METHOD FOR TRANSFERRING A USEFUL LAYER ONTO THE FRONT FACE OF A SUBSTRATE

A two-phase heat treatment method addresses the issue of crack formation and delamination in SmartCut™ technology by maturing defects and initiating a controlled fracture, ensuring a stable and efficient transfer of the useful layer onto the support substrate.

FR3126809B1Active Publication Date: 2024-10-25SOITEC SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2021009287
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-06
Publication Date
2024-10-25
Estimated Expiration
2041-09-06

AI Technical Summary

Technical Problem

Existing methods for transferring a useful layer onto a support substrate using SmartCut™ technology face issues with crack formation and delamination at the interface between the donor and manipulator substrates due to differing thermal expansion coefficients, leading to uncontrolled fractures and partial transfers.

Method used

A two-phase heat treatment process is employed, with a first phase to mature defects and prevent fracture initiation, followed by a second phase at a lower temperature to initiate a controlled fracture along the weakened zone, minimizing the risk of cracks and delamination.

Benefits of technology

The method effectively transfers the useful layer to the support substrate at a lower temperature, reducing the likelihood of cracks and delamination, thereby stabilizing the interface and ensuring a controlled transfer process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000013_0000
    Figure 00000013_0000
  • Figure 00000013_0001
    Figure 00000013_0001
  • Figure 00000013_0002
    Figure 00000013_0002
Patent Text Reader

Abstract

The invention relates to a method for transferring a useful layer (15) onto a support substrate (20), the method comprising: a) supplying a donor substrate (10) which includes a donor layer (12); b) forming a weakening zone (14) by implanting species into the donor layer (12), which, together with the latter, defines a useful layer (15); c) assembling the support substrate (20) with the donor substrate (10); d) a heat treatment comprising a first and a second phase, the first phase, of a first duration, comprising a rise to a first temperature, and is adapted to allow the maturation of defects and prevent the initiation of a fracture in said zone (14), the second phase, of a second duration, comprising a plateau at a second temperature, lower than the first temperature, and is adapted to initiate a fracture along the weakening zone. Figure 1D
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR TRANSFERRING A USEFUL LAYER TO A FRONT FACE OF A SUPPORT SUBSTRATE FIELD OF THE INVENTION

[0001] The present invention relates to the field of heterogeneous structures.

[0002] In particular, the present invention relates to a method of transferring a useful layer onto a support substrate involving SmartCut™ technology.

[0003] In particular, the method according to the present invention relates to a method for limiting the fracture temperature in order to reduce the risk of cracks and / or delamination appearing.

[0004] The method according to the present invention is then advantageously implemented for the manufacture of a piezoelectric substrate on an insulator. TECHNOLOGICAL BACKGROUND OF THE INVENTION

[0005] Document FR3068508A1 discloses a method for transferring a useful layer onto a support substrate. In particular, document FR3068508A1 discloses a method for transferring, using a SmartCut™ method, a useful layer onto a support substrate.

[0006] The transfer method described in document FR3068508A1 comprises, in this regard, the following steps:

[0007] aO) a step of providing a donor substrate which comprises, from a front face to a rear face, a donor layer resting on one face of a manipulator substrate;

[0008] bO) a step of implanting species via the front face in the donor layer so as to form a weakening zone which extends along a plane parallel to the front face and which delimits with said front face a useful layer;

[0009] cO) a step of assembling the front face of the donor substrate with a main face of a support substrate;

[0010] dO) a heat treatment step intended to initiate the propagation of a fracture wave within the weakening zone and thus transfer the useful layer onto the main face of the support substrate.

[0011] This method is advantageously implemented when the materials forming the useful layer and the support substrate have different thermal expansion coefficients. More particularly, the method disclosed in document FR3068508A1, in order to limit the risks of an uncontrolled fracture or of a partial and / or defective transfer of the useful layer, proposes to consider a handling substrate made of a material having a coefficient of thermal expansion similar to that of the material forming the support substrate.

[0012] Nevertheless, the consideration of such a donor substrate remains problematic.

[0013] Indeed, the interface formed between the donor layer and the manipulator substrate is sensitive to heat treatment. In particular, this interface can be the site of the appearance of cracks and / or delamination of the donor layer.

