Semi-finished products comprising a thermoplastic resin
The described process for mixing and heating reinforcing fibers with thermoplastic resin to achieve a higher crystallization temperature in semi-products addresses thermal degradation issues, resulting in high-quality composite materials with improved flow properties and reduced defects.
Patent Information
- Application Number
- FR2019000411
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-01-17
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is a need for semi-products with good flow properties and minimal thermal degradation to manufacture high-quality composite materials, particularly in industries like aeronautical, space, automotive, and sports equipment, where existing methods result in defects due to thermal degradation of thermoplastic resins during composite material production.
A process involving mixing reinforcing fibers with a thermoplastic resin, heating the resin to a temperature above its melting point, and optionally calendering, resulting in a semi-product with a crystallization temperature higher than the resin's, using methods like infrared irradiation and inert atmospheres to minimize thermal degradation.
The process produces semi-products with minimal thermal degradation, ensuring high-quality composite parts with improved flow properties and reduced defects, characterized by a crystallization temperature greater than the resin's, enhancing the manufacturing process.
Smart Images

Figure 00000024_0000 
Figure 00000024_0001 
Figure 00000025_0000
Abstract
Description
Title of the invention: Semi-finished products comprising a thermoplastic resin Field of invention
[0001] The present invention relates to a semi-finished product comprising reinforcing fibers and a thermoplastic resin. The present invention also relates to a method for manufacturing the semi-finished product, a method for manufacturing a composite part, and the composite part obtained from this semi-finished product. Technical background
[0002] Composite materials combining a thermoplastic resin with reinforcing fibers are of great interest in many fields due to their excellent mechanical properties for a low weight, particularly in the aeronautics and space industry, but also in the automobile industry and sports equipment.
[0003] These composite materials, which may be made of long, continuous or short fibers for example, can be obtained by conventional composite transformation processes using liquid resins (thermosetting or thermoplastic) or plastics processing processes (injection, resin transfer molding (RTM), injection molding, compression molding, (thermo)stamping, filament winding, etc.).
[0004] These composite materials are generally manufactured by assembling / stacking and consolidating semi-finished products made up of resin-coated reinforcing fibers such as pre-impregnated materials in the form of unidirectional sheets, wicks or woven fabrics.
[0005] These semi-finished products can be obtained for example by impregnating the fibers, which are generally unidirectional and continuous, with the resin. There are different processes, in which the resin can be either melted, dissolved in a solvent, in powder form, in a fluidized bed, or dispersed in an aqueous solution. The impregnated fibers are then, if necessary, freed from the solvent or aqueous solution and then heated in order to melt the retained resin and form the semi-finished product. It is also possible to provide the thermoplastic resin within the reinforcing fibers by intimate mixing (co-mixing) of reinforcing fibers with thermoplastic fibers brought to be melted to form the resin surrounding the reinforcing fibers. This semi-finished product is characterized by a homogeneous distribution of the resin (then called matrix) around the reinforcing fibers.
[0006] The document by lyer et al. in Journal of Thermoplastic composite materials, 1990 (p.325-355) describes the parameters which are essential for the development of a process for impregnating fibres with a dry powder of thermoplastic material.
[0007] Document US 3,742,106 describes a method for manufacturing a semi-finished product comprising passing the spread glass fibers through a bed of thermoplastic material powder and heating the fibers so as to melt the thermoplastic material and form a matrix of thermoplastic material around the fibers.
[0008] The article by Miller et al. in Composites Part A, 1998 (p.773-782) describes two methods of impregnating fibers with a thermoplastic material: the first method comprising mixing the reinforcing fibers with the thermoplastic material in fiber form and the second method comprising mixing the reinforcing fibers with the thermoplastic material in powder form.
[0009] The article by Funck et al. in Composites Manufacturing, 1995 (pp. 189-192) describes improved methods of heating thermoplastic tape (prepreg tape) by laser or direct flame heating.
[0010] The paper "Thermal Degradation Effects on Consolidation and Bonding in the Thermoplastic Fiber-Placement Process" by Fink et al. (Army Research Laboratory-ARL-TR-2238, June 2000) concerns the effects of thermal decomposition of polyetherketoneketone (PEKK) during a semi-finished product consolidation process.
[0011] The article by Tadini et al. in Aerospace Science and Technology, 2017 (p.106-116) concerns the analysis of the chemical degradation of PEKK-based composites for aeronautical components at high temperature.
[0012] The article by Patel et al. in Polymer Degradation and Stability, 2010 (p.709-718) presents different mechanisms of decomposition of PEEK and different products formed due to this decomposition.
[0013] The article by Vasconcelos et al. in Materials Research, 2013 (p.227-235) concerns the evaluation of the decomposition kinetics of PEEK in nitrogen as well as in synthetic air atmospheres.
[0014] There is still a need to provide a semi-finished product having good properties, in particular good flow properties, and exhibiting minimal degradation, in particular thermal degradation, for the manufacture of high-quality composite materials. Summary of the invention
[0015] The invention relates firstly to a method for manufacturing a semi-finished product, comprising the following steps:
[0016] • the supply of reinforcing fibers and a thermoplastic resin having a crystallization temperature Tcresine; • mixing the reinforcing fibers with the thermoplastic resin; • heating to melt the thermoplastic resin and for the bring to a temperature above the melting temperature of the resin; and • optionally, a calendering step;
[0017] the semi-finished product being characterized by a crystallization temperature Tcsemi.product, the Tcsemi product being greater than or equal to the Tcresine.
[0018] In some embodiments, the melting of the thermoplastic resin is carried out by heating the reinforcing fibers, or the thermoplastic resin, or both of the reinforcing fibers and the thermoplastic resin.
[0019] In some embodiments, heating is performed by infrared irradiation, UV irradiation, microwave irradiation, laser irradiation, convection heating or high frequency wave heating, and preferably by infrared irradiation.
[0020] In some embodiments, at least a portion of the thermoplastic resin melting step is performed under an inert atmosphere.
