Manufacturing process for a paved structure
The method addresses contamination and pollution issues in semiconductor sticker manufacturing by using a UV-sensitive adhesive film and mineral-based paste to create a cohesive mineral material, enhancing mechanical resistance and enabling efficient functionalization and thin film transfer.
Patent Information
- Application Number
- FR2022006643
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-06-30
AI Technical Summary
Existing methods for manufacturing paved structures using semiconductor materials involve significant particle and metal contamination, organic pollution, and difficulty in rectifying sticker heights and polishing due to adhesive tape usage, leading to erosion and incompatibility with subsequent functionalization operations.
A method involving a vignetted structure with UV-sensitive adhesive film and mineral-based paste is used, where stickers are glued with a mineral-based paste, pressure is applied to fill spaces, and a heat treatment densifies the paste to form a cohesive mineral material, facilitating rectification and functionalization.
This method reduces contamination and organic pollution, enhances mechanical resistance and adhesive force, allowing for flat surface formation and efficient implantation of ionic species, enabling collective technological steps like thin film transfer.
Smart Images

Figure 00000020_0000 
Figure 00000020_0001 
Figure 00000020_0002
Abstract
Description
Title of the invention: Method for manufacturing a paved structure
[0001] The present invention relates to the field of transferring a sticker made of semiconductor material onto a support substrate. In particular, the present invention relates to a method for manufacturing a paved structure suitable for subsequent functionalization operations including in particular a film transfer by steps of implantation of ionic species, bonding and fracture.
[0002] A method of paving a support with vignettes is already known in the prior art. This method consists of fixing a source substrate on a first rigid frame by means of a first adhesive tape (also well known under the English terminology 'tape') sensitive to ultraviolet rays. The source substrate is then cut into vignettes according to the desired geometry using a diamond saw. After exposure of the first adhesive tape, the vignettes are repositioned on a second rigid frame provided with a second adhesive tape sensitive to ultraviolet rays according to the desired positioning. Then the surface of the vignettes is glued by direct gluing on the surface of a handle substrate and the second tape is exposed to separate the vignettes from the second rigid frame.After a consolidation annealing of the direct bonding, the vignettes undergo technological steps such as for example steps of transferring thin film taken from the surface of the vignettes onto a receiving support using a Smart Cut TM process.
[0003] However, this known paving process involves many disadvantages. On the one hand, cutting the tiles with a diamond saw causes significant particulate and metallic contamination. On the other hand, the use of adhesive tape causes organic pollution which is difficult to clean before carrying out the first direct bonding. There are cleaning and surface preparation solutions which are effective but they are aggressive and incompatible with the presence of the adhesive tape which holds the tiles. Finally, it is difficult to rectify the different heights of the tiles and then polish their surface because the space between the tiles leads to greater erosion of the edges of the tiles, which are more exposed to attack by the polishing device.
[0004] One of the aims of the present invention is to overcome at least one of these drawbacks. To this end, the present invention provides a method of manufacturing a paved structure comprising: - a) provision of a vignetted structure comprising a rigid frame, vignettes glued at spaced intervals on the rigid frame provided with a UV-sensitive adhesive film, such as an acrylate polymer, - b) gluing the stickers to a support substrate using a paste mineral base so as to form a stack, - c) applying pressure to the stack so that the mineral-based paste fills the space between the stickers, - d) exposing the UV-sensitive adhesive film, - e) separation of the rigid frame and the vignettes secured to the support substrate, and - f) application of a heat treatment so as to transform the mineral-based paste into a cohesive mineral material to obtain the paved structure.
[0005] The method of the invention allows the transfer of the vignettes onto a support substrate by bonding via a mineral-based paste. This bonding is less restrictive in terms of surface preparation than direct bonding by molecular adhesion. The heat treatment according to step f) allows the densification of the mineral-based paste, the elimination of the organic elements and the aggregation and / or sintering of the grains of the mineral powder constituting the paste, as will be seen in detail later, to lead to the production of a cohesive mineral material. This cohesive mineral material has sufficient mechanical strength and adhesive force to carry out a possible operation of rectification of the vignettes in order to form a flat surface as well as a possible implantation of ionic species in order to carry out a transfer by Smart Cut™.
[0006] The application of pressure to the stack according to step c) is carried out so that the mineral-based paste fills the space between the vignettes until it comes into contact with the UV-sensitive adhesive film.
[0007] For example, the pressure applied to the stack according to step c) is of the order of ten kN, and in particular the pressure is between 5 and 10 kN.
[0008] Concretely, the heat treatment of step f) is carried out in stages.
[0009] According to one possibility, the heat treatment of step f) is carried out at a temperature between room temperature and a temperature of approximately 450°C depending on the material(s) constituting the vignettes and the mineral-based paste used to obtain a cohesive mineral material. For example, for a mineral-based paste of the 'glass frit FX-11-036' type from the company Ferro, the temperature is maintained at 125°C for 30 min then at 300°C for 60 min then at 425°C for 90 min so as to obtain the desired cohesive mineral material.
[0010] According to one arrangement, the method comprises, after step f), a step g) of planarizing the upper surface of all the vignettes, so that the vignettes collectively form a flat surface. The presence of the cohesive mineral material facilitates grinding and polishing because the edge of the vignettes is less exposed than when they are glued by direct gluing without filling material in the space separating the vignettes. In addition, obtaining such a flat surface facilitates the performance of collective technological steps, such as functionalizations or thin film reports.
