Partition wall crossing
The partition crossing design with a metallic housing and tellurium oxide-based glass sleeve addresses robustness issues by eliminating thermoplastic interfaces, ensuring high hermeticity and mechanical strength under severe conditions.
Patent Information
- Application Number
- FR2023003007
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-04
AI Technical Summary
Existing partition crossings in the electronics industry face issues with robustness at high temperatures and pressures due to multiple material interfaces, particularly with thermoplastic materials like PEEK, which have significant thermal expansion deviations and limited temperature resistance.
A partition crossing design using a metallic housing with a glass sleeve made of tellurium oxide-based glass, surrounded by a copper or copper alloy pin, eliminating thermoplastic components and ensuring electrical insulation, mechanical resistance, and hermetic sealing, with a glass composition that matches the thermal expansion coefficient of the metal components.
The design achieves high hermeticity and mechanical strength at extreme conditions, reducing differential expansion issues and maintaining sealing integrity under high pressure and temperature, with improved thermal resistance and reduced interface complexity.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Partition wall penetration technical field
[0001] The present exposition relates to a partition wall penetration and a method for manufacturing such a partition wall penetration. Previous technique
[0002] In the field of electronics, bulkhead feedthroughs are devices allowing one or more lines to pass through a partition, such as the casing of a machine or the enclosure of a room, without compromising the sealing of the partition.
[0003] One of the most widely used solutions to date is described in US patent 7,364,451 B2. However, these bulkhead fittings have the drawback of requiring five different types of components for four different types of materials, not counting the elastomer seal that provides a watertight connection between the bulkhead fitting and the bulkhead itself. These bulkhead fittings thus comprise 1) a metal pin, 2) a glass insert, 3) several ceramic inserts, 4) a metal housing, and 5) a thermoplastic housing.
[0004] These partition penetrations thus present multiple interfaces between different materials, which makes them not very robust at high temperature due to the differential expansion phenomena appearing at each of the interfaces.
[0005] In particular, the thermoplastic material used for part of the housing of this bulkhead fitting belongs to the PEEK (PolyEther Ether Ketone) group which has a coefficient of thermal expansion of the order of 50 ppm / °C, which represents a significant difference compared to the coefficients of thermal expansion of the metallic and ceramic components of these same bulkhead fittings.
[0006] Moreover, thermoplastic materials of the PEEK group, although among the most efficient in terms of thermal and mechanical resistance, have a glass transition temperature around 150°C and a melting temperature around 350°C.
[0007] However, in the energy industry, bulkhead penetrations can be subjected to extremely severe operating conditions: they can be simultaneously exposed to very high pressures, up to 2000 bar, and high temperatures, exceeding 200°C. It is therefore understandable that this known configuration is not satisfactory for such demanding applications.
[0008] Other bulkhead penetration configurations are also known, notably in US patents 7,901,247 B2 and US patents 7,442,081 B2, but all these configurations also include a housing element made of thermoplastic material, making them unsuitable for the intended high-pressure and high-temperature applications.
[0009] There is therefore a real need for a bulkhead penetration and a manufacturing process for such a bulkhead penetration which are free, at least in part, from the disadvantages inherent in the aforementioned known configurations. Description of the invention
[0010] The present description relates to a partition wall penetration, comprising a metallic housing comprising a front surface, a rear surface and a peripheral surface, configured to be engaged in a through-hole of a partition, the peripheral surface of the housing comprising at least one peripheral groove configured to receive a seal intended to be crushed between the housing and the internal surface of the opening, at least one metallic pin, having a diameter greater than or equal to 1 mm, passing completely through the housing and protruding, on one side, from the front surface of the housing and, on the other side, from the rear surface of the housing, and at least one cylindrical, glass sleeve surrounding said at least one pin from the front surface to the rear surface of the housing so as to electrically isolate said at least one pin from the housing, in which said at least one pin is made of copper or copper alloy, said pin possibly having undergone a surface treatment, in which the sleeve material is a tellurium oxide-based glass having the composition consisting of, in molar percentage: - 50 to 80% of TeO2, advantageously 50 to 70%; - from 8 to 40% ZnO, advantageously from 15 to 35%; - 2 to 25% TiO2, advantageously 2 to 10% - from 0 to 20% of an oxide axOy, advantageously from 2 to 10%, a being an element chosen from the group consisting of Ba, Ce, Er, Sb, Y, La and B, x being an integer equal to 1 or 2 and y an integer equal to 1, 2 or 3; - possibly ZnF2 at a concentration of 2 to 10%, advantageously 3 to 8%, - and the inevitable impurities, provided that ZnF2 is present when axOy is BaO, said composition being essentially free of lead oxide, sodium oxide, potassium oxide and vanadium oxide.
