ILLUMINABLE LAMINATED VEHICLE GLAZING AND VEHICLES WITH SUCH GLAZING

The optical protection layer in vehicle glazing with LEDs addresses contamination issues by isolating the outer surface, using refractive index and thickness optimization to maintain light guidance efficiency and absorption, thus preserving light intensity and pattern integrity.

FR3141380B1Active Publication Date: 2024-10-18SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022011149
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-26
Publication Date
2024-10-18
Estimated Expiration
2042-10-26

AI Technical Summary

Technical Problem

Existing vehicle glazing with light-emitting diodes (LEDs) suffers from light output reduction due to contamination on the outer surface, leading to altered light patterns and reduced visibility, as grazing angles cause significant absorption of guided light by contaminants.

Method used

Incorporation of an optical protection layer with a specific refractive index and thickness to isolate the outer surface from contamination, utilizing angular filtering and evanescent waves to maintain light guidance efficiency, combined with tinted layers to absorb grazing rays and reduce contamination interaction.

Benefits of technology

The optical protection layer effectively prevents contamination-induced light absorption, preserving light intensity and pattern integrity by minimizing interaction with contaminants, ensuring consistent and efficient light output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000033_0000
    Figure 00000033_0000
  • Figure 00000033_0001
    Figure 00000033_0001
  • Figure 00000034_0000
    Figure 00000034_0000
Patent Text Reader

Abstract

The invention proposes an illuminable vehicle glazing comprising: - a partially tinted laminated glazing with a minimum refractive index n2 between first and second glass sheets n2>n0, n0 being the index of the second glass sheet - a light source (4) coupled to the second glass sheet, - means for extracting light - on the F4 face side an optical protection layer with a refractive index n1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: ILLUMINABLE LAMINATED GLAZING FOR A VEHICLE AND VEHICLE WITH SUCH GLAZING

[0001] The present invention relates to an illuminable laminated vehicle glazing, in particular a road vehicle glazing with light-emitting diodes.

[0002] Light-emitting diodes (LEDs) have been used for several years to light signaling devices (traffic lights, etc.), turn signals and position lights in motor vehicles. The advantage of diodes is their long lifespan, luminous efficiency, robustness, low energy consumption and compactness, making the devices using them more durable and requiring reduced maintenance.

[0003] More recently, light-emitting diodes have been used for automobile roofs, in particular panoramic laminated roofs with lighting by light-emitting diodes as described in document WO2010049638. The light emitted by the diodes is introduced through the edge into the interior glazing forming a guide, the light being extracted from the glazing by a transparent diffusing layer on the glazing, the surface of which defines the light pattern, such as a flat enamel containing dielectric diffusing particles.

[0004] It is possible to further improve the light rendering in the illuminated roof or more broadly in the illuminated glazing of a vehicle, in particular to improve the perception of the light pattern.

[0005] To this end, the present invention relates to an illuminable (or luminous) laminated glazing for a vehicle, in particular a road vehicle (car, truck, public transport: bus, coach, etc.) or a rail vehicle (train, metro, tram), preferably curved, preferably a roof or even side glazing, a windshield, or even a rear window, comprising:

[0006] - a first transparent sheet (curved), in mineral glass, possibly tinted (mass-colored), in particular gray or green, first glass sheet (transparent) comprising a first exterior main face called face F1, a second interior main face called face F2 (bare or coated with a functional coating - transparent - in particular of at most 200nm), typically with a refractive index nv of at least 1.5 and even at most 1.6 or 1.55, in the visible (at a reference wavelength in particular chosen from 550nm to 600nm, for example 550nm, which is preferably in the spectral range of the light source mounted or to be mounted)

[0007] - a second transparent (curved) sheet, preferably made of mineral glass or organic, in particular clear or preferably extra-clear glass, in particular with a thickness of at most 2.1 mm, with a third main face called face F3 and a fourth main face called face F4 (facing the interior of the vehicle), second sheet with a refractive index nO of at least 1.5 and possibly at most 1.6 or 1.55, in the visible, in particular at a reference wavelength chosen in particular from 550nm to 600nm, for example 550nm, which is preferably in the spectral range of the light source (mounted or to be mounted)

[0008] between the faces F2 and F3, one or more intermediate layers (for example at most 5, 4, 3, or 2 intermediate layers), dielectric, transparent, with given refractive indices in the visible (at the reference wavelength), comprising a polymer lamination interlayer, in particular the intermediate layer(s) are the interlayer layers,

[0009] the first sheet being tinted and / or among the intermediate layer(s) a first layer being tinted, in particular a first tinted interlayer,

[0010] when several intermediate layers, interlayers, are tinted, the first tinted layer is the tinted layer closest to the face F3,

[0011] n2 being the lowest refractive index in the visible range among the refractive indices of the intermediate layer(s) (in particular interlayer) between the face F3 and up to and including the first tinted layer or up to the face F2 in the absence of a tinted intermediate layer, with n2 <n0, notamment à la longueur d’onde de référence, et de préférence n2<n0 pour toute la gamme spectrale, et typiquement n2<nv (en particulier si deuxième feuille en verre minéral).

[0012] The glazing according to the invention further preferably comprises a light source (preferably polychromatic, with a wide spectral range of at least 100 nm, in particular white) in optical coupling with the second sheet forming a light guide. In particular, the light source (preferably diodes) is peripheral, preferably offset from the clear glass. The light source can be removable, added, sold separately from the glazing or as a kit. The light source can extend linearly (bar(s) of diodes).

[0013] The glazing according to the invention further comprises means for extracting (guided) light, light guided in the second sheet (light extraction means linked to the first sheet, in optical or even direct contact with the face F3 or the face F4 or in the second sheet).

[0014] The glazing according to the invention further preferably comprises a light source (preferably polychromatic) optically coupled with the second sheet forming a light guide, in particular a peripheral light source, preferably offset from the clear glass, preferably diodes). The light source can be removable, added, sold separately from the glazing or as a kit. The source can extend linearly.

[0015] The glazing further comprises light extraction means, light guided in the second sheet (light extraction means linked to the first sheet, in optical or even direct contact with the F3 face or the F4 face or in the second sheet).

[0016] In addition, the glazing on the F4 face, an optical protection layer, transparent, dielectric, and refractive index ni in the visible, with nl <n2, notamment à la longueur d’onde de référence, et même pour toute la gamme spectrale de la source (notamment source polychromatique, par exemple RGB ou lumière blanche) et d’épaisseur El d’au moins lOOnm ou même d’au moins 200nm et submillimétrique, et de préférence d’au plus lOOpm ou 50pm ou 5pm oulpm ou 500nm.

[0017] With the prior art roof architecture, any contamination of the F4 face is a cause of light extraction and is therefore very visible when the light is on. Indeed, the light bounces off the F4 face, where it can interact with fingerprints or dust.

[0018] According to the invention, the optical protection layer isolates the F4 face in the open air (tin face for example for float glass) from contamination which would come into contact with it. This optical protection layer makes it possible to make the light guide insensitive to surface contamination, without loss of light extraction efficiency.

[0019] The optical protection layer is effective, due to its transparency, its dielectric character, the choice of its refractive index n2 with a reasonable thickness El. Depending on the materials available and the integration of the optical protection layer, El is lowered more or less, and we get closer or closer to n2.

[0020] Its index n2 and its thickness El are in particular adjusted to allow only an evanescent wave at the angles of incidence of the guided mode (beyond the critical angle).

[0021] The optical protection layer is in particular in optical contact with the face F4, on a functional sub-layer (barrier, etc.), in particular mineral, for example of at most 120nm or 100nm for example with a refractive index greater than n2 (and ni) in the visible, in particular at the reference wavelength.

[0022] For simplicity, the optical protection layer (in particular a coating) can be in direct contact with the F4 face (deposition directly on the F4 face).

[0023] The optical protection layer (film or coating) may preferably have a light absorption of at most 3% even at 1% in the visible (at the reference wavelength or even over the entire visible).

[0024] The outer edge or slice of the optical protection layer may be offset from the clear glass, for example defined by a peripheral internal masking layer (forming a peripheral masking frame) between the face F2 and the face F3, in particular the optical protection layer extending under this internal masking layer over at most 10 cm or at most 3 cm.

[0025] For all the refractive indices according to the invention, a reference wavelength can be chosen which is 550nm and even according to the DIN 67507 standard. Preferably, the relationships between refractive indices nl<n2 et n0> n2 are true for the entire visible spectral range of the light source, for all the visible.

[0026] The Applicant has identified that the absorption of visible light by a contaminating layer is not negligible. However, the absorption of visible light at normal incidence remains low because the light passes through it perpendicularly. The interaction between the radiation and the contaminating layer occurs only over the thickness ef of the contaminating layer.

[0027] However, the situation is different for the light of the guided mode, with a contaminating layer directly on the F4 face of the light guide, the guided light being likely to interact with the contaminating layer. The rays of the guided mode are "grazing", propagating along an incidence 0 for example greater than approximately 78° in the configuration with a lower interlayer based on polyvinyl butyral (PVB) and a second sheet of mineral glass.

[0028] Thus, a significant portion of the guided light comes into contact with this contaminating layer at a grazing angle and is therefore likely to be absorbed.

