METHOD FOR THE MANUFACTURE OF PAPER OR CARDBOARD
Patent Information
- Application Number
- DE602021021912
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-22
- Filing Date
- 2021-12-21
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The paper industry faces challenges in achieving improved drainage and machinability in paper production due to rapid and difficult-to-control reactions of polyvinylamine with dialdehydes, which result in high transportation costs and potential machine alterations from polymer gel formation.
A process involving the functionalization of polymers with isocyanates and the addition of compounds with aldehyde functions, followed by reactions within a fibrous suspension, to enhance drainage and dry resistance properties without gel formation, allowing for on-site polymer injection and maintaining machinability.
This process improves drainage and dry resistance properties while preventing polymer gel formation, thus maintaining machine operability and reducing costs by enabling on-site polymer application.
Description
Field of invention
[0001] The present invention relates to a process for the manufacture of paper or cardboard having improved drainage and machinability properties. More specifically, the invention relates to a process involving the preparation of a polymer resulting from functionalization with isocyanates and the addition of compounds comprising at least one aldehyde function before its addition to the fibrous suspension used to manufacture the paper or cardboard.
[0002] The present invention also relates to papers and cardboards with improved physical properties obtained by this process. Prior art
[0003] The paper industry is constantly seeking to optimize its manufacturing processes, particularly in terms of efficiency, productivity, cost reduction and quality of finished products.
[0004] The use of polymers as dry strength, drainability and machinability agents is very widely described.
[0005] Drainage properties relate to the ability of the fiber mat to evacuate or drain the maximum amount of water before drying. Improved drainage properties mean energy savings and increased production capacity.
[0006] Machinability refers to the optimization of the operation of the paper machine by increasing productivity through better drainage on the table, better dryness in the press section, a reduction in breakages through greater cleanliness of the circuits and a reduction in deposits.
[0007] WO 2012 / 017172 describes a method of manufacturing a sheet of paper or board having improved retention and drainage properties.
[0008] WO 00 / 11046 describes a papermaking process improving dry or wet strength.
[0009] Polyvinylamines are known to improve drainage during paper formation. US Patent 8,262,859 describes that the reaction of polyvinylamine with at least one dialdehyde produces a functionalized polyvinylamine that gives the paper or board improved strength in the wet and / or dry state. However, this reaction is very rapid, difficult to control, and is carried out in a very dilute medium, which results in a significant cost for transporting the product from the production site to the papermaking site. This reaction also causes the reaction medium to gel. Therefore, this reaction cannot be undertaken directly at the papermaking site just upstream of the injection of the polymer into the cellulose fiber, as it risks impairing machinability due to deposits generated on the paper machine. Statement of the invention
[0010] Unexpectedly, the Applicant discovered that a papermaking process using a polymer resulting, just upstream of its injection into a fibrous suspension (advantageously a suspension of cellulose fibers), from functionalization by isocyanates and the addition of compounds comprising at least one aldehyde function makes it possible to improve the drainage and dry strength properties. In addition, during this process, no formation of polymer gel is observed, which means that machinability is not impaired.
[0011] More specifically, the invention relates to a method for manufacturing a sheet of paper or cardboard from a fibrous suspension (advantageously a suspension of cellulose fibers), during which a water-soluble polymer P1 comprising at least one non-ionic monomer chosen from acrylamide, methacrylamide, N,N-dimethylacrylamide and acrylonitrile is subjected to a reaction Re1to give a polymer P2, which is then subjected to a reaction Re2 to give a polymer P3, which is injected into the fibrous suspension within 24 hours (less than or equal to 24 hours) from the start of the reaction Re1 ; The reaction Re1 consisting of adding an alkali and / or alkaline earth hydroxide and an alkali and / or alkaline earth hypohalide to the polymer P1 in order to obtain the polymer after 10 seconds to 60 minutes P2 functionalized by isocyanates, The reaction Re2 consisting of adding a compound functionalized by at least one aldehyde or capable of generating at least one aldehyde function on the polymer P2 in order to obtain the polymer P3.
