METHOD FOR MANUFACTURED FLOAT GLASS FROM A MIXTURE OF MINERAL MATERIALS INCLUDING A CALCIUM SILICATE

By using calcium silicate with a fine particle size in the glass manufacturing process, the challenge of achieving homogeneous glass composition and reducing energy consumption is addressed, resulting in improved glass quality and reduced energy costs.

FR3141458B1Active Publication Date: 2024-10-18SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022011322
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-10-18
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Existing glass manufacturing processes face challenges in achieving homogeneous glass composition while minimizing energy consumption and CO2 emissions, primarily due to the use of conventional limestone with large particle sizes that affect heat transfer and glass quality.

Method used

Incorporating calcium silicate with a median grain diameter of less than 400 micrometers into the glass manufacturing process, along with other raw materials, to enhance calcium oxide distribution and reduce energy consumption.

Benefits of technology

The process achieves improved glass homogeneity and reduces energy consumption by up to 10% while maintaining high-quality glass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000019_0000
    Figure 00000019_0000
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a flat glass, comprising the melting of a mixture of raw materials constituting a melting bath, said mixture of raw materials comprising a calcium silicate comprising, by weight percentage, more than 30% of SiO2 and more than 20% of CaO, preferably at least 25% of CaO, CaO and SiO2 together representing more than 60%, or even more than 70% or more than 80% of the total weight of said silicate and in that said silicate is introduced into the mixture in the form of a powder having a median grain diameter of less than or equal to 400 micrometers.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR PRODUCING FLOAT GLASS FROM A MIXTURE OF MINERAL MATERIALS COMPRISING A CALCIUM SILICATE

[0001] The invention relates to the field of glass melting, in particular for the manufacture of float glass as used in particular in the fields of construction or even automobiles.

[0002] Glass is usually prepared by melting in a furnace raw materials comprising silica and at least one silica flux such as sodium carbonate, and at least one alkaline earth (to give the glass resistance to hydrolysis) such as limestone (calcium carbonate) and dolomite (CaMg(CO3)2). During melting, the carbonates release carbon dioxide, the bubbles of which contribute to the stirring of the mass being melted. Furthermore, certain carbonates such as dolomite, even before releasing their CO2, break down into finer particles according to the phenomenon known as decrepitation, which can be quite violent and generate dust which clogs and even corrodes the various conduits equipping the furnaces (chimneys, regenerators, etc.).Removing bubbles from glass generally requires the addition of a refining agent such as sodium sulfate, the release of sulfur oxide from which carries residual carbon dioxide and water bubbles to the glass surface. However, sulfur oxide is a particularly corrosive gas. It is desirable to develop glass manufacturing processes that generate as little CO2 as possible for environmental reasons, while still producing good quality glass at an acceptable cost, particularly from the point of view of the energy expenditure required for glass manufacturing.

[0003] In addition to the release of CO2 directly during the melting process of the raw material bath, it is therefore important to consider the glass manufacturing process as a whole, taking into account other factors such as the cost of the raw materials, their transport or even the energy cost of making said raw materials available and melting them.

[0004] The invention relates to a mixture of raw materials for the preparation of a molten glass whose target composition corresponds to the formulation below, in weight percentage: - SiO2: between 65 and 80%, preferably between 70 and 75%, - Na2O: between 8 and 20%, preferably between 10 and 20%, - CaO: between 5 and 20%, preferably between 5 and 15%, - MgO: between 0 and 10%, preferably between 0 and 7%, - A12O3: between 0 and 10%, preferably between 0.5 and 3%, - K2O: between 0 and 10%, preferably between 0 and 2%, - Iron oxide: 0 to 15%, preferably between 0 and 10%, - other oxide(s): between 0 and 5% cumulative,

[0005] the remainder being made up of unavoidable impurities.

[0006] This mixture of raw materials is intended to be heated to a temperature and under conditions allowing its melting to obtain a glass corresponding to said target composition.