[0014] Thus, an aim of the present invention is to propose a method for transferring a useful layer onto a donor substrate making it possible to prevent the appearance of cracks at the interface formed between the donor layer and the handling substrate and the delamination of the donor layer. BRIEF DESCRIPTION OF THE INVENTION

[0015] The object of the invention is achieved by a method of transferring a useful layer onto a support substrate, the method comprising the following steps:

[0016] a) providing a donor substrate which comprises, from a main face, a donor layer formed of a piezoelectric material, and a manipulator substrate;

[0017] b) the formation of a weakening zone, by implantation of species in the donor layer, parallel to the main face and which delimits with the latter a useful layer;

[0018] c) assembling the support substrate with the donor substrate so as to interpose the donor layer between the manipulator substrate and the support substrate;

[0019] d) a heat treatment which comprises, in order, a first phase and a second phase, the first phase, of a first duration, comprises a temperature increase to a first temperature, and is adapted on the one hand to allow maturation of defects, generated by the species, in the weakening zone, and on the other hand to prevent the initiation of a fracture in said weakening zone, the second phase, of a second duration, comprises a plateau at a second temperature, lower than the first temperature, and is adapted to initiate a fracture along the weakening zone and thus transfer the useful layer to the front face.

[0020] According to one embodiment, step d) also comprises a reinforcement phase preceding the first phase and carried out at a temperature, called the reinforcement temperature, lower than the first temperature, the reinforcement phase being intended to reinforce a bonding energy of an interface formed between the support substrate and the donor substrate during the execution of step c).

[0021] According to one embodiment, the first phase comprises in order: a rise in temperature, a plateau at the first temperature, and a fall in temperature to the second temperature.

[0022] According to one embodiment, the first phase is adjusted according to the conditions for the establishment of species when carrying out step b).

[0023] According to one embodiment, the relative difference between the coefficients of thermal expansion of the materials forming, respectively, the manipulator substrate and the support substrate is less than 10%.

[0024] According to one embodiment, the manipulator substrate comprises a solid substrate on one face of which rests an intermediate layer, the intermediate layer being interposed between the donor layer and the solid substrate, advantageously, the intermediate layer comprises a polymer material.

[0025] According to one embodiment, the first temperature is less than 300°C, advantageously less than 250°C, even more advantageously less than 220°C.

[0026] According to one embodiment, the absolute difference between the first temperature and the second temperature is less than 40°C, and is greater than 30°C.

[0027] According to one embodiment, the second duration is less than 6 hours, advantageously less than 4 hours.

[0028] According to one embodiment, the second temperature is less than 180°C, advantageously less than 170°C.

[0029] According to one embodiment, the species comprise at least one of the elements chosen from: hydrogen ions, helium ions.

[0030] According to one embodiment, the piezoelectric material comprises at least one of the elements chosen from: LiTaO3, LiNbO3, LiA103, BaTiO3, PbZrTiO3, KNbO3, BaZrO3, CaTiO3, PbTiO3, KTaO3.

[0031] According to one embodiment, the assembly step c) is preceded by a step of forming a layer of dielectric material on the donor layer and / or on a front face of the support substrate.

[0032] According to one embodiment, assembly step c) comprises molecular bonding. Brief description of the drawings

[0033] Other characteristics and advantages will appear in the following description of a method for transferring a useful layer onto a support substrate according to the invention, given as non-limiting examples, with reference to the appended figure in which:

[0034] [Fig.lA] [Fig.lA] is a schematic representation of step a) of the method according to the present invention, in particular, [Fig.lA] represents the donor substrate along a section plane perpendicular to a main face of said donor substrate;

[0035] [Fig.lB] [Fig.lB] is a schematic representation of step b) of the method according to the present invention, in particular [Fig.lB] represents the donor substrate along a section plane perpendicular to a main face of said donor substrate and the arrows symbolize the implantation of the species by the main face in order to form the weakening zone;

[0036] [Fig.lC] [Fig.lC] is a schematic representation of step c) of the method according to the present invention, in particular [Fig.lC] represents an assembly formed by the donor substrate and the support substrate, along a section plane perpendicular to the main face of said donor substrate;

[0037] [Fig. 1D] [Fig. 1D] is a schematic representation of the first phase of step d) of the method according to the present invention, in particular [Fig. 1D] represents the maturation of the defects at the level of the weakening zone of the assembly formed by the donor substrate and the support substrate and according to a section plane perpendicular to the main face of said donor substrate;