[0021] In some embodiments, during the step of melting the thermoplastic resin, the combination of reinforcing fibers and thermoplastic resin is provided with a power per unit mass of 10 to 1600 kW / kg, preferably 20 to 1400 kW / kg-
[0022] In some embodiments, heating the thermoplastic resin to a temperature above its melting temperature is carried out to a temperature of 320 to 420°C, and preferably 360 to 400°C.
[0023] In some embodiments, the Tcsemi-product is higher than the Tcresin by 1 to 10°C, and preferably by 4 to 8°C.
[0024] In some embodiments, the thermoplastic resin is one or more poly-aryletherketones selected from polyetherketones, polyetheretherketones, polyetherketoneketones, polyetheretherketoneketones, polyetherketoneetherketones, polyetheretherketoneetherketones, and polyetherdiphenyletherketones, polyetheretherketones, and preferably selected from polyetherketones, polyetherketoneketones, and polyetheretherketones.
[0025] In some embodiments, the reinforcing fibers are carbon fibers and / or glass fibers.
[0026] The invention also relates to a semi-finished product obtained according to the process described above.
[0027] The invention also relates to a method of manufacturing a composite part comprising the following steps:
[0028] • the manufacture of at least two semi-finished products according to the process described above • stacking semi-finished products in at least two layers of semi-finished products; • consolidation of layers of semi-finished products, and • cooling of the layers of consolidated semi-finished products in order to obtain the composite part.
[0029] In certain embodiments, the composite part is characterized by a crystallization temperature Tccomposite, where Tccomposite > Tcresine- 5°C.
[0030] The invention also relates to a method of manufacturing a composite part comprising the following steps:
[0031] • the supply of at least two semi-finished products as described above; • stacking semi-finished products in at least two layers of semi-finished products; • consolidation of layers of semi-finished products, and • cooling of the layers of consolidated semi-finished products in order to obtain the composite part.
[0032] In some embodiments, the composite part is characterized by a crystallization temperature Tccomposite, where Tccomposite > Tcsemi product- 10°C.
[0033] The invention also relates to a composite part obtained according to one of the methods described above.
[0034] In some embodiments, the composite part has a thickness of 0.05 to 150 mm, and / or a length of 0.01 to 100 m, and / or a width of 0.005 to 5 m.
[0035] In some embodiments, the composite part is a part of an air or space vehicle, or a part of a drilling rig, or a part intended to be positioned in contact with or near a vehicle engine or reactor, or a part intended to be subjected to friction.
[0036] The present invention makes it possible to meet the need expressed in the state of the art. It provides more particularly a semi-finished product having good properties, in particular good flow properties, and exhibiting minimal degradation, in particular thermal degradation, for the manufacture of high-quality composite materials.
[0037] It has been discovered by the present inventors that the manufacture of high-quality composite materials depends heavily on the properties of the semi-finished products. Indeed, obtaining semi-finished products with no or minimal degradation makes it possible to obtain the properties suitable for the manufacture of composite parts with few defects. Here, degradation will be defined as a mechanism which tends to initially slow down, then to hinder, the capacity of the semi-finished product to crystallize. This mechanism may be linked to an increase in molecular masses by branching of polymer chains. This degradation, which in the context of the invention is mainly a thermal degradation of the resin in the semi-finished product, must be minimal.The suitable properties of the semi-finished product produced according to the present invention and making it possible to obtain composite parts free from defects are mainly a good flow property as well as a good capacity to crystallize. The present inventors have found that the crystallization temperature of the semi-finished product is an indicator of the good properties of the semi-finished product as well as its . degradation and that a semi-finished product crystallization temperature Tcsemi product greater than or equal to the crystallization temperature of the thermoplastic resin alone Tcresine (before the manufacture of the semi-finished product) allows the production of semi-finished products with good properties and minimal degradation.
[0038] The present inventors have also discovered that when these semi-finished products are used for the manufacture of composite parts, the crystallization temperature of the composite part Tccomposite can also be an indicator of good properties and minimal degradation of the composite part. Brief description of the figures
[0039] [fig. 1 ] shows differential scanning calorimetry (DSC) analysis diagrams for a PEKK resin (A = first heating, B = second heating, C = cooling), where the temperature is represented on the abscissa (°C) and the heat flux is represented on the ordinate (W / g).
[0040] [fig.4] represents differential scanning calorimetry analysis diagrams (DSC) for a PEKK resin (A = first heating, B = second heating, C = cooling), where the temperature is represented on the abscissa (°C) and the heat flux is represented on the ordinate (W / g).
[0041] [fig.2] represents a DSC analysis diagram for a semi-finished product according to the invention (A = first heating, B = second heating, C = cooling), where the temperature is represented on the abscissa (°C) and the heat flow is represented on the ordinate (W / g).
[0042] [fig.3] represents a DSC analysis diagram for a composite part according to the invention (A = first heating, B = second heating, C = cooling), where the temperature is represented on the abscissa (°C) and the heat flow is represented on the ordinate (W / g).
[0043] [fig.5] represents a DSC analysis diagram for a semi-finished product according to a comparative example (A = first heating, B = second heating, C = cooling), where the temperature is represented on the abscissa (°C) and the heat flow is represented on the ordinate (W / g).
[0044] [fig.6] represents a DSC analysis diagram for a composite part according to a comparative example (A = first heating, B = second heating, C = cooling), where the temperature is represented on the abscissa (°C) and the heat flow is represented on the ordinate (W / g). Detailed description
[0045] The invention is now described in more detail and in a non-limiting manner in the following description.
[0046] Method of manufacturing a semi-finished product
[0047] The term "semi-finished product" means a product comprising a resin and reinforcing fibers, which is used as an intermediate product in the manufacture of composite materials. The semi-finished products according to the invention are pre-pregs (or tapes) in the form of a sheet of fibers in a resin matrix. The reinforcing fibers preferably have an essentially unidirectional orientation in the semi-finished product.
[0048] The resin of the semi-finished product is a thermoplastic resin which may comprise one or more thermoplastic materials. Similarly, the reinforcing fibers may consist of fibers of the same nature or fibers of different nature, both in terms of chemical nature (organic, inorganic, mineral, natural, bio-sourced, etc.) and dimensions (diameter, number).