[0029] A ray of the guided mode therefore crosses the contaminating layer over a distance corresponding to: ef / cos (0). The more grazing the angle, the lower cos (0), the more the rays of the guided mode interact with the contaminating layer over a great distance and therefore the greater the proportions of absorbed rays.

[0030] This is why it is possible to observe, depending on the light from the source injected into the guide, an alteration, a chromatic change, a reduction or even an erasure of the luminous zone resulting from the extraction as one moves away from the light injection point due to the high absorption in guided mode at the grazing angles of the contaminating layer.

[0031] To preserve the luminous zone, the inventors therefore chose the optical protection layer having a lower absorption and therefore a better preservation of the guided mode in the sense of its total intensity.

[0032] The optical protection layer is effective, due to its transparency, its dielectric character, the choice of its refractive index n2 with a reasonable thickness El. Depending on the materials available and the integration of the optical protection layer, El is lowered more or less, and we get closer or closer to n2.

[0033] Its index n2 and its thickness El are in particular adjusted to allow only an evanescent wave at the angles of incidence of the guided mode (beyond the critical angle).

[0034] The thickness of the tinted material helps limit heating in the passenger compartment. A tinted intermediate layer (interlayer or a tinted polymer film added, for example example first tinted layer, possibly single) preferably extends over almost the entire glazing, in particular over at least 80% or 90%. For the tinting of an intermediate layer (in particular interlayer or said polymer film) a molecular dye or inorganic pigment can be used.

[0035] A tinted intermediate layer (interlayer, upper and / or lower layer, said tinted film, for example first tinted layer, possibly single) may have a light transmission of at most 50% or 40% or 30% or 20% and even at least 5%. A different tint color may be chosen, identical to that of the first glass sheet. For example, the first tinted glass sheet is green, blue or gray and the first tinted layer, preferably interlayer, (for example PVB) is blue or gray. At least one other intermediate layer, preferably interlayer, clear (for example clear PVB) may be added closer to the face F2 than the first tinted layer or closer to the face F3.

[0036] The invention takes advantage of this thickness of tinted material. Indeed, if the most grazing rays are guided in the second sheet by total internal reflection with the interface with the intermediate layer (lower interlayer for example), other less grazing rays propagating in the glazing by refraction, reach the tinted material and are quickly absorbed after a few rebounds (refraction and reflection). They are therefore quickly absent on face F4, for example after less than 10 cm from the injection zone.

[0037] In particular, the first glass sheet and / or any tinted intermediate layer (PVB interlayer or non-adhesive such as polyethylene terephthalate PET) are sufficiently absorbent (taking into account their absorption coefficients and their thicknesses) so that on a rebound (refraction from face F3 to face F1, then reflection on face F1, refraction up to face F3, the light intensity is reduced by at least 50%. The light intensity can be measured by transmission spectroscopy. Typically the extinction coefficient k, the imaginary part of the complex refractive index for a glass called VG10 from the Applicant of 2 mm or for a tinted PVB of 0.76 mm with TL of 40% is of the order of 108 in the visible (in particular at the reference wavelength for example 550 nm and even over the spectral range of the source).

[0038] The tinted thickness thus creates an angular filtering which makes it possible not to have to manage the less grazing angles. In this zone close to the injection, the glazing can be masked (trimming) for example in favor of a peripheral masking layer as described later).

[0039] The single-layer or multi-layer lamination interlayer is in particular of a thickness of at most 2 cm or 1.2 cm or subcentimetric in particular of at least 0.3 mm, in particular all or part thermoplastic (tinted or not), with for example at least a lower part of the lamination interlayer (tinted or not) called the lower interlayer layer (for example a sheet), of a given thickness preferably of at least 100 pm, in adhesive contact with the face F3.

[0040] The glazing according to the invention is thus tinted (therefore absorbent in the visible, in particular in the spectral range of the light source) over a given thickness of, for example, at least 100 pm or 300 pm:

[0041] - the first sheet being tinted (over its entire thickness, colored in mass)

[0042] - and / or on all or part of the lamination interlayer, preferably thickness submillimeter tinted, for example an upper interlayer, between the F2 face and the lower interlayer, being tinted (mass-colored) and / or the lower interlayer being tinted

[0043] - and / or or a transparent tinted (mass-colored), polymeric (in particular non- adhesive to mineral and / or organic glass), for example with a thickness of at least 30 or 50 pm and better still at most 200 pm, being inserted between the F2 face and the lower interlayer, for example within the lamination interlayer, between the lower interlayer and an upper interlayer.

[0044] For example, it is a thermoplastic film (flexible, curved following the curvature of the glazing), which is: polyester, in particular polyethylene terephthalate (PET), poly(butylene terephthalate) PBT, poly(ethylene naphthalate) (PEN),, polyimide (PI), polyurethane (PU) or cellulose triacetate (TAC), acrylic, polyolefin in particular polypropylene (PP) polycarbonate (PC) or PMMA, (coextruded) film in PET-PMMA poly(vinyl chloride) PVC.

[0045] With a PC or PMMA polymer film, thermoplastic polyurethane (TPU) is preferred (for greater chemical compatibility) as the thermoplastic interlayer. The same applies if a second sheet of PC or PMMA organic glass is chosen, thermoplastic polyurethane (TPU) is preferred as the thermoplastic interlayer (especially the lower one).

[0046] The lamination interlayer (a top interlayer in particular) may have a main face FA in adhesive contact with the bare face F2 or with a functional coating on the face F2. The interlayer (the lower interlayer) may have a main face FB in adhesive contact with the bare face F3 (FB face of the lower interlayer).

[0047] Advantageously, the difference n2-nl is greater than 0.02 or even 0.05 and / or the difference n2-nl is preferably less than 0.3 and even 0.15 or 0.1 (for example at 550nm).

[0048] Unexpectedly, given the angular filtering, it is not necessary to lower ni to 1 or as close to 1 as possible, which would drastically restrict the choice of material. The index ni can be slightly lower than n2 (especially that of an interlayer) to isolate all the light that propagates in the second sheet.

[0049] If ni is too close to n2, the thickness El must be increased further, which can sometimes be detrimental to the mechanical strength, the optical protection layer (appearance of microcracks, etc.).

[0050] It may be desired to have a nI a little further from n2 and increase the thickness El, for example for an optical protection layer which is an organic coating by liquid means. In addition, for a porous layer, in particular silica, the degree of porosity required is then reduced.

[0051] Preferably, for example at 550nm, n1 is greater than or equal to 1.3 or even 1.35 or 1.4, (n2 is in particular at least 1.45 or 1.48) and nO is at least 1.5. El is preferably at least 250nm. In particular, at 550nm, n2=1.485 approximately (and even the lower interlayer is preferably based on PVB), and nO is at most 1.53.

[0052] To characterize the absorption by the contaminating layer of light in guided mode, it is not possible to experimentally determine parameters since the guided mode exists only in the second sheet.

[0053] Furthermore, the nature of the contaminating layer cannot be prejudged in advance; the pessimistic assumption is that the layer absorbs 100% of the light. With this system, the Applicant has determined a specific optical model enabling the reflection in guided mode to be evaluated by simulation, in particular the parameter in guided mode called Rgm, which is the total quantity of light reflected at each reflection on the layer interface. This reflection corresponds to a given angle of incidence (for example, 80° beyond the critical angle of 78° if the second sheet is mineral glass and the lower layer is PVB, according to the Snell-Descartes law, therefore with n0=1.52±0.01, n2=1.485+0.05 at 550nm). Strong absorption in guided mode results in limited values ​​of Rgm.

[0054] The inventors then determined an optical protection layer such that even in the presence of a layer absorbing 100% of the light behind it, it has a higher Rgm parameter, preferably at least 95% or even 97% or even 99%, denoting very low absorption and therefore better preservation of the guided mode in the sense of its total intensity.

[0055] Thus, El and ni are chosen such that the optical protection layer has a parameter Rgm which is the reflection in guided mode at the second sheet / optical protection layer interface of at least 95%, preferably at least 97% and even at least 99%.

[0056] In one embodiment, simulations of this system with a 100% absorbing layer were made and validated with n0=1.52, n2=1.485 at 550nm.

[0057] In particular for Rgm of 95%, the thickness El, in nm, is in a first delimited region of a graph of the thickness El as a function of ni, with a first lower limit included El defined by a first curve Cl of the thickness as a function of ni of the following equation:

[0058] Ela(nl)=bl-an*(nl-nri)-a3i*(nl-nri)3-a5i*(nl-nri)5

[0059] with nri=1.499; bl=122nm; an=30.lnm; a3i=-9.44*10 3nm; a5i=5.69*106nm

[0060] This curve has a vertical asymptote close to n2.

[0061] And preferably, in particular for Rgm of 97%, the thickness El, in nm, is in a second delimited region of said graph (more restricted than the first region), with a second lower limit included Elb, defined by a second curve C2 (above Cl) of the thickness as a function of the following equation:

[0062] Elb(nl)=b2-ai2*(nl-nr2)-a32*(nl-nr)3-a52*(nl-nr2)5

[0063] with nr2=l.495, b2=154nm, ai2=30.5nm, a32=-7.51*10 3nm; a52=3.05*106nm

[0064] And even more preferably, in particular for Rgm of 99%, the thickness El, in nm, is in a third delimited region of said graph (more restricted than the first or second region), with a third lower limit included Elc, defined by a third curve C3 (above Cl and C2) of the thickness as a function of the following equation:

[0065] Elc(nl)=b3-ai3*(nl-nr3)-a33*(nl-nr3)3-a53*(nl-nr3)5

[0066] With nr3=l,492, b3=211nm; an=34,4nm; a33=-6,43*10 3nm; a53=l,99*106nm.

