PIEZOELECTRIC DEVICE PRINTED EMPILE
The use of a PEDOT:PSS mixture with specific molecules addresses adhesion issues in piezoelectric devices, enabling stable, defect-free multi-layer structures for improved performance.
Patent Information
- Application Number
- FR2022013221
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-13
AI Technical Summary
Existing piezoelectric devices face issues with poor adhesion between PVDF and PEDOT:PSS layers, leading to wrinkles and potential short circuits due to solvent solubility of PEDOT:PSS, which affects the stability and performance of stacked piezoelectric capacitors.
A piezoelectric device is developed with a mixture of PEDOT:PSS and specific molecules, including an epoxy group-containing molecule and a sodium phosphonate, sodium sulfonate, or sodium carboxylate, to enhance adhesion and stability, allowing for multiple organic piezoelectric layers without short circuits.
The solution provides a homogeneous PEDOT:PSS layer with improved adhesion to PVDF, enabling multiple stacked organic piezoelectric layers without defects, enhancing device performance and reliability.
Smart Images

Figure 00000015_0000 
Figure 00000015_0001 
Figure 00000015_0002
Abstract
Description
Title of the invention: STACKED PRINTED PIEZOELECTRIC DEVICE Technical field
[0001] The present invention relates to the general field of piezoelectric devices based on organic material.
[0002] The invention relates to a stacked printed piezoelectric device.
[0003] The invention also relates to a method of manufacturing such a device.
[0004] The invention finds applications in numerous industrial fields, and in particular in the field of electromechanical devices, ultrasonic transducers for medical diagnosis, for energy recovery, in the field of force or pressure sensors.
[0005] The invention is particularly interesting for the manufacture of miniaturized devices. STATE OF THE PRIOR ART
[0006] Piezoelectric materials are materials that become electrically polarized under the action of mechanical stress and, conversely, can deform when an electric field is applied.
[0007] Piezoelectric technology printed by screen printing on flexible support is well known. For example, the article by Aliane et al. (“Impact of crystallization onferro-, piezo- andpyro-electric characteristics in thinfilm P(VDF-TrFE)”, Organic Electronics (2015), 25, 92-98) describes a printed piezoelectric device comprising a stack formed of an organic layer 40 of copolymers of vinylidene fluoride and trifluoroethylene (P(VDF-TrFE)) arranged between two electrodes 10, 20 made of poly(3,4-ethylenedioxythiophene) (PEDOT) and sodium poly(styrene sulfonate) (PSS) (denoted PEDOT:PSS) on a flexible support 30 made of polyethylene naphthalate or polyethylene terephthalate ([Fig.l]).
[0008] Generally speaking, piezoelectricity is mainly used to manufacture actuators or motors in the automotive or aeronautical fields or in the field of robotics. They are both fast (< 1 ms) and have a high resolution due to the direct conversion of electrical energy into mechanical energy.
[0009] The manufacture of actuator-type technologies requires stacking several piezoelectric capacitors vertically on top of each other ([Fig.2]). The device then comprises an alternation of piezoelectric layers 40 and first electrode 10 or second electrode 20. The displacement obtained is proportional to the number of piezoelectric layers (noted n). This displacement can be defined by the following equation (1): ,X7 ? (1) naked
[0010] The first electrodes 10 are electrically connected by means of a first via 51 filled with an electrically conductive material. The second electrodes 20 are electrically connected by means of a second via 52 filled with an electrically conductive material.
[0011] The organic piezoelectric material, based on polyvinylidene fluoride (PVFD), is generally deposited on the PEDOT:PSS electrodes by printing.
[0012] However, PVDF and PEDOT:PSS have poor adhesion to each other and PEDOT:PSS is soluble in the PVDF solvent. Wrinkles then form in the PVDF deposited on the PEDOT:PSS layer ([Fig.3]), which can subsequently cause short circuits. Statement of the invention
[0013] An aim of the present invention is to propose a piezoelectric device overcoming the drawbacks of the prior art, and in particular, a device avoiding short circuits.