[0012] In other words, the method of manufacturing a sheet of paper or cardboard from a fibrous suspension, according to the invention, comprises the following steps: a) injection of a polymer P3 in a suspension of cellulose fibers, b) formation of a sheet of paper or cardboard, c) drying of the sheet of paper or cardboard, the polymer P3 being prepared, prior to step a), according to the reactions Re1 has Re2, from a water-soluble polymer P1 of at least one non-ionic monomer chosen from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile: Re1 : preparation of a polymer P2comprising isocyanate functions by reaction for 10 seconds to 60 minutes between (i) an alkali metal hydroxide and / or an alkaline earth metal hydroxide, (ii) an alkali metal hypohalide and / or an alkaline earth metal hypohalide and (iii) the polymer P1, Re2 : preparation of a polymer P3 by reaction between (iv) a compound comprising at least one aldehyde function or a compound capable of generating at least one aldehyde function and (v) the polymer P2 comprising isocyanate functions, the polymer P3 being injected into the fibrous suspension during step a) within 24 hours of the start of the reaction Re1.
[0013] This process is advantageously devoid of a decarboxylation step (elimination of COz) after the reaction Re1. In fact, this would consume the isocyanate functions necessary for carrying out the reaction Re2.The process is advantageously devoid of a decarboxylation step (removal of COz) after the reaction Re2, especially when the reaction Re2 is partial (reaction of part of the isocyanate functions).
[0014] In the remainder of the description and in the claims, all polymer dosages expressed in gt -1< or kg.t -1< are given as weight of active polymer per tonne of dry matter. The dry matter corresponds to the dry extract obtained after evaporation of the water from the fibrous suspension used in a process for manufacturing a sheet of paper or cardboard. The dry matter is generally based on cellulose fibres and fillers, advantageously consisting of cellulose fibres and fillers. The term "cellulose fibres" encompasses any cellulose entity, including fibres, fines, microfibrils or nanofibrils. By fibrous suspension is meant the thick pulp or the diluted pulp which are based on water and cellulose fibres. The thick pulp ( Thick Stock ) , having a mass concentration of dry matter greater than 1%, or even greater than 3%, is upstream of the mixing pump ( fan pump ) . The diluted paste ( Thin Stock ), having a mass concentration of dry matter generally less than 1%, is located downstream of the mixing pump.
[0015] The term "polymer" refers to both homopolymers and copolymers.
[0016] An amphoteric polymer is a polymer comprising cationic charges and anionic charges, preferably as many anionic charges as cationic charges.
[0017] As used herein, the term "water-soluble polymer" means a polymer that gives an aqueous solution without insoluble particles when dissolved under stirring for 4 hours at 25°C and with a concentration of 20 gL -1< in water.
[0018] Value ranges include lower and upper bounds. Thus, the value ranges "between 0.1 and 1.0" and "from 0.1 to 1" include the values 0.1 and 1.0.
[0019] The water-soluble polymer P1contains at least one non-ionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, acrylonitrile. Optionally, it may also contain anionic and / or cationic and / or zwitterionic monomers.
[0020] The anionic monomers are preferably chosen from the group comprising monomers having a carboxylic acid function and their salts, including acrylic acid, methacrylic acid, itaconic acid, maleic acid; monomers having a sulfonic acid function and their salts; including acrylamido tert-butyl sulfonic acid (ATBS), allyl sulfonic acid and methallyl sulfonic acid, and their salts, and monomers having a phosphonic acid function and their salts.
[0021] Generally, salts of anionic monomers of polymers P1 has P5are salts of an alkali metal, an alkaline earth metal or an ammonium (preferably a quaternary ammonium).
[0022] The cationic monomers are preferably selected from the group comprising quaternized or salified dimethylaminoethyl acrylate (ADAME), quaternized or salified dimethylaminoethyl methacrylate (MADAME), diallyldimethylammonium chloride (DADMAC), acrylamidopropyltrimethylammonium chloride (APTAC), and methacrylamidopropyltrimethylammonium chloride (MAPTAC).
[0023] Advantageously, the cationic monomer salts of the polymers P1 has P5 are salts of a halide, preferably the chloride.
[0024] The zwitterionic monomers are preferably chosen from the group comprising sulfobetaine monomers such as sulfopropyl dimethylammonium ethyl methacrylate, sulfopropyl dimethylammonium propylmethacrylamide, or sulfopropyl 2-vinylpyridinium; phosphobetaine monomers, such as phosphato ethyl trimethylammonium ethyl methacrylate; and carboxybetaine monomers.
[0025] Preferably, the water-soluble polymer P1 is non-ionic. In other words, it preferably only comprises non-ionic monomers. Even more preferably, P1 is a homopolymer of acrylamide or methacrylamide.