[0067] And El is preferably at most 3pm or even at most 1.5pm.

[0068] If El of at most Ipm is preferred, it is necessary to have at least 1.466, 1.4685, 1.453 respectively. If El of at most 800nm ​​is preferred, it is necessary to have at least 1.461, 1.453, 1.438 respectively. If El of at most 600nm is preferred, it is necessary to have at least 1.442, 1.43, 1.40 respectively. If the thickness El can be at least 1.2 pm (self-supporting film, liquid coating) it is possible to have at least 1.472, 1.470, 1.461 respectively.

[0069] Beyond respectively 1.3pm, 1.6pm, 2.2pm ni is in the widest possible range as long as nl <n2.

[0070] The optical protection layer may comprise, or be, a so-called protective coating, preferably single-layer, on the F4 face (preferably in direct contact).

[0071] The minimum depends on the type of material and the deposition process.

[0072] For example, the thickness E1 is provided to be at least 300nm, 400nm, 500nm, 800nm ​​and preferably at most 5pm or 3pm or even at most 1.5pm.

[0073] The protective coating may be deposited on the second flat glass sheet before the toughening bending operation (and therefore must be toughenable). Otherwise the optical protective coating may be deposited (preferably by liquid means) on the second curved glass sheet, particularly if the protective coating is organic. Typically, the toughening bending operation is at a temperature of at least 600°C.

[0074] The protective coating can be deposited after lamination, in particular if the protective coating is adhesive with a supporting element, for example a tempered glass.

[0075] The protective coating may be mineral, and on the second glass sheet preferably mineral preferably silica-based coating (dense or preferably porous) in particular sol-gel with El at most 1.5 or 1.1 pm or Ipm. Preferably the second glass sheet is then mineral in the case of a sol-gel deposition involving elimination of pore-forming agent by heat treatment (for example during bending-tempering).

[0076] The protective coating preferably comprises (in particular consists of):

[0077] - sol-gel layer based on porous silica and El is at most Ipm, better still at most 800 nm and even 700 nm, to avoid the risk of cracks, nor can easily go up to 1.3

[0078] - or oxide-based layer (silica-based etc.) deposited by physical phase vapor (PVD) such as magnetron sputtering and El is at most Ipm better at most 700 nm and even 400 nm because the deposition is very slow,

[0079] - or a porous silica-based layer obtained from a SiOxCyHz layer deposited by a combination of plasma-assisted chemical process (PECVD) and magnetron sputtering, with El preferably at most 500nm, and after (bending)-quenching becoming (more) porous silica, for example a method of depositing such a layer described in patent application WO2012172266.

[0080] In magnetron sputtering the silica layer may contain one or more other elements such as aluminum and the refractive index may be 1.48.

[0081] The proportion of pore volume can be limited and controlled in particular by sol-gel method.

[0082] The protective coating may comprise (be made up of) a layer based on porous silica, in particular sol-gel, in particular ni is at most 1.44, optionally with a sub-layer of dense silica, in particular sol-gel, with a refractive index greater than ni (for example at least 0.02 or 0.05), of 1.45. This sub-layer preferably has a thickness of at least 5 nm, in particular at most 120 nm, for example between 50 nm or 80 nm and 120 nm.

[0083] The protective coating may comprise (be made up of) a porous silica-based layer, in particular sol-gel, with a porosity of less than 20% or 10% by volume, in particular ni is at least 1.4 or 1.42 or 1.44.

[0084] The structuring of the sol-gel layer into pores is linked to the sol-gel type synthesis technique, which makes it possible to condense the essentially mineral material (i.e. mineral or organic-mineral hybrid) with a suitably chosen pore-forming agent, in particular of well-defined size(s) and / or shape(s) (elongated, spherical, oval, etc.). The pores may preferably be empty or possibly filled.

[0085] We can thus choose silica made from tetraetoxysilane (TEOS),

[0086] We can adjust the refractive index according to the pore volume. We can use as a first approximation the following relationship for calculating the index ni:

[0087] nl=f.na+(lf).npores where f is the volume fraction of the material constituting the layer (here silica) and na is its refractive index (here silica) and npores is the pore index generally equal to 1 if they are empty.

[0088] The thickness of the optical protection layer can also be adjusted by choosing the appropriate solvent level.

[0089] The pores may be closed, done by removing a particulate pore-forming agent.

[0090] The smallest characteristic dimension of the pores, in particular closed pores (and preferably the largest dimension as well) may be greater than or equal to 30 nm and preferably less than 200 or 100 nm or even 80 nm, and less than EL. The porosity may also be monodisperse in size.

[0091] The optical protection layer, in particular a coating, preferably a single layer, may comprise (be made up of) an organic or organic-inorganic hybrid layer, in particular an acrylate, polymethacrylate (varnish, etc.) layer.

[0092] It is possibly in contact with a film, for example glass, with a thickness of at most 600 pm then bonded to the F4 face.

[0093] El is for example at most 50pm or 10pm or 5pm micronic or even at most 800nm ​​or 700nm. The upper and / or lower limit may depend on the deposition process.

[0094] It is preferred that the optical protection layer (the protective coating) be single-layer and on the F4 face, for simplicity.

[0095] As an organic-inorganic hybrid sol-gel layer, a layer based on methyltriethoxysilane (MTEOS), an organosilane with a non-reactive organic group, can be chosen. MTEOS is an organosilane which has three hydrolyzable groups and whose organic part is a methyl, non-reactive.

[0096] Even if an optical protection layer in the form of a coating on the F4 face is preferred (for its simplicity and compactness), other embodiments of the invention can be envisaged.

[0097] Alternatively, one can choose to stick a fluoropolymer (thermoplastic) optical protective film on the F4 face and bond it to a transparent film (polymer or preferably clear or extra-clear glass, in particular ultra-thin or 'UTG' of at most 600pm 300pm. The fluoropolymer film can be based on or even made of one of the following materials:

[0098] - perfluoroalkoxy PFA, in particular of about 1.3

[0099] - poly(vinylidene fluoride) PVDF, in particular of about 1.4% ni

[0100] - ethylene Chlorotrifluoroethylene ECTFE - ethylene tetrafluoroethylene ETFE, more precisely poly(ethylene-co-tetrafluoroethylene, in particular of about 1.4 - the perfluorinated ethylene propylene copolymer FEP or (Fluorinated Ethylene Propylene in English) in particular of ni of approximately 1.3 - polytetrafluoroethylene PTFE, in particular of about 1.3% ni, polyvinyl fluoride (Polyvinyl Fluoride or PVF).

[0101] In one configuration, the optical protection layer, preferably single-layer, may comprise an adhesive layer, made of crosslinked polymer material (film or coating) on ​​the face F4 (preferably in direct contact) and in contact with an internal main face Fi of a transparent film (polymer or preferably clear or extra-clear glass, in particular ultra-thin or 'UTG' of at most 600 pm or 300 pm). Glass is preferred for mechanical durability.

[0102] The optical protection layer is an optical glue (OCA for optically clear adhesive in English, LOCA if liquid).

[0103] For the manufacture of the optical protection layer, crosslinkable adhesives can be used which harden when their components react (photocrosslinkable in particular under ultraviolet, thermocrosslinkable etc.) or when a solvent evaporates. In all cases there is a chemical reaction in order to create chemical bonds for crosslinking, crosslinked polymer then defined by the formation of a 3D network of polymer chains linked by chemical bonds.

[0104] Thus the way in which the crosslinkable adhesive hardens depends on its nature, some (photo)crosslinking in particular by the supply of energy of the ultraviolet (UVA) or visible (400-405nm) type, others crosslinking at room temperature with the addition of a hardener by chemical reaction. Other crosslinkable adhesives are crosslinked by chemical reaction initiated and promoted by the supply of thermal energy.

[0105] Liquid deposition of the crosslinkable adhesive can be done by spray coating, curtain coating, flow coating, roller coating, slot die, dip coating, blade coating, screen printing, inkjet, drop casting, or filling a cavity with a syringe in particular.

[0106] Preferably, the optical protective layer may preferably be photo-crosslinked by ultraviolet, for example comprises a polymer matrix photo-crosslinked by ultraviolet.

[0107] In one configuration, the optical protection layer, preferably single-layer, comprises (is) in particular:

[0108] - an adhesive film preferably with a thickness of at least 30 pm (more ma- (pulpable, less risk of creases) and better at most 100pm or 50pm preferably pressure-sensitive film, preferably chosen from polymers based on acrylate, urethane acrylate or fluoro urethane acrylate or silicone

[0109] - or an adhesive coating preferably with a thickness of at least 800nm ​​or Ipm, or even at least 100m.

[0110] In one configuration, the optical protection layer is an adhesive film based on a crosslinked polymer, in particular of at least 30 μm, preferably a pressure-sensitive film, preferably chosen from polymers based on acrylate, urethane acrylate or fluoro urethane acrylate or silicone.