[0014] For this, the present invention proposes a piezoelectric device comprising a substrate covered by a stack,
[0015] the stack comprising organic piezoelectric layers, first electrodes and second electrodes, each organic piezoelectric layer being arranged between a first electrode and a second electrode,
[0016] each organic piezoelectric layer preferably comprising a polymer matrix of PVDF, a PVDF copolymer or a PVDF terpolymer,
[0017] the first electrodes and the second electrodes being made of a mixture comprising PEDOT:PSS, a first molecule having an epoxy group and a second molecule, the second molecule being a sodium phosphonate, a sodium sulfonate or a sodium carboxylate.
[0018] The invention is fundamentally distinguished from the prior art by the use of an electrode comprising a mixture of PEDOT:PSS and at least two other particular molecules.
[0019] The molecule having an epoxy group makes it possible to crosslink the PEDOT:PSS and to form a protective network with respect to the solvent(s) used to deposit the upper layer (i.e. the piezoelectric layer).
[0020] Advantageously, the mixture comprises from 2 to 5% by mass of first molecule having an epoxy group. Preferably,
[0021] Advantageously, the first molecule is chosen from the (3-Glycidyloxypropyl)trimethoxysilane, 3-Glycidoxypropyldimethylethoxysilane and Glycidyl 2,2,3,3-tetrafluoropropyl ether.
[0022] Preferably, the first molecule is an alkoxysilane. Thus, the alkoxide groups form ionic bonds with the PEDOT:PSS, replacing the PSS-, which stabilizes the deposition and adhesion of the PVDF on the PEDOT:PSS layer.
[0023] Preferably, the first molecule having the epoxy group is 3-Glycidyloxypropyl)trimethoxysilane. This molecule has a relatively low crosslinking temperature (140°C), which is compatible with polymer substrates.
[0024] The second molecule is a charged molecule having a sodium ion. In particular, the second molecule being a sodium phosphonate, a sodium sulfonate or a sodium carboxylate. The presence of this molecule improves the adhesion of the PEDOT:PSS to the piezoelectric material, in particular PVDF, and facilitates connections during crosslinking of the PEDOT:PSS.
[0025] Advantageously, the mixture comprises from 2 to 10% by mass of second molecule.
[0026] Advantageously, the second molecule is chosen from the monosodium salt of 3-(Trihydroxysilyl)propyl methylphosphonate (also called sodium 3-(Trihydroxysilyl)propyl methylphosphonate), the hydrated sodium salt of Fosmidomycin, the sodium salt of 1-Hexanesulfonic acid and the hydrated sodium salt of (2E)-Pentenedioic acid.
[0027] Preferably, the second molecule is a phosphonate, i.e. an organophosphorus molecule having an RPO(OR')(OR”) group, in which R, R' and R” represent, independently of each other, a hydrogen atom, an alkyl group or an aryl group.
[0028] Preferably, it is sodium 3-(Trihydroxysilyl)propyl methylphosphonate.
[0029] Advantageously, the mixture comprises at least 70% by mass of PEDOT:PSS.
[0030] Advantageously, the mixture further comprises 2,2,3,3,3-Pentafluoro-l-propanol. This molecule allows the epoxy molecules to be linked together and facilitates the deposition of the upper PVDF layer by modifying the surface energy.
[0031] Advantageously, the mixture comprises from 0.1 to 1% by mass of 2,2,3,3,3-Pentafluoro-1-propanol.
[0032] Advantageously, the mixture further comprises sorbitan. Sorbitan improves the miscibility of the different species of the formulation and facilitates printing. It has a favorable effect on the hydrophilic-hydrophobic balance of the mixture.
[0033] Advantageously, the mixture comprises from 0.1 to 1% by mass of sorbitan.
[0034] Advantageously, the mixture comprises between 2 and 5% by mass of (3-Glycidyloxypropyl)trimethoxysilane, between 2 and 10% by mass of 3-(Trihydroxysilyl)propyl methylphosphonate, at least 70% by mass of PEDOT:PSS. Preferably, the mixture further comprises 1% by mass of Sorbitan and 1% by mass of 2,2,3,3,3-Pentafluoro-l-propanol.