[0026] The polymer P1may be linear, structured or crosslinked. The crosslinking agents allowing the structuring may in particular be chosen from sodium allyl sulfonate, sodium methallyl sulfonate, sodium methallyl disulfonate, methylenebisacrylamide, triallylamine and triallylammonium chloride.
[0027] Polymer structuring P1 can also be obtained with at least one polyfunctional compound containing at least 3 heteroatoms chosen from N, S, O, P and each having at least one mobile hydrogen. This polyfunctional compound can in particular be a polyethyleneimine or a polyamine.
[0028] The polymer P1 has a weight-average molecular weight of between 100,000 and 20 million, preferably between 250,000 and 5 million daltons.
[0029] According to the present invention, the weight average molecular weight of the polymer P1is determined by measuring the intrinsic viscosity. The intrinsic viscosity can be measured by methods known to those skilled in the art and can in particular be calculated from the reduced viscosity values for different concentrations by a graphical method consisting of plotting the reduced viscosity values (on the y-axis) as a function of the concentrations (on the x-axis) and extrapolating the curve to zero concentration. The intrinsic viscosity value is read off the y-axis or using the least squares method. Then, the weight-average molecular weight can be determined by the well-known Mark-Houwink equation: η = K M α [η] represents the intrinsic viscosity of the polymer determined by the solution viscosity measurement method, K represents an empirical constant, M represents the molecular weight of the polymer, α represents the Mark-Houwink coefficient, α and K depend on the particular polymer-solvent system. Tables known to those skilled in the art give the values of α and K depending on the polymer-solvent system.
[0030] The reaction Re1 consists of adding (i) an alkali metal hydroxide and / or an alkaline earth metal hydroxide and (ii) an alkali metal hypohalide and / or an alkaline earth metal hypohalide (iii) to the polymer P1 in order to obtain the polymer P2 functionalized by isocyanates.
[0031] Advantageously, the alkali hydroxide is soda (sodium hydroxide) and the alkali hypohalide is sodium hypochlorite.
[0032] The reaction Re1 is advantageously carried out on the polymerP1 at a polymer mass concentration P1 between 0.5 and 20% in aqueous solution, preferably between 1 and 10%.
[0033] For the reaction Re1, the Alpha coefficient = moles of hypohalide (alkaline and / or alkaline-earth) / moles of non-ionic monomer(s) of the polymer P1 is between 0.1 and 1.0 and the coefficient Beta = moles of hydroxide (alkaline and / or alkaline earth) / moles of hypohalide (alkaline and / or alkaline earth) is between 0.5 and 4.0.
[0034] The Alpha coefficient allows us to determine the quantity of isocyanate functions formed during the reaction Re1 from the non-ionic monomers of the polymer P1 (acrylamide, methacrylamide, N,N-dimethylacrylamide and acrylonitrile). This is not the Mark-Houwink coefficient denoted α.
[0035] The reaction Re1 is carried out at a temperature between 30°C and 60°C.
[0036] Thus, according to a particular embodiment, the reaction Re1 can be made from an aqueous solution having a polymer mass concentration P1 between 0.5 and 20%, at a temperature between 30°C and 60°C and in the presence of an Alpha coefficient between 0.1 and 1.0, the Alpha coefficient being the ratio between the number of moles of hypohalide and the number of moles of non-ionic monomer of the polymer P1.
[0037] The reaction Re2 consists of adding a compound comprising at least one aldehyde function or a compound capable of generating at least one aldehyde function on the polymer P2 in order to obtain the polymer P3.
[0038] The reaction Re2 is advantageously carried out on the polymer P2 at a polymer mass concentration P2 between 0.5 and 20% in aqueous solution, preferably between 1 and 5%.
[0039] Advantageously, the reaction Re2 takes place by direct addition of the compound comprising at least one aldehyde function or of the compound capable of generating at least one aldehyde function in the reaction medium (aqueous solution) resulting from the reaction Re1.
[0040] The reaction Re2 is carried out at a temperature between 10°C and 60°C, preferably between 20 and 40°C.
[0041] Without wishing to be limited by any theory, it would seem that, during the reaction Re2, the isocyanate functions of the polymer P2 react with aldehyde functions, for example to form imine functions of the type -N=C(HR 1< ).
[0042] The compound comprising at least one aldehyde function has a molecular weight advantageously less than or equal to 200 g.mol -1< .