[0049] The thermoplastic material may be one or more polyaryletherketones (PAEK).
[0050] By "PAEK" is meant polymers comprising units of formula (-Ar-X-) as well as units of formula (-Ar'-Y-), in which:
[0051] • Ar and Ar' each denote a divalent aromatic radical; • Ar and Ar' may preferably be chosen from 1,3-phenylene, 1,4-phenylene, 4,4'-biphenylene, 1,4-naphthylene, 1,5-naphthylene and 2,6-naphthylene, optionally substituted; • X denotes an electron-withdrawing group, which may preferably be chosen from the carbonyl group and the sulfonyl group; • Y denotes a group chosen from an oxygen atom, a sulfur atom, an alkylene group, such as in particular -CH2- and isopropylidene.
[0052] Among the X units, at least 50 mol.%, preferably at least 70 mol.% and more particularly, at least 80 mol.% of the X units represent a carbonyl group. In certain embodiments, all the X units denote a carbonyl group.
[0053] Among the Y units, at least 50 mol.%, preferably at least 70 mol.% and more particularly at least 80 mol.% of the Y units represent an oxygen atom. In certain embodiments, all the Y units denote an oxygen atom.
[0054] Thus, in certain embodiments, the PAEK is a polymer comprising, or preferably consisting of, units of formula (-Ar-CO-) as well as units of formula (-Ar'-O-), the Ar and Ar' units being as defined above.
[0055] In certain embodiments, the PAEK is a poly-ether-ketone-ketone (PEKK), comprising a succession of repeating units of the type -(Ari-O-Ar2-CO-Ar3 -CO)n-, each Arb Ar2 and Ar3 independently representing a divalent aromatic radical, preferably a phenylene.
[0056] In the above formula, as in all the formulas that follow, n represents an integer.
[0057]
[0058]
[0059]
[0060]
[0061]
[0062]
[0063]
[0064]
[0065]
[0066]
[0067]
[0068]
[0069] The bonds on either side of each Arb motif Ar2 and Ar3 can be of the para, or meta, or ortho type (preferably of the para or meta type). In some embodiments, the PEKK comprises a succession of repeating units of the following formula (IA) and / or formula (IB): (IA) OO Units of formula (IA) are units derived from isophthalic acid (or I units), while units of formula (IB) are units derived from terephthalic acid (or T units). In the PEKK used in the invention, the mass proportion of T units relative to the sum of the T and I units can vary from 0 to 5%; or from 5 to 10%; or from 10 to 15%; or from 15 to 20%; or from 15 to 20%; or from 20 to 25%; or from 25 to 30%; or from 30 to 35%; or from 35 to 40%; or from 40 to 45%; or from 45 to 50%; or from 50 to 55%; or from 55 to 60%; or from 60 to 65%; or from 65 to 70%; or from 70 to 75%; or from 75 to 80%; or from 80 to 85%; or from 85 to 90%; or from 90 to 95%; or from 95 to 100%. Ranges of 35 to 100%, particularly 55 to 85% and more specifically 60 to 80%, are particularly suitable. In all ranges set out in this application, the terminals are included unless otherwise stated. In some embodiments, the PAEK is a polyether-ether-ketone (PEEK), comprising a succession of repeating units of the type -(ArrO-Ar2-O-Ar3-CO)n-, each ArB Ar2 and Ar3 independently representing a divalent aromatic radical, preferably a phenylene. The bonds on either side of each Arb motif Ar2 and Ar3 can be of the para, or meta, or ortho type (preferably of the para or meta type). In some embodiments, the PEEK comprises a succession of repeating units of formula (II): and / or a succession of repeating units of formula (III):
[0070]
[0071]
[0072]
[0073]
[0074]
[0075]
[0076]
[0077]
[0078]
[0079] and / or a succession of repeating units of formula (IV): and / or a succession of repeated motifs of formula (V): (V) ★ n In some embodiments, PAEK is a polyether ketone (PEK), comprising a succession of repeating units of the type -(ArrO-Ar2-CO)n-, each An and Ar2 independently representing a divalent aromatic radical, preferably a phenylene. The bonds on either side of each An and Ar2 motif can be of the para, or meta, or ortho type (preferably of the para or meta type). In some embodiments, the PEK comprises a succession of repeating units of formula (VI): In some embodiments, the PEK comprises a succession of repeating units of formula (VII): (VII)
[0080]
[0081]
[0082] In this formula, as in the following formulas, x and y represent whole numbers. In some embodiments, the PEK comprises a succession of repeating units of formula (VIII): (VIII)
[0083]
[0084]
[0085]
[0086]
[0087]
[0088]
[0089]
[0090]
[0091] In some embodiments, the PAEK is a poly-ether-ether-ketone-ketone (PEEKK), comprising a succession of repeating units of the type -(Ari-O-Ar2-O-Ar3 -CO-Ar4-CO)n-, each Arb Ar2, Ar3 and Ar4 independently representing a divalent aromatic radical, preferably a phenylene. The bonds on either side of each Arb motif Ar2, Ar3 and Ar4 can be of the para, or meta, or ortho type (preferably of the para or meta type). In some embodiments, the PEEKK comprises a succession of repeating units of formula (IX): In some embodiments, the PAEK is a polyether-ether-ether-ketone (PEEEK), comprising a succession of repeating units of the type -(Ari-O-Ar2-O-Ar3 -O-Ar4-CO)n-, each Arb Ar2, Ar3 and Ar4 independently representing a divalent aromatic radical, preferably a phenylene. The bonds on either side of each Arb motif Ar2, Ar3 and Ar4 can be of the para, or meta, or ortho type (preferably of the para or meta type). In some embodiments, the PEEEK comprises a succession of repeating units of formula (X): (X) r In some embodiments, the PAEK is a poly-ether-ketone-ether-ketone-ketone (PEKEKK), comprising a succession of repeating units of the type -(Ari-O-Ar2-CO-Ar3-O-Ar4-CO-Ar5-CO)n-, each Arb Ar2, Ar3, Ar4 and Ar5 independently representing a divalent aromatic radical, preferably a phenylene.