[0007] The originality of the present invention lies in the choice of raw materials. Indeed, contrary to the prejudices generally present in the field, and illustrated by the previously cited publications, it has been discovered that it is possible to use silicates as raw material in a flat glass manufacturing process to limit the energy consumption of its manufacturing process while maintaining good homogeneity of the final glass.

[0008] According to the invention, it has in fact been found by the applicant company that the granulometry of such mineral raw materials must also be taken into account for the preparation of the initial mixture in order to limit the energy consumption of such a flat glass manufacturing process.

[0009] Thus, according to a first aspect, for soda-lime-silica glasses, among the different oxides constituting the glass, calcium oxide is the one which most impacts the homogeneity of the glass due to the difference between its optical index and that of silica, the main constituent of the glass network. CaO is however necessary in the composition of flat glass: inexpensive, easy to find in nature, it reinforces the hydrolytic resistance and helps to control the viscosity and the liquidus temperature of the molten bath of raw materials.

[0010] However, a non-homogeneous glass can easily exhibit "waves", i.e. areas where the refractive index varies locally due to a variation in composition. Sometimes, even if the variation is less than 0.1% by weight of calcium oxide, not detectable by conventional analytical methods, these variations lead to optically observable distortions.

[0011] For soda-lime-silica glass intended for the production of flat glass, the standard limestone has a PSD (PSD for particle size distribution) such that the median diameter D50 is of the order of or greater than 600 microns, with maximum particle sizes of up to 2 or even 3 mm. In order to improve the homogeneity of the glass, it may be considered to reduce the particle size distribution of the raw material and particularly the PSD of the limestone used in the initial bath of raw materials, as shown by the publication "Influence of limestone grain size on glass homogeneity, Glass Technology, Society of Glass Technology, 2010, 51 (3), pp.116".

[0012] In a conventional glass melting furnace as illustrated in the attached [Fig.l], another aspect of the raw materials is also to be taken into account if such a reduction in the PSD is envisaged.

[0013] [Fig.l] schematically illustrates a furnace 2 for melting raw materials. The raw materials are introduced as a mixture into the furnace 7 in the form of a compact lump 1. The lump 1 initially floats on the molten glass 6. The lower surface of the lump first melts due to the convection of the molten glass under the effect of electrical resistance 4 (electrical boosting) arranged in the lower part of the furnace. A bubbler 8 increases the convection of the glass and thus mechanically induces better homogeneity of the glass. The upper surface of the lump is also heated by radiation thanks to a series of burners 3 positioned at the side walls of the furnace as shown schematically by [Fig.l] below. After melting of the lump, a foaming phenomenon 5 is observed due to the refining of the glass.

[0014] It has been demonstrated by the experiments carried out by the applicant company that the efficiency of heating by the burners 3 is linked to the emissivity of the raw materials used and in particular of the source of calcium used. Thus, a raw material with low emissivity produces a thermal mirror on the surface of the tile, which reduces the melting kinetics and increases the energy consumption of the furnace to achieve the same degree of melting.

[0015] Therefore, if we act on the particle size distribution (PSD) of the raw material and particularly the PSD of the calcium source used, a major drawback is that the emissivity of the raw material decreases. Thus, a lower emissivity results in a less efficient heat transfer. As a result, if the use of a limestone with a finer particle size allows on the one hand to improve the chemical and optical homogeneity of the glass and in particular the distribution of calcium oxide in the final glass, on the other hand it increases the energy consumption of the furnace since the energy transfer will be less favorable.

[0016] On the basis of these two antagonistic effects, it is customary to use, as a raw material source of calcium (or CaO in the final glass), limestone whose median diameter is of the order of 600 micrometers, or even greater than 600 micrometers.

[0017] The object of the present invention is thus to propose a glass manufacturing process allowing a homogeneous distribution of calcium oxide in said final glass, while reducing the energy consumption necessary for said manufacturing.