[0038] [Fig.lE] [Fig.lE] is a schematic representation of the second phase of step d) of the method according to the present invention, in particular [Fig.lE] represents the fracture leading to the detachment of the useful layer from the donor layer with a view to its transfer to the front face of the support substrate;

[0039] [Fig.2] [Fig.2] is a schematic representation of the donor substrate along a section plane perpendicular to a main face of said donor substrate and according to a particular embodiment of the present invention, in particular, according to this embodiment, the manipulator substrate comprises a solid substrate on one face of which rests an intermediate layer, so that said intermediate layer is interposed between the solid substrate and the donor layer;

[0040] [Fig.3] [Fig.3] is a graphical representation of a heat treatment that can be implemented within the framework of the present invention, in particular the horizontal axis represents the time in hours, and the vertical axis represents the temperature in degrees Celsius;

[0041] [Fig.4A] [Fig.4A] is a graphical representation of a heat treatment, called the first treatment, capable of being implemented for the determination of parameters relating to the execution of step d), in particular the horizontal axis represents the time in hours, and the vertical axis represents the temperature in degrees Celsius;

[0042] [Fig.4B] [Fig.4B] is a graphical representation of a heat treatment, called second treatment, capable of being implemented for the determination of parameters relating to the execution of step d), in particular the horizontal axis represents the time in hours, and the vertical axis represents the temperature in degrees Celsius;

[0043] [Fig.4C] [Fig.4C] is a graphical representation of a heat treatment, called third treatment, capable of being implemented for the determination of parameters relating to the execution of step d), in particular the horizontal axis represents the time in hours, and the vertical axis represents the temperature in degrees Celsius;

[0044] [Fig.5] [Fig.5] illustrates a donor substrate which comprises a layer of dielectric materials, called the first layer, resting on the donor layer;

[0045] [Fig.6] [Fig.6] illustrates a support substrate which comprises a layer of materials dielectric (for example silicon dioxide), called the second layer, resting on the front face of the support substrate. DETAILED DESCRIPTION OF THE INVENTION

[0046] For the sake of simplification of the description to come, the same references are used for identical elements or elements ensuring the same function in the state of the art or in the different modes of implementation of the method described.

[0047] The figures are schematic representations which, for the sake of readability, are not to scale. In particular, the thicknesses of the layers are not to scale relative to the lateral dimensions of these layers.

[0048] The present invention relates to a method for transferring a useful layer onto a front face of a support substrate.

[0049] In particular, the method comprises carrying out steps a) to d). In particular, step a) comprises providing a donor substrate. The latter is provided, from a main face, with a donor layer formed of a piezoelectric material, and a manipulator substrate.

[0050] Step b) comprises the formation of a weakening zone, by implantation of species, in the donor layer, which extends parallel to the main face and which delimits with the latter a useful layer.

[0051] Step c) comprises assembling the donor layer with a front face of a support substrate.

[0052] Step d) comprises a heat treatment which comprises, in order, a first phase and a second phase. The first phase, of a first duration, comprises a temperature increase to a first temperature, and is adapted on the one hand to initiate a maturation of defects, generated by the species, in the weakening zone, and on the other hand to prevent the initiation of a fracture in said weakening zone. The second phase comprises a plateau at a second temperature, lower than the first temperature, and is of a second duration so as to initiate a fracture along the weakening zone and thus transfer the useful layer to the front face.

[0053] Figures 1A to 1E are schematic representations of the different steps implemented in the method of transferring a useful layer onto the front face of a support substrate according to the present invention.

[0054] [Fig. 1A] is an illustration of a step a) which comprises providing a donor substrate 10. In this regard, the donor substrate 10 comprises, from a main face 11, a donor layer 12 formed of a piezoelectric material, and a manipulator substrate 13. In other words, the donor layer 12 rests on a face of the manipulator substrate 13.

[0055] The formation of the donor substrate 10 may for example comprise, in order, a step of bonding a piezoelectric substrate to one face of a manipulator substrate, and a step of thinning the piezoelectric substrate in order to form the donor layer. The formation of the donor substrate 10 may also comprise a heat treatment step intended to reinforce the bonding interface formed between the donor layer and the manipulator substrate 13. The formation of the donor substrate 10 set out above is given only by way of example and is therefore not such as to limit the scope of the present invention.