[0092] The bonds on either side of each Arb motif Ar2, Ar3, Ar4 and Ar5 may be of the para, or meta, or ortho type (preferably of the para or meta type).
[0093] In some embodiments, the PAEK is a poly-ether-ether-ketone-ether-ketone (PEEKEK), comprising a succession of repeating units of the type -(Ari-O-Ar2-O-Ar3-CO-Ar4-O-Ar5-CO)n-, each Arb Ar2, Ar3, Ar4 and Ar5 independently representing a divalent aromatic radical, preferably a phenylene.
[0094] The bonds on either side of each Arb motif Ar2, Ar3, Ar4 and Ar5 may be of the para, or meta, or ortho type (preferably of the para or meta type).
[0095] In some embodiments, the PAEK is according to the most general formula shown below, in which certain Ar and / or Ar' units represent a divalent radical derived from diphenyl or biphenol.
[0096] In some embodiments, PAEK is a poly-ether-diphenyl-ether-ketone (PEDEK), comprising a succession of repeating units of the type -(Ari-ODO-Ar2-CO)n-, each Ari and Ar2 independently representing a divalent aromatic radical, preferably a phenylene, and D representing a divalent radical derived from diphenyl.
[0097] The bonds on either side of each An and Ar2 motif may be of the para, or meta, or ortho type (preferably of the para or meta type).
[0098] In certain embodiments, the PEDEK comprises a succession of repeating units of formula (XI):
[0100] Blends of the preceding PAEKs may also be used, as well as copolymers of the preceding PAEKs.
[0101] The PAEK resin may comprise one or more additional polymers not belonging to the PAEK family.
[0102] Preferably, the mass content of PAEK in the PAEK resin is greater than or equal to 50%, preferably 60%, more preferably 70%, more preferably 80% and more preferably 90%.
[0103] In some embodiments, the PAEK resin consists essentially of one or more PAEKs.
[0104] Advantageously, the thermoplastic resin comprises PEK, PEEK or PEKK as a thermoplastic material. PEKK is particularly preferred.
[0105] In some embodiments, the thermoplastic resin may have a glass transition temperature Tg of 120 to 200°C, preferably 140 to 170°C. The Tg is determined by differential scanning calorimetry (DSC) according to EN ISO 11357-4:2014.
[0106] In some embodiments, the thermoplastic resin may have a melting temperature Tm of 250 to 400°C, preferably 300 to 350°C. The Tm is determined by differential scanning calorimetry (DSC) according to EN ISO 11357-4:2014.
[0107] In some embodiments, the thermoplastic resin may have a Tcresine crystallization temperature of 220 to 310°C, preferably 245 to 285°C. This crystallization temperature may also be determined by differential scanning calorimetry (DSC) according to EN ISO 11357-4:2014 but with cooling at 20°C / min.
[0108] The reinforcing fibers used for the manufacture of semi-finished products can be chosen from all the fibers capable of being used as reinforcement in the manufacture of parts made of composite materials.
[0109] Thus, it may in particular be glass fibers, quartz fibers, carbon fibers, graphite fibers, silica fibers, metal fibers such as steel fibers, aluminum fibers or boron fibers, ceramic fibers such as silicon carbide or boron carbide fibers, synthetic organic fibers such as aramid fibers or poly(p-phenylene benzobi-soxazole) fibers, better known by the acronym PBO, or PAEK fibers, or mixtures of such fibers.
[0110] Preferably, these are carbon fibers or glass fibers, and more particularly carbon fibers.
[0111] The fibers are preferably not sized. When they are sized, the sizing is preferably adapted to the resin, in particular in that it does not cause degradation products harmful to the resin.
[0112] The average diameter of the reinforcing fibers may be in particular from 2 to 20 μm, preferably from 4 to 15 μm, more preferably from 6 to 10 μm. The average diameter of the fibers may be measured by microscopic analysis.
[0113] The method of manufacturing a semi-finished product according to the invention may comprise the following steps:
[0114] * providing the reinforcing fibers and a thermoplastic resin as described above; • mixing the reinforcing fibers with the thermoplastic resin; • heating to melt the thermoplastic resin and to raising the temperature of the thermoplastic resin to a temperature above the melting temperature of the resin; and • optionally a calendering step.
[0115] The second step and the third step thus allow the impregnation of the reinforcing fibers with the thermoplastic resin.
[0116] Thus, the semi-finished products according to the invention can be manufactured by unwinding in an aligned manner and putting under tension strands of fibers initially wound into reels, arranged adjacent to each other; then carrying out the impregnation with the resin.
[0117] The number of strands arranged adjacently may be in particular from 10 to 300, preferably from 20 to 200, more preferably from 30 to 100, for example about 50. Each strand may comprise in particular from 300 to 50,000 fibers, preferably from 1,000 to 50,000 fibers, more preferably from 3,000 to 50,000 fibers, more preferably from 6,000 to 50,000 fibers, more preferably from 6,000 to 48,000 fibers, more preferably from 6,000 to 24,000 fibers, more preferably from 12,000 to 24,000 fibers, for example about 12,000 fibers.
[0118] The mixing can be carried out by introducing and circulating the reinforcing fibers in a bath of aqueous resin dispersion. The fibers mixed with thermoplastic resin powder are then removed from the bath and freed from water, for example by drying in an infrared oven. Then, melting the thermoplastic resin and then raising the temperature of the thermoplastic resin to a temperature above its melting temperature allows the fibers to be coated with the resin. The coated fibers obtained are then, if necessary, shaped, for example by calendering. This step can allow the semi-finished product to be textured and dimensioned.
[0119] Alternatively, the mixing may be carried out by introducing and circulating the reinforcing fibers in a bath of resin dissolved in a solvent, followed by drying, evaporating the solvent and melting the thermoplastic resin and calendering as described above.
[0120] Alternatively, mixing may be carried out by arranging the reinforcing fibers in a fluidized bed of resin powder, then melting the thermoplastic resin and calendering as described above.