[0011] In this configuration, it is understood that the glass sleeve completely passes through the partition penetration and therefore emerges on both sides of the partition, thus being exposed to the environments, possibly very different, on each side of the partition.
[0012] Such a configuration is made possible by the glass composition selected by the inventors. Indeed, this glass composition offers both good electrical insulation between the metallic pin and the metallic housing, good mechanical and thermal resistance of the seal between the pin and the housing and, above all, good airtightness ensuring good sealing of the bulkhead penetration, including at high pressure and high temperature.
[0013] In particular, ZnO gives the glass composition good stability. TiO2, for its part, provides excellent durability to the glass. Furthermore, the optional additional axOy oxide improves the stability, wettability, and / or coefficient of thermal expansion of the glass.
[0014] The MIL-STD-883 standard of April 2016 is one of the standards specifying the method for measuring the leakage rate of electronic components. According to conditions A4, the component is hermetically sealed (using a gasket and appropriate tightening) onto a vacuum chamber. It is advantageous to have the lowest possible pressure in this chamber for optimal sensitivity. Indeed, the lower the pressure, the fewer gas molecules there are in the chamber and therefore the less residual helium, which reduces background noise. The standard specifies a pressure below 0.13 mbar (0.11 µTr). This chamber is connected to a mass spectrometer calibrated to achieve the expected helium leakage rate. Calibration must be performed at each period of use, using a calibrated diffusion leak. The airtightness of the assembly must be checked with a flat metal plate.This is done by spraying the plate with helium using a spray gun. If the detector does not detect helium during this check, the assembly is correct and the parts can be tested in the same way, by spraying them with helium.
[0015] A good level of watertightness for a bulkhead penetration (for example, 1 x 10¹¹ mbar-l / s) depends primarily on the sealing achieved at the interfaces between the conductive metallic components and those made of insulating mineral materials. The inventors have thus measured that the resulting bulkhead penetrations exhibit a level of watertightness less than or equal to 10¹¹ mbar-l / s measured according to this Mil-STD-883 standard of April 2016.
[0016] The resulting bulkhead penetrations retain this good level of airtightness after the repeated thermal shock test defined in one of the standards Mil-DTL-26482 of February 2017, Mil-DTL-38999 of February 2015 and Mil-DTL-83723 of November 2009. This test, the methodology of which varies according to the standards, is considered the most relevant and is applied systematically for the airtight version.
[0017] Therefore, since this glass composition selected by the inventors ensures the desired airtightness, even when the glass sleeve completely passes through the bulkhead penetration, the use of a thermoplastic element directly in contact with the pin over at least part of its length is no longer necessary. The inventors then took advantage of this improved glass sleeve to propose a completely metallic housing, also completely passing through the partition wall, without any thermoplastic portion or even insert.
[0018] Thus, in the absence of thermoplastic material exposed to the severe environmental conditions of the bulkhead penetration, the mechanical and thermal resistance of the bulkhead penetration is improved.
[0019] Furthermore, the use of a fully metallic housing improves the robustness, dimensional stability, aesthetic appearance, and assembly options of the bulkhead fitting. It also reduces the number of interfaces between the various components of the bulkhead fitting, which improves its high-temperature performance, particularly with regard to differential expansion issues.
[0020] In this respect, this glass composition has the additional advantage of having a coefficient of thermal expansion close to that of metallic materials, in particular those used for the housing and the spindle.
[0021] The coefficient of thermal expansion is measured in the context of this presentation on a TMA from TA instrument (TMA 2940), with a ramp of 2° / min from 30 °C to 250 °C.
[0022] Advantageously, the composition of the tellurium oxide-based glass is free of Bi2O3.
[0023] More advantageously, the composition of the tellurium oxide-based glass is free of Al2O3, F and / or PbF2.
[0024] In general, the unavoidable impurities in the composition of tellurium oxide-based glass can be chosen from lead (Pb), iron (Fe), copper (Cu), arsenic (As), antimony (Sb), calcium (Ca), carbonate (CO3), magnesium (Mg), potassium (K), sodium (Na), phosphorus (P), chlorine (Cl), silicon (Si), sulfur (S) and mixtures thereof.
[0025] The total content of unavoidable impurities is generally less than or equal to 0.1105% (1105 ppm).