[0111] The crosslinked polymer material of the adhesive optical protection layer is for example chosen from polymers based on polyacrylate, in particular urethane acrylate or fluorourethane acrylate or fluorosilicone acrylate, polysiloxanes, silicone, in particular polydimethylsiloxane, epoxy polymer or polyepoxides, polyurethane, polyvinyl acetate, polyester. In particular, the crosslinked polymer material of the adhesive optical protection layer is preferably chosen from a polymer based on acrylate, in particular urethane acrylate or silicone acrylate or based on silicone, and the polymer further having a fluorinated function

[0112] The following may be mentioned as crosslinkable liquid (UV) adhesive for liquid deposition:

[0113] - urethane acrylate-based adhesive, for example from the company Norland, in particular product called LOCA Norland NOA 1315 (ni = 1.315) which is an aliphatic urethane acrylate,

[0114] - fluorourethane acrylate based adhesive, for example from the company Shin-A, in particular the product called SFA 335 (ni = 1.335-1.339) or SFA 387 (ni = 1.385-1.389),

[0115] - acrylate-based adhesive, for example in particular the product called UZ181A (nor = 1.47) from the company AKChemTeck, or the product called UVEKOL S15 (ni = 1.44) from the company Allnex.

[0116] Mention may be made of liquid adhesives based on fluorourethane acrylate, for example from the company Shin-A, in particular the product called LOCA Shin-A 335 (ni = 1.335-1.339) or 387 (ni = 1.385-1.389).

[0117] In particular, pressure-sensitive adhesive (PSA) film sticks by contact after applying mechanical pressure.

[0118] As a low PSA index film based on acrylate, we can cite the product called CS986 (ni = 1.47) from the company Nitto.

[0119] As a low PSA index film based on silicone, we can cite the product called Opt Alpha Gel from the company Taica (nl = 1.41).

[0120] Regarding the silicone, polydimethylsiloxane, PDMS or dimethicone, which is an organomineral polymer from the siloxane family, is preferred.

[0121] A pressure-sensitive adhesive, abbreviated PSA and commonly referred to as a self-adhesive, is an adhesive that forms a bond when pressure is applied to it so as to secure the adhesive to the surface to be bonded. No solvent, water, or heat is required to activate the adhesive.

[0122] As the name "pressure sensitive" suggests, the degree of bonding between a given surface and the self-adhesive binder is influenced by the amount of pressure used to apply the adhesive to the target surface and the nature and density of the physical bonds formed between the adhesive and the substrate (mineral or organic glass sheet).

[0123] PSAs are generally designed to form a bond and maintain it at room temperature.

[0124] PSAs can be made of rubber, polyurethane, acrylic ester polymer, polysiloxane.

[0125] PSAs are generally based on an elastomer coupled with a suitable additional adhesive agent or "tackifying" agent (e.g., an ester resin). The elastomers may preferably be based on:

[0126] - acrylates, which may be sufficiently tacky to not require a ta agent additional modifier.

[0127] - silicone, requiring special tackifying agents such as resins of silicate of type "MQ", composed of monofunctional trimethyl silane ("M") which has reacted with quadrifunctional silicon tetrachloride ("Q"), silicone-based PSAs are for example polydimethylsiloxane gums and resins dispersed in xylene or a mixture of xylene and toluene

[0128] or possibly:

[0129] - styrene-based block copolymers such as Styrene block copolymers butadiene-styrene (SBS), styrene-ethylene / butylene-styrene (SEBS), styrene-ethylene / propylene (SEP), styrene-isoprene-styrene (SIS),

[0130] - vinyl ethers.

[0131] - of nitriles.

[0132] PSA adhesives are marketed as rolls of double-sided adhesive with a liner on each side to protect the PSA film.

[0133] Silicone-based PSAs include Dow Corning® adhesives such as 2013 Adhesive, 7657 Adhesive, Q2-7735 Adhesive, Q2-7406 Adhesive, Q2-7566 Adhesive, 7355 Adhesive, 7358 Adhesive, 280A Adhesive, 282 Adhesive, 7651 Adhesive, 7652 Adhesive, 7356 Adhesive or Taica adhesives such as OPT alpha GEL® such as K120E, K90E or MRK adhesives such as MR3050, MR3080.

[0134] Examples of acrylate-based PSAs that may be mentioned are Nitto adhesives such as CS98210U, CS98210UK or Tesa® adhesives such as OCA 69206, OCA 69208, OCA 69405.

[0135] The glazing according to the invention, in particular the roof, may comprise between the face F2 and the face F3 an electrically controllable device with a stack (dielectric support) / electrode / active layer / electrode / (dielectric support) for example between two sheets of the lamination interlayer (PVB etc.). The following electrically controllable devices may be chosen:

[0136] - variable blur device: an optical valve device (SPD for suspended particle device in English) with liquid crystals, with a stack (dielectric support) / electrode / active layer / electrode / (dielectric support) for example between two sheets of the lamination interlayer (PVB etc.),

[0137] - variable tint device: an electrochromic device for example.

[0138] This device is, for example, entirely or partly opposite or offset from the guided light extraction means, and preferably between the face F2 and the first tinted layer (tinted upper interlayer for example).

[0139] Indeed, between the face F3 and the first tinted layer, it is preferable to avoid any metallic layer (electrode etc.) (pure or nitrided for example) or even transparent conductive oxide or even any layer with an extinction coefficient k, imaginary part of the complex refractive index, of at least 105 in the visible (in particular at the reference wavelength for example 550nm and even over the spectral range of the source).

[0140] The laminated glazing according to the invention may also comprise an infrared-reflecting or absorbing layer, on the F2 face or on a transparent polymer film (PET etc.) between two interlayers, in particular a so-called low-emissivity thin-layer stack comprising at least one metallic layer such as silver (and even 2 or 3 or 4), the or each silver layer being arranged between dielectric layers. In this configuration, the first tinted layer (preferably interlayer) is closer to the F3 face than this low-emissivity stack and the first glass sheet is clear and even any layer (interlayer etc.) between the F3 face and the low-emissivity stack.

[0141] More broadly, between the first tinted layer and the face F3, it is preferable to avoid any metallic layer (pure or nitrided for example) or even transparent conductive oxide, having an extinction coefficient k imaginary part of the complex refractive index, of at least 105 in the visible (in particular at the reference wavelength for example 550nm and even over the spectral range of the source),

[0142] The lamination interlayer may be single-layer or multi-layer (in particular multi-layer, two, three or four adhesive layers, in particular adhesive films or sheets. The interfaces between layers (sheet) are not necessarily discernible. The lamination interlayer may incorporate elements (not adhesive to the glass) such as functional polymer films or electro-optical elements, sensors, of various extents (all or part of the glazing). For example, two PVB sheets in a PVB / non-adhesive polymer film stack with the glass / PVB etc.

[0143] It is also preferable to choose a lamination interlayer that is as blurry as possible, i.e. at most 1.5% and even at most 1%.

[0144] Preferably, the lamination interlayer comprises one or more polymer sheets (lower interlayer layer, upper interlayer layer, etc.).The polymers are chosen from polyvinyl butyral (PVB), polyurethanes (PU), polyureas, ethylene vinyl acetate (EVA), polyolefins (including polyethylene (PE), polypropylene (PP) or polyisobutylene (P-IB)), polyvinyl chloride and its derivatives (for example poly(vinyl dichloride) (PVDC)), styrenic polymers (for example polystyrene (PS), acrylostyrene butadiene (ABS), styrene acrylonitrile (SAN)), polyacrylics (including polyacrylonitrile (PAN) and poly(methyl methacrylate) (PMMA)), polyesters (including poly(ethylene terephthalate) (PET) and poly(butylene terephthalate) (PBT)), polyoxymethylene (POM), polyamides (PA), fluorinated polymers such as polychlorotrifluoroethylene (PCTFE), polycarbonates (PC), aromatic polysulfones including polysulfone (PSU), polyphenylene ether (PPE), epoxy (EP) alone or in a mixture and / or copolymer of several of them.

[0145] The lamination interlayer may be at least one sheet based on PVB or PU (flexible) or thermoplastic without plasticizer (ethylene / vinyl acetate copolymer (EVA), etc.), each sheet having for example a thickness between 0.2 mm and 1.1 mm, in particular 0.38 and 0.76 mm.

[0146] Preferably, any PVB-based interlayer (in sheet form) comprises from 70% to 75% PVB, 25 to 30% plasticizer and less than 1% adjuvants. There are also PVB sheets with little or no plasticizer such as the film "MOWITAL LP BF" from the company KURARAY. Also, the lamination interlayer may be or comprise a sheet based on poly(vinyl butyral) (PVB) containing less than 15% by weight of plasticizers, preferably less than 10% by weight and even better less than 5% by weight and in particular without plasticizer and in particular with a thickness of at most 0.15 mm, in particular from 25 to 100 pm, 40 to 70 pm and even 50 pm, for example the product Kuraray Mowital®.