[0011] In practice, step g) of planarization is carried out by lapping then by chemical-mechanical polishing, so as to achieve a surface roughness of the vignettes compatible with direct bonding, for example a surface roughness < 0.5 nm RMS measured by AFM on a scan of 1*1pm2.
[0012] According to one possibility, the method comprises, after step g) of planarization, a step h) of selective chemical etching of the exposed face of the paved structure, so as to etch the cohesive mineral material more quickly than the exposed surface of the vignettes.
[0013] The chemical attack is carried out in particular by an aqueous solution of HF at 10% vol. for a duration allowing a removal of a few tens of nanometers of the cohesive mineral material relative to the surface of the vignettes.
[0014] According to one possibility, the method comprises before step a): - a step i) of removable bonding between a source substrate of vignettes and a handle substrate, - a step ii) of vignetting of the source substrate glued to the handle substrate, in particular carried out by photolithography and etching, so as to individualize the vignettes, - a step iii) of fixing the stickers in a spaced manner on the rigid frame provided with the UV-sensitive adhesive film, and - a step iv) of dismantling the handle substrate from the vignettes, so as to obtain the vignetted structure provided in step a).
[0015] These steps of preparing the vignetted structure without using a diamond saw limit particulate and metallic contamination of the vignettes.
[0016] According to one possibility, the removable bonding according to step i) is obtained by the use of an adhesive layer and a removable layer at the bonding interface between the source substrate and the handle substrate. Indeed, the removable layer limits the adhesion energy with the adhesive layer so as to allow the disassembly of step iv) at the interface between the removable layer and the adhesive layer by the insertion of a wedge at said interface.
[0017] Concretely, the removable layer is made of a material chosen from a chlorinated compound, such as octadecyltrichlorosilane, and a fluorinated polymer, such as Novec™ 2702 supplied by 3M™, Novec™ 1720 from 3M™, the Optool fluorinated polymer developed by Daikin®, perfluorodecyltrichlorosilane, or perfluorodecyldimethyl-chlorosilane.
[0018] According to one characteristic, the adhesive layer is made of a material chosen from thermoplastic polymers, for example a BrewerBOND® 305 supplied by the company Brewer Science.
[0019] Conveniently, the material of the removable layer is spread on the surface of the handle substrate. Since subsequent cleaning of the removable layer is difficult, it is preferable to place it on the handle substrate and place the adhesive layer on the source substrate.
[0020] Step iv) of disassembly also includes the removal of the adhesive layer by cleaning the vignetted structure using in particular D-limonene then isopropanol when the adhesive layer is made of BrewerBOND® 305. These components are inert with respect to the vignetted structure.
[0021] According to an alternative embodiment of the vignetted structure provided in step a), the removable bonding according to step i) is obtained by the use of an adhesive dry film, chosen from silicone-based polymers, in particular SPIS DFTA23 available in the professional range of Shin-Etsu®. This adhesive dry film is simple to use, it does not require spreading by centrifugation or an annealing step. It makes it possible to achieve sufficient adhesion energy for producing the vignetting of the source substrate without preventing the disassembly of step iv) of the substrate-handle by inserting a wedge at the interface.
[0022] Once the handle substrate has been dismantled, step iv) of the method further comprises removing by simple cleaning the dry adhesive film from the surface of the vignettes with a solution comprising p-menthol and then a solution comprising isopropanol. This solution is inert with respect to the vignetted structure.
[0023] According to an alternative embodiment of the vignetted structure, the method uses a laser treatment vignetting technology, which consists of laser damage cutting, well known under the name 'Stealth Dicing' (SD) and for example described in the following articles: Masayoshi Kumagai et al, IEEE TRANSACTIONS ON SEMICONDUCTOR MANUFACTURING, VOL. 20, NO. 3, AUGUST 2007, Cereno, DI and Wickramanayaka, S, 2017 IEEE 67TH ELECTRONIC COMPONENTS AND TECHNOLOGY CONFERENCE (ECTC 2017), pp.358-363, and Gaudiuso, C; Volpe, A and Ancona, A, Mar 2020, MICROMACHINES 11.
[0024] Also, according to this alternative, the method comprises before step a): - a step j) of laser treatment of a source substrate glued to a support frame provided with a UV-sensitive adhesive tape so as to preform cutting lines within the source substrate, the cutting lines being intended to form the vignettes, - a step jj) of extending the adhesive tape so as to cause the source substrate to break along the preformed cutting lines and form the stickers, and - a step jjj) of fixing the vignettes on the rigid frame provided with a film UV-sensitive adhesive, and - a step jjjj) of separating the support frame and the vignettes comprising the exposure of the UV-sensitive adhesive tape, so as to obtain the vignetted structure provided in step a).
[0025] This alternative avoids the use of photolithography and etching steps in the source substrate in order to provide the vignettes.
[0026] According to one possibility, the rigid frame and the UV-sensitive adhesive film respectively used in step iii) or in step jjj) have a diameter greater than that of the source substrate,
[0027] and the method comprises respectively in step iii) or jjj) the fixing of the vignettes by increasing the space between the vignettes, by modifying the initial position of the vignettes and / or by fixing vignettes of several source substrates on a single support substrate of a diameter greater than that of the source substrate.
[0028] According to one possibility, the method further comprises after step f), and for example after step g) or h): - a step k) of implanting ionic species in the vignettes of the paved structure so as to create a weakening plane in each vignette delimiting a thin film between the implanted face and said weakening plane, - a step 1) of molecular bonding of the implanted face of the vignettes on a receiving substrate, - a step m) of fracture at the level of the weakening plane, in particular by applying a heat treatment, so as to collectively transfer the thin film of each vignette onto the receiving substrate.