[0026] For the purposes of this presentation, "tellurium oxide-based glass" means any glass whose main component of composition is tellurium oxide (TeO2), advantageously of which TeO2 is present in a higher content than the other components, even more advantageously in a content of at least 50% molar percentage, even more advantageously of at least 60% molar percentage.
[0027] More generally, for the purposes of this exposition, a material is considered to be based on a given element when that element is the principal element of the material's composition, advantageously when that element is present in a higher proportion than the other components, even more advantageously in a proportion of at least 50% by molar percentage, and even more advantageously in a proportion of at least 60% by molar percentage molar.
[0028] In some embodiments, the housing has a length, measured between its front surface and its rear surface, greater than or equal to 10 mm, preferably greater than or equal to 30 mm.
[0029] In certain embodiments, the peripheral surface of the housing includes a shoulder delimiting two portions of the housing having different contours. This shoulder can act as a stop when fixing the bulkhead fitting into the bulkhead.
[0030] In some embodiments, the housing is configured to be fixed in the partition passage.
[0031] In some embodiments, the housing includes a fixing portion configured to cooperate with a fixing portion of the partition passage, the fixing portion preferably including at least one thread.
[0032] In certain embodiments, the alloy or metal of the housing has a coefficient of thermal expansion greater than 16 ppm / °C. Thus, the metal of the housing has a coefficient of thermal expansion relatively close to the other materials of the bulkhead penetration, which reduces the phenomena of differential expansion.
[0033] In some embodiments, the alloy or metal of the housing is stainless steel, in particular 304L or 316L. These alloys have a coefficient of thermal expansion of the order of 17 ppm / °C.
[0034] In certain embodiments, the alloy or metal of the housing is chosen from the group consisting of nickel and nickel-based alloys, in particular Ni-Fe, Ni-Fe-Cr or Ni-Fe-Cr-Mo. These alloys have a coefficient of thermal expansion of the order of 13 ppm / °C.
[0035] In certain embodiments, the bulkhead fitting includes at least one seal installed in said at least one peripheral groove in the peripheral surface of the housing. This seal is useful for reducing leakage flow in the bulkhead passage once the bulkhead fitting is fixed.
[0036] In certain embodiments, said at least one seal is an O-ring.
[0037] In certain embodiments, said at least one seal is an elastomeric seal.
[0038] In some embodiments, the partition penetration comprises two joints, installed each in a different peripheral groove of the peripheral surface of the housing, configured to be crushed between the housing and the internal surface of the passage.
[0039] In some embodiments, said at least one spindle has a diameter greater than or equal to 2 mm, preferably greater than or equal to 3 mm.
[0040] In some embodiments, said at least one pin is solid.
[0041] In certain embodiments, said at least one pin has a length greater than or equal to 30 mm, preferably greater than or equal to 50 mm.
[0042] In certain embodiments, said at least one pin protrudes at least 5 mm, preferably at least 10 mm, from each of the front and rear surfaces of the housing.
[0043] In certain embodiments, said at least one pin comprises, at at least one of its ends, a welding barrel or a crimping barrel.
[0044] In certain embodiments, said at least one pin is made of a copper-based alloy comprising beryllium, zinc, nickel, tin, and / or zirconium, optionally coated. It may, in particular, be a Cu-Be or Cu-Be-Co alloy. These alloys offer a good compromise between electrical, mechanical, and thermal properties. Furthermore, they have a coefficient of thermal expansion between 16 and 18 ppm / °C.
[0045] In certain embodiments, at least one pin is provided with a coating comprising at least one nickel-based layer at least 1 µm thick. Such a nickel layer promotes the adhesion of the glass sleeve to the pin, thereby improving the hermeticity of the bulkhead penetration, particularly at high pressure and high temperature.
[0046] In some embodiments, the thickness of the nickel-based layer is between 1 and 10 pm, preferably between 4 and 8 pm.
[0047] In some embodiments, the nickel-based layer comprises phosphorus, the content of which is preferably between 6 and 9% by mass.
[0048] In certain embodiments, the nickel-based layer of the coating on at least one pin is oxidized, at least on the surface. This further promotes the adhesion of the glass to the pin. In particular, glass composed of TZT or TZTC oxides has a strong affinity for the oxidized Ni-P alloy.
[0049] In some embodiments, the coating of at least one pin includes a copper-based underlayer at least 0.1 µm thick. Preferably, this underlayer is made of pure copper, with any unavoidable impurities. This copper underlayer promotes adhesion of the nickel layer to the pin, thereby further improving the seal of the bulkhead penetration.