[0056] The piezoelectric material forming the donor layer 12 may comprise at least one of the elements chosen from: LiTaO3, LiNbO3, LiA103, BaTiO3, PbZrTiO3, KNbO3, BaZrO3, CaTiO3, PbTiO3, KTaO3.

[0057] The manipulator substrate 13 may comprise any type of material, and more particularly a semiconductor material such as silicon, or an insulating material such as glass.

[0058] According to a particular embodiment, and as illustrated in [Fig. 2], the manipulator substrate may comprise a bulk substrate 13a (bulk substrate according to English terminology) on one face of which rests an intermediate layer 13b. More particularly, the intermediate layer 13b is, according to this particular embodiment, interposed between the bulk substrate 13a and the donor layer 12.

[0059] The solid substrate 13a may comprise any type of material, and more particularly a semiconductor material such as silicon, or an insulating material such as glass.

[0060] The intermediate layer 13b may comprise an insulating material, and more particularly a polymer material, which provides an adhesion function between the solid substrate 13a and the donor layer 12.

[0061] The relative difference between the coefficients of thermal expansion of the materials forming, respectively, the manipulator substrate and the support substrate may be less than 10%. Such a consideration will make it possible to limit the stresses likely to appear during the execution of a heat treatment of step d) described in the remainder of the statement.

[0062] Step a) is followed by a step b) shown in [Fig.lB].

[0063] In particular, step b) comprises the formation of a weakening zone 14, by implantation of species in the donor layer 12. More particularly, the weakening zone extends in a plane parallel to the main face 11 and delimits with the latter a useful layer 15.

[0064] By “weakening zone” is meant an area along which a fracture wave is likely to propagate in order to cause the detachment of the layer useful 15 of the donor layer 12.

[0065] It is further understood, without it being necessary to specify it, that the implanted species are chosen so as to be able to cause, by thermal activation, on the one hand a maturation of defects within the weakening zone and on the other hand the propagation of a fracture wave along the weakening zone.

[0066] The implantation of species can in particular implement an ionic implantation, and more particularly, an implantation of hydrogen ions and / or helium ions.

[0067] The implantation conditions, in terms of dose of implanted species and implantation energy, condition the thickness of the useful layer 15. By way of example, and for a donor layer 12 made of LiTaO3, a dose of hydrogen ions of between 1E16 at / cm2 and 5E17 at / cm2, with an implantation energy of between 30keV and 300keV makes it possible to form a useful layer 15 with a thickness of between 200 nm and 2000 nm.

[0068] The method according to the present invention also comprises the execution of a step c) ([Fig.lC]).

[0069] Step c) comprises the assembly of the donor substrate 10 and the support substrate 20 so as to interpose the donor layer 12 between the support substrate 20 and the manipulator substrate 13.

[0070] Thus, and as illustrated in [Fig. 1C], step c) comprises the assembly comprising bringing the main face 11 into contact with a front face 21 of a support substrate 20.

[0071] The invention is however not limited to this aspect, and it is possible to consider a step of forming a layer of dielectric material on the donor layer and / or on the front face of the support substrate preceding step c).

[0072] In this regard, [Fig.5] illustrates a donor substrate 10 which comprises a layer of dielectric materials (for example silicon dioxide), called first layer 17 resting on the donor layer.

[0073] Alternatively or additionally, the layer of dielectric material may be formed on the front face of the support substrate 20. In this regard, [Fig. 6] illustrates a support substrate 20 which comprises a layer of dielectric materials (for example silicon dioxide), called second layer 22 resting on the front face of the support substrate 20.

[0074] In such a case, the first layer 17 and / or the second layer 22 is found, at the end of the execution of step c), interposed between the donor layer and the support substrate.

[0075] The assembly step c) may comprise molecular bonding which results, when the free faces of the donor and support substrates are brought into contact, in the propagation of a bonding wave and consequently in adhesion between said faces. The invention is not limited to the sole implementation of molecular bonding. In this respect, it is possible to consider bonding by compression or thermocompression, bonding by means of an adhesive layer.

[0076] Step c) is then followed by a heat treatment step d) intended to initiate a fracture wave along the weakening zone in order to cause the detachment of the useful layer 15 and consequently transfer the latter to the front face 21 of the support substrate 20.

[0077] However, in order to prevent the occurrence of cracks or delamination of the donor layer at the interface formed between said donor layer 12 and the manipulator substrate 13, the heat treatment is carried out in such a way that the initiation of the fracture wave occurs at the lowest possible temperature.