[0043] Preferably, the compound comprising at least one aldehyde function is chosen from glyoxal, glutaraldehyde, furan-dialdehyde, 2-hydroxyadipaldehyde, succinaldehyde, starch dialdehyde, 2,2-dimethoxyethanal and combinations thereof. Even more preferably, the compound comprising at least one aldehyde function is glyoxal.
[0044] The compound capable of generating at least one aldehyde function has a molecular weight advantageously less than or equal to 500,000 g.mol -1< , more advantageously less than or equal to 100,000 g.mol -1< , for example less than or equal to 50,000 g.mol -1< . It has a molecular weight advantageously greater than or equal to 500 g.mol -1< , for example greater than or equal to 1,000 g.mol -1< .
[0045] According to one embodiment, the compound capable of generating at least one aldehyde function is a polyepoxide, for example polyethylene glycol diepoxide or polyethylene glycol triepoxide. In this case, it is a precursor of a compound comprising at least one aldehyde function.
[0046] According to another embodiment, the compound capable of generating at least one aldehyde function is preferably a polymer P5 non-ionic, cationic, anionic or amphoteric resulting from the reaction between at least one compound comprising at least one aldehyde function and at least one base polymer P4 of at least one non-ionic monomer chosen from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile.
[0047] The base polymer P4 may be non-ionic, cationic or anionic or amphoteric. It is advantageously water-soluble.
[0048] The polymer P4may comprise a cationic monomer which is preferentially selected from the group comprising quaternized or salified dimethylaminoethyl acrylate (ADAME), quaternized or salified dimethylaminoethyl methacrylate (MADAME), dimethyldiallylammonium chloride (DADMAC), acrylamidopropyltrimethylammonium chloride (APTAC), and methacrylamidopropyltrimethylammonium chloride (MAPTAC).
[0049] The polymer P4 may comprise an anionic monomer which is preferentially chosen from 2-acrylamido-2-methylpropane sulfonic acid, acrylic acid, methacrylic acid, itaconic acid, and / or their salts.
[0050] The compound comprising at least one aldehyde function reacting on P4 to give P5is advantageously chosen from glyoxal, glutaraldehyde, furan-dialdehyde, 2-hydroxyadipaldehyde, succinaldehyde, starch dialdehyde, 2,2-dimethoxyethanal and combinations thereof. Even more preferably, the compound comprising at least one aldehyde function is glyoxal.
[0051] The polymer P5 has a molecular weight advantageously between 100,000 g.mol -1< and 2,000,000 g.mol -1< , for example between 120,000 g.mol -1< and 1,000,000 g.mol -1< .
[0052] According to a preferred embodiment, the polymer P5 is obtained by reaction of a compound comprising at least one aldehyde function and at least one base polymer P4 within a maximum of 12 hours before being added to the polymer P2. This is the time between the start of the reaction and the addition to P2.
[0053] For the reaction Re2of the process of the invention, between 2 and 50%, preferably between 5 and 30% of compound comprising at least one aldehyde function or of compound capable of generating at least one aldehyde function are added to the polymer P2, the percentages being expressed by weight relative to the weight of the polymer P2.
[0054] Thus, some or all of the isocyanate functions of the polymer P2 can be functionalized.
[0055] According to a particular embodiment, an excess of compound comprising at least one aldehyde function or of compound capable of generating at least one aldehyde function may be added. In this case, during the reaction Re2, the molar quantity of aldehyde functions is greater than that of isocyanate functions.
[0056] The polymer P3 is advantageously used immediately after the reaction Re2, without purification.
[0057] According to a preferred embodiment, the polymer P3 is introduced into the white water and / or the thick paste and / or the mixture formed by the white water and the thick paste after homogenization of the fibrous suspension in the dilution pump (fan pump).
[0058] Advantageously, the polymer P3 can also be introduced into the papermaking process at the level of the forming table or the size press (coater), for example by spraying.
[0059] Between 0.25 and 15 kg.t -1< , and preferably between 0.5 and 5 kg.t -1< of polymer P3 are added to the fibrous suspension.
[0060] The fibrous suspension encompasses the possible use of different cellulosic fibers: virgin fibers, recycled fibers, chemical pulp, mechanical pulp, micro-fibrillated cellulose or nano-fibrillated cellulose. The fibrous suspension also encompasses the use of these different cellulosic fibers with all types of fillers such as TiO 2 , CaCO 3 (ground or precipitated), kaolin, organic fillers and their mixtures.