[0147] The lamination interlayer may be acoustic, in particular comprising or consisting of an acoustic PVB (three-layer, four-layer, etc.). Thus, the lamination interlayer may comprise at least one so-called middle layer made of viscoelastic plastic material with vibro-acoustic damping properties, in particular based on polyvinyl butyral and plasticizer, and the interlayer, and further comprising two external layers made of standard PVB, the middle layer being between the two external layers. Mention may be made of the acoustic PVBs described in the patent applications WO2012 / 025685, WO2013 / 175101, in particular tinted as in WO2015079159.

[0148] The first glass sheet and the second (mineral) glass sheet may preferably be curved (by bending methods known to those skilled in the art). The curved glazing is generally curved in two directions.

[0149] The mineral glass sheet can be produced by the “float” process, which allows a perfectly flat and smooth sheet to be obtained, or by stretching or rolling processes.

[0150] The tin face of the second mineral glass sheet may be the F3 face or the F4 face. The tin face of the first glass sheet may be the F1 face or the F2 face.

[0151] Examples of glass include float glass of conventional soda-lime composition, possibly hardened or tempered thermally or chemically, an aluminum or sodium borosilicate or any other composition.

[0152] In one embodiment, the glazing comprises an internal, peripheral, opaque masking layer between the face F3 and the face F2, and even covering the periphery of the optical protection layer, in particular an internal masking layer in contact with the face F2 (coating on the face F2 or on an interlayer in contact with the face F2), in particular defining the clear of the window. And / or the glazing may comprise an internal, peripheral, opaque masking layer on the face F4, in particular congruent or of a width less than the width of the internal masking layer.

[0153] The opaque, internal peripheral masking layer is in particular an enamel (black etc.) on the face F2. It may be an opaque coating on a thermoplastic adhesive layer, in particular an upper interlayer, in particular PVB, for example an opaque coating based on PVB and with a coloring agent on a main face of a PVB layer facing face F2 or face F3.

[0154] The internal masking layer may be 2mm or 3mm (less than 1cm or 5mm) from the edge of the glazing or even up to the edge. The internal masking layer may be a strip framing the glazing (windshield, roof, etc.), particularly black. The entire periphery is opaque to hide bodywork elements or joints or to protect an adhesive for mounting on the vehicle. This internal masking layer may delimit the clear glass. It may be advantageous for the external edge of the optical protection layer to be masked by the internal masking layer and not to be in the clear glass.

[0155] The width of the internal masking layer along the sides of a motor vehicle roof is generally less than that at the front or even the rear.

[0156] In particular for an automobile roof:

[0157] - the width of the internal (and even inner) masking layer along the edges longitudinal can be at most 30cm, in particular 10 to 20cm,

[0158] - the width of the internal (and even inner) masking layer along the edge rear side may be at most 30cm, in particular at least 1 or 5cm, and along the front side edge at most 60cm, in particular at least 1 or 5cm.

[0159] The width of the inner masking layer is preferably greater than that of the inner masking layer.

[0160] The inner, peripheral masking layer may be on the F4 face, in particular facing the inner masking layer (and even of identical nature, for example, an enamel, in particular black, on a second mineral glass sheet). The inner masking layer may be 2 mm or 3 mm (less than 1 cm or 5 mm) from the edge of the glazing or even up to the edge. The inner masking layer, in particular black, may be a strip and even a frame.

[0161] The internal and / or interior masking layer may be an organic or mineral binder (fused glass frit) with an organic or inorganic coloring agent, in particular a molecular dye or inorganic pigment.

[0162] The internal and / or interior masking layer is preferably a continuous layer (flat with a solid edge or alternatively a gradient edge (set of patterns).

[0163] The thickness of the intermediate layer(s) between face F2 and face F3 is preferably at most 1.5 mm or 1.1 mm or 0.9 mm and in particular the thickness of the interlayer lamination layer(s) being at most 1.1 mm or 0.9 mm. The thickness between face F1 and face F4 is preferably at most 9 mm or 7 mm, in particular for a road vehicle.

[0164] The first sheet is preferably made of mineral glass, possibly tempered, in particular if intended to be the outer sheet and if the second sheet is made of organic glass. In particular for road glazing, the first (outer) sheet is preferably at most 2.5 mm thick, even at most 2.2 mm - in particular 1.9 mm, 1.8 mm, 1.6 mm and 1.4 mm - and even at least 0.7 mm thick.

[0165] The second sheet may have a thickness of at least 0.7 mm, possibly less than that of the first outer glass sheet, even at most 2.2 mm - in particular 1.9 mm, 1.8 mm, 1.6 mm and 1.4 mm - or even at most 1.3 mm or at most 1 mm.

[0166] The total thickness of the first and second glass sheets is preferably strictly less than 5 or 4 mm, even 3.7 mm.

[0167] The first and second sheets of glass may be of substantially identical size, for example generally rectangular shape. The first sheet (if external) may have a larger size than the second sheet (if internal), thus exceeding this second sheet over at least part of its periphery, possibly a smaller second sheet (passenger compartment side) with a recessed edge, in particular of at most 10 or 5 cm from the edge of the first sheet of glass, on a edge or several edges (longitudinal and / or lateral) in particular or all around.

[0168] The first sheet may be a clear glass with an athermal or even heating functional coating on the F2 face.

[0169] The first mineral glass sheet may be based on silica, soda-lime, preferably silicosodo-lime, or even aluminosilicate, or even borosilicate. It may have a weight content of total iron oxide (expressed in the form Fe2O3) of at least 0.4% and preferably at most 1.5%.

[0170] The second mineral glass sheet may in particular be based on silica, soda-lime, silico-sodo-lime, or aluminosilicate, or borosilicate. To limit absorption, it has a weight content of total iron oxide (expressed in the form Fe2O3) of at most 0.05% (500 ppm), preferably at most 0.03% (300 ppm) and at most 0.015% (150 ppm) and in particular greater than or equal to 0.005%. The redox of the second glass sheet is preferably greater than or equal to 0.15.

[0171] In this text, the light transmission is calculated from the transmission spectrum between 380 and 780 nm taking into account illuminant A and the CIE 1964 reference observer (10°).

[0172] The light transmission and tint of each of the glass sheets are adjusted by the chemical composition of the glass and the thickness of the glass sheet. The chemical composition of the glass comprises a colorless base, preferably soda-lime-silica (but other glasses may be used, in particular borosilicate or aluminosilicate glasses), as well as a coloring part. The coloring part comprises in particular one or more colorants chosen from transition metal oxides - in particular iron oxides (ferrous and ferric), cobalt oxide, chromium oxide, nickel oxide, rare earth oxides, in particular erbium oxide, and selenium.

[0173] The first tinted glass sheet is a glass sheet having, for example, a light transmission of between 50 and 80%, in particular between 60 and 75%. It comprises a coloring part, for example consisting of iron oxides, in a total content of between 0.4 and 1.2% by weight, in particular between 0.6 and 1.1% by weight. The glasses obtained are then green, possibly yellowish or blueish-green depending on the proportion of ferrous iron. According to other examples, cobalt oxide, selenium and / or erbium oxide are added in order to impart a tint, for example blue or gray.

[0174] Better still, the first tinted glass sheet is a glass sheet having, for example, a light transmission of between 5 and 50%, in particular between 8 and 40% and even at most 20%. It comprises a coloring part, for example consisting of iron oxides, in a total content of between 1.0 and 2.3 by weight, in particular between 1.1 and 2.0% by weight, as well as cobalt and chromium oxides and / or selenium. The coloring part comprises, for example, the following colorants, in the weight contents defined below: Fe2O3 (total iron) from 1.2 to 2.3%, in particular from 1.5 to 2.2%, CoO from 50 to 400 ppm, in particular from 200 to 350 ppm, Se from 0 to 35 ppm, in particular from 10 to 30 ppm. The redox is preferably between 0.1 and 0.4, in particular between 0.2 and 0.3. Redox is understood to mean the weight ratio between the ferrous iron content (expressed as FeO) and the total iron content (expressed as Fe2O3). The glasses obtained are in particular green or gray.

[0175] The second sheet may be made of organic glass, in particular based on polyurethane (PU), polycarbonate (PC), poly(methyl methacrylate) (PMMA), poly(vinyl chloride) (PVC).

[0176] The second organic glass sheet may be flexible to follow the curvature of the first curved sheet or the second organic glass sheet may be preformed.

[0177] With organic glass such as PC or PMMA, thermoplastic polyurethane (TPU) or a crosslinked polymer material is preferred (for greater chemical compatibility) to PVB as the lower interlayer. Thermoplastic or thermoset EVA can also be chosen.

[0178] In the present invention, the expression tempered glass means thermally tempered glass in the absence of any precision, and preferably tempered glass during a glass bending operation.

[0179] The second glass sheet is a clear (or extra-clear) sheet having, for example, a light transmission of at least 85%, or even at least 90%. It generally does not include any coloring part except for unavoidable impurities, in particular iron oxides, in a total content of between 0.005 and 0.200% by weight, in particular between 0.010 and 0.150% by weight, or even between 0.030 and 0.120% by weight.