[0078] In this regard, the heat treatment comprises two phases called, respectively, first phase and second phase.

[0079] [Fig.3] graphically represents an example of heat treatment that can be implemented when performing step d).

[0080] In particular, [Fig. 3] represents the time along the horizontal axis and the temperature imposed on the assembly formed by the donor substrate 10 and the support substrate 20 along the vertical axis. The first phase comprises in order: a rise in temperature A, a plateau at the first temperature B, and a fall in temperature C to the second temperature.

[0081] The first phase (illustrated in [Fig.lD]), of a first duration dl, comprises a rise in temperature up to the first temperature Tl, and is adapted on the one hand to allow maturation of defects 16, generated by the species, in the weakening zone, and on the other hand to prevent the initiation of a fracture in said weakening zone.

[0082] By "defect maturation" is meant the formation and growth of bubbles in the plane of the weakening zone. This maturation is activated by the supply of thermal energy.

[0083] The second phase (illustrated in [Fig.lE]), of a second duration d2, comprises a plateau at the second temperature T2, lower than the first temperature T1, and is adapted to initiate a fracture along the weakening zone and thus transfer the useful layer to the front face.

[0084] It is understood, without it being necessary to specify it, that the second phase is executed in continuity with the first phase.

[0085] Step d) may in particular be carried out in a batch oven, under a controlled and more particularly inert atmosphere. The invention is not limited to the implementation of a batch oven. In particular, a rapid annealing oven may also be considered.

[0086] Considering a two-phase heat treatment makes it possible to initiate a fracture wave, and consequently a transfer of the useful layer 15 onto the support substrate 20, at a lower temperature than those currently envisaged in the state of the art.

[0087] Advantageously, the first phase may be preceded by a phase of reinforcing the interface formed during the assembly of the donor substrate and the support substrate. The reinforcing phase is in this respect carried out at a temperature, called the reinforcing temperature Tr, lower than the first temperature.

[0088] It is understood, without it being necessary to specify it, that the first phase is adjusted according to the conditions of implantation of the species during the execution of step b).

[0089] In particular, the heat treatment conditions, and more particularly the first temperature T1, the second temperature T2, the first duration d1 and the second duration d2 can be determined empirically.

[0090] In this regard, and by way of example, Figures 4A to 4C are graphic representations of different heat treatments imposed on batches of 25 assemblies obtained at the end of step c). During the execution of each of these heat treatments, the inventors identified the times of detection of the initiation of a fracture likely to occur within each of the assemblies.

[0091] Thus, [Fig.4A] graphically represents a heat treatment, called first heat treatment, for which the first and second temperatures are equal to, respectively, 200°C and 160°C, while the first and second durations are equal to, respectively, 7 min and 6 hours.

[0092] [Fig.4B] graphically represents a heat treatment, called second heat treatment, and which differs from the first heat treatment in that the second temperature and the second duration are equal, respectively, to 170°C and 4 hours.

[0093] [Fig.4C] graphically represents a heat treatment, called third heat treatment, and which differs from the first heat treatment in that the first and second durations are equal to, respectively, 20 min and 4 hours.

[0094] During the execution of the first treatment, the inventors were able to observe that 8 assemblies out of the 25 present in the heat treatment furnace did not suffer any fracture.

[0095] The consideration of a second higher temperature (170°C) during the execution of the second treatment ([Fig.4B]) makes it possible to initiate a fracture wave within each of the 25 assemblies in the second phase of said treatment. However, the initiation of a fracture wave of two of the 25 assemblies is only observed after the end of the plateau of the second phase. The conditions imposed during the execution of this second annealing does not allow the required stability to be conferred on the process according to the present invention.

[0096] Considering a longer maturation stage (first phase) when carrying out the third treatment leads to the initiation of a fracture wave during the first phase (more particularly during the decrease in temperature C). Such a heat treatment does not allow stabilization of step d).

[0097] Based on these results, the inventors estimate that the optimal parameters of the heat treatment for the implantation conditions considered are as follows:

[0098] - temperature Tl= 200 °C,

[0099] - duration dl = 15 min,

[0100] - temperature T2=170 °C,

[0101] - duration d2 = 4 hours.

[0102] The above principles thus make it possible to determine the optimal heat treatment conditions for carrying out step d).

