Reinforced wiper blade for windshield wiper
Incorporating raw kaolin as a reinforcing filler in a bio-sourced elastomer blend for windshield wiper blades addresses environmental concerns and enhances mechanical properties, achieving improved rigidity and elasticity.
Patent Information
- Application Number
- FR2022009893
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-09-29
AI Technical Summary
Existing windshield wiper blades made from petrochemical materials face environmental concerns and require improved mechanical properties, particularly rigidity and elasticity, while reducing reliance on carbon black fillers.
Incorporating aluminosilicate, specifically raw kaolin with a lamellar structure and a specific surface area of 15 to 45 m2/g, as a reinforcing filler in a bio-sourced elastomer blend of natural rubber and ethylene-propylene-diene monomer (EPDM) to enhance cohesion and mechanical properties without sulfur vulcanization.
The use of raw kaolin improves the mechanical properties and homogeneity of the elastomer mixture, providing enhanced rigidity and resistance to mechanical stress, while reducing the environmental impact by minimizing petrochemical content.
Smart Images

Figure 00000013_0000 
Figure 00000013_0001
Abstract
Description
Title of the invention: Reinforced wiping blade for windshield wiper blade
[0001] The invention relates to a wiping blade for a windshield wiper, in particular composed in part of bio-sourced materials.
[0002] Motor vehicles are commonly equipped with windshield wiper systems to ensure washing and / or wiping of the windshield and to prevent the driver's vision of his surroundings from being disturbed. The wiper blades of such a system are conventionally driven by arms performing a back-and-forth angular movement. These blades rub against the outer surface of the window, for example the windshield, and evacuate the water by bringing it out of the driver's field of vision. In a conventional version, the blades are made in the form of articulated levers which hold the wiper blade at several points. In a more recent version called "fiat blade" (for "flat blade"), the blades are made in the form of a semi-rigid assembly which holds the wiper blade along its entire length.
[0003] Generally speaking, a wiper blade is made of elastically deformable material based on an elastomer supplemented with additives, in particular to improve its mechanical properties, elasticity, resistance to wear, to external aggressions or to facilitate the implementation of the manufacturing process. This may for example be reinforcing fillers, plasticizer, vulcanizing agent, agent for protection against UV radiation, oxidation, ozone and / or wear. These additives remain necessary to obtain a material having sufficient properties, in particular in terms of mechanical strength, sliding properties and without generating excessive noise to be used in the automotive industry to manufacture wiper blades.
[0004] Both the elastomer and the additives are in most cases petrochemical products. However, the growing desire to protect the environment and reduce CO2 emissions is leading to limiting the use of such petrochemical products.
[0005] In the rubber industry, it is possible to use natural rubber as a basic elastomer which is very efficient in terms of its elasticity and its intrinsic mechanical properties. Natural rubber comes from rubber cultivation, which makes it a bio-sourced material. Combined with bio-sourced fillers and plasticizers, the use of natural rubber makes it possible to considerably reduce the rate of materials from petrochemicals.
[0006] Application EP3546302 describes materials for a broom wiper blade wiper blades in which the elastomer is composed of a mixture of natural rubber, in particular non-functionalized, and EPDM (ethylene-propylene-diene monomer) of bio-sourced origin; EPDM fulfills the functions of anti-UV and anti-ozone agent, thus reducing the addition of other additives. In these materials, the vulcanization system does not use sulfur, which involves the use of activators or accelerators that can be harmful to the environment, but the vulcanization system is peroxide-based.
[0007] This peroxide vulcanization system allows for better homogeneity of crosslinking between the two elastomeric phases, and thus better elasticity of the final product. The advantage of this better cohesion in terms of elasticity nevertheless has the disadvantage of generating weaker mechanical properties than with sulfur vulcanization.
[0008] Indeed, the peroxide crosslinking network, consisting of CC bridges, is more sensitive to strong elongations (such as greater than 100%) than a sulfur network, consisting of mono and polysulfide bridges which make it possible to achieve high elongation levels (such as greater than 300%).
[0009] Obtaining mechanical properties suitable for its use, and in particular the rigidity of the wiping blade prepared from this material, requires the addition of reinforcing fillers. Such fillers are typically carbon black, which is massively produced by the petrochemical industry, by incomplete combustion of hydrocarbons.
[0010] It is desirable to replace, at least partially, carbon black with fillers of bio-sourced origin, with a view to reducing the environmental footprint of the finished product.