[0180] The second sheet of glass may (depending on the aesthetic rendering, the desired optical effect, the purpose of the glazing, etc.) be a clear glass (for example light transmission Tl greater than or equal to 90% for a thickness of 4 mm), for example a glass of standard soda-lime composition such as Planilux® from the company Saint-Gobain Glass, and even extra-clear (for example TL greater than or equal to 91.5% for a thickness of 4 mm), for example a soda-lime-silica glass with less than 0.05% of Fe III or Fe2O3 such as Diamant® glass from Saint-Gobain Glass, or Optiwhite® from Pilkington, or B270® from Schott, or another composition described in document WO04 / 025334.

[0181] The glass of the first sheet of glass may have undergone chemical or thermal treatment such as hardening, annealing or tempering (for better mechanical resistance in particular) or bending, and is generally obtained by the float process.

[0182] The luminous glazing may have a non-zero light transmission TL in all or part of the clear glass (generally framed by a masking layer). For glazing which is a roof, a non-zero light transmission TL is preferred, and even at least 0.5% or at least 2% and at most 10% and even at most 8%.

[0183] The second glass sheet may alternatively be made of organic glass (preferably rigid, semi-rigid) such as polymethyl methacrylate (PMMA) - preferably with lamination interlayer (PU) -, polycarbonate (PC) - preferably with lamination interlayer PVB -.

[0184] In particular, the following can be chosen as the first glass sheet / lamination interlayer / second glass sheet: - mineral glass / PVB (acoustic etc.) / mineral glass, - or mineral glass / lamination interlayer / polycarbonate,

[0185] For guidance, the second sheet of mineral glass is preferably clear and even extra-clear or made of clear and even extra-clear organic glass.

[0186] For thermal insulation, the first sheet of glass (or other layer) is tinted and preferably over-tinted.

[0187] It is preferred that the first tinted layer and the intermediate layer(s) under the first tinted layer have an extinction coefficient k, imaginary part of the complex refractive index of at most 106 or 107 in the visible (in particular at the reference wavelength for example 550nm and even over the spectral range of the source).

[0188] The (visible) light source is preferably:

[0189] - a set of light-emitting diodes (on a first circuit support printed like a PCB for “printed circuit board” in English), in particular a strip,

[0190] - or a light source which comprises a coupled extractor optical fiber with primary light source (light-emitting diode(s) etc.),

[0191] The diodes can be (pre)assembled on one or more PCB supports (PCB for Printed Circuit Board in English) or supports with electrical power supply tracks, the PCB supports being able to be fixed to other supports (profiles, etc.). The PCB support is generally thin, in particular with a thickness less than or equal to 3 mm, or even 1 mm, or even 0.1 mm or less if necessary than the thickness of a lamination interlayer. Several PCB supports can be provided, in particular if the areas to be illuminated are very distant from each other. The PCB support can be made of flexible, dielectric or electrically conductive material (metal such as aluminum etc.), be composite, plastic, etc.

[0192] Preferably, the light source is located on a part of the glazing located inside the vehicle trim, which has the essential function of hiding it from the eyes of the vehicle passengers as well as protecting it from dust and external aggressions.

[0193] The light source (diodes etc.) can be spaced from the second sheet of glass or glued for example to the edge.

[0194] We want to see the luminous zone inside the passenger compartment (case of a roof in particular or signaling, information for the driver or any other passenger).

[0195] The glazing may comprise several light sources, in particular light-emitting diodes. Naturally, it is possible to have several light sources (one or more series of diodes) coupled to the second sheet.

[0196] The injection of light from the light source in optical coupling with the second sheet, preferably a set of light-emitting diodes, is for example:

[0197] - by a slice of the second sheet of glass, possibly with a notch

[0198] - or by a wall delimiting a closed hole in the second sheet of glass, in particular a hole offset from a window clear, facing an internal masking layer,

[0199] - or by a light redirection element, local like an optical film re director, side face F3 or face F4, the light source then being opposite or offset from face F4, in particular direct optical coupling or via an optic, in particular light source and light redirection element offset by a window clear, facing an internal masking layer.

[0200] The extraction (diffusing) zone is for example at least 0.5mm wide, or less 1mm, or even at least 1cm, and even at least 5cm (width naturally to be distinguished from thickness), solid zone and / or comprising a set of discontinuous patterns (discrete, punctate (3D), for example geometric, linear (2D) in particular distinct or identical for example spaced at least 0.5mm apart), the diffusing zone being able to occupy a surface area of ​​length preferably greater than 5cm and even 10cm.

[0201] The diffusing zone can occupy at least 60%, 70%, 80%, 90% of the main face of the glazing, preferably being spaced from the optical coupling by at least 20mm.

[0202] The luminous glazing may comprise a plurality of diffusing zones of identical or distinct size and / or shape. The extraction zone may therefore cover part or all of the laminated glazing depending on the lighting or the desired effect (in the form of strips arranged on the periphery of one of the faces to form a luminous frame, logos or patterns, etc.).

[0203] The diffusing zone can be in several zones, for example each with patterns, identical or distinct, continuous or discontinuous, and can be of any geometric shape (rectangular, square, triangular, circular, oval, etc.), and can form a design, a sign (arrow, letter, etc.).

[0204] The luminous glazing may comprise several light extraction zones (diffusing layers) to form several luminous zones on the glazing.

[0205] For example, the light extraction means comprise:

[0206] - a texturing of the second sheet, face F3 or face F4 and even in contact with the overlying optical protection layer

[0207] - or an extractor film on the second sheet, face F3 or face F4 and in contact with the overlying optical protection layer

[0208] - or a diffusing layer comprising a binder and diffusing particles and / or pores, on the second sheet, face F3 or face F4 and in contact with the overlying optical protection layer

[0209] - or a local diffusing zone in the second sheet, comprising particles diffusing and / or pores, or laser engraving.

[0210] In particular, the means for extracting the guided light comprise (or even consist of) a diffusing layer comprising diffusing elements in a matrix (organic or mineral, for example enamel) to form a diffusing zone (luminous in the on state).

[0211] The diffusing elements preferably comprise and even consist essentially of particles (dielectric, organic or mineral, for example metal oxides) dispersed and bound by the matrix, particles with a size of at most 30 pm or at most 10 pm. The particles are for example chosen from particles of TiO2, SiO2, CaCO3, ZnO, Al2O3, ZrO2.

[0212] The diffusing layer may be on the main face FB of the lamination interlayer directly. The other main face of the lamination interlayer (in adhesive contact with a glass sheet) may be bare or coated, in particular at the periphery, with a masking layer (black ink, etc.).

[0213] The thickness of the diffusing layer can be at most 20 pm and even at most 10 pm and even at least 1 pm.

[0214] The diffusing layer is for example a transparent coating, the matrix being organic and transparent. The transparent matrix, in particular deposited by liquid means, may be made of a material chosen from a polymeric binder such as a paint, in particular a lacquer, or a resin. In particular, the transparent matrix may consist essentially of resin, in particular PVB resin. In particular, the transparent coating may comprise and even consist essentially of resin, in particular PVB resin, and diffusing elements, in particular diffusing particles, in particular of at least 50 nm, 80 nm or 100 nm and preferably of at most 30 pm or 10 pm or 1 pm. The transparent diffusing coating may consist essentially of the resin and said diffusing elements (particles and / or pores, etc.), in particular particles. The resin may be chemically compatible with the interlayer of lamination which is for example a PVB. The resin can be a PVB resin with the lamination interlayer which is a PVB.

[0215] The glazing is preferably a roof, which can be opening or fixed.

[0216] The invention also relates to a road vehicle incorporating the glazing defined above.

[0217] In the present application, the term “road vehicle” means a car, in particular a utility vehicle (van, minivan, relay) weighing less than 3.5 tonnes (light utility vehicle) or a truck or a shuttle, a small public or private transport vehicle. The side windows may be in sliding doors. The luminous glazing may be in a rear door.

[0218] The present invention will be better understood and other details and advantageous characteristics of the invention will appear on reading the examples of luminous vehicle glazing according to the invention illustrated.

[0219] [Fig-1] - [Fig.l] represents a schematic sectional view of a laminated roof motor vehicle light according to the invention in a first embodiment

[0220] [Fig.l'] - [Fig.l]' represents a schematic front view of the roof of [Fig.l]

[0221] [Fig.l”] - [Fig.l]” shows a graph with three curves Cl, C2, C3 indicating the minimum thickness Elmin as a function of ni

[0222] [Fig.2] - [Fig.2] represents a schematic sectional view of a luminous laminated glazing of a motor vehicle in a second embodiment by injection of peripheral light

[0223] [Fig.2'] - [Fig.2]' represents a schematic sectional view of a luminous laminated glazing of a motor vehicle which is a roof mounted in a vehicle

[0224] [Fig.3] - [Fig.3] represents a schematic sectional view of a luminous laminated glazing of a motor vehicle in a third embodiment by injection of peripheral light

[0225] [Fig.4] - [Fig.4] represents a schematic sectional view of a luminous laminated glazing of a motor vehicle in a fourth embodiment by injection of peripheral light

[0226] [Fig.4'] - [Fig.4]' represents a schematic front view of the glazing of [Fig.4]

[0227] [Fig.5] - [Fig.5] represents a schematic sectional view of a luminous laminated glazing of a motor vehicle in a fifth embodiment by injection of light via an internal glass wall

[0228] [Fig.5'] - [Fig.5]' represents a schematic front view of the glazing of [Fig.5].