[0035] The PEDOT:PSS layer obtained is homogeneous and has good adhesion to the PVDF.
[0036] It is thus possible to have a device with several stacked organic piezoelectric layers. Advantageously, the stack comprises at least 2 organic piezoelectric layers, preferably at least 5 organic piezoelectric layers, and even more preferably at least 7 organic piezoelectric layers. It can comprise up to 15 layers.
[0037] The invention also relates to a method of manufacturing a piezoelectric device comprising a substrate covered by a stack,
[0038] the stack comprising organic piezoelectric layers, first electrodes and second electrodes, each organic piezoelectric layer being arranged between a first electrode and a second electrode,
[0039] each organic piezoelectric layer preferably comprising a polymer matrix of PVDF, a PVDF copolymer or a PVDF terpolymer,
[0040] the first electrodes and the second electrodes being formed by depositing, on the organic piezoelectric layers, a solution comprising a solvent, PEDOT:PSS, a first molecule having an epoxy group and a second molecule, the second molecule being a sodium phosphonate, a sodium sulfonate or a sodium carboxylate.
[0041] Advantageously, the mixture comprises between 2 and 5% by mass of (3-Glycidyloxypropyl)trimethoxysilane, between 2 and 10% by mass of 3-(Trihydroxysilyl)propyl methylphosphonate and at least 70% by mass of PEDOT:PSS.
[0042] Advantageously, the mixture further comprises 1% by mass of Sorbitan and / or 1% by mass of 2,2,3,3,3-Pentafluoro-1-propanol.
[0043] Other characteristics and advantages of the invention will emerge from the additional description which follows.
[0044] It goes without saying that this additional description is given only as an illustration of the subject of the invention and must in no case be interpreted as a limitation of this subject. Brief description of the drawings
[0045] The present invention will be better understood on reading the description of exemplary embodiments given purely for informational purposes and in no way limiting, with reference to the appended drawings in which:
[0046] [Fig.l], previously described, is a schematic cross-sectional representation of a piezoelectric device having a layer of piezoelectric material according to the prior art.
[0047] [Fig. 2], previously described, is a schematic cross-sectional representation of a piezoelectric device having several layers of organic piezoelectric material according to the prior art.
[0048] [Fig. 3], previously described, is a photograph obtained under an optical microscope of a layer of PVDF deposited on a layer of PEDOT:PSS, according to a method of the prior art.
[0049] [Fig.4A] and
[0050] [Fig.4B] are schematic cross-sectional representations of different piezoelectric devices having several layers of organic piezoelectric material according to different particular embodiments of the invention.
[0051] [Fig.5A] and
[0052] [Fig.5B] are photographs obtained under an optical microscope, at different magnifications, of a stack of 5 stages comprising an alternation of PEDOT:PSS layers and PVDF layers, according to a particular embodiment of the invention.
[0053] [Fig.6] is a graph obtained with a profilometer representing the thickness as a function of the distance, the measurement having been carried out on the stack of figures 5A and 5B.
[0054] [Fig.7] is a graph obtained with a profilometer representing the thickness as a function of the distance, the measurement having been carried out on a stack of 7 stages, the stack comprising an alternation of layers of PEDOT:PSS and layers of PVDF, according to another particular embodiment of the invention.
[0055] The different parts represented in the figures are not necessarily on a uniform scale, in order to make the figures more readable.
[0056] DETAILED DESCRIPTION OF PARTICULAR EMBODIMENTS
[0057] Although this is in no way limiting, the invention particularly finds applications in the field of piezoelectric devices, in particular capacitances of the Metal / Composite / metal type.
[0058] The invention is particularly interesting for underwater sonar and ultrasonic transducer applications for medical diagnosis, but also for energy recovery or for force or pressure sensors or actuators.