[0061] The polymer P3can be used within the papermaking process in combination with other products such as mineral or organic coagulants, dry strength agents, wet strength agents, natural polymers such as starches or carboxymethylcellulose (CMC), inorganic microparticles such as bentonite microparticles and colloidal silica microparticles, organic polymers of any ionic nature (non-ionic, cationic, anionic, or amphoteric) and which may be (without limitation) linear, branched, crosslinked, hydrophobic, or associative.
[0062] The following examples illustrate the invention without, however, limiting its scope. Examples of embodiments of the invention Procedures used in application testing: a) Types of pasta used
[0063] Virgin fiber pulp: Wet pulp is obtained by disintegrating dry pulp to obtain a final aqueous concentration of 1% by weight. It is a neutral pH pulp composed, by weight, of 90% bleached virgin long fibers, 10% bleached virgin short fibers, and 30% additional GCC (ground calcium carbonate) (Hydrocal ®< 55 from Omya) relative to the weight of the fibers.
[0064] Recycled fiber pulp: Wet pulp is obtained by disintegrating dry pulp to obtain a final aqueous concentration of 1% by weight. It is a pH-neutral pulp composed of 100% recycled cardboard fibers. b) Drainage Performance Assessment (DDA)
[0065] The DDA (Dynamic Drainage Analyzer) can automatically determine the time (in seconds) required to drain a fibrous suspension under vacuum. The polymers are added to the wet pulp (0.6 liters of 1.0% by weight pulp) in the DDA cylinder while stirring at 1000 rpm: T=0 s: Stirring of the paste T=20 s: Addition of the polymer T=30 s: Stop stirring and drain under vacuum at 200 mbar (1 bar = 10 5< Pa) for 70 seconds.
[0066] The pressure under the fabric is recorded as a function of time. When all the water is evacuated from the fibrous mat, the air passes through it, causing a break in slope to appear on the curve representing the pressure under the fabric as a function of time. The time, expressed in seconds, recorded at this break in slope corresponds to the drainage time. The shorter the time, the better the vacuum drainage. c) Performance in DSR application (dry strength), grammage at 90 gm -2 <
[0067] The necessary quantity of paste is taken in order to obtain a final sheet with a weight of 90 gm -2< .
[0068] The wet paste is introduced into the dynamic farmhouse vat and kept stirring. The various components of the system are injected into this paste according to the predefined sequence. A contact time of 30 to 45 seconds is generally observed between each addition of polymer.
[0069] Paper trusses are produced with an automatic dynamic trusses: a blotter and the forming fabric are placed in the bowl of the dynamic trusses before starting the rotation of the bowl at 1000 rpm -1< and building the water wall. The treated pulp is spread over the water wall to form the fibrous mat on the forming fabric.
[0070] Once the water is drained, the fibrous mat is recovered, pressed under a press delivering 4 bar, then dried at 117°C. The resulting sheet is conditioned overnight in a room with controlled humidity and temperature (50% relative humidity and 23°C). The dry strength properties of all the sheets obtained by this procedure are then measured.
[0071] Burst is measured with a Messmer Buchel M 405 burst tester according to TAPPI T403 om-02. The result is expressed in kPa. The burst index, expressed in kPa.m 2 < / g, is determined by dividing this value by the weight of the sheet tested.
[0072] The dry breaking length is measured in the machine direction using a Testometric AX tensile tester according to TAPPI T494 om-01. The result is expressed in km. Products tested in application trials: Polymer P1
[0073] 310 g of water are introduced into a 1 liter reactor equipped with a mechanical stirrer, a thermometer, a condenser and a nitrogen gas immersion rod. The pH of the reaction medium is adjusted to 3.3 using a pH buffer (NaOH 30% by weight in water and H 3 PO 4 75% by weight in water). The medium is heated and maintained at a temperature between 79 and 81 ° C using a water bath. Using two continuous pours, 400 g of acrylamide at 50% by weight in water, 0.28 g of N,N-methylene-bis-acrylamide at 100%, 237.8 g of water and 2.40 g of sodium methallyl sulfonate at 100% are incorporated (pour 1) for 180 minutes. Casting 2, 0.48 g of 100% sodium persulfate and 48 g of water are incorporated for 180 minutes. The polymer is left at 80°C for 120 minutes after the end of casting.