[0018] More specifically, the present invention relates to a method for manufacturing a glass having a target composition, comprising the melting of a mixture of raw materials constituting a melt bath, said target composition meeting the following criteria, in weight percentages:

[0019] SiO2: between 65 and 80%, preferably between 70 and 75%,

[0020] Na2O: between 8 and 20%, preferably between 10 and 20%,

[0021] CaO: between 5 and 20%, preferably between 5 and 15%,

[0022] MgO: between 0 and 10%, preferably between 0 and 7%,

[0023] A12O3: between 0 and 10%, preferably between 0.5 and 3%,

[0024] K2O: between 0 and 10%, preferably between 0 and 2%,

[0025] Iron oxide: 0 to 15%, preferably between 0 and 10%,

[0026] other oxide(s): between 0 and 5% cumulative,

[0027] the remainder being made up of unavoidable impurities,

[0028] said method being characterized in that the mixture of raw materials comprises a calcium silicate comprising, in weight percentage, more than 30% of SiO2 and more than 20% of CaO, preferably at least 25% of CaO, CaO and SiO2 together representing more than 60%, or even more than 70% or even more than 80% of the total weight of said silicate and in that said calcium silicate is introduced into the mixture in the form of a powder whose median grain diameter is less than or equal to 400 micrometers.

[0029] According to preferred but non-limiting modes of the scope of the present invention:

[0030] - Said calcium silicate has the following composition, in weight percentages: - SiO2: between 30 and 60%, preferably between 40 and 55%, - CaO: between 25 and 55%, preferably between 35 and 50%, - Fe2O3: between 0 and 4%, for example between 0.1 and 0.5%, - A12O3: between 0 and 8%, for example between 0.5 and 2%, - CO2: between 0 and 20%, in particular between 0 and 15%, - less than 5% of other oxides, preferably less than 3% of other oxides. - Said calcium silicate is introduced into the mixture in the form of a powder whose median grain diameter is between 20 micrometers and 400 micrometers, preferably between 30 micrometers and 350 micrometers, and very preferably between 40 micrometers and 300 micrometers. - Said calcium silicate is introduced into the mixture in the form of a powder whose maximum diameter is less than 1500 micrometers, preferably less than 1250 micrometers and very preferably less than 1000 micrometers. - The raw material mix includes: - said calcium silicate, - silica, particularly in the form of sand, - at least one source of sodium preferably chosen from sodium hydroxide sodium NaOH, sodium carbonate Na2CO3 or a mixture of sodium hydroxide NaOH and sodium carbonate Na2CO3> - optionally at least one source of magnesium chosen from an oxide mixed magnesium with at least one element selected from the group consisting of Si, Ca or magnesium hydroxide, optionally feldspar (K,Na)AlSi3O8, or another source of aluminum such as hydrated or calcined alumina, or phonolite or nepheline or slag optionally limestone CaCO3 optionally dolomite, optionally recycled glass cullet. The raw material mixture includes sodium hydroxide as a sodium source. The raw material mixture comprises a magnesium silicate as a source of magnesium, said mineral magnesium silicate preferably comprising, in weight percentage, more than 30% SiO2 and more than 10% MgO, preferably more than 15% MgO, MgO and SiO2 together representing more than 60%, or even more than 70% or even more than 75% of the total weight of said source. The said source of magnesium is a magnesium silicate having the following composition, in weight percentages: SiO2: between 40 and 55%, preferably between 45 and 50%, A12O3: between 0 and 10%, for example between 1 and 10%, MgO: between 20 and 40%, preferably between 25 and 35%, Fe2O3: between 0 and 4%, for example between 1 and 3%, less than 5% of other oxides, preferably less than 3% of other oxides, possibly water, in particular present in said source in the form of hydroxide(s), preferably in an amount of less than 20% and in particular between 5 and 15%. The said source of magnesium is a magnesium silicate having the following composition, in weight percentages: SiO2: between 55 and 70%, preferably between 58 and 65%, A12O3: between 0 and 10%, for example between 1 and 10%, MgO: between 20 and 40%, preferably between 25 and 35%, Fe2O3: between 0 and 4%, for example between 0.5 and 2%, less than 5% of other oxides, preferably less than 3% of other oxides, possibly water, in particular present in said source in the form of hydroxide(s), preferably in an amount of less than 20% and in particular between 5 and 15%. The said source of magnesium is a magnesium silicate having the following composition, in weight percentages: - SiO2: between 30 and 50%, preferably between 35 and 45%, - A12O3: between 0 and 10%, for example between 1 and 5%, - MgO: between 25 and 45%, preferably between 30 and 40%, - Fe2O3: between 0 and 10%, for example between 5 and 10%, - less than 5% of other oxides, preferably less than 3% of other oxides, - optionally water, in particular present in said source in the form of hydroxide(s), preferably in an amount of less than 20% and in particular between 5 and 15%. - The said source of magnesium is a magnesium hydroxide corresponding to the following composition, in percentages by weight: - MgO: between 50 and 75%, preferably between 55 and 70%, - H2O: between 10 and 35%, preferably between 25 and 35%, - SiO2: between 0 and 10%, for example between 0.5 and 5%, - CaO: between 0 and 5%, for example between 0.5 and 2%, - Fe2O3: between 0 and 4%, for example between 0.5 and 2%,