[0050] In some embodiments, the thickness of the copper-based sublayer is between 0.2 and 1 pm.
[0051] In some embodiments, the bulkhead fitting comprises several pins, possibly at least ten and even at least twenty pins, each pin having a diameter greater than or equal to 1 mm, passing completely through the housing and protruding, on one side, on the front surface of the housing and, on the other side, on the rear surface of the housing, in which a separate glass sleeve surrounds each pin at least from the front surface to the rear surface of the case. It is thus possible to run several channels using a single bulkhead penetration, which simplifies the enclosure configuration and reduces the risk of leakage. Furthermore, the use of individual sleeves allows the characteristics, particularly the thickness, of each sleeve to be adapted to the specific requirements of the pin it surrounds.
[0052] In some embodiments, at least two pins have different diameters.
[0053] In certain embodiments, said at least one sleeve has a thickness greater than or equal to 0.3 mm, preferably greater than or equal to 0.7 mm, for example between 0.3 and 2.0 mm, preferably between 0.7 and 1.5 mm.
[0054] In some embodiments, the partition penetration comprises several sleeves having different thicknesses.
[0055] In some embodiments, the composition of the tellurium oxide-based glass comprises axOy oxide selected from the group consisting of Y2O3, CeO2, Sb2O3, Er2O3, La2O3, B2O3 and BaO, in particular from the group consisting of CeO2, Sb2O3, La2O3, Y2O3 and B2O3, more particularly CeO2.
[0056] In certain embodiments, the coefficient of thermal expansion of the tellurium oxide-based glass composition is between 11 and 22 ppm / °C, advantageously between 12 and 16 ppm / °C. This coefficient of thermal expansion is then close to or even lower than that of the spindle and the housing, which reduces the phenomenon of differential expansion and therefore increases the resistance of the bulkhead penetration at high temperature.
[0057] In certain embodiments, the tellurium oxide-based glass composition has a chemical durability of between 1.106 and 1.108 g / (cm2.min) determined by soxhlet at 95°C in demineralized water continuously renewed according to ISO16797 of April 2004.
[0058] In certain embodiments, the tellurium oxide-based glass composition has a glass transition temperature (Tg) below 500°C, advantageously between 250 and 400°C, and in particular between 300 and 380°C. A low glass transition temperature allows for a glass-to-metal seal at a lower temperature. However, a glass transition temperature (Tg) that is too low is not advantageous for the purposes of the present invention, as it is necessary to obtain a partition penetration with a temperature resistance up to 200°C. A glass transition temperature (Tg) that is too low for the glass leads to thinning of the glass at these operating temperatures, which can result in a loss of airtightness. The Tg is measured using a DSC (Differential Scanning Calorimetry): DSC setaram (DSC 131). The measurement is carried out from 20 to 580 °C with a ramp of 10 °C / min. The temperatures Tg and Tx are the onset temperatures (temperatures at the beginning of the phenomenon)..
[0059] In certain embodiments, said at least one sleeve is sealed between said at least one pin and the housing by glass / metal sealing.
[0060] In some embodiments, the bulkhead penetration has a helium leakage rate less than or equal to 10 11 mbar.l / s at 2000 bars and 200°C.
[0061] The present description also relates to a method for manufacturing a bulkhead fitting according to any one of the preceding embodiments, comprising the following successive steps a) supply of a metallic casing comprising a front surface, a rear surface and a peripheral surface; b) supply of a pin, made of copper or copper alloy, possibly coated, having a diameter greater than or equal to 1 mm; (c) supply of a cylindrical glass preform based on tellurium oxide having the composition as defined in any of the preceding embodiments, the cylindrical preform having a longitudinal passage; d) insertion of the pin into the longitudinal passage of the cylindrical preform and insertion of the assembly formed by the pin and the cylindrical preform into a through passage of the housing; e) maintaining contact between the spindle, the cylindrical preform and the housing using suitable tooling; f) heating the assembly formed by the spindle, the cylindrical preform and the housing to a temperature and for a time sufficient to achieve the glass-to-metal seal; and g) recovery of the sealed assembly.
[0062] Thanks to such a process, using glass preforms having a composition conforming to those described above, it is possible to obtain a bulkhead penetration as presented above, with the advantages and technical effects indicated. In particular, the use of such a glass-to-metal sealing step using glass preforms makes it possible to obtain very good adhesion of the glass to both the pin and the housing, and thus to achieve very good levels of airtightness, including at high pressure and high temperature.