[0074] The polymer solution P1 obtained has a pH of 5.7, a polymer weight concentration of 20% and a viscosity of 6000 cps. Polymers P2
[0075] Preparation of a solution of P1 at 10% by weight in water, by diluting 20 g of a solution of P1 at 20% by weight in water with 20 g of water. The polymer solution is heated to 50°C.
[0076] A mixture of 14.6% sodium hypochlorite (by weight in water) and 30% sodium hydroxide (by weight in water) is prepared based on the alpha and beta coefficients for the reaction Re1. When the polymer solution P1 is at 50°C, the mixture of sodium hypochlorite and soda is added on P1. After 30 seconds of reaction, water is added. The polymer is obtained. P2 (Table 1: list of polymers P2). P2 Table 1: Polymers Alpha coefficient Beta coefficient Sodium hypochlorite Soda Water P2-A 0,35 2 10,05 5,25 144,70 P2-B 0,5 2 14,35 7,50 138,15 P2-C 0,7 2 20,10 10,50 129,40 P2-D 0,05 2 1,44 0,75 157,81 P2-E 0,35 6 10,05 15,75 134,20 Polymers P3
[0077] 3 minutes after obtaining the polymers P2,1.7 g of glyoxal (40% by weight in water) is added to carry out the reaction Re2, or 17% by weight relative to the polymer. The polymers are obtained P3-A1, P3-B1 And P3-C1. 3 minutes after obtaining the polymer P2-B, 6.5 g of polymer P5 and 25 g of water are added to carry out the reaction Re2, or 11% by weight relative to the polymer. The polymer is obtained P3-B3. 3 minutes after obtaining the polymers P2, the pH is adjusted to 10 and 0.67 g of glycerol triglycidyl ether (GE-100) is added to carry out the reaction Re2, or 17% by weight relative to the polymer. The polymers are obtained P3-A5 And P3-B5. 3 minutes after obtaining the polymers P2, the pH is adjusted to 10 and 0.67 g of Pentaerythritol tetraglycidyl ether (GE-500) is added to carry out the reaction Re2, or 17% by weight relative to the polymer. The polymers are obtained P3-A6 And P3-B6. Polymer P4
[0078] In a 1 liter reactor equipped with a mechanical stirrer, a thermometer, a condenser and a nitrogen gas dipstick, 153 g of water, 67 g of 64% diallyldimethylammonium chloride and 5.0 g of sodium hypophosphite are introduced. The pH of the reaction medium is adjusted to 2.5 using 96% sulfuric acid. The medium is heated and maintained at a temperature between 79 and 81°C using a water bath. Using two continuous pours, 715 g of 50% by weight acrylamide are incorporated in water for 135 minutes (pour 1). Pour 2, 4.0 g of 100% sodium persulfate and 56 g of water are incorporated for 160 minutes. The polymer is left at 80°C for 30 minutes after the end of casting. 1 g of 40% sodium bisulfite (by weight in water) is added before aging for 60 minutes at 80°C.
[0079] The polymer solution P4obtained has a pH of 5.2, a weight concentration of 40% and a viscosity of 2300 cps. Polymer P5
[0080] In a 1000 ml stirred reactor, 211 g of polymer P4 and 745 g of demineralized water are introduced. The reactor is equipped with a pH measuring probe. After 10 minutes of stirring, the pH is adjusted to 11.2 with a 30% by weight sodium hydroxide solution in water. The temperature is maintained between 19 and 26°C.
[0081] 42 g of glyoxal at 40% by weight in water are added. pH control and viscosity monitoring allow a product of 20 cps (end of reaction viscosity) to be obtained. When this viscosity is reached, the reaction is stopped by lowering the pH to less than 3.5 by adding H 2 SO 4 at 92% by weight in water. The final viscosity and pH are recorded. The polymer is obtained P5 at a weight concentration of 7.5%.
[0082] For all viscosity measurements, the viscometer is a Brookfield type, with an LV1 module and a speed of 60 rpm. Polymer P3 - THIS (counter-examples)
[0083] 3 minutes after obtaining the polymer P2-D, 1.7 g of Glyoxal (40% by weight in water) is added to carry out the reaction Re2, or 17% by weight relative to the polymer. The polymer is obtained P3 - CE-1. This is not stable and forms a solid gel. 3 minutes after obtaining the polymer P2-E, 1.7 g of Glyoxal (40% by weight in water) is added to carry out the reaction Re2, or 17% by weight relative to the polymer. We obtain the Polymer P3 - CE-2. Application testing Drainage performance (DDA).