[0121] The heating mentioned above may consist of heating the reinforcing fibers (which itself allows the thermoplastic resin to be heated), or heating the thermoplastic resin directly, or heating the entire set of reinforcing fibers and the thermoplastic resin.
[0122] Thus, heating can be carried out by infrared irradiation, UV irradiation, microwave irradiation, laser irradiation, convection heating, wave heating high frequency or hot air heating. Preferably, heating is carried out by infrared irradiation.
[0123] For example, the heating may be heating of the reinforcing fibers by infrared irradiation, or heating of the thermoplastic resin by convection.
[0124] Heating can be carried out in several stages, for example by applying different powers from one stage to another. For example, several ovens can be used, each having a different power, or an oven with separate heating zones. By "heating power" is meant here the electrical power consumed by the oven.
[0125] Preferably, the heating is of decreasing intensity, that is to say that a first heating power (for example infrared irradiation) is first applied, then a second heating power (for example infrared irradiation) lower than the first, then optionally a third heating power (for example infrared irradiation) lower than the first, and possibly so on.
[0126] Preferably, the reinforcing fibers are at a distance of 2 to 25 cm, and preferably 6 to 15 cm from the radiation source.
[0127] The heating can for example be carried out at a maximum power of 25 to 60 kW, preferably 30 to 50 kW.
[0128] The heating time (from the start of heating until no further heating is applied) may be in particular from 3 to 150 seconds, and preferably from 10 to 80 seconds. Thus, the heating time may in particular be from 3 to 10 seconds; or from 10 to 20 seconds; or from 20 to 30 seconds; or from 30 to 40 seconds; or from 40 to 50 seconds; or from 50 to 60 seconds; or from 60 to 70 seconds; or from 70 to 80 seconds; or from 80 to 90 seconds; or from 90 to 100 seconds; or from 100 to 110 seconds; or from 110 to 120 seconds; or from 120 to 130 seconds; or from 130 to 140 seconds; or from 140 to 150 seconds.
[0129] During heating, the power absorbed per kg of all the reinforcing fibers and the thermoplastic resin makes it possible to bring the thermoplastic resin to its melting temperature and to exceed it to bring the resin to a temperature above its melting temperature to obtain the semi-finished product. This power can in particular be from 10 to 1600 kW / kg, preferably from 20 to 1400 kW / kg. Thus, this absorbed power can be from 10 to 100 kW / kg; or from 100 to 200 kW / kg; or from 200 to 300 kW / kg; or from 300 to 400 kW / kg; or from 400 to 500 kW / kg; or from 500 to 600 kW / kg; or from 600 to 700 kW / kg; or from 700 to 800 kW / kg; or 800 to 900 kW / kg; or from 900 to 1000 kW / kg; or from 1000 to 1100 kW / kg; or from 1100 to 1200 kW / kg; or from 1200 to 1300 kW / kg; or from 1300 to 1400 kW / kg; or from 1400 to 1500 kW / kg; or from 1500 to 1600 kW / kg.
[0130] This absorbed power can be calculated using the following formula: 101311 P =^x{[Cpx(Tf-23)] + [(l-Vm)xAHf]\
[0132] The power per unit mass P is measured in kW / kg. Cp represents the heat capacity of the set of reinforcing fibers and thermoplastic resin, and is expressed in J / kg.°C, Tf represents the melting temperature of the resin in °C, Vm represents the volume ratio of reinforcing fibers, AHf represents the enthalpy of fusion of the resin in J / kg (which can be determined by DSC according to standard EN ISO 11357-4: 2014) and Dm represents the mass flow rate of semi-finished product expressed in kg / s.
[0133] During the heating step, a line speed of 2 to 80 m / min, preferably 5 to 40 m / min, for example 10 to 20 m / min may be used.
[0134] During the heating step, the thermoplastic resin must reach a temperature above its melting temperature to allow the semi-finished product to be manufactured. This temperature may in particular be 320 to 420°C, preferably 360 to 400°C. Also, the reinforcing fibers may reach a maximum temperature of 300 to 440°C, preferably 360 to 400°C in the case of the impregnation of PAEK-type thermoplastics. The temperature of the reinforcing fibers may be measured using a pyrometer or a thermal camera.
[0135] According to some embodiments, at least a portion of the melting of the thermoplastic resin is carried out under an inert atmosphere. Preferably, the entire step of melting the thermoplastic resin is carried out under an inert atmosphere.
[0136] By "melting under an inert atmosphere" is meant a melting in which the product to be melted is brought into contact with a gas mixture essentially free of oxygen. Melting under an inert atmosphere can be carried out, for example, in an enclosure filled with nitrogen or another inert gas mixture, or in an enclosure filled with air but with a sweep of inert gas mixture (for example nitrogen) over the molten product.
[0137] The calendering step can be carried out in particular by a heating calendering device. The temperature during calendering can in particular be from 20 to 350°C, preferably from 140 to 240°C.
[0138] The semi-finished product is generally in the form of a more or less wide ribbon (we can speak of a sheet or sheet from a certain width) and more or less thick. These semi-finished products preferably have the following dimensions:
[0139] • a thickness of 0.05 to 1 mm, preferably 0.15 to 0.4 mm; • a length of 0.01 m to 25,000 m for glass fiber products for example and at 10,000 m for carbon fiber tapes. • a width of 0.005 m to 5 m, preferably 0.01 m to 5 m.
[0140] Preferably, the semi-finished products according to the invention comprise from 1 to 99% by weight, preferably from 30 to 90%, in particular from 50 to 80% by weight, and in particular from 60 to 70% by weight of reinforcing fibers.
[0141] Preferably, the semi-finished products according to the invention comprise from 1 to 99% by weight, preferably from 10 to 70%, in particular from 20 to 50% by weight, and in particular from 30 to 40% by weight of resin.
[0142] The semi-finished products according to the invention may have a crystallization temperature Tcsemi-finished product of 220 to 320°C, preferably of 245 to 295°C determined by differential scanning calorimetry (DSC) according to standard EN ISO 11357-4: 2014 during cooling at 20°C / min.