[0063] In certain embodiments, the process further comprises, after step b) and before step d), the following step: b') pretreatment of the spindle resulting in the spindle being coated with at least one nickel-based layer at least 1 pm thick. As explained previously, such a nickel layer promotes the adhesion of the glass to the pin.
[0064] In some embodiments, step b') includes at least the following step: b2) nickel plating of the spindle. This step can be, in particular, an autocatalytic nickel plating step, preferably of the medium-phosphorus type. Autocatalytic nickel plating is preferred to electrolytic nickel plating because it allows for the easier production of thicker deposits.
[0065] In some embodiments, step b2) is carried out between 75 and 100°C, preferably between 85 and 90°C, for a period of between 15 and 30 minutes, preferably between 20 and 25 minutes.
[0066] In some embodiments, step b') comprises, after step b2), the following step: b3) steaming at at least 45°C for at least 3 minutes. This step allows at least part of the surface of the nickel layer to be oxidized. As explained previously, this further facilitates the attachment of the glass to the spindle.
[0067] In some embodiments, step b3) is carried out between 45 and 85°C, preferably between 55 and 75°C, for a duration of between 3 and 10 minutes, preferably between 3 and 7 minutes.
[0068] In some embodiments, step b') includes, before step b2), the following step: bl) copper plating of the spindle. This step can notably involve cyanide plating. As explained previously, such a copper layer promotes the adhesion of the nickel layer to the pin.
[0069] In some embodiments, step bl) is carried out between 50 and 70°C, preferably between 55 and 65°C, for a duration of between 0.5 and 2 minutes, preferably between 0.5 and 1.5 minutes.
[0070] In some embodiments, step bl) is carried out with a current density between 0.5 and 2 A / dm2, preferably between 0.7 and 1.3 A / dm2.
[0071] In some embodiments, step b') further includes at least one degreasing step, preferably cathodic and / or anodic, a pickling step and / or a rinsing step.
[0072] In certain embodiments, the process further comprises, after step b) and before step d), the following step: b*) mechanical alteration of all or part of the area which will be covered by the glass sleeve resulting in the surface of the spindle having a roughness Ra of at least 3.2 pm, preferably at least 6.3 pm. This step, carried out for example by sandblasting, increases the roughness of the surface of the spindle, which promotes the adhesion of the glass to the spindle.
[0073] In some embodiments, step b*) is carried out so as to obtain a roughness Ra between 3.2 and 50 pm, preferably between 6.3 and 30 pm. Such roughness allows good adhesion of the glass to the spindle, even when one or more coatings are deposited on the spindle after the mechanical alteration stage.
[0074] In certain embodiments, when the process includes a pretreatment step b') of the spindle, step b*) is carried out before step b'). This avoids altering the coating(s) deposited on the spindle.
[0075] In some embodiments, the process further comprises, after step g), the following step: h) installation of a seal in a peripheral groove on the peripheral surface of the housing.
[0076] In some embodiments, step b) includes the provision of several pins, step c) includes the provision of several preforms and step d) includes the insertion of each pin into the longitudinal passage of a separate preform and the insertion of the assembly into a single housing.
[0077] In some embodiments, the temperature of step f) is between 350 and 500°C, preferably between 400 and 500°C.
[0078] In some embodiments, the duration of step f) is between 30 and 80 minutes.
[0079] The aforementioned features and advantages, as well as others, will become apparent from the following detailed description, examples of bulkhead penetration implementation, and the proposed manufacturing process. This detailed description refers to the attached drawings. Brief description of the drawings
[0080] The attached drawings are schematic and are intended primarily to illustrate the principles of the exposition.
[0081] In these drawings, from one figure to another, identical elements (or parts of elements) are identified by the same reference numerals. In addition, elements (or parts of elements) belonging to different embodiments but having a similar function are identified in the figures by numerical reference numerals incremented by 100, 200, etc.
[0082] [Fig. 1] Fig. 1 is a cross-sectional view of a first example of a crossing of partition.
[0083] [Fig.2] [Fig.2] is a cross-sectional view of the bulkhead penetration of [Fig.1], fixed in a partition wall.
[0084] [Fig.3] Fig.3 is a cross-sectional view of an alternative embodiment of the first example of a partition wall penetration.
[0085] [Fig. 4] Fig. 4 is a cross-sectional view of another example of a bulkhead penetration including several pins. Description of the implementation methods
[0086] To make the explanation more concrete, examples of bulkhead penetrations and methods for manufacturing such bulkhead penetrations are described in detail below, with reference to the accompanying drawings. It should be noted that the invention is not limited to these examples.