[0029] According to one arrangement, steps k, 1 and m) are repeated n times on the negative obtained at the end of step m), the negative comprising the support substrate and the vignettes, so as to carry out n new collective transfers of the thin film of each vignette onto a receiving support.
[0030] According to another possibility, the method comprises after step f), and for example after step g) or h) the carrying out of technological steps collectively on the vignettes of the paved structure.
[0031] Conveniently, the mineral-based paste comprises a mineral powder, a binder and a homogenizing solvent.
[0032] Concretely, the mineral powder comprises grains having a size less than or equal to one tenth of the inter-chip space between the adjacent vignettes so as to facilitate the filling of the inter-chip space during step c). This limitation in size makes it easier to fill the inter-chip spaces with the mineral-based paste. Then the densification / sintering obtained by the heat treatment according to step f) makes it possible to solidify and enlarge these grains leading to the obtaining of the cohesive mineral material.
[0033] According to other characteristics, the method of manufacturing a paved structure comprises one or more of the following optional characteristics considered alone or in combination: - The mineral-based paste is spread prior to gluing in step b) on the exposed face of the vignettes and / or on the support substrate. - Step d) of exposure is carried out before step c) of applying pressure. - Step d) of exposure is carried out after step c) of applying pressure. - The removable layer and the adhesive layer formed according to step i), are annealed by applying a heat treatment. - The source substrate is formed by at least one material constituting the tiles of the paved structure and comprises at least one semiconductor material, notably chosen from column IV and columns III / V of the periodic table of elements. - The materials of the vignettes are chosen from semiconductor materials, in particular chosen from column IV and columns III / V of the periodic table of elements and for example silicon, Ge, InP, AsGa, SiC, glass, alumina, sapphire, LNO, LTO and quartz. - The tiles of the paved structure are all made of the same single material. - The paved structure includes tiles of different materials. - Each of the tiles in the paved structure is made up of a composite structure, the composite structure comprising different or identical materials. - The space between two adjacent vignettes of the vignette structure is between 100 and 200 micrometers. - Each vignette has a main face of polygonal shape, for example square or rectangular, or an oval or circular shape. - Step ii) includes a step of removing the vignettes at the edge of the handle substrate, the main face of which has a shape different from that of the majority of the vignettes. - Mineral-based paste is formed solely by mineral powder, binder and homogenizing solvent. - The mineral powder is chosen from metallic powders, metalloid powders, ceramic powders and a combination of these powders, in particular metalloid or ceramic powders so as to avoid a metallic contamination and for example a powder of a composition identical to that of the vignettes. Metal powders are chosen from silver, copper, tin and tungsten for example. Metalloid powders are chosen from silicon, germanium, and antimony, for example. Ceramic powders are chosen from oxides and silicates, for example SiO2, GeO2, Al2O3, TiO2, mica, etc. The mineral-based paste is composed so as to have the necessary properties to be able to be spread by screen printing or by tape casting. The quantity of homogenizing solvent is chosen so that said mineral-based paste has a viscosity between 10 and 500 Pa.s. The homogenization solvent is chosen in particular from N-methyl-2-pyrrolidone, terpinol, and limonene. The nature of the binder of the mineral-based paste is chosen so as to give cohesion to the mineral-based paste. The binder of the mineral-based paste is chosen from mineral materials, organic materials and a combination of these materials. The mineral materials forming the binder of the mineral-based paste are chosen from doped glass of the alkaline polysilicate Li2Si50n type, a poly-phosphate (NaPO3)n, and a phosphate H2LiPO4. The organic materials forming the binder of the mineral-based paste are polymeric materials, such as polyvinylidene fluoride, polyvinylpyrrolidone, ethyl cellulose, or polyethylene glycol. The mineral-based paste is made of 'glass frit FX-11-036' compound available from Ferro. The mineral-based paste is made up of a mixture of a silica mineral powder (Aerosil® R202 - 5g), an ethyl cellulose binder (Sigma Aldrich® -0.5g) and a Terpinol homogenization solvent (Sigma Aldrich® - 5g). The repetition n times of steps k, 1 and m) on the negative obtained at the end of step m), comprises first carrying out step g) of planarization of the upper surface of all the vignettes, and / or a step h) of selective chemical attack of the exposed face of the paved structure, so as to remove the work-hardened zone by the implantation of ionic species according to step k) previously carried out, and obtain the removal of the cohesive mineral material from the mineral-based paste relative to the surface of the vignettes. The steps described above are repeated n times until the residual thickness of the stickers is no longer sufficient to carry out a transfer film collective. - The rigid frame is a metal frame, such as DISCO® metal frames, or a rigid frame made of any other material that is non-contaminating under the conditions of use. - The handle substrate is made of silicon. - The support substrate is made of silicon. - The UV-sensitive adhesive film and tape are made of acrylate polymer, particularly compound 'SP-537T-230' available from Furukawa Electric.
[0034] Other aspects, aims and advantages of the present invention will appear better on reading the following description of different variant embodiments thereof, given by way of non-limiting example and with reference to the appended drawings. The figures do not necessarily respect the scale of all the elements represented so as to improve their readability. Dotted lines symbolize a weakening plane formed in a substrate. In the remainder of the description, for the sake of simplification, identical, similar or equivalent elements of the different embodiments bear the same numerical references.