[0143] The Tcsemi produced by the semi-finished products according to the invention is greater than or equal to the Tcresine (i.e. the crystallization temperature of the thermoplastic resin alone before the manufacture of the semi-finished product).
[0144] According to certain embodiments, the Tcsemi.product is equal to Tcresine. Alternatively, the Tcsemi-product is higher than the Tcresine by 1 to 10°C and preferably by 4 to 8°C. The Te semi-product may for example be 1 to 2°C; or 2 to 4°C; or 4 to 6°C; or 6 to 8°C; or 8 to 10°C higher than or equal to the Tc^ne-
[0145] The semi-finished products of the invention may also further comprise fillers (other than reinforcing fibers) and / or functional additives. Among the functional additives, one or more surfactants, UV stabilizers, thermal stabilizers, light stabilizers, impact modifiers, plasticizers, expanding agents and / or biocidal agents, thermally and / or electrically conductive particles, colorants, flame retardants, flame retardants, etc. may in particular be included.
[0146] The fillers may in particular be mineral fillers such as alumina, silica, calcium carbonate, titanium dioxide, glass beads, carbon black, graphite, graphene and carbon nanotubes.
[0147] The total quantity of fillers and additives is preferably less than or equal to 5% by weight, more preferably 2% by weight, more preferably 1% by weight in the semi-finished product.
[0148] Additives and / or fillers, when present, may preferably be incorporated during impregnation with the resin.
[0149] Process for manufacturing composite parts
[0150] The manufacturing process of a composite part involves:
[0151] • the stacking of at least two semi-finished products; • the consolidation of semi-finished products, and • cooling of semi-finished products to obtain the composite part.
[0152] The thermoplastic resin may be identical or different from one semi-finished product to another forming the same composite part. Preferably, the thermoplastic resin is of the same nature (for example PEK or PEKK or PEEK) in all of the semi-finished products of the composite part. It may possibly have a different grade from one semi-finished product to another, for example a different viscosity, a different molecular weight or a different melting temperature. Alternatively, the grade of the thermoplastic resin is the same in all the semi-finished products of the composite part.
[0153] The composite part obtained from this process is characterized by a crystallization temperature Tccomposite.
[0154] When the thermoplastic resin of the different semi-finished products is the same, or when the semi-finished products are the same, the temperature Tccomposite can be compared to the temperature Tcresine of the starting resin, or to the temperature Tcsemi-finished product of the semi-finished products used for the manufacture of the part.
[0155] Thus, in embodiments, Tccomposite > Tcresin- 5°C. Thus, the difference between Tcresin and Tccomposite may be less than 5°C; or less than 4°C; or less than 3°C; or less than 2°C; or less than 1°C.
[0156] In embodiments, Tccomposite > Tcsemi product- 10°C. Thus, the difference between the Tcsemi product and the Tccomposite may be less than 10°C; or less than 9°C; or less than 8°C; or less than 7°C; or less than 6°C; or less than 5°C; or less than 4°C; or less than 3°C; or less than 2°C; or less than 1°C.
[0157] The Tccomposite of a composite part according to the invention may be from 210 to 320°C and preferably from 245 to 295°C determined by differential scanning calorimetry (DSC) according to standard EN ISO 11357-4: 2014 during cooling at 20°C / min.
[0158] The composite parts are obtained for example by first manufacturing a preform, in particular by placing or draping the pre-impregnated semi-finished products in a mold. The composite part is then obtained by consolidation, a step during which the preform is heated, generally under pressure in an autoclave, so as to assemble the semi-finished products by fusion. Preferably, the semi-finished products manufactured according to the invention can be consolidated outside of an autoclave, for example under a vacuum cover placed in an oven. Such equipment is more economical than an autoclave, and therefore advantageous to use. However, it allows a lower level of compression than an autoclave.
[0159] Thus, when the consolidation is carried out in an autoclave, the pressure applied in the autoclave may be from 1 to 20 bar and preferably from 7 to 10 bar. Thus, the pressure applied in the autoclave may in particular be from 1 to 1.5 bar; or from 1.5 to 2 bar; or from 2 to 2.5 bar; or from 2.5 to 3 bar; or from 3 to 3.5 bar; or from 3.5 to 4 bar; or from 4 to 4.5 bar; or from 4.5 to 5 bar; or from 5 to 5.5 bar; or from 5.5 to 6 bar; or from 6 to 6.5 bar; or from 6.5 to 7 bar; or from 7 to 7.5 bar; or from 7.5 to 8 bar; or from 8 to 8.5 bar; or from 8.5 to 9 bar; or from 9 to 9.5 bar; or from 9.5 to 10 bar; or from 10 to 10.5 bar; or from 10.5 to 11 bar; or from 11 to 11.5 bar; or from 11.5 to 12 bar; or from 12 to 12.5 bar; or from 12.5 to 13 bar; or from 13 to 13.5 bar; or from 13.5 to 14 bar; or from 14 to 14.5 bar; or from 14.5 to 15 bar; or from 15 to 15.5 bar; or from 15.5 to 16 bar; or from 16 to 16.5 bar; or from 16.5 to 17 bar; or from 17 to 17.5 bar; or from 17.5 to 18 bar; or from 18 to 18.5 bar; or from 18.5 to 19 bar; or from 19 to 19.5 bar; or from 19.5 to 20 bar.
[0160] When the consolidation is carried out in a vacuum tank, the pressure applied in the vacuum tank may be from 50 to 900 mbar and preferably from 300 to 800 mbar. Thus, the pressure applied in the vacuum tank may in particular be from 50 to 100 mbar; or 100 to 150 mbar; or 150 to 200 mbar; or 200 to 250 mbar; or 250 to 300 mbar; or 300 to 350 mbar; or 350 to 400 mbar; or 400 to 450 mbar; or 450 to 500 mbar; or 500 to 550 mbar; or 550 to 600 mbar; or 600 to 650 mbar; or from 650 to 700 mbar; or from 700 to 750 mbar; or from 750 to 800 mbar; or from 800 to 850 mbar; or from 850 to 900 mbar.