[0031] less than 5% of other oxides, preferably less than 3% of other oxides. - The raw materials of said melt include said calcium silicate and a source of magnesium such as a magnesium silicate, in particular as described above. - Recycled glass cullet is introduced into the melting bath. - Recycled glass cullet represents between 5 and 70% of the total weight of the bath of merger.

[0032] The invention also relates to a mixture of raw materials as described above and comprising in particular a calcium silicate comprising, in weight percentage, more than 30% of SiO2 and more than 20% of CaO, preferably more than 25% of CaO, CaO and SiO2 together representing more than 60%, or even more than 70% or even more than 80% of the total weight of said silicate and in which said silicate is introduced into the mixture in the form of a powder whose median grain diameter is less than or equal to 400 micrometers.

[0033] The present invention relates in particular to a mixture of raw materials comprising: - said calcium silicate, - silica, in particular in the form of sand, - at least one source of sodium preferably chosen from sodium hydroxide sodium NaOH, sodium carbonate Na2CO3 or a mixture of sodium hydroxide NaOH and sodium carbonate Na2CO3> - optionally at least one source of magnesium chosen from a mixed oxide of magnesium with at least one element chosen from the group consisting of Si, Ca or magnesium hydroxide, - optionally feldspar (K,Na)AlSi3O8, or another source of aluminum such as hydrated or calcined alumina, or phonolite or nepheline or slag - optionally limestone CaCO3> - optionally dolomite, - optionally recycled glass cullet.

[0034] Unless otherwise indicated, all particle size values ​​(median diameter D50, maximum diameter Dmax) in the present description and the claims are given by mass and are obtained by conventional sieving techniques, in particular for the calcium silicate according to the invention.

[0035] The invention will be better understood on reading the following examples intended to illustrate its advantages, without of course the invention being considered as limited to these, in any of the aspects described. Examples

[0036] In the following examples, different mixtures of raw materials were prepared in order to compare a mixture as currently used for the manufacture of glass for an identical final glass composition, which has substantially the following composition:

[0037] [Tables 1] Elements Percentage weight % SiO2 73.1 CaO 9.5 MgO 2.0 A12O3 1.1 Fe2O3 0.1 Na2O 13.5 k2o 0.3 Example 1 (prior art)

[0038] According to a first example, a glass corresponding to the preceding composition is synthesized, according to current techniques.

[0039] Table 2 below gives the proportions of the different raw materials and the final composition of the glass thus obtained:

[0040] [Tables2] D50 (pm) kg / tonne glass SiO2 TiO2 A12O 3 Fe2O 3 CaO MgO Na2 O K2O SO3 Sand 376 559 99.4 0.1 0.4 0.1 0.0 0.0 0.0 0.1 0.0 Feldspar 187 39 70.0 0.1 16.8 0.3 0.4 0.1 5.7 6.4 0.0 Soda ash 365 174 0.0 0.0 0.0 0.0 0.0 0.0 58.2 0.0 0.0 Dolomite 615 81 1.0 0.0 0.2 0.1 33.0 19.0 0.0 0.0 0.0 Limestone 596 88 0.1 0.0 0.0 0.0 55.6 0.4 0.0 0.0 0.0 Sodium sulfate NM 8 0.0 0.0 0.0 0.0 0.0 0.0 43.2 0.0 55.9 Cullet - 200 73.4 0.1 1.1 0.1 9.8 2.0 13.6 0.3 0.2 Final glass composition 73.1 0.1 1.1 0.1 9.5 2.0 13.5 0.3 0.5

[0041] NM: Not Measured

[0042] The particle size of the different raw materials is obtained by sieving.