[0035] [Fig.l] is a schematic view illustrating a step i) and ii) of the method according to an embodiment of the invention.
[0036] [Fig.2] is a schematic view illustrating a step iii) of the method according to the mode of production of [Fig.l] and supply of the vignetted structure a).
[0037] [Fig.3] is a schematic view illustrating steps b) to d) of the method according to the embodiment of [Fig.l].
[0038] [Fig.4] is a schematic view illustrating steps e) and f) of the method of realization of [Fig.l].
[0039] [Fig.5] is a schematic view illustrating steps g) and h) then step k) of implantation according to an embodiment of the invention.
[0040] [Fig.6] is a schematic view illustrating steps 1) and m) of the method according to one embodiment of the invention.
[0041] [Fig.7] is a schematic view illustrating a step j) of the method according to a pos feasibility of carrying out the invention.
[0042] [Fig.8] is a schematic view illustrating steps jj) to jjjj) of the method according to the embodiment of [Fig.7].
[0043] [Fig.9] is a schematic view illustrating a step jjj) or iii) of transferring vignettes of several source substrates on a single frame of larger diameter according to an alternative embodiment of the invention.
[0044] As illustrated in Figures 1 to 6, the method according to the invention comprises the preparation of a vignetted structure 50, the transfer of vignettes 1 onto a support substrate S3 so as to obtain a paved structure 100, steps of functionalizing the vignettes 1, and / or of carrying out a collective transfer of a thin film 2 taken from each of the vignettes 1 onto a receiving substrate S4.
[0045] The method for manufacturing a tiled structure 100 firstly comprises a step of detachable bonding of a source substrate SI onto a handle substrate S2 ([Fig.l]- step i) followed by a vignetting step comprising photolithography of the surface of the source substrate SI then etching in the source substrate SI forming trenches 3 to delimit spaced vignettes 1 ([Fig.l]- step ii). A rigid frame 4 provided with a UV-sensitive adhesive film 5 is provided to fix the vignettes 1 thereto ([Fig.2]- step iii). The handle substrate S2 is then detached at the detachable bonding interface so as to obtain the vignetted structure 50 which will be provided in step a) of the method ([Fig.2] - step iv).
[0046] The vignettes 1 are then glued onto a support substrate S3 covered with a mineral-based paste 6 to form a stack 7 ([Fig.3]). Pressure is applied on either side of the stack 7 so as to ensure that the space 3 between the vignettes 1 is filled with the mineral-based paste 6 ([Fig.3], steps b and c). A step d) of exposing the UV-sensitive adhesive film 5 is then carried out ([Fig.3]) before separating the rigid frame 4 from the vignettes 1 secured to the support substrate S3, ([Fig.4] - step e).
[0047] A heat treatment is applied for: - allow the elimination of organic components from the mineral-based paste 6, - densify the mineral paste 6 by aggregation and / or sintering of the mineral grains.
[0048] At the end of the heat treatment, only the mineral part of the paste 6' remains ([Fig.4], step f). The cobblestone structure 100 is then obtained. This heat treatment and this structuring of the cohesive mineral material 6' also make it possible to increase the adhesion energy of the vignettes 1 on the support substrate S3. A step g) of planarization of the upper surface 8 of the set of vignettes 1 is then carried out so that the vignettes 1 collectively form a flat surface ([Fig.5]). Depending on the materials used and the planarization method carried out, step g) is not sufficient to obtain a shrinkage of the cohesive mineral material 6' relative to the surface of the vignettes 1 (or it is deliberately limited to reduce costs), which risks hindering a future collective transfer by Smart Cut™ of the vignettes 1 onto a receiving substrate S4.A step h) of selective chemical etching is then carried out so as to obtain a shrinkage of between 10 and 20 nm of the cohesive mineral material 6' derived from the mineral-based paste 6 in the space 3 between the vignettes 1 ([Fig.5]).
[0049] The paved structure 100 thus prepared is advantageously used for a collective transfer of thin film 2 coming from the vignettes 1 onto a receiving substrate S4. For this To do this, a step k) of implanting ionic species is carried out in the vignettes 1 so as to create a weakening plane 9 delimiting a thin film 2 in each vignette 1, the thin film 2 being between the implanted surface and the weakening plane 9 ([Fig.5]). The implanted paved structure 100 is then used for molecular bonding on a receiving substrate S4 according to step 1) of the method ([Fig.6]). This is followed by a step m) of fracture at the weakening plane 9 so as to collectively transfer the thin film 2 of each vignette 1 onto the receiving substrate S4 and obtain a new paved structure by direct bonding ([Fig.6]). The negative 11 obtained at the end of the fracture of the paved structure 100 comprises the support substrate S3 and the thinned vignettes 1. This negative 11 is advantageously reused after planarization, polishing etc... in new collective transfer of thin film 2 of the vignettes 1 onto a new receiving substrate S4 ([Fig.5])..
[0050] An alternative embodiment of the method according to the invention differs from that described above in that the vignetted structure 50 is prepared using a 'stealth dicing' technology ([Fig.7]). This alternative embodiment comprises: - a step j) of laser treatment of a source substrate SI glued to a support frame 12 provided with a UV-sensitive adhesive tape 13, so as to preform cutting lines 14 within the source substrate SI, the cutting lines 14 being intended to form the vignettes 1 ([Fig.7]), - a step jj) of extending the adhesive tape 13 so as to cause the source substrate SI to break along the preformed cutting lines 14 and form the vignettes 1, ([Fig.8]), - a step jjj) of fixing the vignettes 1 on a rigid frame 4 provided with a UV-sensitive adhesive film 5, and a step jjjj) of separating the support frame 12 and the plurality of vignettes 1 comprising the exposure of the UV-sensitive adhesive tape 13, ([Fig.8]) so as to obtain the vignetted structure 50 provided in step a).