[0059] For this, the present invention proposes a piezoelectric device comprising a stack formed of several layers of piezoelectric materials 400-412 (Figures 4A and 4B). Twelve organic piezoelectric layers are shown in the figures, but the stack could have more than twelve organic piezoelectric layers or fewer than twelve organic piezoelectric layers. The stack has at least two organic piezoelectric layers.
[0060] Each organic piezoelectric layer 400 is disposed between a first electrically conductive electrode 100 and a second electrically conductive electrode 200.
[0061] The electrodes of the stack are therefore alternately first electrodes 100-106 then second electrodes 200-206.
[0062] In other words, the stack successively comprises:
[0063] - a first electrode, preferably positioned on a substrate, preferably a flexible substrate,
[0064] - N x (a sub-stack formed of an organic piezoelectric layer, a second electrode, an organic piezoelectric layer, a first electrode, an organic piezoelectric layer), and
[0065] - a second electrode.
[0066] N is an integer greater than or equal to 1.
[0067] The first electrodes 100-106 (or sometimes noted 100 for simplification) and the second electrodes 200-206 (or sometimes noted 200 for simplification) locally cover the layers of piezoelectric materials.
[0068] Advantageously, the first electrodes 100-106 and the second electrodes 200-206 are made of the same material.
[0069] The electrodes 100-106, on the one hand, and the electrodes 200-206, on the other hand, are electrically connected to each other, for example by means of vias 510, 520 and / or contact connections 530, 540 ([Fig.4A]).
[0070] Alternatively, the first electrodes 100-106 are electrically connected by means of a first via 510 filled with a first electrically conductive material and the second electrodes 200-206 are electrically connected by means of a second via 520 filled with a second electrically conductive material ([Fig.4B])•
[0071] The first electrodes 100-106 are electrically insulated from the second electrodes 200-206.
[0072] Vias 510, 520 pass through the stack from one side to the other. The first via 510 passes through all organic piezoelectric layers 400-412. The second via 520 passes through all organic piezoelectric layers 400-412.
[0073] The filling of the vias 510, 520 is preferably carried out during the deposition of the first electrodes 100-106 and during the deposition of the second electrodes 200-206. In other words, the material forming the first electrodes 100-106 and the material forming the second electrodes 200-206 fills the vias 510, 520 as and when of the formation of electrodes.
[0074] Advantageously, the first electrically conductive material and the second electrically conductive material are identical.
[0075] Even more advantageously, the material of the first electrodes 100-106, the material of the second electrodes 200-206, the first electrically conductive material filling the first via 510 and the second electrically conductive material filling the second via 520 are identical. Preferably, it is PEDOT:PSS. The upper part of the vias 510,520 may be made of another electrically conductive material (for example silver), if the vias are not completely filled after the formation of the stack.
[0076] Advantageously, the first via 510 and the second via 520 have the same shape and / or the same dimension.
[0077] Contact connections 530, 540 may also be present.
[0078] The organic piezoelectric layer 400 preferably comprises a polymer matrix made of PVDF, a PVDF copolymer or a PVDF terpolymer, or a resin, for example epoxy or a thermoplastic polyurethane (TPU).
[0079] It may be a copolymer of vinylidene fluoride and at least one other monomer copolymerizable with VDF. Advantageously, the copolymer comprises at least 50 mol%, preferably at least 70 weight%, even more preferably at least 90 mol% of VDF.
[0080] By way of illustration, the copolymerizable monomer(s) are, for example, chosen from chlorotrifluoroethylene (CTFE), chlorofluoroethylene (CFE), hexafluoropropylene (HFP), trifluoroethylene (VF3), methyl methacrylate (MMA), tetrafluoroethylene (TFE), and perfluoro(alkyl vinyl) ethers such as perfluoro(methyl vinyl) ether (PMVE).
[0081] For example, the copolymer is a poly(vinylidene fluoride-trifluoroethylene) PVDF / TrFe copolymer, also noted P(VDF-TrFe).
[0082] It can also be a terpolymer. For example, a PVDF / CTFE / CFE terpolymer will be chosen.