[0043] The measurements are carried out on approximately 100g of representative sample (accuracy of 102g). The test sample is placed on the upper sieve of the column (Standard NF X 11501). The column is stirred for 5 minutes in a ROTAP sieve machine (Retsch AS200 TAP). The residue from the first sieve containing the grains is weighed (accuracy of 10 2g). The residue from each sieve is added, proceeding in the same way, to those from the previous sieves, and the cumulative mass is noted each time.

[0044] The results are expressed as a cumulative % relative to the final total mass MF.

[0045] X1% = M1 x 100 / MF

[0046] XI = % of cumulative rejection on sieve 1

[0047] Ml = mass of cumulative rejects on sieve 1

[0048] MF = final mass of product.

[0049] This calculation will be carried out for each nominal sieve opening.

[0050] The D50 is calculated from an interpolation of the upper and lower grain sizes closest to 50%.

[0051] In particular, the D50 is classically determined by the following equation:

[0052] D50 = [T<50%] + (50% - [X<50%]) x ([T<50%] - [T>50%]) / ([X<50%] - [X>50%])

[0053] With:

[0054] T<50% = Sieve opening less than 50% of rejection

[0055] T>50% = Sieve opening greater than 50% of rejection

[0056] X<50% =% of cumulative refusal on T<50%

[0057] X>50% =% of cumulative refusal on T>50%

[0058] We can thus deduce the particle size distribution by weight as reported in tables 2 to 4. Example 2 (comparative)

[0059] In this example, the same raw materials were used as in example 1 but a limestone with a finer grain size was used, i.e. D50 equal to 114 micrometers. Example 3:

[0060] In this example the mixture of raw materials is this time as described in table 3 below.

[0061] In this initial mixture, another mineral material consisting of a calcium silicate according to the invention, i.e. with a median diameter D50 equal to 107 micrometers, was introduced as a reagent to replace the limestone.

[0062] Analysis by conventional techniques shows that this natural mineral material corresponds to the composition described in table 3 below:

[0063] [Tables3] kg / ton glass SiO 2 TiO 2 A12O 3 Fe2O 3 CaO Mg O Na2 O K2O SO3 Sand 537 99.4 0.1 0.4 0.1 0.0 0.0 0.0 0.1 0.0 Feldspar 38 70.0 0.1 16.8 0.3 0.4 0.1 5.7 6.4 0.0 Soda ash 174 0.0 0.0 0.0 0.0 0.0 0.0 58.2 0.0 0.0 Dolomite 81 1.0 0.0 0.2 0.1 33.0 19.0 0.0 0.0 0.0 Limestone 53 0.1 0.0 0.0 0.0 55.6 0.4 0.0 0.0 0.0 Calcium Silicate 44 52.2 0.0 0.6 0.4 44.7 0.5 0.1 0.1 0.0 Sodium Sulfate 8 0.0 0.0 0.0 0.0 0.0 0.0 43.2 0.0 55.9 Cullet 200 73.4 0.1 1.1 0.1 9.8 2.0 13.6 0.3 0.2 Final Glass Composition 73.1 0.1 1.1 0.1 9.5 2.0 13.5 0.3 0.5 Example 4:

[0064] In this example, the same raw materials were used as in example 3 but a calcium silicate with a higher particle size was used, i.e. D50 equal to 826 micrometers.