[0051] According to yet another alternative embodiment which differs from the method described above, the method comprises in step iii) or jjj) the provision respectively of a support frame 12 or a rigid frame 4 provided with a UV-sensitive adhesive film 5 having a diameter greater than that of the source substrate SI, for example 300 nm and 100 nm respectively, so as to fix vignettes 1 of several source substrates SI on a single rigid frame 4' or support frame 12' ([Fig.9]). The fixing according to step iii) or jjj) is then advantageously carried out by a device for handling and transferring vignettes (Pick and Place) allowing the independent handling of each of the vignettes 1 or of a plurality of vignettes 1 at the same time. The following steps are carried out as previously described using a support substrate S3 and a receiving substrate S4 of a diameter at least equal to the diameter of the disc defined by the thumbnails 1 on the rigid frame 47support frame 12' (not shown).
[0052] Detailed examples of embodiments of the method according to the invention follow below. Example 1
[0053] A removable layer 16 of a fluoropolymer (Novec™ 2702) is formed by spreading on a silicon handle substrate S2 (200 mm in diameter and 725 μm thick), and the assembly is annealed at 150°C for 30 min. The thickness of the fluoropolymer film is of the order of 10 nm.
[0054] An adhesive layer 15 is formed by spreading 40 μm of a BrewerBOND® 305 adhesive resin on a silicon source substrate SI (200 mm in diameter and 725 μm thick) before bonding with the handle substrate S2 at 210°C so as to obtain a removable bond at the interface between the adhesive layer 15 and the removable layer 16 of fluoropolymer ([Fig.l] - step i).
[0055] The source substrate SI is thinned by mechanical abrasion using a diamond wheel until it reaches a thickness of 500 pm. The surface is then wet cleaned. Photolithography of the source substrate SI makes it possible to define vignettes 1 of 8x8 mm2 with a space 3 of 100 pm between adjacent vignettes 1 ([Fig.l], step ii).
[0056] The vignettes 1 thus obtained have a thickness of 500 micrometers. They are then glued onto a rigid DISCO® metal frame 4 using a UV-sensitive adhesive film 5 'SP-537T-230' available from the company Furukawa ([Fig.2], step iii). The handle substrate S2 is then detached by inserting a wedge at the interface between the adhesive layer 15 and the removal layer 16 (step iv). The adhesive layer 15 is removed by cleaning with D-limonene and then isopropanol. The vignetted structure 50 comprising vignettes 1 glued by an adhesive film 5 onto a rigid frame 4 is thus obtained ([Fig.2]) and can be provided according to step a) of the method of the invention.
[0057] On a silicon support substrate S3 (200 mm in diameter and 725 μm thick) is spread by screen printing approximately 100 μm of mineral-based paste 6 “glass frit FX-11-036” from the company Ferro. The UV-sensitive adhesive film 5 of the vignetted structure 50 is exposed by UV irradiation (step d) then the support substrate S3 is brought into contact with the vignettes 1 so as to form a stack 7 (step b) while applying a pressure of 5 kN ([Fig. 3], step c). According to a variant, it is possible to expose the UV-sensitive adhesive film 5 (step d) after contacting.
[0058] The rigid frame 4 is separated from the stack 7 consisting of the support substrate S3 and the vignettes 1 ([Fig.4], step e). Annealing by applying a heat treatment at 125°C for 30 min, then 300°C for 60 min and 425°C for 90 min ([Fig.4], step f) allows the transformation of the mineral-based paste 6 into mineral material cohesive mineral material 6' and obtaining the paved structure 100. The vignettes 1 are secured to the support substrate S3 and the space 3 between the vignettes 1 is filled. The surface of the vignettes 1 is planarized by a mechanical lapping step then a thorough chemical-mechanical polishing step (step g). The polishing speed of the cohesive mineral material 6' from the glass frit is higher than the polishing speed of the silicon, which leads to a shrinkage of the cohesive mineral material 6' of approximately 20 nm compared to the surface of the silicon vignettes 1 ([Fig.5]).
[0059] The paved structure 100 thus prepared is subjected to an implantation of hydrogen ions with an energy of 150 keV and a dose of 5.1016 ions / cm2 ([Fig.5], step k). A silicon receiving substrate S4 (200 mm in diameter and 725 pm thick) is oxidized so as to form a 500 nm SiO2 film on its surface (not shown). The receiving substrate S4 is then prepared so as to achieve direct bonding with the implanted face of the vignettes 1 ([Fig.6], step 1). Annealing at 500°C makes it possible to obtain a fracture at the level of the embrittlement plane 9 and a thin film 2 with a thickness of 1.2 pm coming from each of the vignettes 1 is transferred onto the receiving substrate S4 ([Fig.6], step m). A chemical-mechanical polishing of the negative 11 obtained at the end of step m) comprising the support substrate S3 and the vignettes 1 allows a new use in a thin film transfer process 2 as previously described according to steps k to m). Example 2
[0060] A removable layer 16 of 10 nm of fluorinated polymer (Novec™ 1720) is formed by spreading on a silicon handle substrate S2 (200 mm in diameter and 725 pm thick), and the assembly is annealed at 135°C for 15 min.