[0083] According to a first embodiment, the polymer is ferroelectric. For example, it is PVDF (polyvinylidene fluoride), poly(vinylidene fluoride-trifluoroethylene), denoted P(VDF-TrFE) or PVDF-CTFE.
[0084] Preferably, the organic piezoelectric layers 400-412 are made of P(VDF-TrFE) or based on P(VDF-TrFE).
[0085] According to another embodiment variant, the polymer is not a ferroelectric polymer: it may be PVDF-HFP.
[0086] The organic piezoelectric layer 400 may be a composite material. For example, the layer may comprise, in addition to the polymer matrix, particles ferroelectrics and, possibly, PEDOT:PSS particles.
[0087] For example, the ferroelectric particles are made of BaTiO3 (BTO), PZT (lead zirconate titanoate), AIN, ZnO, or even SBN (Sr-Ba-Nb oxide) or SBT (Sr-Ba-Ti oxide).
[0088] The thickness of the piezoelectric material layer 400 ranges, for example, from 1 pm to 100 pm, preferably from 1 to 50 pm, more preferably from 3 to 100 pm. It is, preferably, between 4 pm and 6 pm. For example, the organic piezoelectric layers 400-412 have a thickness of 3.6 pm.
[0089] Each layer of piezoelectric material 400 is arranged between a first electrode 100 called the lower electrode and a second electrode 200 called the upper electrode.
[0090] The first electrodes 100-106 and the second electrodes 200-206 have, for example, a thickness of Ipm.
[0091] The first electrodes 100-106 and the second electrodes 200-206 are made of a material formed from a mixture of PEDOT:PSS and other particular molecules.
[0092] The electrodes 100, 200 are based on PEDOT:PSS (poly(3,4-ethylenedioxythiophene ...). By based on PEDOT:PSS, it is meant that the material forming the electrode comprises at least 50% by mass of PEDOT:PSS. Preferably, the material forming the electrode comprises at least 70% by mass of PEDOT:PSS.
[0093] In particular, the mixture comprises:
[0094] - PEDOT:PSS,
[0095] - the first molecule having an epoxy group, the first molecule being preferably an alkoxysilane,
[0096] - a second molecule, the second molecule being a sodium phosphonate, a sodium sulfonate or a sodium carboxylate,
[0097] - possibly sorbitan,
[0098] - optionally 2,2,3,3,3-Pentafluoro-l-propanol.
[0099] Preferably, the mixture comprises:
[0100] - at least 70% by mass of PEDOT:PSS,
[0101] - from 2 to 5% by mass of the first molecule having an epoxy group, the first molecule preferably being an alkoxysilane,
[0102] - from 2 to 10% by mass of second molecule, the second molecule being preferably a sodium phosphonate,
[0103] - optionally from 0.1 to 1% by mass of sorbitan,
[0104] - optionally from 0.1 to 1% by mass of 2,2,3,3,3-Pentafluoro-l-propanol.
[0105] Advantageously, the first molecule having an epoxy group is chosen from (3-Glycidyloxypropyl)trimethoxysilane (CAS 2530-83-8), 3-Glycidoxypropyldimethylethoxysilane (CAS 65799-47-5) and Glycidyl 2,2,3,3-tetrafluoropropyl ether (CAS 19932-26-4).
[0106] It is possible to choose a fluoroepoxy.
[0107] Preferably, the first molecule is an alkoxysilane.
[0108] Preferably, the first molecule is (3-Glycidyloxypropyl)trimethoxysilane.
[0109] Preferably, the second molecule is chosen from the monosodium salt 3-(Trihydroxysilyl)propyl methylphosphonate (also noted as sodium methylphosphonate 3-(Trihydroxysilyl)propyl) (CAS 84962-98-1)), the sodium salt Fos-midomycin (also called monosodium salt of P-[3-(formylhydroxyamino)propyl]-phosphonic acid (CAS 66508-53-0)), the sodium salt of 1-Hexanesulfonic acid (CAS 2832-45-3) and the sodium salt of (2E)-Pentenedioic acid (also called hydrated salt of Sodium trans-glutaconate (C5H6O4 • xNa+ • yH2O).