[0011] The use of fillers based on calcined kaolin has thus been proposed in WO2017 / 194776. However, to improve its performance, calcined kaolin must generally be functionalized, in particular by silane chains; the silane risks deactivating during storage or mixing, which makes the use of these functionalized kaolins delicate and not very robust.
[0012] Replacement reinforcing fillers must preserve the elastic properties of the material while ensuring its rigidity and resistance to mechanical stresses.
[0013] It has been found within the scope of the present invention that the use of natural fillers such as raw kaolin makes it possible to achieve these and other objectives.
[0014] This is why the present invention relates to a wiper blade for a windscreen wiper, at least a part of said blade comprising a material based on (i) elastomer containing natural rubber and ethylene-propylene-diene monomer (EPDM), vulcanized with peroxide and (ii) at least one additive, characterized in that the additive is an aluminosilicate having a specific surface area of 15 to 45 m2 / g and in particular a lamellar structure.
[0015] The invention is based on the use of aluminosilicate having specific surface characteristics, making it possible to improve the cohesion of the mixture of elastomer and additives, and to reinforce the solidity thereof.
[0016] The invention also relates to the use of a lamellar aluminosilicate, in particular raw kaolin, with a specific surface area of 15 to 45 m2 / g, preferably 20 to 40 m2 / g, for the manufacture of a wiper blade for a windscreen wiper, said wiper blade for a windscreen wiper comprising an elastomer-based material containing natural rubber and ethylene-propylene-diene monomer (EPDM) and essentially free of sulfur.
[0017] Aluminosilicates which are particularly suitable for implementing the invention are kaolins, and more particularly raw kaolin.
[0018] Indeed, unlike kaolins previously used as reinforcing filler such as calcined kaolins, which have a round structure, raw kaolin has a lamellar structure. This is retained in the particles based on raw kaolin. It is thus possible to obtain particles having a larger specific surface area, and to obtain better interaction with the rubber when mixing the composition.
[0019] The aluminosilicate and in particular the raw kaolin according to the invention is in the form of particles with an average size of less than 9 pm, i.e. 95% of the population of all the particles has a size of less than 9 pm. According to certain embodiments, the size of the particles is less than 8 pm.
[0020] Advantageously, the average size of the aluminosilicate particles is approximately 1 μm. The average size is generally greater than 0.1 μm, or even greater than or equal to 0.3 μm.
[0021] By particle size is meant the largest dimension of said particle, in the case where it has an irregular shape.
[0022] The average particle size is determined by methods known to those skilled in the art, such as, for example, laser diffraction.
[0023] The specific surface area of the aluminosilicate particles is from 15 to 45 m2 / g, which means that it can be 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44 or 45 m2 / g. The specific surface area is advantageously from 20 to 40 m2 / g, in particular from 20 to 30 m2 / g, in particular about 20 m2 / g.
[0024] In a material for a wiper blade for a windscreen wiper according to the invention, all or part of the reinforcing fillers may consist of aluminosilicate in the form of particles as defined in the present text.
[0025] The material can thus comprise from 10 to 35% of aluminosilicate, in particular 14 to 35% and in particular 14 to 19% of aluminosilicate, by weight relative to the total weight of the material.
[0026] These quantities can also be expressed in phr (for "parts per hundred of rubber") corresponding, in French, to pce (parts per hundred of elastomer), the material containing from 25 to 75 phr of aluminosilicate, advantageously from 25 to 35 phr.
[0027] Kaolins particularly suitable for implementing the invention may in particular be chosen from kaolins originating from 3 quarries:
[0028] -Imerys Quarry / La Gare / CLERAC (17),
[0029] -Kaolin Quarry 3 Meudon QUESSOY (22),
[0030] -Cementori de la Gomal / L'Arboç TARRAGONA (Spain)
[0031] According to certain embodiments of the invention, the reinforcing fillers are made entirely of aluminosilicate.
[0032] According to other embodiments, the reinforcing fillers of the material comprise other constituents, and in particular they may comprise carbon black.
[0033] The aluminosilicate may constitute from 40 to 100% by weight of the reinforcing fillers, in particular from 45 to 70% of the reinforcing fillers.
[0034] According to one embodiment, the additive present in the material further comprises at least one agent chosen from plasticizers, UV protection agents, antioxidants and vulcanization agents.