[0087] Fig. 1 represents, in section along a vertical plane passing through its main axis A, a first example of a partition crossing 1. It includes a metal housing 10, a metal pin 20, a glass sleeve 30 and two elastomer seals 40.
[0088] The housing 10 has a shape of revolution about the principal axis A. It thus comprises a front surface 11, a rear surface 12, and a peripheral surface 13. The front surfaces 11 and rear surfaces 12 are planar and orthogonal to the principal axis A. The peripheral surface 13 comprises a main portion 13a, having the largest diameter, and a reduced portion 13b, having a diameter smaller than that of the main portion 13a; a radial shoulder 14 is thus formed at the junction between the main portion 13a and the reduced portion 13b. The peripheral surface 13 also comprises a projection portion 13c, with a diameter smaller than that of the main portion 13a; a radial shoulder 15 is thus formed at the junction between the main portion 13a and the projection portion 13c.
[0089] The peripheral surface 13 has, at the level of its main portion 13a, at least one peripheral groove 16, here two in number, circumferential and extending 360° along the peripheral surface 13.
[0090] The peripheral surface 13 also has, at the level of its reduced portion 13b, a thread 17. The peripheral surface 13 further has, at the level of its projection portion 13c, a circumferential bead 18.
[0091] The metal casing 10 further includes a longitudinal passage 19 extending axially, along the main axis A, from the front surface 11 to the rear surface 12, the longitudinal passage 19 thus opening out on each side of the partition penetration 1.
[0092] In this example, the housing 10 measures 3.7 cm axially between its front surface 11 and rear surface 12; the diameter of its main portion 13a measures 1 cm.
[0093] The metal pin 20 takes the form of a straight and solid rod extending axially along the longitudinal passage 19 of the housing 10. The metal pin 20 protrudes on each side of the housing 10. Each end of the pin 20 can be rounded.
[0094] In this example, the diameter of the pin 20 is 1.6 mm; the length of the pin is 5.7 cm; it protrudes 1 cm on each side from the front surface 11 and the rear surface 12.
[0095] The glass sleeve 30 is provided around the metal pin 20 so as to electrically isolate the latter from the metal housing 10. The glass sleeve extends from the front surface 11 of the housing 10 to its rear surface 12, thus having the same length as the housing 10.
[0096] In this example, the length of the glass sleeve 30 is thus equal to 3.7 cm; its thickness is equal to 0.9 mm.
[0097] Finally, the partition passage 1 includes two elastomeric O-rings 40, each O-ring 40 being installed in a peripheral groove 16 of the housing 10.
[0098] Fig. 2 then represents the same partition crossing 1 installed and fixed in a partition 90. This partition 90 has a longitudinal passage 91 completely traversing the partition 90 between its front surface 92 and its rear surface 93.
[0099] The passage 91 has a main portion 91a, of larger diameter, and a reduced portion 91b, of smaller diameter than the main portion 91a; a radial shoulder 94 is thus formed at the junction between the main portion 91a and the reduced portion 91b. The reduced portion 91b further includes a threaded hole 95.
[0100] The diameter of the main portion 91a of the passage 91 is adjusted to the diameter of the main portion 13a of the housing 10, and the diameter of the reduced portion 91b of the passage 91 is adjusted to the diameter of the reduced portion 13b of the housing 10. Thus, the bulkhead fitting 1 can be inserted into the passage 91 of the bulkhead by screwing the thread 17 of the housing 10 into the threaded hole 95 of the passage until the shoulder 14 of the housing is abutted against the shoulder 94 of the passage 91. The sealing of the assembly is achieved by adjusting the diameters and by compressing the O-rings 40 between the bottom of the peripheral grooves 16 of the housing 10 and the internal surface of the passage 91 of the bulkhead 90.
[0101] Figure 3 shows a partition wall penetration 101 according to an alternative embodiment. In this alternative embodiment, the metal housing 110 and the glass sleeve 130 are unchanged. However, the metal pin 120 is configured differently.
[0102] Indeed, in this variant, the metal pin 120 includes, at one of its ends, in this case its rear end, a welding barrel 121 in place of a simple rod.
[0103] Fig. 4 represents another example of a bulkhead penetration 201 comprising several metal pins 220.