[0065] Table 4 below shows the granulometric characteristics determined according to the method previously described for the different sources of calcium used as raw material in the previous examples:

[0066] [Tables4] “Coarse” limestone “Fine” limestone “Fine” calcium silicate “Coarse” calcium silicate Example 1 2 3 4 D50 (pm) 596 114 107 826 Max grain size (pm) 2000 250 800 4000 Proportion of grains <100 pm (%) 6 30 42 <5

[0067] The following measurements are carried out:

[0068] 1°) The emissivity of the calcium sources used is measured from the spectra of reflectance using the law of conservation of energy for opaque materials: absorbance a(X, T) + reflectance p(X, T) = 1. Applying Kirchhoff's law, the spectral emittance can be expressed in terms of total reflectance,

[0069] e(X, T) = a(X, T)

[0070] with: em = i L ... /

[0071] where Bt is the spectral irradiance of the black body at temperature T of 2000°C, corresponding to the temperature of the air-gas flame of the burner.

[0072] The measurements of the hemispherical reflectance at room temperature are carried out with a 150 mm integrating sphere mounted on a Lambda spectrophotometer are carried out between 300 and 2500 nm, using as a reflectance reference, a Spectralon plate.

[0073] For easy handling, the samples are pressed by applying a force of 0.4 tonnes / cm2 and wetted with 10% water prior to measurement.

[0074] 2°) The mixtures of the above examples are melted in a glass melting furnace typical soda-lime based on flame technology shown schematically in [Fig.l] below.

[0075] Measurement of the energy consumed in the furnace for melting the mixtures:

[0076] During the various fusion tests corresponding to the examples above, the gas consumption is adjusted in order to maintain a profile temperature similar to inside the oven and at every point of it. This deduces a gas consumption and therefore energy required to reach the same heating point.

[0077] 3°) Homogeneity in CaO in the final glass:

[0078] A sample is melted in a cylindrical platinum crucible from the same mixture of raw materials as described previously. The sample is heated in air at 1480°C for 2 hours. The cooled glass is then cored and cut to obtain a blade comprising the cross-section of the cylinder. This blade was polished, carbon-metallized and analyzed using an electron microprobe at 15 kV. The analysis consisted of determining the mass percentage of CaO over the entire height of the blade (or of the melted sample) over 100 measurement points, the measurement step was 250 microns.

[0079] It is thus possible on this basis to calculate the average of the CaO concentration and the standard deviation. A criterion of homogeneity in CaO in the glass is provided by the ratio standard deviation divided by the average concentration (oCao / [CaO]).

[0080] The results obtained are reported in Table 5 below:

[0081] [Tables5] Example 1 2 3 4 Calcium source “Coarse” limestone “Fine” limestone “Fine” calcium silicate “Coarse” calcium silicate Emissivity 0.57 0.20 0.27 0.44 Glass homogeneity (Ocao / [CaO]) (%) 5.5 NM 3.5 >5 Energy consumed by the first burner in the furnace Reference >Ref. -10% / Ref NM

[0082] Example 3 according to the invention, in which a source of calcium consisting of a calcium silicate according to the invention is used as raw material for said melt, allows an energy adjustment on the first burner 1 (closest to the charging, i.e. the entry of the raw materials into the furnace) in the sense of a reduction in energy expenditure of approximately 10%. Also, in the sense previously described, the homogeneity of calcium oxide appears to be improved in the case of example 3 according to the invention.

[0083] To assess the optical quality (or homogeneity) of the glass, the "shadowgraph" technique is used, which reveals variations in refractive index and / or local variations in thickness. Depending on the type of defect, it is possible to filter only the defects due to variations in refractive index or chemical homogeneity, as described in publication WO2002012869A1. Periodically, samples are collected from all along the ribbon and the intensity of the defects is measured (0 if nothing, 1 if the defect is barely visible, 2 if the defect is more visible, etc.), each intensity value being defined using reference samples.

[0084] An evaluation or “rating” is thus determined which is the average calculated from the intensities of the glasses, as defined using said reference samples and on a production of glass with a thickness of 9.5 mm.

[0085] The results obtained for the glasses of examples 1 and 3 are reported in table 6 below.

[0086] [Tableauxô] Shadowgraph rating [daily average] Example 1 Example 3 Production (9.5mm thick) 1.1 0.7

[0087] It can be seen that example 3 according to the invention has fewer defects than reference example 1.