[0035] In particular, the additive comprises at least one plasticizer. A plasticizer is a component making the material more flexible and / or easier to use for the manufacture of a wiping blade (made of elastomeric material). Generally speaking, plasticizers are often compositions comprising fatty acids, in particular mineral or vegetable oils.
[0036] In particular, a bio-sourced plasticizer will be used, preferably a bio-sourced oil.
[0037] The bio-sourced oil may be chosen from vegetable oils and / or fats but also from animal oils and / or fats, or a mixture of these.
[0038] The vegetable oil and / or fat is in particular chosen from sunflower oil, olive oil, rapeseed oil, linseed oil, coconut oil, castor oil, soybean oil and mixtures thereof. The bio-sourced plasticizing agent may in particular be sunflower oil.
[0039] The elastomer contains ethylene-propylene-diene monomer (EPDM), the EPDM being at least partly bio-sourced. The EPDM may thus comprise up to 70% bio-sourced ethylene, preferably between 40 and 60%.
[0040] For the purposes of the present invention, the term “bio-sourced” designates a product which is not of fossil origin but is obtained from renewable resources. Where appropriate, it also designates a biological process. “Of fossil origin” means: any product derived from petroleum or coal or petroleum or coal derivatives, including traditional fuel products derived from petrochemicals.
[0041] Bio-sourced ethylene can for example be produced from ethanol obtained from at least one plant material, the plant material being chosen in particular from sugar cane, beet, a woody plant or a mixture of these.
[0042] Such mixtures of natural rubber and EPDM are described in application EP3546302.
[0043] In particular, an elastomer consisting of a mixture of natural rubber and EPDM produced half from ethanol from sugar cane cultivation will be used.
[0044] Advantageously, the material comprises:
[0045] between 30 and 45% by weight of natural rubber, preferably between 35 and 40% by weight,
[0046] between 10 and 20% by weight of at least partly bio-sourced EPDM, preferably between 15 and 20% by weight,
[0047] between 35 and 55% by weight of reinforcing filler, preferably between 40 and 45% by weight, and
[0048] between 1 and 10% by weight of plasticizer, preferably between 2 and 5% by weight.
[0049] The wiping blade material may contain more than 50% and up to 85% recycled and / or bio-sourced material.
[0050] The composition may further contain one or more treatment promoters, including chemical base lubricants such as steric acid.
[0051] Materials according to the invention have properties of elasticity and tensile strength thanks to the presence of aluminosilicate, in particular raw kaolin in the form of particles as defined above, which make them suitable for use in the manufacture of wiper blades for windscreen wipers.
[0052] The choice of aluminosilicate particles, in particular raw kaolin, meeting the criteria described above makes it possible both to give the material a good level of reinforcement and to obtain a mixture of good homogeneity in terms of dispersion of the filler; the mixture adapts well to the process of preparing the wiping blade, in particular to the slitting process. The wiping blades made of material according to the invention ensure good wiping quality.
[0053] The use of aluminosilicate particles can be used in the manufacture of wiper blades for windshield wipers, wherein the manufacturing process comprises a peroxide-based vulcanization step of the elastomer mixture of the material.
[0054] Preferably, the material of the wiping blade does not contain sulfur. Preferably, the material of the wiping blade also does not contain zinc oxide.
[0055] The wiper blades for windscreen wipers having the characteristics and composition according to the present invention can in particular be obtained by extrusion of the material described in the present application.
[0056] According to another embodiment, the wiper blade is obtained by molding the containing material described above. Brief description of the figures
[0057] The invention will be better understood on reading the following description given solely by way of example and with reference to the appended drawings in which:
[0058] [Fig-1] represents a wiping blade of a windscreen wiper blade according to the invention
[0059] [Fig.2] shows the stress / strain curves of parts prepared from a material containing no filler, containing carbon black, containing raw kaolin and containing calcined kaolin.
[0060] [Fig.3a] represents the specific surface area / elongation modulus curve at 50%.
[0061] [Fig.3b] represents the specific surface area / elongation modulus curve at 25%.
[0062] According to [Fig.l], the wiping blade 1 of a windscreen wiper blade according to the invention has an elongated shape and is intended to be carried by a body of the blade (not shown). The blade 1 comprises a lip 3 and a heel 5 which are connected by a hinge 7. The lip 3, heel 5, hinge 7 assembly forms a basic body of the blade 1.