[0110] Advantageously, the second molecule is a sodium phosphonate.
[0111] Preferably, it is sodium 3-(Trihydroxysilyl)propyl methylphosphonate.
[0112] Sorbitan may be present in trace amounts in the composite. Trace amounts are defined as less than 0.2%. Sorbitan may be found on the surface of the material. The benzene ring and / or OH groups of sorbitan make it easily identifiable, for example, by FTIR or XPS (chemical analysis technique).
[0113] Advantageously, the stack comprises at least 2 organic piezoelectric layers, preferably at least 5 organic piezoelectric layers, even more preferably at least 7 piezoelectric layers.
[0114] The stack is arranged on a substrate 300. It can be positioned at the edge of the substrate 300 ([Fig.4A]) or offset from the edge of the substrate 300 ([Fig.4B]).
[0115] The substrate 300 is, advantageously, a flexible type substrate. For example, it is a simple plastic substrate such as a film of polyethylene terephthalate (PET), polyimide (PI), polyethylene naphthalate (PEN), polycarbonate (PC), thermoplastic polyurethane (TPU) or polydimethylsiloxane (PDMS). It may also be a paper substrate.
[0116] The invention also relates to a method of manufacturing such a device. The method comprises the following steps:
[0117] a) forming a first electrode 100,
[0118] b) forming on the first electrode 100, for example by screen printing, an organic piezoelectric layer 400,
[0119] c) forming a second electrode 200 on the organic piezoelectric layer 400,
[0120] d) forming on the second electrode 200, for example by screen printing, an organic piezoelectric layer 400,
[0121] e) optionally repeating steps a), b), c) and d) until a stack with the desired number of piezoelectric layers 400 is formed.
[0122] It is possible to obtain stacks comprising up to 15 layers of composite material.
[0123] The device is made from the substrate 300. The material of the substrate 300 can first be cleaned in order to remove organic residues present thereon. The type of cleaning implemented will depend on the material of the substrate.
[0124] Step a) and / or step c) can be carried out by vapor deposition (PVD) by evaporation (“sputtering” in English), screen printing, spraying or even by inkjet.
[0125] Preferably, step a) and / or step c) are carried out by depositing, by screen printing, a composition (or formulation) comprising the various constituents of the electrode indicated above and a solvent. The screen printing deposition device may comprise a fabric screen or a metal stencil.
[0126] The composition can be mixed with glass beads.
[0127] The solvent is, for example, triethylphosphate, trimethylphosphate or tetrahydrofuran (THF).
[0128] In the case where vias are present in the device, as the stack of the piezoelectric device is formed, the materials of the first electrodes 100-106 and the materials of the second electrodes 200-206 fill, respectively, the first via 510 and the second via 520.
[0129] If the vias 510,520 are not completely filled, it is possible to add another electrically conductive element, for example a silver ink.
[0130] During step b), the layer of piezoelectric material 400 can be deposited by spin coating. Other types of localized deposition can be used such as screen printing or spraying or even inkjet deposition. Preferably, the piezoelectric layer is deposited by screen printing. In one pass, the thickness deposited is between 1 and 20 μm. It is possible to superimpose several layers by screen printing until the desired final thickness is reached.
[0131] For the actuators, at least five layers and preferably ten layers of composites will be deposited, intercalated between two electrodes, according to the following sequence: N x (electrode / composite / electrode).
[0132] The method also comprises a step of crystallizing the layer of pyroelectric material, to improve its pyroelectric performance. This irradiation is for example carried out with UV flash light, with a flash duration, or pulse duration, of between approximately 500 ps and 2 ms, a fluence (energy delivered per unit area) of between approximately 15 J / cm2 and 25 J / cm2, and with light of wavelength of between approximately 200 nm and 380 nm. The number of flashes, or The pulses of UV light produced during this irradiation vary depending on the thickness over which the pyroelectric material is to be crystallized. For example, for a thickness of P(VDF-TrFe) equal to approximately 2 pm, the irradiation can be implemented with a fluence equal to approximately 17 J / cm2, a pulse duration equal to approximately 2 ms and a number of pulses equal to 5.