[0229] [Fig.6] - [Fig.6] represents a schematic sectional view of a luminous laminated glazing of a motor vehicle in a sixth embodiment by injection of light passing through a glass

[0230] [Fig.6'] - [Fig.6]' represents a schematic front view of the glazing of [Fig.6].

[0231] It is specified that for the sake of clarity the different elements of the objects represented do not are not necessarily reproduced to scale

[0232] [Fig.l] represents a schematic sectional view here, side view, of a luminous laminated vehicle roof 100 according to the invention in a first embodiment by peripheral lighting. [Fig.l]' represents a schematic front view of the roof of [Fig.l].

[0233] This is a laminated car roof, 100 rectangular and curved, which comprises:

[0234] - a first sheet of glass 1, for example rectangular (of dimensions 300X300 mm for example), with a tinted composition (Venus VG10 or TSA 4+ glass marketed by the company Saint-Gobain Glass) for example with a thickness equal to 2.1 mm, with a first main face 11 corresponding to the face Fl, a second main face 12 on the inner side called F2 and an edge (longitudinal edges 10 and 10'), the face F2 being possibly coated with an athermal silver coating 16' or even heating, etc.,

[0235] - a second sheet of glass, preferably mineral, 2, of the same dimensions as the first sheet 1, forming internal glazing, passenger compartment side, made of mineral glass, having a third main face 11 corresponding to face F3 and a fourth main face 12 which is face F4, and an edge (longitudinal slices 21 and 22 - for example a sheet of sodium-calcium silico glass, extra-clear such as Diamant glass marketed by the company Saint-Gobain Glass, of thickness equal for example to 2.1 mm, glass with a refractive index nO of the order of 1.52 at 550 nm or Optiwhite glass of 1.95 mm,

[0236] - between the face F2 and the face F3 an intermediate layer comprising at least one interlayer of lamination 3, with a slice 30 here longitudinal possibly offset from the longitudinal slices 10, 10' towards the center of the glass (therefore set back), here a single layer (a single sheet) 31 of clear or tinted PVB of 0.76mm in adhesive contact with the athermal coating 16' (or with the face F2 in its absence) and in adhesive contact with the face F3 and of refractive index n2 in the visible with n2 <n0.

[0237] The second face F2 comprises an internal masking layer 7 forming a masking frame, for example a black enamel, delimiting a window clear 16 (daylight) here rectangular (see [Fig.l]').

[0238] Light-emitting diodes 4 extend along the longitudinal coupling edge 21 of the second glass sheet 2. These are front-emitting diodes. Thus, these diodes 4 are aligned on a PCB support 5, for example a parallelepiped strip. The PCB support 5 is fixed, for example, by glue 7 (or double-sided adhesive) on the edge of the face.

[0239] Alternatively, the light source may be one or more primary sources (diodes, etc.) coupled directly to a guide, along the coupling edge, for example an extractor optical fiber with a light exit zone.

[0240] The luminous glazing 100 may have a plurality of extraction zones 6 for the light guided in the second sheet, in particular of given geometry (rectangular, square, round, etc.). For example, it is a diffusing layer 6 (enamel, ink, screen printing, etc.) which is a coating on the third face F3 and even alternatively or cumulatively on the fourth face F4, a diffusing layer preferably in the clear glass 16. Alternatively, it may be a local extractor film placed or glued locally on the third face F3 or even the fourth face F4 (in relief or with a diffusing layer or diffusing in mass).

[0241] For example, the distance between the extraction 6 and the diodes is at least 10 or 40 mm. For example, the extraction occupies from 10 to 100% of the glass clear,

[0242] Several series of diodes 4 (one edge, two edges, three edges, over the entire periphery) can be provided, controlled independently and even of different colors. Diodes emitting white or colored light can be chosen for ambient lighting, reading lighting, etc. Red light can be chosen for signaling, possibly alternating with green light. The diode support 5 can be glued to the edge 21.

[0243] The light ray (after refraction on the edge 21) propagates by total internal reflection (at the level of the face F3 and the face F4) in the second sheet 1 forming a light guide.

[0244] According to the invention, the face F4 comprises an optical protection layer 151, with a refractive index of ni in the visible with ni < n2. This is a coating, the deposition is by any means (liquid, physical in vapor phase (magnetron etc.), chemical in vapor phase etc.) and of thickness EL

[0245] [Fig.l]” shows a graph with three curves Cl, C2, C3 indicating the minimum thickness El min as a function of ni.

[0246] For a contamination layer absorbing 100% of the light, the inventors then determined how to achieve with the optical protection layer a higher Rgm parameter, preferably at least 95% or even 97% or even 99% denoting very low absorption and therefore better preservation of the guided mode in the sense of its total intensity.

[0247] Thus, El and ni are chosen such that the optical protection layer has a parameter Rgm which is the reflection in guided mode at the second sheet / optical protection layer interface of at least 95%, preferably at least 97% and even at least 99%.

[0248] In one embodiment, simulations were carried out and validated with n0=1.52, n2= 1.485.

[0249] For Rgm of 95%, the thickness El, in nm, is in a first delimited region of a graph of the thickness El as a function of ni, with a first lower limit included Ela defined by a first curve Cl of the thickness as a function of ni of the following equation:

[0250] Ela(nl)=bl-an*(nl-nri)-a3i*(nl-nri)3-a5i*(nl-nri)5

[0251] with nri=1.499; bl=122nm; an=30.lnm; a3[=-9.44*10 3nm; a5i=5.69*106nm

[0252] And preferably, for Rgm of 97%, the thickness El in nm, is in a second bounded region of said graph (more restricted than the first region), with a second lower limit included Elb, defined by a second curve C2 (above Cl) of the thickness as a function of ni of the following equation

[0253] Elb(nl)=b2-ai2*(nl-nr2)-a32*(nl-nr)3-a52*(nl-nr2)5

[0254] with nr2=l.495, b2=154nm; ai2=30.5nm;a32=-7.51*10 3nm; a52=3.05*106nm

[0255] And even more preferably, for Rgm of 99%, the thickness El in nm, is in a third delimited region of said graph (more restricted than the first or second region), with a third lower limit included Elc, defined by a third curve C3 (above Cl and C2) of the thickness as a function of the following equation:

[0256] Elc(nl)=b3-ai3*(nl-nr3)-a33*(nl-nr3)3-a53*(nl-nr3)5

[0257] With nr3=l,492 b3=211nm; ai3=34,4nm; a33=-6,43*10 3nm; a53=l,99*106nm

[0258] And El is preferably at most 3pm or even at most 1.5pm.

[0259] If El of at most Ipm is preferred, it is necessary to be at least 1.466, 1.4685, 1.453 respectively. If El of at most 800nm ​​is preferred, it is necessary to be at least 1.461, 1.453, 1.438 respectively. If El of at most 600nm is preferred, it is necessary to be at least 1.442, 1.43, 1.40 respectively.

[0260] If the thickness can be at least 1.2 pm (self-supporting film, liquid coating) we can have at least 1.472, 1.470, 1.461.

[0261] Beyond respectively 1.3pm, 1.6pm, 2.2pm ni is in the widest possible range as long as nl <n2.

[0262] For example, if we want a very thin optical protection layer, we choose nl = 1.35 and El = 500nm.

[0263] For example, if we can produce a thicker optical protection layer, we choose ni very close to n2 (at most 1.46 approximately) and El = Ipm, for example a porous silica sol-gel layer with at most 10% by volume of pores.

[0264] Alternatively, an acrylate optical protection layer is chosen, for example with nl= 1.4 with El from 600nm or even 1 or 2 pm if this facilitates deposition. It is possible to choose to glue an ultra-thin clear glass for mechanical protection.

[0265] An adhesive layer can also be chosen as optical protection layer 151. in particular adhesive coating (LOCA) including UV crosslinked or PSA film, adhesive layer is then in contact with ultra thin clear glass.

[0266] Furthermore, as a variant, the second sheet is made of organic glass, in particular based on polyurethane (PU), polycarbonate (PC), poly(vinyl chloride) (PVC), poly(methyl methacrylate) (PMMA). With an organic glass such as PC or PMMA, thermoplastic polyurethane (TPU) or a thermoplastic or thermoset EVA is preferred (for greater chemical compatibility) to PVB as an interlayer. Ni and El are adjusted as a function of n2.

[0267] In all these examples the anti-dirt, fingerprint, dust function is fulfilled by the optical protection layer. Any dust or fingerprint will not interact with the light and will therefore not light up when the light source is turned on. Even if the optical protection layer is in contact with the air, it is not necessary for it to be very low, close to 1, which is of course more difficult to obtain.

[0268] This laminated luminous glazing 100 can alternatively form a front windshield with internal signaling. The diffusing layer forms, for example, an anti-collision signal, in particular forming a band along the lower longitudinal edge. For example, the light comes on (red) when a vehicle in front is too close.

[0269] This laminated luminous glazing 100 can alternately form a front or rear quarter panel. The diffusing layer 6 forms, for example, interior signage or a decorative pattern, etc.

[0270] [Fig.2] represents a schematic sectional view of a luminous laminated glazing of a motor vehicle 200 in a second embodiment by injection of peripheral light.