[0161] During consolidation of the preform, the temperature of the semi-finished products can increase to a maximum temperature, higher than the melting temperature of the thermoplastic resin, then remain constant.
[0162] The maximum temperature is preferably set at a value which is 5 to 50°C higher than the melting temperature of the resin, preferably 10 to 40°C higher than the melting temperature of the resin, preferably 20 to 30°C higher than the melting temperature of the resin, and for example 25°C higher than the melting temperature of the resin.
[0163] The maximum temperature may be, depending on the case, 300 and 450°C, preferably 320 to 400°C, and for example 375°C. In certain embodiments, the maximum heating temperature may be 300 to 320°C; or 320 to 340°C; or 340 to 360°C; or 360 to 380°C; or 380 to 400°C; or 400 to 420°C; or 420 to 450°C.
[0164] The consolidation of a preform is followed by its cooling in order to solidify the composite part. Thus, the temperature is reduced to a temperature below the melting temperature of the resin.
[0165] In the manufacturing processes of composite parts, the semi-finished products or preforms are subjected to different thermal cycles under pressure or under vacuum in order to assemble them together to form the composite part and / or to shape it.
[0166] In some embodiments, a number of semi-finished products may be positioned side by side and edge to edge on a plane. In this case, the reinforcing fibers of the semi-finished products may be oriented in the same direction. Thus, the semi-finished products may form a layer of thickness that corresponds to the thickness of a semi-finished product. In some embodiments, the plane on which the semi-finished products are positioned may be curved. In some embodiments, the semi-finished products may be positioned on a mandrel, such as a circular mandrel. In other embodiments of realization, the semi-finished products can be positioned in such a way that a slight overlap is possible on each of the edges of the semi-finished products. These placements of semi-finished products can be carried out for example using an automated deposition means of the AFP (Automated Fiber Placement) type. Alternatively, these placements can be carried out using a filament winding process. Thus, a layer of semi-finished products can consist of one or more semi-finished products positioned next to each other. This layer of semi-finished products preferably has the following dimensions:
[0167] • a thickness of 0.05 to 1 mm, preferably 0.15 to 0.4 mm; • a length of 0.01 to 100 m, preferably 0.1 to 10 m; • a width of 0.005 to 5 m, preferably 0.01 to 5 m.
[0168] A preform is an assembly of a certain number of layers of semi-finished product. The number of layers in a preform can vary from 1 to 200, preferably from 6 to 48.
[0169] Thus, the number of layers in a preform can vary from 1 to 150 layers, preferably from 4 to 100, and ideally from 6 to 48.
[0170] Thus, a preform according to the invention may for example comprise from 1 to 10; or from 10 to 20; or from 20 to 30; or from 30 to 40; or from 40 to 50; or from 50 to 60; or from 60 to 70; or from 70 to 80; or from 80 to 90; or from 90 to 100; or from 100 to 110; or from 110 to 120; or from 120 to 130; or from 130 to 140; or from 140 to 150 layers of semi-finished products.
[0171] The reinforcing fibers preferably have a substantially unidirectional orientation in each layer of semi-finished products. The unidirectional orientation of the reinforcing fibers may be the same from one layer to the next, i.e., two adjacent layers of semi-finished products have unidirectional orientations of reinforcing fibers that substantially form an angle of 0° to each other. Preferably, however, the unidirectional orientation of the reinforcing fibers differs from one layer of semi-finished products to another. More preferably, two adjacent layers of semi-finished products have unidirectional orientations of reinforcing fibers that substantially form an angle of about 90° to each other; or that substantially form an angle of about 45° to each other.
[0172] In some embodiments, two adjacent semi-finished product layers may have unidirectional orientations of reinforcing fibers that essentially form an angle of 0 to 20°; or 20 to 45°; or 45 to 60°; or 60 to 90° relative to each other; these angles may be counted positively and / or negatively.
[0173] The composite parts thus manufactured by consolidation of the preforms can be further transformed, in order to obtain assemblies of complex composite parts. Thus, it is possible to co-consolidate composite parts, a process gener- ration carried out in an autoclave by means of a new thermal cycle, or to weld parts together by local heating.
[0174] The composite parts that are obtained with the method according to the invention may be parts of an air or space vehicle, or parts of a drilling installation (for hydrocarbon fields), or any part located in contact with or in proximity to an engine (for example a marine, land or air vehicle engine) or a reactor, and in particular seals, connectors, sheaths and structural parts. They may also be parts intended to be subjected to friction, that is to say parts in moving contact with one or more surfaces, in use. Such parts may in particular be supports, rings, valve seats, gears, pistons, piston rings, valve guides, compressor blades, seals and engine components. Examples
[0175] The following examples illustrate the invention without limiting it.
[0176] Example 1 - Manufacture of semi-finished product and composite part according to the invention
[0177] To study the properties and degradation of a semi-finished product comprising carbon fibers and PEKK as thermoplastic resin, as well as of a composite part also comprising carbon fibers and the same thermoplastic resin, the crystallization temperature of the PEKK resin alone was first measured at Tcresine=263°C by DSC analysis as illustrated in Figure 1 (C).
[0178] Then, a semi-finished product was manufactured from this PEKK resin and carbon fibers by a powder fluidized bed impregnation process as described in document WO 2018 / 115736.
[0179] The heating of the impregnated carbon fibers was carried out in an infrared oven with a power of 40% for 2 s, a power of 20% for 3.5 s and a power of 0% for 3.5 s. The powers indicated are percentages of maximum power delivered by the infrared modules, i.e. 36 kW for the first IR oven and 48 kW for each of the following two.
[0180] The speed of the semi-finished product in the infrared oven was 5 m / min and the total energy supplied during heating was 2.2 kW.min.
[0181] The calendering was carried out at a calender temperature of 230°C, the product being maintained at a temperature above its melting point, i.e. 380°C.