[0103] Advantageously, the first temperature T1 is less than 300°C, advantageously less than 250°C, even more advantageously less than 220°C.

[0104] Still advantageously, the absolute difference between the first temperature T1 and the second temperature T2 is less than 40°C, and is greater than 30°C. For example, the second temperature T2 is less than 180°C, advantageously less than 170°C.

[0105] Advantageously, the second duration d2 is less than 6 hours, advantageously less than 4 hours.

[0106] Carrying out the heat treatment of step d) according to the terms of the present invention makes it possible to limit the temperature of the stage during which the initiation of a fracture wave is likely to occur. This aspect makes it possible to limit the stresses at the interface formed between the donor layer and the manipulator substrate, and possibly in the intermediate layer if it is considered.

[0107] In other words, the heat treatment, as considered in the present invention, limits the occurrence of cracks and / or delamination as described in the section "TECHNOLOGICAL BACKGROUND OF THE INVENTION".

[0108] Of course, the invention is not limited to the embodiments described and variant embodiments can be made without departing from the scope of the invention as defined by the claims.

Claims

Claims

1. A method of transferring a useful layer (15) onto a support substrate (20), the method comprising the following steps: a) providing a donor substrate (10) which comprises, from a main face, a donor layer (12) formed of a piezoelectric material, and a manipulator substrate (13), the donor layer (12) resting on one face of the manipulator substrate (13); b) forming a weakening zone (14), by implantation of species in the donor layer (12), parallel to the main face and which delimits with the latter a useful layer (15); c) assembling the support substrate (20) with the donor substrate (10) so as to interpose the donor layer (12) between the manipulator substrate (13) and the support substrate (20);d) a heat treatment which comprises, in order, a first phase and a second phase, the first phase, of a first duration, comprises a temperature increase to a first temperature, and is adapted on the one hand to allow maturation of defects, generated by the species, in the weakening zone (14), and on the other hand to prevent the initiation of a fracture in said weakening zone (14), the second phase, of a second duration, comprises a plateau at a second temperature, lower than the first temperature, and is adapted to initiate a fracture along the weakening zone (14) and thus transfer the useful layer (15) onto the support substrate (20).;

2. Method according to claim 1, in which step d) also comprises a reinforcement phase preceding the first phase and carried out at a temperature, called reinforcement temperature, lower than the first temperature, the reinforcement phase being intended to reinforce a bonding energy of an interface formed between the support substrate (20) and the donor substrate (10) during the execution of step c).

3. Method according to claim 1 or 2, in which the first phase comprises in order: a rise in temperature, a hold at the first temperature, and a fall in temperature to the second temperature.

4. Method according to one of claims 1 to 3, in which the first phase is adjusted according to the conditions of implantation of the species during the execution of step b).

5. Method according to one of claims 1 to 4, in which the relative difference between the coefficients of thermal expansion of the materials forming, respectively, the manipulator substrate (13) and the support substrate (20) is less than 10%.

6. Method according to one of claims 1 to 5, in which the manipulator substrate (13) comprises a solid substrate on one face of which rests an intermediate layer, the intermediate layer being interposed between the donor layer (12) and the solid substrate, advantageously, the intermediate layer comprises a polymer material.

7. Method according to one of claims 1 to 6, in which the first temperature is less than 300°C, advantageously less than 250°C, even more advantageously less than 220°C.

8. Method according to one of claims 1 to 7, in which the absolute difference between the first temperature and the second temperature is less than 40°C, and is greater than 30°C.

9. Method according to one of claims 1 to 8, in which the second duration is less than 6 hours, advantageously less than 4 hours.

10. Method according to one of claims 1 to 9, in which the second temperature is less than 180°C, advantageously less than 170°C.

11. Method according to one of claims 1 to 10, in which the species comprise at least one of the elements chosen from: hydrogen ions, helium ions.

12. Method according to one of claims 1 to 11, in which the piezoelectric material comprises at least one of the elements chosen from: LiTaO3, LiNbO3, LiA103, BaTiO3, PbZrTiO3, KNbO3, BaZrO3, CaTiO3, PbTiO3, KTaO3.

13. Method according to one of claims 1 to 12, in which the assembly step c) is preceded by a step of forming a layer of dielectric material on the donor layer (12) and / or on a front face (21) of the support substrate (20).

14. Method according to one of claims 1 to 13, in which step c) of assembly comprises molecular bonding.