[0133] The pyroelectric material, having possibly undergone a previous crystallization, is then subjected to annealing, for example, carried out at approximately 130°C for approximately 60 min, to finalize the total crystallization of the pyroelectric material.
[0134] The crystallization of the pyroelectric material can therefore be carried out in two stages: firstly, irradiation by UV light pulse to properly crystallize the second face of the layer of pyroelectric material in order to increase its thermal conductivity, then thermal annealing completing the crystallization for the rest of the pyroelectric material not crystallized by the previous irradiation.
[0135] When the pyroelectric material is a copolymer based on P(VDF-TrFe), a polarization step of the pyroelectric material is carried out before its use. This step can be carried out, for example, by applying a direct current voltage to its terminals, via the electrodes, in order to improve the pyroelectric coefficient of this material. This polarization is carried out only once for the entire lifetime of the pyroelectric material. This polarization by direct current can be done at room temperature or hot (up to about 100°C). When the polarization is carried out at room temperature, it is possible to apply a direct voltage up to about 150V / pm of thickness of the pyroelectric layer for a duration for example between a few seconds and a few minutes. For example, a voltage of 120V / pm will be applied for 20s.When the polarization is carried out hot, for example at a temperature of about 90°C, a direct voltage for example between about 50 V and 80 V per micron of thickness of the pyroelectric layer can be applied for a duration for example between about 1 min and 5 min. The temperature is then lowered until it reaches room temperature, then the electric field applied to the pyroelectric material, via the applied direct voltage, is stopped. Such polarizations allow the PVDF to reach pyroelectric coefficients between about 20 and 45 pC / (m2.K). .
[0136] The molecules inside the pyroelectric layer 400 remain oriented in this way, even when the material is no longer subjected to this electric field. The material can be polarized in this way by applying an initial polarization voltage to the terminals of the electrodes. A thickness of pyroelectric material less than or equal to approximately 2 μm will preferably be chosen in order to promote the polarization of the pyroelectric material of this capacity, and the level of the electrical voltage applied between the electrodes to achieve the initial polarization of the pyroelectric material (when the pyroelectric material is to be initially polarized).
[0137] Annealing is advantageously carried out at the end of the process, or between the different steps. The annealing is, for example, at a temperature between 100°C and 150°C, preferably around 100°C to remove residual traces of solvent and / or finalize the crystallization of the pyroelectric material 400.
[0138] At the end of the method, contact resumptions 530, 540 are advantageously carried out.
[0139] Illustrative and non-limiting examples of an embodiment:
[0140] In the following example, the substrate is a 50 pm thick PI substrate. On this substrate, a stack comprising alternating layers based on PEDOT:PSS to form the electrodes and P(VDF-TRFE) or P(VDF-TRFE)-based layers to form the piezoelectric material was deposited. The stack comprises 5 layers of P(VDF-TRFE).
[0141] The electrodes are formed from a mixture comprising:
[0142] - at least 70% by mass of PEDOT:PSS,
[0143] - from 2 to 5% by mass of (3-Glycidyloxypropyl)trimethoxysilane,
[0144] - from 2 to 10% by mass of sodium 3-(Trihydroxysilyl)propyl methylphosphonate,
[0145] - 1% by mass of sorbitan,
[0146] - 1% by mass of 2,2,3,3,3-Pentafluoro-l-propanol.
[0147] The lower electrode 100 is deposited by screen printing and then subjected to two heat treatments: a first annealing at 60°C for 5 min and a second annealing at 150°C for 20 minutes.
[0148] The P(VDF-TRFE) piezoelectric layer is deposited by screen printing, then it is subjected to heat treatment (annealing at 150°C for 5 minutes).