Claims

Claims

1. A method of manufacturing a glass having a target composition, comprising melting a mixture of raw materials constituting a melt bath, said target composition meeting the following criteria, in weight percentages: SiO2: between 65 and 80%, preferably between 70 and 75%, Na2O: between 8 and 20%, preferably between 10 and 20%, CaO: between 5 and 20%, preferably between 5 and 15%, MgO: between 0 and 10%, preferably between 0 and 7%, Al2O3: between 0 and 10%, preferably between 0.5 and 3%, K2O: between 0 and 10%, preferably between 0 and 2%, Iron oxide: 0 to 15%, preferably between 0 and 10%, other oxide(s): between 0 and 5% cumulatively, the remainder consisting of unavoidable impurities, said process being characterized in that the mixture of raw materials comprises a calcium silicate comprising, in weight percentage, more than 30% of SiO2 and more than 20% of CaO, preferably at least 25% of CaO, CaO and SiO2 together representing more than 60%,or even more than 70% or even more than 80% of the total weight of said silicate and in that said calcium silicate is introduced into the mixture in the form of a powder whose median grain diameter is less than or equal to 400 micrometers, in which said calcium silicate has the following composition, in weight percentages: - SiO2: between 30 and 60%, - CaO: between 25 and 55%, - Fe2O3: between 0 and 4%, - A12O3: between 0 and 8%, - CO2: between 0 and 20%, - less than 5% of other oxides.,

2. Manufacturing process according to claim 1, wherein said calcium silicate has the following composition, in weight percentages: - SiO2: between 40 and 55%, - CaO: between 35 and 50%, - Fe2O3: between 0.1 and 0.5%, - A12O3: between 0.5 and 2%, - CO2: between 0 and 15%, - less than 3% of other oxides.

3. Method according to one of the preceding claims, in which said calcium silicate is introduced into the mixture in the form of a powder whose median grain diameter is between 20 micrometers and 400 micrometers, preferably between 30 micrometers and 350 micrometers, and very preferably between 40 micrometers and 300 micrometers.

4. Method according to one of the preceding claims, wherein said calcium silicate is introduced into the mixture in the form of a powder whose maximum diameter is less than 1500 micrometers, preferably less than 1250 micrometers and very preferably is less than 1000 micrometers.

5. Method according to one of the preceding claims, in which the mixture of raw materials comprises: - said calcium silicate, - silica, in particular in the form of sand, - at least one source of sodium preferably chosen from sodium hydroxide NaOH, sodium carbonate Na2CO3 or a mixture of sodium hydroxide NaOH and sodium carbonate Na2CO3> - optionally at least one source of magnesium chosen from a mixed oxide of magnesium with at least one element chosen from the group consisting of Si, Ca or a magnesium hydroxide, - optionally feldspar (K,Na)AlSi3O8, or another source of aluminum such as a hydrated or calcined alumina, or phonolite or nepheline or a slag - optionally limestone CaCO3 - optionally dolomite, - optionally recycled glass cullet.

6. A method according to the preceding claim, wherein the mixture of raw materials comprises sodium hydroxide as a sodium source.

7. A method according to any preceding claim, wherein the mixture of raw materials comprises a magnesium silicate as a source of magnesium, said mineral magnesium silicate preferably comprising, in weight percentage, more than 30% SiO2 and more than 10% MgO, preferably more than 15% MgO, MgO and SiO2 together representing more than 60%, or even more than 70% or even more than 75% of the total weight of said source.

8. Method according to the preceding claim, in which said magnesium source is a magnesium silicate corresponding to the following composition, in weight percentages: - SiO2: between 40 and 55%, preferably between 45 and 50%, - Al2O3: between 0 and 10%, for example between 1 and 10%, - MgO: between 20 and 40%, preferably between 25 and 35%, - Fe2O3: between 0 and 4%, for example between 1 and 3%, - less than 5% of other oxides, preferably less than 3% of other oxides, - optionally water, in particular present in said source in the form of hydroxide(s), preferably in an amount of less than 20% and in particular between 5 and 15%.