[0104] In this other example, the housing 210 is configured similarly to the housing 10 of the first example, except that its diameter is larger to accommodate a greater number of pins 220. The metal housing 210 thus comprises a front surface 211, a rear surface 212, and a peripheral surface 213 comprising a peripheral groove 216, a shoulder 214, and a thread 217. On the other hand, the housing 210 includes several longitudinal passages 219, all parallel, extending along the main axis A from the front face 211 to the rear face 212.
[0105] Each metal pin 220 is analogous to the metal pin 20 of the first example, except that their diameters may vary, both in relation to the first example and among themselves. Thus, in the example shown in [Fig. 4], the central pin is thicker than the peripheral pins. Although not shown, at least some pins 220 may of course include a solder barrel analogous to that of [Fig. 3].
[0106] Each metal pin 220 is further fitted with an individual glass sleeve 230. Each glass sleeve 230 is analogous to that of the first example, except that their thicknesses may vary, both in relation to the first example and among themselves. Thus, in the example shown in [Fig. 4], the sleeve of the central pin is thicker than the sleeves of the peripheral pins.
[0107] Examples of manufacturing processes for such bulkhead penetrations will now be described.
[0108] Example 1 - In this first example, corresponding to the example shown in [Fig.1], the housing 10 is made of 304L stainless steel (Fe-74%, Cr-18%, Ni-8%) having the reference UNS S30403.
[0109] The pin 20 is obtained from a 1.6 mm pin made of copper and beryllium alloy (Cu-97.5%, Be-2.0%, Co-0.5%), generally known as Cu-Be and under the reference UNS C17200. This pin is then subjected to the following pretreatment.
[0110] The spindle is first subjected to a sandblasting operation over all or part of the area that will be covered by the glass sleeve 30. This sandblasting step mechanically alters the surface condition of the spindle to obtain a roughness Ra greater than 6.3 pm. This sandblasting is followed by a double rinsing.
[0111] The spindle is then subjected to cathodic degreasing, carried out at 40°C, for 2 minutes, and with a current density of 1 A / dm2, followed by anodic degreasing, carried out at 40°C, for 1 minute, and with a current density of 1 A / dm2. These degreasings are followed by a double rinse.
[0112] The spindle is then subjected to METEX M629 pickling, carried out at 30°C for 1 minute. This pickling is followed by a double rinse.
[0113] The pin is then subjected to cyanide plating at 60°C for 1 minute, with a current density of 1 A / dm². This cyanide plating step provides the Cu-Be pin with a surface layer of pure copper with a thickness between 0.2 and 1.0 µm. This step is followed by a double rinse.
[0114] The copper-plated pin is then subjected to MP nickel plating, carried out at 88°C, for 22 minutes. This MP (medium phosphorus) nickel plating step, also called chemical or autocatalytic nickel plating, applies a surface layer of nickel-phosphorus alloy to the spindle, which adheres well to the pure copper sublayer. This nickel-phosphorus alloy layer has a phosphorus content of between 6 and 9% by mass and a thickness of at least 6 µm. This step is followed by a double rinse.
[0115] The pin, thus copper-plated and then nickel-plated, is subsequently baked at 65°C for 5 minutes. This baking step allows for controlled oxidation of the Ni-P alloy layer, which will promote the subsequent adhesion of the glass of the sleeve 30.
[0116] Thus, at the end of these pretreatment steps, a pin 20 is obtained ready to be mounted in the housing 10.
[0117] A cylindrical glass preform is then provided, this cylindrical preform being intended to form the glass sleeve 30. This glass has a so-called TZT composition including tellurium oxide, zinc oxide and titanium oxide. More precisely, in this first example, the composition of the glass is as follows: TeO2 -65%, ZnO -30%, TiO2 -5% (in molar percentages).
[0118] The cylindrical preform is then engaged around the spindle 20 and the assembly is inserted into the longitudinal passage 19 of the housing 10. Then, to perform the glass-to-metal seals, the metal-glass preform assembly is held in place using suitable tooling. Heating is carried out in an oven, without a protected atmosphere, at 420°C for 45 minutes.
[0119] The partition penetration 1 thus obtained then exhibits a mechanical resistance to pressure of 2000 bar and a thermal resistance to temperature of 280°C.
[0120] The insulation resistance is measured using a megohmmeter under 500V DC. The insulation resistances obtained reach the detection limit of the device (20 Gohm).
[0121] Helium tightness is measured using a helium leak detector (Adixen ASM 142) according to MIL-STD-883, conditions A4. The resulting bulkhead penetration exhibits a level of tightness expressed as a helium leak rate of less than 10 11 mbar.l / s according to this measurement method defined by the Mil-STD-883 standard of April 2016.
