquid paint on said silver layer, then a step of drying said layer of liquid paint.

13. The process as claimed in the preceding claim, wherein the stack of thin layers is deposited by magnetron sputtering.