[0061] An adhesive layer 15 is formed by spreading 40 μm of a BrewerBOND® 305 adhesive resin on a silicon source substrate SI (200 mm in diameter and 725 μm thick) before bonding with the handle substrate S2 at 210°C so as to obtain a removable bond at the interface between the adhesive layer 15 and the fluoropolymer layer 16 ([Fig.l], step i).
[0062] A photolithography in the silicon of the source substrate SI makes it possible to define vignettes 1 of 20x20 mm2 with a space 3 of 200 pm between the adjacent vignettes 1 (step ii).
[0063] The vignettes 1 thus obtained are glued onto a DISCO® metal frame using an adhesive film 5 'SP-537T-230' available from the company Furukawa (step iii). The handle substrate S2 is then detached by inserting a wedge at the interface between the adhesive layer 15 and the disassembly layer ([Fig.2], step iv). The adhesive layer 15 is then removed by cleaning with D-limonene and then isopropanol so as to obtain the vignetted structure 50.
[0064] On a silicon S3 support substrate (200 mm in diameter and 725 pm thickness) is spread by screen printing approximately 100 μm of mineral-based paste 6 "glass frit FX-11-036" from the company Ferro ([Fig.3]). The UV-sensitive adhesive film 5 of the vignetted structure 50 is exposed by UV irradiation (step d) then the vignettes 1 at the edge of the rigid frame 4 which do not have the desired shape (for example square) are removed using a suitable tool for handling and transferring vignettes (Pick and Place).
[0065] The support substrate S3 is then brought into contact with the vignettes 1 so as to form a stack 7 ([Fig.3] step b) while applying a pressure of 5 kN (step c).
[0066] The rigid frame 4 is separated from the stack 7 consisting of the support substrate S3 and the vignettes 1 ([Fig.4], step e). Annealing by applying a heat treatment at 125°C for 30 min, then 300°C for 60 min and 425°C for 90 min (step f) allows the transformation of the mineral-based paste into cohesive mineral material 6' and the obtaining of the paved structure 100. The vignettes 1 are integral with the support substrate S3 and the space 3 between the vignettes 1 is filled. The surface of the vignettes 1 is planarized by a mechanical lapping step then a chemical-mechanical polishing step ([Fig.5], step g) is applied lightly to avoid significant wear of the consumables. However, since light polishing does not allow sufficient removal of cohesive mineral material 6' to be achieved, selective chemical attack completes it with an aqueous solution of HF at 10% vol.during Imn (step h) and allows to achieve a sufficient shrinkage of the cohesive mineral material 6' from the "glass frit" for example 10 nm relative to the surface of the silicon. The paved structure 100 thus prepared can be used as a donor substrate of thin film 2 of Si in a Smart Cut™ transfer process (implantation, bonding, fracture). Example 3
[0067] Stealth Dicing technology is used to cut ten 100mm diameter InP SI source substrates into 10x10mm2 chips. To do this, the SI source substrates are each arranged on a UV-sensitive adhesive tape 13 arranged on a support frame 12. A laser processing step is performed in each of the source substrates so as to preform cutting lines 14 within the source substrate (step j - [Fig.7]). The adhesive tape 13 is then stretched so as to cause the source substrate to break along the preformed cutting lines 14 and form the vignettes 1 ([Fig.8], step jj).
[0068] A rigid frame 4' of a dimension adapted to plates with a diameter of 300 mm and provided with a UV-sensitive adhesive film 5 is used to transfer the vignettes 1 of the ten source substrates SI ([Fig.9]) using a suitable tool for handling and transferring vignettes (Pick and Place). The non-square vignettes 1 at the edge of the frame have been removed beforehand (not shown).
[0069] On a silicon support substrate S3 (300 mm in diameter and 725 μm thick) is spread by screen printing approximately 100 μm of mineral-based paste 6 “glass frit FX-11-036” from the company Ferro. The support substrate S3 is brought into contact with the vignettes 1 so as to form a stack 7 (as in [Fig.3], step b) while applying a pressure of 10 kN (step c).
[0070] The UV-sensitive adhesive film 5 is exposed by UV and the rigid frame 4 is separated from the stack 7 consisting of the support substrate S3 and the vignettes 1 ([Fig.4], step e). Annealing by applying a heat treatment at 125°C for 30 min, then 300°C for 60 min and 350°C for 300 min (step f) allows the transformation of the mineral-based paste 6 into cohesive mineral material 6' and the obtaining of the paved structure 100. The vignettes 1 are secured to the support substrate S3 and the space 3 between the vignettes 1 is filled. The surface of the vignettes 1 is planarized by a mechanical lapping step then a light chemical-mechanical polishing step (step g).
[0071] In order to increase the shrinkage obtained by the chemical-mechanical polishing of step g), it is completed by a selective chemical attack with an aqueous solution of HF at 10% vol. for 1 min ([Fig.5] - step h). This allows a shrinkage of cohesive mineral material 6' from the "glass frit" of approximately 10 nm relative to the surface of the InP.