[0063] The heel 5 allows the blade 1 to be hooked into the body of the wiper. The lip 3 is intended to be in contact with the outer surface of a window such as a windshield for wiping purposes.
[0064] The hinge 7 is formed by a thin strip of material which gives the blade a certain flexibility and allows it to tilt when the direction of movement of the blade changes, in other words a forward and backward tilting movement of the lip.
[0065] The blade 1 is obtained by a conventional manufacturing process known to those skilled in the art.
[0066] Advantageously, at least a portion of the blade 1 comprises the material as described above, in particular the basic body of the blade comprises this material. It is thus possible to envisage embodiments in which, for example:
[0067] - only lip 3 comprises the material,
[0068] - only heel 5 includes the material,
[0069] - the entire blade 1 comprises the material.
[0070] If necessary, all or part of the surface of the blade 1 can also be treated so as to modify it, for example by graphitization, plasma treatment, halo generation, ion implantation and / or coating deposition. Such treatment makes it possible to strengthen the mechanical, wiping and / or wear resistance properties of the blade.
[0071] The wiping blade 1 may thus comprise a single-layer or multi-layer coating. The coating covers the base body of the blade 1.
[0072] Example 1: preparation of a composition
[0073] An example of a formulation of material used for the manufacture of a wiping blade in accordance with the invention is given here for illustrative purposes. The quantities are indicated as a percentage by weight.
[0074] natural rubber (NR) 44%
[0075] EPDM made partly from cane sugar 11%
[0076] carbon black 19%
[0077] raw kaolin 14%
[0078] rapeseed oil 4.4%
[0079] Wingstay L antioxidant 0.4%
[0080] Calcium Oxide 2.8%
[0081] treatment promoter 1.1%
[0082] In a 2nd step we mix with
[0083] Luperox 101XL45-sp2 3.3%
[0084] Total phr 178.7 including 25 phr of raw kaolin
[0085] The units can also be expressed in phr (for parts per hundred of rubber) corresponding, in French, to pce (parts per hundred of elastomer).
[0086] Carbon black is the product Spheron 5000A
[0087] Luperox 101XL45-sp2 is a DPBH peroxide: dibutyl peroxide hexane
[0088] The treatment promoter / anti-dispersant agent is a mixture of fatty alcohol, fatty acid and fatty acid ester, such as Aflux® 42 marketed by the company Lanxess.
[0089] The antioxidant used in this example is 2,2,4-Trimethyl-1,2-dihydroquinoline
[0090] Renewable material (%) NR+ U2 EPDM + oil 56
[0091] Product of natural origin (%) 16
[0092] Non-petrochemical material (%) 72
[0093] The Mooney viscosity ML(l+4)100°C of the material measured according to ISO289 is 43 units
[0094] The roasting time (Scorch t5) at 130°C is 23.7 minutes
[0095] The vulcanization kinetics were measured according to the ISO3417 RPA Vulca standard nization Def. 0.5° / Freq. 100 cpm - 210°C / 10' - T0+1 day
[0096] ts2 (min) 0.29
[0097] t90 (min) 0.69
[0098] Vulcanization takes 1'18” at 210°C
[0099] Tests were also carried out to test the properties of this material, in particular the mechanical properties.
[0100] Tensile strength measurements or tensile test were carried out according to ISO 37 at 500 mm / min. The results are summarized below
[0101] Shore A (pts) 65
[0102] Tensile test - 500 mm / min
[0103] Initial tensile properties
[0104] Modulus 50% (MPa) 2.2
[0105] Modulus 100% (MPa) 4.7
[0106] Breaking strength (MPa) 11
[0107] Elongation at break (%) 200
[0108] The elongation of the material subjected to 50% elongation after 22 hours at 70°C or 85°C (50% elongation set in English) was measured according to ISO 2285.
[0109] 50% Elongation Set 72h at 85°C (%) 18.2
[0110] 50% Elongation Set 72h at 70°C (%) 12 Example 2
[0111] To evaluate the performance of using raw kaolin as a reinforcing filler, 3 rubber mixtures were made with the same formulation, but varying only the type of filler: raw kaolin, calcined kaolin, and carbon black control.
[0112] The charges used for the study are as follows:
[0113] Raw kaolin - Argirec B24 Imerys - 22 m2 / g
[0114] Calcined Kaolin - Metasial V800 - 6 m2 / g
[0115] Carbon Black BC1031 (Birla) - 41 m2 / g
[0116] The formulas are shown in Table 1 below.