[0182] DSC analysis of the semi-finished product obtained according to this process made it possible to measure the crystallization temperature of the semi-finished product Tcsemi_product=268°C as illustrated in Figure 2 (C).
[0183] The Tcsemi produced is therefore superior to Tcresine.
[0184] A composite part was then manufactured from semi-finished products such as manufactured above. It results from the assembly by juxtaposition and consolidation of 23 plies in 0° orientation. Each ply is made up of 12 mm wide and 0.25 mm thick strips. These plies were deposited using an automated strip placement robot equipped with LASER heating. Consolidation was carried out in an autoclave at a plateau temperature of 375°C for 30 min (temperature rise with a ramp at 10°C / min and cooling at -10°C / min). The nitrogen pressure in the autoclave was kept constant (7 bars), with the vacuum level applied to the part being set at 100 mbar.
[0185] DSC analysis of the composite part made it possible to measure the crystallization temperature of the composite part Tccomposite=261°C as illustrated in Figure 3 (C).
[0186] Tccomposite therefore presents a difference of 2°C with Tcresine.
[0187] Example 2 - Comparative example
[0188] Another semi-finished product was made from a PEKK resin (having a Tcresine crystallization temperature of 273°C according to DSC analysis and as illustrated in Figure 4 (C)) and carbon fibers.
[0189] The same impregnation method as in Example 1 was used.
[0190] Heating of the impregnated carbon fibers was carried out in an infrared oven with a power of 65% for 2 s, a power of 65% for 3.5 s and a power of 55% for 3.5 s. The power percentages correspond to the power emitted by the infrared modules, this power being indicated as a maximum percentage of the power that a module can provide. Here each module has a maximum power of 48 kW.
[0191] The speed of the semi-finished product in the infrared oven was 5 m / min and the total energy supplied during heating was 10.3 kW.min.
[0192] The calendering was carried out at a temperature of 230°C.
[0193] DSC analysis of the semi-finished product obtained according to this process made it possible to measure the crystallization temperature of the semi-finished product Tcsemi product=267°C as illustrated in Figure 5 (C).
[0194] The Tcsemi produced in this case is lower than the Tcresine.
[0195] A composite part was then manufactured from semi-finished products as manufactured above using the same process as in the previous example.
[0196] DSC analysis of the composite part made it possible to measure the crystallization temperature of the composite part Tccomposite=249°C as illustrated in Figure 6 (C).
[0197] Tccomposite therefore presents a difference of 25°C with Tcresine-
Claims
Claims
1. A method of manufacturing a semi-finished product, comprising the following steps: • providing reinforcing fibers and a thermoplastic resin having a crystallization temperature Tcresine; • mixing the reinforcing fibers with the thermoplastic resin; • heating to melt the thermoplastic resin and to bring it to a temperature higher than the melting temperature of the resin; and • optionally, a calendering step; the semi-finished product being characterized by a crystallization temperature Tcsemi-finished product, the Tcsemi-finished product being greater than or equal to the Tcresine>in which the heating is carried out by infrared irradiation, UV irradiation, microwave irradiation, laser irradiation, convection heating or high-frequency wave heating, and preferably by infrared irradiation.
2. The method of claim 1, wherein the melting of the thermoplastic resin is carried out by heating the reinforcing fibers, or the thermoplastic resin, or the combination of the reinforcing fibers and the thermoplastic resin.
3. Manufacturing method according to one of claims 1 to 2, in which at least part of the step of melting the thermoplastic resin is carried out under an inert atmosphere.
4. Method according to one of claims 1 to 3, in which, during the step of melting the thermoplastic resin, the combination of reinforcing fibers and thermoplastic resin is provided with a power per unit mass of 10 to 1600 kW / kg, preferably 20 to 1400 kW / kg.
5. A method according to any one of claims 1 to 4, wherein the heating of the thermoplastic resin to a temperature above its melting temperature is carried out up to a temperature of 320 to 420°C, and preferably 360 to 400°C.
6. A method according to any one of claims 1 to 5, wherein the Tcsemi produced is higher than the Tcresin by 1 to 10°C, and preferably by 4 to 8°C.
7. A method according to any one of claims 1 to 6, wherein the thermo-resin moplastic is one or more polyaryletherketones selected from polyetherketones, polyetheretherketones, polyetherketoneketones, polyetheretherketoneketones, polyetherketoneetherketoneketones, polyetheretherketoneetherketones, polyetheretherketoneketones, and polyetherdiphenyletherketones, polyetheretherketones, and preferably selected from polyetherketones, polyetherketoneketones, and polyetheretherketones.
8. Method according to one of claims 1 to 7, in which the reinforcing fibers are carbon fibers and / or glass fibers.
9.
10. Semi-finished product obtained according to the method of one of claims 1 to 8. Method for manufacturing a composite part comprising the following steps: • manufacturing at least two semi-finished products according to the method of one of claims 1 to 8; • stacking the semi-finished products in at least two layers of semi-finished products; • consolidating the layers of semi-finished products, and • cooling the layers of consolidated semi-finished products in order to obtain the composite part.
11. The method of claim 10, wherein the composite part is characterized by a crystallization temperature Tccomposite, where Tccomposite > Te - 5°C -1- ^resined
12. A method of manufacturing a composite part comprising the following steps: • providing at least two semi-finished products according to claim 9; • stacking the semi-finished products into at least two layers of semi-finished products; • consolidating the layers of semi-finished products, and • cooling the layers of consolidated semi-finished products in order to obtain the composite part.
13. The method of claim 12, wherein the composite part is characterized by a crystallization temperature Tccomposite, where Tccomposite > Te —1O°CA ^semi-product JV -•
14. Composite part obtained according to the method of one of claims 10 or 11, or according to the method of one of claims 12 or 13.
15. A composite part according to claim 14, having a thickness of 0.05 to 150 mm, and / or a length of 0.01 to 100 m, and / or a width of 0.005 to 5 m.
16. A composite part according to one of claims 14 or 15, which is a part of an air or space vehicle, or a part of a drilling installation, or a part intended to be positioned in contact with or near a vehicle engine or a reactor, or a part intended to be subjected to friction.