[0072] The paved structure 100 thus prepared is subjected to an implantation of hydrogen ions with an energy comprised between 60 and 100 keV and a dose comprised between 6 and 7.1016 ions / cm2 depending on the thickness of the InP film to be transferred ([Fig.6], step k). A silicon receiver substrate S4 (300 mm in diameter and 725 pm thick) is oxidized so as to form a 200 nm SiO2 film on its surface. The receiver substrate S4 is then prepared so as to achieve direct bonding with the implanted face of the vignettes 1 ([Fig.6], step 1). Annealing at 280°C makes it possible to obtain a fracture at the level of the embrittlement plane 9 and a thin film 2 originating from each of the vignettes 1 is transferred onto the receiver substrate S4 (step m). A chemical-mechanical polishing of the negative 11 obtained at the end of step m) comprising the support substrate S3 and the vignettes 1 allows a new use in a thin film transfer process 2 as previously described according to steps k to m). Example 4:
[0073] A dry adhesive film in SPIS DFTA23 (Shin Etsu®) is deposited by spreading on a silicon S2 handle substrate with a diameter of 200 mm (725 μm thick),
[0074] A removable bonding of the handle substrate S2 with a 200 mm diameter germanium source substrate SI is carried out at 90°C ([Fig.l], step i). A photolithography of the germanium source substrate SI makes it possible to define vignettes 1 of 2x12 mm2 with a space 3 between the adjacent vignettes 1 of 200 pm (step ii).
[0075] The vignettes 1 thus obtained are stuck on a rigid metal DISCO® frame 4 using an adhesive film 5 'SP-537T-230' available from the company Furukawa ([Fig.2], step iii). The handle substrate S2 is then detached by inserting a wedge at the interface of the removable bonding ([Fig.2], step iv).
[0076] The dry adhesive film in SPIS DFTA23 is then removed by cleaning with p-menthol and then isopropanol. The vignetted structure 50 comprising vignettes 1 glued by an adhesive film 5 in SP-537T-230 on a rigid frame 4 is thus obtained. Said UV-sensitive adhesive film 5 is exposed by UV irradiation ([Fig.3], step d).
[0077] A silica-based mineral-based paste 6 is prepared by mixing 5 g of silica (Aerosil® R 202), 0.5 g of ethyl cellulose (Sigma-Aldrich®) and 5 g of terpinol (Sigma-Aldrich®). Approximately 100 μm of this mineral-based paste 6 is spread by screen printing on a silicon support substrate S3 (200 mm in diameter and 725 μm thick) before contacting with the vignettes 1 so as to form a stack 7 ([Fig. 3], step b) while applying a pressure of 5 kN (step c).
[0078] The rigid frame 4 is separated from the stack 7 consisting of the support substrate S3 and the vignettes 1 ([Fig.4], step e). Annealing by applying a heat treatment at 100°C for 60 min, then 425°C for 120 min (step f) allows the transformation of the mineral-based paste 6 into cohesive mineral material 6' and the obtaining of the paved structure 100. The vignettes 1 are integral with the support substrate S3 and the space 3 between the vignettes 1 is filled. The surface of the vignettes 1 is planarized by a mechanical lapping step then a chemical-mechanical polishing step (step g).
[0079] After this step g) a selective chemical attack with an aqueous solution of HF at 10% vol. for 1 min makes it possible to set back the cohesive mineral material 6' by approximately 10 nm relative to the surface of the silicon ([Fig.5], step h). The paved structure 100 thus prepared can be used as a donor substrate for a thin film 2 of Ge in a collective transfer process using Smart Cut™ technology (implantation, bonding and fracture). Example 5:
[0080] Silicon plates with a diameter of 200 mm and a thickness of 725 μm are used.
[0081] A removable layer 16 of fluorinated polymer (Optool Daikin®) is formed by spreading on a silicon handle substrate S2 (200 mm in diameter and 725 μm thick) ([Fig.l]).
[0082] An adhesive layer 15 is formed by spreading 40 μm of a BrewerBOND® 305 adhesive resin on a silicon source substrate SI (200 mm in diameter and 725 μm thick) before bonding with the handle substrate S2 at 210°C so as to obtain a removable bond at the interface between the adhesive layer 15 and the fluoropolymer layer 16 ([Fig.l], step i).
[0083] A photolithography in the silicon of the source substrate SI makes it possible to define vignettes 1 of 8x8 mm2 with a space 3 of 100 pm between the adjacent vignettes 1 (step ii).
[0084] The vignettes 1 thus obtained are glued onto a DISCO® metal frame using an adhesive film 5 'SP-537T-230' available from the company Furukawa ( [Fig.2], step iii). The handle substrate S2 is then detached by inserting a wedge at the interface between the adhesive layer 15 and the disassembly layer (step iv). The adhesive layer 15 is removed by cleaning with D-limonene and then isopropanol. The vignetted structure 50 comprising vignettes 1 glued by an adhesive film 5 onto a rigid frame 4 is thus obtained.
[0085] On a silicon support substrate S3 (200 mm in diameter and 725 μm thick) is spread by screen printing approximately 100 μm of mineral-based paste 6 “glass frit FX-11-036” from the company Ferro. The UV-sensitive adhesive film 5 of the vignetted structure 50 is exposed by UV irradiation ([Fig. 3], step d) then the support substrate S3 is brought into contact with the vignettes 1 so as to form a stack 7 (step b) while applying a pressure of 5 kN (step c).