[0084] Note: As the tests are carried out in series, a blank is redone each time. • Series 1
[0085] Table 2: Drainage depending on the polymer P2 or P3 Alpha Drainage(s) 1.7 kg / T 3.4 kg / T P2-A 0,35 17.46 14,46 P2-B 0,5 16,16 13,05 P2-C 0,7 15,88 12,88 P3-A-1 0,35 16,01 12,00 P3-B-1 0,5 14,58 10,89 P3-C-1 0,7 14,11 11,09 White 29,29
[0086] An improvement in drainage is observed with increasing alpha coefficient. Polymers P3 exhibit improved performance compared to polymers P2 for the same alpha coefficient. This demonstrates the benefit generated by the reaction Re2. • Series 2
[0087] Table 3: Drainage according to polymer Alpha Drainage(s) 1.7 kg / T 3.4 kg / T P2-B 0,5 18,34 13,03 P3-B-1 0,5 16,87 12,51 P3 B-3 0,5 17,52 12,73 P5 / 32,65 35,11 CE-3 0,5 21,69 15,04 White 34,4 CE-3 : simultaneous addition of a polymer P2 and a polymer P5 without prior mixing into the paper pulp during the draining sequence.
[0088] The glyoxalated polymer P5 alone does not present any interest in drainage. An improvement in drainage is observed with polymers P3 compared to a polymer P2. Adding the polymer P5 during of the reaction Re2 on the polymer P2 allows for a more efficient polymer to be obtained. • Series 3
[0089] Table 4: Drainage as a function of polymer Alpha Drainage(s) 1.7 kg / T 3.4 kg / T P2-A 0,35 24,29 18,61 P3-A-5 0,35 18,17 12,54 P3-A-6 0,35 18,73 12,66 P2-B 0,5 20,88 14,77 P3-B-5 0,5 17,88 12,34 P3-B-6 0,5 17,25 11,95 White 34,25
[0090] Improved drainage is observed with polymers P3 resulting from the addition of an epoxy to the polymer P2, during the reaction Re2. • Series 4
[0091] Table 5: Drainage as a function of polymer Alpha / Beta Drainage(s) 1.7 kg / T 1.7 kg / T + 0.6 kg / T PA 3.4 kg / T P2-B 0,5 / 2 17,06 12,05 13,2 P3-B-1 0,5 / 2 16,6 11,83 12,09 P3-CE-1 0,05 / 2 Freeze P3-CE-2 0,5 / 6 21,31 16,82 16,04 White 32,97 PA: Copolymer of acrylamide and acrylic acid (70 / 30, mol %) in the form of an aqueous dispersion
[0092] The polymer of the invention added with an anionic polymer PA generates improved drainage. The polymer P3-CE-2 having a beta coefficient greater than 4 does not provide performance in DDA. The P3-CE-1 polymer having an alpha coefficient of 0.05 is not usable. • Series 5
[0093] Table 6 Drainage as a function of polymer Alpha Drainage(s) 1.7 kg / T P2-B 0,5 17,53 P3-B-1 0,5 16,25 CE-5-3 18,88 CE-6-5 27,62 White 33,26 CE-5-3 And CE-6-5 are from US patent 8,262,859 (examples 3 and 5)
[0094] Glyoxalated polyvinylamines CE-5-3 And CE-6-5 have less efficient drainage than the polymer P3. Performance in DSR application (dry strength, Paste pH 6.5
[0095] Table 7: Dry strength as a function of polymer % Burst index % DBL SM % DBL ST White réf. réf. réf. P2-B 15 % 9 % 14 % P3-B-1 18 % 12 % 26 % P3-B-5 19 % 10 % 18 % P3-B-6 19 % 17 % 18 % CE-5-3 9 % 9 % 19 % CE-6-5 2 % 4 % 9 %
[0096] Burst performance is improved by the use of polymer P3 compared to Polymers P2 and to the CE counterexamples. The same trend is observed for the measurement of breaking length in the forward direction (DBL SM) and in the cross direction (DBL ST).