9. Method according to claim 7 in which said magnesium source is a magnesium silicate corresponding to the following composition, in weight percentages: - SiO2: between 55 and 70%, preferably between 58 and 65%, - Al2O3: between 0 and 10%, for example between 1 and 10%, - MgO: between 20 and 40%, preferably between 25 and 35%, - Fe2O3: between 0 and 4%, for example between 0.5 and 2%, - less than 5% of other oxides, preferably less than 3% of other oxides, - optionally water, in particular present in said source in the form of hydroxide(s), preferably in an amount of less than 20% and in particular between 5 and 15%.

10. The method of claim 7 wherein said source of magnesium is a magnesium silicate having the following composition, in weight percentages: - SiO2: between 30 and 50%, preferably between 35 and 45%, - A12O3: between 0 and 10%, for example between 1 and 5%, - MgO: between 25 and 45%, preferably between 30 and 40%, - Fe2O3: between 0 and 10%, for example between 5 and 10%, - less than 5% of other oxides, preferably less than 3% of other oxides, - optionally water, in particular present in said source in the form of hydroxide(s), preferably in an amount of less than 20% and in particular between 5 and 15%.

11. Method according to one of claims 1 to 6, in which said source of magnesium is a magnesium hydroxide corresponding to the following composition, in weight percentages: - MgO: between 50 and 75%, preferably between 55 and 70%, - H2O: between 10 and 35%, preferably between 25 and 35%, - SiO2: between 0 and 10%, for example between 0.5 and 5%, - CaO: between 0 and 5%, for example between 0.5 and 2%, - Fe2O3: between 0 and 4%, for example between 0.5 and 2%, less than 5% of other oxides, preferably less than 3% of other oxides.

12. A method according to any preceding claim wherein the raw materials of said molten bath comprise said calcium silicate and a source of magnesium such as a magnesium silicate.

13. Method according to one of the preceding claims, in which recycled glass cullet is introduced into the melting bath.

14. Method according to the preceding claim, in which the recycled glass cullet represents between 5 and 70% of the total weight of the melt.

15. Mixture of raw materials for the manufacture of a glass having a target composition meeting the following criteria, in weight percentages: SiO2: between 65 and 80%, preferably between 70 and 75%, Na2O: between 8 and 20%, preferably between 10 and 20%, CaO: between 5 and 20%, preferably between 5 and 15%, MgO: between 0 and 10%, preferably between 0 and 7%, A12O3: between 0 and 10%, preferably between 0.5 and 3%, K2O: between 0 and 10%, preferably between 0 and 2%, Iron oxide: 0 to 15%, preferably between 0 and 10%, other oxide(s): between 0 and 5% cumulatively, the remainder being made up of unavoidable impurities, said mixture comprising a calcium silicate comprising, in weight percentage, more than 30% of SiO2 and more than 20% of CaO, preferably more than 25% of CaO, CaO and SiO2 together representing more than 60%, or even more than 70% or even more than 80% of the total weight of said silicate and in which said silicate of calcium is introduced into the mixture in the form of a powder whose median grain diameter is less than or equal to 400 micrometers, in which said calcium silicate has the following composition, in weight percentages: - SiO2: between 30 and 60%, - CaO: between 25 and 55%, - Fe2O3: between 0 and 4%, - A12O3: between 0 and 8%, - CO2: between 0 and 20%, - less than 5% of other oxides.

16. Mixture of raw materials according to the preceding claim comprising: - said calcium silicate, - silica, particularly in the form of sand, - at least one source of sodium preferably chosen from sodium hydroxide NaOH, sodium carbonate Na2CO3 or a mixture of sodium hydroxide NaOH and sodium carbonate Na2CO3> - optionally at least one source of magnesium chosen from a mixed oxide of magnesium with at least one element chosen from the group consisting of Si, Ca or a magnesium hydroxide, - optionally feldspar (K,Na)AlSi3O8, or another source of aluminum such as hydrated or calcined alumina, or phonolite or nepheline or slag optionally limestone CaCO3> optionally dolomite, optionally recycled glass cullet.