[0117] [Tableauxl] phr % Mix 1 Mix 2 Mix 3 60.8 Natural Rubber 100 100 100 Raw Kaolin 50 - - 30.4 Calcined Kaolin - 50 - Carbon Black N550 - - 50 Antioxidant 1.5 1.5 1.5 0.9 Antiozonant 1 2 2 2 1.2 Antiozonant 2 2 2 2 1.2 ZnO 4 4 4 2.4 Stearic Acid 0.8 0.8 0.8 0.5 Sulfur 0.75 0.75 0.75 0.5 Thiuram Accelerator 1.5 1.5 1.5 0.9 MBTS Accelerator 2 2 2 1.2
[0118] The mixtures are vulcanized according to industrial cycle time conditions 47170°C
[0119] Tensile strength measurements or tensile test were carried out according to ISO 37 at 500 mm / min. The results are summarized in the table below
[0120] [Tables2] Mix 1 Mix 2 Mix 3 Modulus 10% (MPa) 0.36 0.28 0.47 Modulus 25% (MPa) 0.69 0.56 0.89 Modulus 50% (MPa) 1.12 0.92 1.47
[0121] The traction / elongation curves are shown in [Fig.2] and compared with that of an unfilled mixture.
[0122] These results clearly highlight the interest of the raw kaolin filler, which has a reinforcing power superior to that of calcined kaolin. Example 3
[0123] The relationship between specific surface area and modulus has been studied.
[0124] By reporting the values of the 50% module obtained and the specific surface values specific characteristics of each of the 3 fillers used, we clearly see that the more the specific surface increases, the higher the modulus, and therefore the stronger the reinforcing power.
[0125] We obtain a quasi-linear relationship with a good correlation coefficient of 0.9887 very close to 1.
[0126] [Tables3] Module 50 (%) 1.12 0.92 1.47 Specific surface area (m2 / g) 22 6 Calcined kaolin 41 Black N550 Raw kaolin
[0127] Figure number 3 represents the corresponding graph
[0128] The correlation coefficient is even better for the values of modulus 25 and modulus 10%, respectively 0.9948 and 0.9983
[0129] These levels of elongation are close to those corresponding to the deformations encountered by the windshield wiper blade during use.
Claims
Claims
1. Wiper blade for a windscreen wiper, at least a portion of said blade comprising a material based on (i) an elastomer containing natural rubber and ethylene-propylene-diene monomer (EPDM), vulcanized with peroxide and (ii) at least one additive, characterized in that the additive is an aluminosilicate having a specific surface area of 20 to 40m2 / g, and in particular a lamellar structure.
2. Wiper blade for windscreen wiper according to claim 1, characterized in that the aluminosilicate is a kaolin.
3. Wiper blade for a windscreen wiper according to at least one of claims 1 or 2, characterized in that the material contains 14 to 35% aluminosilicate by weight relative to the total weight of the material.
4. Wiper blade for a windscreen wiper according to at least one of claims 1 to 3, characterized in that the aluminosilicate is in the form of particles with an average size of less than 9 μm.
5. Wiper blade for a windscreen wiper according to at least one of claims 1 to 4, characterized in that the aluminosilicate is a kaolin
6. raw. Wiper blade for windscreen wiper according to at least one of claims 1 to 5, characterized in that the EPDM contains up to 70% bio-sourced ethylene.
7. Wiper blade for windscreen wiper according to at least one of claims 1 to 6, characterized in that the additive further comprises at least one agent chosen from fillers, plasticizers, antioxidants and vulcanizing agents.
8. Wiper blade for a windscreen wiper according to at least one of claims 1 to 7, characterized in that the material contains at least one bio-sourced plasticizing agent.
9. Use of a lamellar aluminosilicate, with a specific surface area of 20 to 40 m2 / g, for the manufacture of a wiper blade for a windshield wiper, said wiper blade for a windshield wiper comprising an elastomer-based material containing natural rubber and ethylene-propylene-diene monomer (EPDM) and not containing sulfur.
10. Use of an aluminosilicate according to claim 9, characterized in that the manufacture of the wiper blade for a windscreen wiper includes a peroxide-based vulcanization step of the elastomer mixture.
11. Use of a lamellar aluminosilicate according to at least one of claims 9 or 10, characterized in that the lamellar aluminosilicate is a raw kaolin.