[0149] The upper electrode 200 is deposited by screen printing and then subjected to two heat treatments: a first annealing at 60°C for 5 min and a second annealing at 150°C for 20 minutes.
[0150] These technological sequences are repeated for each stage.
[0151] The stack obtained was characterized. It does not have any holes or folds (Figures 5A and 5B). It has a thickness of approximately 50 pm ([Fig.6]).
[0152] A 7-tier stack was also fabricated using the same steps as described previously. The stack has a thickness of approximately 100 pm ([Fig.7]). For comparison, a PEDOT:PSS layer has a thickness of 5 pm.
[0153] The stack obtained does not present any defects (in particular folds) like the devices of the prior art.
Claims
Claims
1. A piezoelectric device comprising a substrate (300) covered by a stack, the stack comprising organic piezoelectric layers (400), first electrodes (100) and second electrodes (200), each organic piezoelectric layer (400) being disposed between a first electrode (100) and a second electrode (200), each organic piezoelectric layer (400) preferably comprising a polymer matrix of PVDF, a PVDF copolymer or a PVDF terpolymer, or a resin, characterized in that the first electrodes (100) and the second electrodes (200) are made of a mixture comprising PEDOT:PSS, a first molecule having an epoxy group and a second molecule, the second molecule being a sodium phosphonate, a sodium sulfonate or a sodium carboxylate.
2. Device according to claim 1, characterized in that the first molecule having an epoxy group is chosen from (3-Glycidyloxypropyl)trimethoxysilane, 3-Glycidoxypropyldimethylethoxysilane and Glycidyl 2,2,3,3-tetrafluoropropyl ether.
3. Device according to one of claims 1 and 2, characterized in that the mixture comprises from 2 to 5% by mass of first molecule having an epoxy group.
4. Device according to any one of the preceding claims, characterized in that the second charged molecule having a sodium ion is chosen from the monosodium salt of 3-(Trihydroxysilyl)propyl methylphosphonate, the hydrated sodium salt of Fosmidomycin, the sodium salt of 1-Hexanesulfonic acid and the hydrated sodium salt of (2E)-Pentenedioic acid.
5. Device according to any one of the preceding claims, characterized in that the mixture comprises from 2 to 10% by mass of second charged molecule having a sodium ion.
6. Device according to any one of the preceding claims, characterized in that the mixture comprises at least 70% by mass of PEDOT:PSS.
7. Device according to any one of the preceding claims, characterized in that the mixture comprises sorbitan.
8. Device according to any one of the preceding claims, characterized in that the mixture comprises from 0.1 to 1% by mass of 2,2,3,3,3-pentafluoro-l-propanol.
9. Device according to any one of the preceding claims, characterized in that the mixture comprises between 2 and 5% by mass of (3-Glycidyloxypropyl)trimethoxysilane, between 2 and 10% by mass of 3-(Trihydroxysilyl)propyl methylphosphonate, at least 70% by mass of PEDOT:PSS, 1% by mass of Sorbitan and 1% by mass of 2,2,3,3,3-pentafluoro-l-propanol.
10. A method of manufacturing a piezoelectric device comprising a substrate (300) covered by a stack, the stack comprising organic piezoelectric layers (400), first electrodes (100) and second electrodes (200), each organic piezoelectric layer (400) being arranged between a first electrode (100) and a second electrode (200), each organic piezoelectric layer (400) preferably comprising a polymer matrix of PVDF, a PVDF copolymer or a PVDF terpolymer, characterized in that the first electrodes (100) and the second electrodes (200) are formed by depositing, on the organic piezoelectric layers (400), a solution comprising a solvent, PEDOT:PSS, a first molecule having an epoxy group and a second molecule, the second molecule being a sodium phosphonate, a sodium sulfonate or a sodium carboxylate.
11. Method according to claim 10, characterized in that the mixture comprises between 2 and 5% by mass of (3-Glycidyloxypropyl)trimethoxysilane, between 2 and 10% by mass of 3-(Trihydroxysilyl)propyl methylphosphonate and at least 70% by mass of PEDOT:PSS.