Claims
1. A method for producing a sheet of paper or cardboard from a fibrous suspension, comprising the following steps: a) injecting a polymer P3 into a cellulose fiber suspension, b) forming a sheet of paper or cardboard, c) drying the sheet of paper or cardboard, the polymer P3 being prepared, prior to step a), from a water-soluble polymer P1 of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile, the P1 polymer being subjected to a Re1 reaction to give a P2 polymer, which is then subjected to a Re2 reaction to give the P3 polymer, which is injected into the fibrous suspension within 24 hours of the start of the Re1 reaction ; - the Re1 reaction consisting in preparing a P2 polymer comprising isocyanate functions by reaction for 10 seconds to 60 minutes between (i) an alkali hydroxide and / or an alkaline-earth hydroxide, (ii) an alkali hypohalide and / or an alkaline-earth hypohalide and (iii) the polymer P1, the Re1 reaction being carried out at a temperature between 30°C and 60°C, with a coefficient Alpha = moles of hypohalide / moles of non-ionic monomer of the water-soluble polymer P1 is between 0.1 and 1.0 and a coefficient Beta = moles of hydroxide / moles of hypohalide is between 0.5 and 4.0, the P1 polymer having a weight average molecular weight between 100,000 and 20 million, - the Re2 reaction consisting in preparing a P3 polymer by reaction between (iv) a compound comprising at least one aldehyde function or a compound which can generate at least one aldehyde function, and (v) the P2 polymer comprising isocyanate functions, the Re2 reaction being carried out at a temperature between 10°C and 60°C, by adding to the P2 polymer between 2% and 50% of compound comprising at least one aldehyde function or of compound capable of generating at least one aldehyde function, % by weight with respect to the weight of the P2 polymer.
2. The method according to claim 1, characterized in that the P1 polymer is non-ionic.
3. The method according to claim 1 or 2, characterized in that the P1 polymer is an acrylamide or methacrylamide homopolymer.
4. The method according to one of claims 1 to 3, characterized in that, for the Re2 reaction, the compound comprising at least one aldehyde function is chosen from glyoxal, glutaraldehyde, furan-dialdehyde, 2-hydroxyadipaldehyde, succinaldehyde, starch dialdehyde, 2,2-dimethoxyethanal and combinations thereof.
5. The method according to any one of claims 1 to 4, characterized in that, for the Re2 reaction, the compound comprising at least one aldehyde function is glyoxal.
6. The method according to any of claims 1 to 5, characterized in that for the Re2 reaction, the compound that can generate at least one aldehyde function is a polyepoxide.
7. The method according to one of claims 1 to 6, characterized in that, for the Re2 reaction, the compound which can generate at least one aldehyde function is a nonionic, cationic, anionic, or amphoteric P5 polymer resulting from the reaction between a compound comprising at least one aldehyde function and at least one base polymer P4 comprising at least one nonionic monomer chosen from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile.
8. The method according to claim 7, characterized in that the base polymer P4 further comprises a cationic monomer selected from the group comprising quaternized or salified dimethylaminoethyl acrylate (ADAME) quaternized or salified dimethylaminoethyl methacrylate (MADAME), dimethyldiallylammonium chloride (DADMAC), acrylamidopropyltrimethylammonium chloride (APTAC), and methacrylamidopropyltrimethylammonium chloride (MAPTAC).
9. The method according to claim 7 or 8, characterized in that the base polymer P4 further comprises an anionic monomer of the selected from 2-acrylamido-2-methylpropane sulfonic acid, acrylic acid, methacrylic acid, itaconic acid, and / or salts thereof.
10. The method according to one of claims 7 to 9, characterized in that the P5 polymer is obtained by reaction between a compound comprising at least one aldehyde function and at least one base polymer P4 within a maximum of 12 hours before being added to the P2 polymer.
11. The method according to one of the claims 1 to 10, characterized in that the P3 polymer is introduced into the white water and / or into the thick stock and / or into the mixture formed by the white water and the thick stock after homogenization of the fibrous suspension in the fan pump.
12. The method according to any of claims 1 to 11, characterized in that the P1 polymer has a weight average molecular weight between 250,000 and 5 million daltons.
13. The method according to one of the claims 1 to 12, characterized in that: - the Re1 reaction is carried out from an aqueous solution having a mass concentration of polymer P1 of between 0.5 and 20%, at a temperature of between 30°C and 60°C; - the Re2 reaction is carried out in the presence of the P2 polymer and from 5 to 30% of compound comprising at least one aldehyde function or of compound capable of generating at least one aldehyde function, by weight relative to the P2 polymer.