[0086] The rigid frame 4 is separated from the stack 7 consisting of the support substrate S3 and the vignettes 1 due to the prior exposure of the film 5 ([Fig.4], step e). Annealing by applying a heat treatment at 125°C for 30 min, then 300°C for 60 min and 425°C for 90 min (step f) allows the transformation of the mineral-based paste 6 into cohesive mineral material 6' and the obtaining of the paved structure 100. The vignettes 1 are integral with the support substrate S3 and the space 3 between the vignettes 1 is filled. The surface of the vignettes 1 is planarized by a mechanical lapping step then a chemical-mechanical polishing step ([Fig.5], step g). The polishing speed of the cohesive mineral material 6' from the glass frit is higher than the polishing speed of the silicon, which leads to a shrinkage of the cohesive mineral material 6' of approximately 20 nm relative to the surface of the silicon vignettes 1 (no performance of step h) in this example).
[0087] The paved structure 100 thus prepared can be used as a donor substrate for a thin film 2 of Si in a Smart Cut™ transfer process (implantation, bonding, fracture) as described above.
[0088] Thus the present invention proposes a method for manufacturing a tiled structure 100 comprising vignettes made of semiconductor material and configured to be used as a donor substrate and collectively transfer the thin film of each vignette onto a receiving substrate by Smart Cut™, while limiting the number of surface cleaning steps as well as the cycle time.
Claims
Claims
1. A method of manufacturing a paved structure (100) comprising: - a) providing a vignetted structure (50) comprising a rigid frame (4), vignettes (1) glued in a spaced manner on the rigid frame (4) provided with a UV-sensitive adhesive film (5), - b) gluing the vignettes (1) to a support substrate (S3) by means of a mineral-based paste (6) so as to form a stack (7), - c) applying pressure to the stack (7) so that the mineral-based paste (6) fills the space (3) between the vignettes (1), - d) exposing the UV-sensitive adhesive film (5), - e) separating the rigid frame (4) and the vignettes (1) secured to the support substrate (S3), and - f) applying a heat treatment so as to transform the mineral-based paste (6) into a cohesive mineral material (6') to obtain the structure paved (100).
2. A method of manufacturing a paved structure (100) according to claim 1, comprising after step f) a step g) of planarizing the upper surface (8) of all the vignettes (1), so that the vignettes (1) collectively form a flat surface.
3. Method for manufacturing a paved structure (100) according to claim 2, comprising after step g) of planarization, a step h) of selective chemical etching of the exposed face of the paved structure (100), so as to etch the cohesive mineral material (6') more quickly than the exposed surface of the vignettes (1).
4. Method for manufacturing a paved structure (100) according to one of claims 1 to 3, comprising before step a): - a step i) of removable bonding between a source substrate (SI) of vignettes (1) and a handle substrate (S2), - a step ii) of vignetting the source substrate (SI) bonded to the handle substrate (S2), so as to single out the vignettes (1), - a step iii) of fixing the vignettes (1) in a spaced manner on the rigid frame (4) provided with the UV-sensitive adhesive film (5), and - a step iv) of dismantling the handle substrate (S2) from the vignettes (l), so as to obtain the vignetted structure (50) provided in step a).
5. A method of manufacturing a paved structure (100) according to one of claims 1 to 3, comprising before step a): - a step j) of laser treatment of a source substrate (SI) glued to a support frame (12) provided with a UV-sensitive adhesive tape (13) so as to preform cutting lines (14) within the source substrate (SI), the cutting lines (14) being intended to form the vignettes (1), - a step jj) of extending the adhesive tape (13) so as to cause the source substrate (SI) to break along the preformed cutting lines (14) and form the vignettes (1), and - a step jjj) of fixing the vignettes (1) to the rigid frame (4) provided with a UV-sensitive adhesive film (5), and - a step jjjj) of separating the support frame (12) and the vignettes (1) comprising the exposure of the adhesive tape (13) sensitive to UV, so as to obtain the vignetted structure (50) provided in step a).
6. A method of manufacturing a paved structure (100) according to one of claims 4 or 5, wherein the rigid frame (4') and the UV-sensitive adhesive film (5) respectively used in step iii) or step jjj) have a diameter greater than that of the source substrate (SI), and wherein step iii) or step jjj) comprises fixing stickers (1) by increasing the space (3) between the stickers (1), by modifying the initial position of the stickers (1) and / or by fixing stickers (1) of several source substrates (SI) on a single rigid frame (4') of a diameter greater than that of the source substrate (SI).
7. Method for manufacturing a paved structure (100) according to one of claims 1 to 6, further comprising after step f): - a step k) of implanting ionic species in the vignettes (1) of the paved structure (100) so as to create a weakening plane (9) in each vignette (1) delimiting a thin film (2) between the implanted face and said weakening plane (9), - a step 1) of molecular bonding of the implanted face of the vignettes (1) on a receiving substrate (S4), - a step m) of fracture at the level of the weakening plane (9), so as to collectively transfer the thin film (2) of each vignette (1) onto the receiving substrate (S4) and obtain a negative comprising the support substrate and the vignettes (1).
8. Method for manufacturing a paved structure (100) according to claim 7, in which steps k, 1 and m) are repeated n times on the negative obtained at the end of step m), the negative comprising the support substrate and the vignettes (1), so as to carry out n new collective transfers of the thin film of each vignette (1) onto a receiving support (S4).
9. A method of manufacturing a paved structure (100) according to one of claims 1 to 8, wherein the mineral-based paste (6) comprises a mineral powder, a binder and a homogenizing solvent.
10. A method of manufacturing a paved structure (100) according to claim 9, wherein the mineral powder comprises grains having a size less than or equal to one tenth of the inter-chip space (3) between the adjacent vignettes (1) so as to facilitate the filling of the inter-chip space (3) during step c).