[0271] This second embodiment differs from the first embodiment firstly in that side-emitting diodes 4 are housed in a recess (peripheral notch) of the wafer 21. Thus these diodes 4 are aligned on a PCB support 5, for example a parallelepiped strip, preferably as opaque as possible (not transparent) and their emitting faces are parallel to the PCB support and opposite the wafer 21 in the recessed wafer part. The PCB support is fixed for example by glue 5' (or a double-sided adhesive) on the edge 121 of the face F2 12, and here is engaged in a groove between the faces F2 and F3 made possible by the sufficient withdrawal of the wafer 30 from the interlayer 3. The peripheral masking strip 7 in opaque enamel (black) can mask the PCB support 5 and even the outgoing light in this area.

[0272] The distance between the diodes and the wafer 10 is reduced as much as possible, for example from 1 to 2 mm. The space between each chip and the optically coupled wafer 10 can be protected from any pollution: water, chemical, etc., this in the long term as during the manufacture of the luminous glazing 100.

[0273] The luminous glazing 200 also has a polymeric encapsulation 8, for example made of black polyurethane, in particular PU-rim (in-mold reaction in English). It is double-sided at the edge of the glazing. This encapsulation ensures long-term sealing (water, cleaning product, etc.). The encapsulation also provides a good aesthetic finish and allows other elements or functions to be integrated (reinforcing inserts, etc.). As described in document WO2011092419 or document WO2013017790, the polymeric encapsulation may have a through-hole closed by a removable cover for placing or replacing the diodes.

[0274] The roof 200 can form, for example, a fixed luminous panoramic roof of a motor vehicle such as a car, mounted from the outside on the bodywork 8' via an adhesive 61' as shown in [Fig.2]'.

[0275] [Fig. 3] represents a schematic sectional view of a luminous laminated glazing 300 of a motor vehicle in a third embodiment by injection of peripheral light.

[0276] A peripheral inner masking layer 7' is on the fourth face F4 14 in particular of width less than the width of the inner masking layer 7. For example a black enamel or a black ink on an intermediate layer (PVB interlayer etc.).

[0277] Furthermore, the diode support 5 is L-shaped with a part facing the fourth face F4 14. For example, the second sheet 2 is smaller than the first sheet 1, so the diodes are under the protruding part of the second face 121. The diodes are side-emitting or front-emitting.

[0278] The optical protection layer 151 is adjacent to the inner masking layer 7' and optionally spaced or in contact with the inner masking layer 7'.

[0279] [Fig.4] represents a schematic sectional view of a luminous laminated glazing 400 of a motor vehicle in a fourth embodiment by injection of peripheral light. [Fig.4]' represents a schematic front view of the glazing of [Fig.4],

[0280] This embodiment differs from the first embodiment in that a second diode module 4', 5' is added along the opposite longitudinal edge 22.

[0281] [Fig.5] represents a schematic sectional view of a luminous laminated glazing unit of a motor vehicle 500 in a fifth embodiment by injection of light via an internal glass wall. [Fig.5]' represents a schematic front view of the glazing unit of [Fig.5].

[0282] This embodiment differs from the first mode 100 by the injection of light and the location of the light source 4.

[0283] Diodes 4 on a support 5 are in a through hole 18 (offset from the glass clear 16), of circular shape, of the second glass sheet 2 delimited by a wall internal 17 and closed by a cover 50 such as a metal sheet or any other optical shutter on the third face F3 13. The diode support 5 forms a cover glued by an adhesive 61 to the fourth face F4 14.

[0284] And as shown in [Fig.5]' the means have been doubled by adding other diodes 4 in another through hole 18 (offset from the window clear 16), of circular shape closed by another cover 50. The holes are here on the lateral front edge side of the roof 20.

[0285] The internal masking layer 7 is often wider at the front than at the rear edge 20'.

[0286] [Fig.6] represents a schematic sectional view of a luminous laminated glazing unit for a motor vehicle 600 in a sixth embodiment by injection of light passing through a glass. [Fig.6]' represents a schematic front view of the glazing unit of [Fig.6].

[0287] This embodiment differs from the first mode 100 by the injection of light and the location of the light source 4.

[0288] Diodes 4 (here with front emission) on a support 5 are opposite (or offset) the fourth main face 14 and the optical coupling with the second sheet 2 is done via a light redirection element for guidance, local such as an optical redirector film 9, reflector, on the third main face F3 side (or fourth main face F4) for example facing the internal masking layer 7.

[0289] For example, it is a polymer prismatic film with prisms 93 and a flat part 94 glued or fixed by suction to the third face F3 13 and with a thickness between 100 and 300 pm covered by the interlayer 31. The film forms a longitudinal strip like the linear type light source 4 along a longitudinal edge of the roof for example.

[0290] The means can therefore be doubled by adding another light source, another redirecting film along the other longitudinal edge 10'.

Claims

Claims

1. Laminated vehicle glazing (100 to 600) comprising: - a first sheet (1), transparent, made of mineral glass, with a first outer main face called face F1 (11) and a second inner main face called face F2 (12), - a second sheet (2), transparent, made of organic or mineral glass, with a third main face called face F3 (13) and a fourth main face called face F4 (14), second sheet with refractive index nO in the visible, - between face F2 and face F3, one or more intermediate, dielectric, transparent layers, with given refractive indices in the visible, comprising an interlayer of polymer lamination (3), the first sheet being tinted and / or among the intermediate layer(s) a first layer being tinted, when several intermediate layers are tinted, the first tinted layer is the tinted layer closest to face F3,n2 being the lowest refractive index among the refractive indices of the intermediate layers between the F3 face and up to and including the first tinted layer or up to the F2 face in the absence of a tinted intermediate layer, with n2 <n0 - de préférence une source de lumière en couplage optique avec la deuxième feuille formant un guide de lumière, - des moyens d’extraction de lumière guidée (6, 6’) dans la deuxième feuille, caractérisé en ce qu’il comporte sur la face F4 une couche de protection optique (151), transparente, diélectrique, et d’indice de réfraction ni dans le visible avec ni < n2 et d’épaisseur El d’au moins lOOnm et submillimétrique.,

2. Vehicle glazing according to the preceding claim, characterized in that the difference n2-nl is greater than 0.02 and preferably less than 0.

3.

3. Vehicle glazing according to one of the preceding claims, characterized in that n2-nl is less than 0.

15.

4. Vehicle glazing according to one of the preceding claims, characterized in that ni is greater than or equal to 1.3 or 1.4, and nO is at least 1.5 and El is at least 250nm.

5. Vehicle glazing according to one of the preceding claims ca- characterized in that the thickness El is in a first delimited region of a graph of the thickness El, in nm, as a function of ni, with a first lower limit included Ela defined by a first curve Cl of the thickness as a function of ni of the following equation: Ela(nl)=bl-an*(nl-nri)-a3i*(nl-nri)3-a5i*(nl-nri)5 with nri=l,499; bl=122nm; an=30,lnm; a3i=-9,44*10 3nm; a5i=5,69*10 6nm and preferably El is at most 3pm.

6. Vehicle glazing according to one of the preceding claims, characterized in that the optical protection layer comprises a so-called protective coating, preferably single-layer, on the F4 face.

7. Vehicle glazing according to claim 6 characterized in that the protective coating is mineral, and on the second sheet of mineral glass, preferably a protective coating based on silica, in particular sol-gel, with El at most 1.5 pm or even 1.1 pm.

8. Vehicle glazing according to one of claims 6 or 7 characterized in that the protective coating comprises a layer based on porous silica, in particular sol-gel, optionally with a dense silica sub-layer, in particular sol-gel.

9. Vehicle glazing according to one of claims 6 to 8, characterized in that the protective coating comprises a layer based on porous silica, in particular sol-gel, with a porosity of less than 20% or 10% by volume.

10. Vehicle glazing according to one of claims 1 to 7 characterized in that the optical protection layer comprises an organic or organic-mineral hybrid layer, in particular an acrylate or polymethacrylate layer.

11. Vehicle glazing according to one of claims 1 to 5 characterized in that the optical protection layer comprises an adhesive layer, made of crosslinked polymer material, on the face F4, in contact with an internal main face Fi of a transparent film, preferably a glass with a thickness of at most 600 pm.

12. Vehicle glazing according to the preceding claim, characterized in that the optical protection layer comprises an adhesive film preferably with a thickness of at least 30 pm and better still at most 100 pm, preferably a pressure-sensitive film, preferably chosen from polymers based on acrylate, urethane acrylate or fluoro urethane acrylate or silicone.

13. Vehicle glazing according to one of the preceding claims, characterized in that the light extraction means (6, 6') comprise: - a texturing of the second sheet, face F3 or face F4 and in contact with the overlying optical protection layer - or an extractor film on the second sheet, face F3 or face F4 and in contact with the overlying optical protection layer - or a diffusing layer comprising a binder and diffusing particles and / or pores, on the second sheet, face F3 or face F4 and even in contact with the overlying optical protection layer - or a local diffusing zone in the second sheet, comprising diffusing particles and / or pores, or laser engraving.

14. Vehicle glazing according to one of the preceding claims, characterized in that the glazing is a roof, the second sheet of glass is made of extra-clear mineral glass.

15. Vehicle, in particular a road vehicle, incorporating at least one glazing unit according to one of the preceding claims.