[0122] The bulkhead fitting retains the same level of airtightness after a so-called thermal shock test defined in the Mil-DTL-38999 standard of February 2015 which consists of subjecting the bulkhead fitting to 10 cycles of passing from cold water at 4°C to hot water at 90°C in less than 5 seconds for each pass.
[0123] In particular, comparative tests were carried out to compare the present example The test was performed using a similar configuration in which the pin is supplied and sealed without the pretreatment step. Among these tests, the pumping time required to reach a pressure below 300 mbar in the chamber, the wall of which includes the bulkhead penetration to be tested, was measured. Generally, the glass-to-metal seal is considered good and sufficiently airtight when this pumping time is less than 15 seconds.
[0124] During these comparative tests, more than 30% of the wall penetrations including a pin that had not undergone the pretreatment of Example 1 exhibited pumping times exceeding 15 seconds. Conversely, this percentage was reduced to practically 0 for wall penetrations where the pin had undergone this pretreatment.
[0125] Moreover, all the materials chosen have the additional advantage of not containing any substance or chemical element subject to the restriction stipulated by the European RoHS (Restriction of Hazardous Substances) directive.
[0126] Other embodiments have been tested and are presented below. Only the differences from Example 1 are shown.
[0127] Example 2 - In a second example, the components are as follows: - 1 304L stainless steel case (Fe-74%, Cr-18%, Ni-8%) referenced in UNS S30403; - 1 pin with a diameter of 1.6 mm made of Cl7200 alloy, having received the pretreatment of Example 1; and - 1 TZTC glass insulator preform with a nominal composition in molar percentages (TeO2-65%, ZnO-27%, TiO2-5%, CeO2-3%).
[0128] The bulkhead penetration is obtained by a glass / metal sealing operation at 420°C for 45 minutes, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead penetration exhibits a level of airtightness below 1011 mbar.l / s and retains the same airtightness after the same thermal shock test.
[0129] Example 3 - In a third example, the components are as follows: - 1 304L stainless steel case (Fe-74%, Cr-18%, Ni-8%) referenced in UNS S30403; - 1 pin with a diameter of 1.6 mm made of C23000 alloy having received the pretreatment of Example 1; - 1 TZTC glass insulator preform with a nominal composition in molar percentages (TeO2-65%, ZnO-27%, TiO2-5%, CeO2-3%).
[0130] The bulkhead penetration is achieved by a glass / metal sealing operation at 420°C for 45 minutes, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead penetration exhibits a level of airtightness below 10 11 mbar.l / s and retains the same airtightness after the same thermal shock test.
[0131] Example 4 - In a fourth example, the components are as follows: - 1 Ni-Fe alloy case called Invar with a nominal composition (Ni-36%, Fe-64%) referenced in UNS K93600; - 1 pin with a diameter of 1.6 mm made of Cl7200 alloy, having received the pretreatment of Example 1; and - 1 TZTC glass insulation preform with a nominal composition in molar percentages (TeO2-65%, ZnO-20%, TiO2-7%, CeO2-8%).
[0132] The bulkhead penetration is achieved by a glass / metal sealing process at 430°C for 60 minutes, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead penetration exhibits a level of airtightness below 1011 mbar.l / s and retains the same airtightness after the same thermal shock test.
[0133] Example 5 - In a fifth example, the components are as follows: - 1 Ni-Cr-Fe alloy case with a nominal composition (Ni-76%, Cr-16%, Fe-8%) referenced in UNS N06600; - 1 pin with a diameter of 1.6 mm made of Cl7200 alloy, having received the pretreatment of Example 1; and - 1 TZTC glass insulation preform with a nominal composition in molar percentages (TeO2-60%, ZnO-20%, TiO2-10%, CeO2-10%).
[0134] The bulkhead penetration is obtained by a glass / metal sealing process at 400°C for 1 hour, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead penetration exhibits a level of airtightness below 10¹¹ mbar.l / s and retains the same airtightness after the same thermal shock test.
[0135] Example 6 - In a sixth example, the components are as follows: - 1 Ni-Cr-Fe alloy case with a nominal composition (Ni-64%, Cr-15%, Fe-5%, Mo-16%) referenced in UNS N10276; - 1 pin with a diameter of 1.6 mm made of Cl7200 alloy, having received the pretreatment of Example 1; and - 1 TZTC glass insulator preform with a nominal composition in molar percentages (TeO2-60%, ZnO-20%, TiO2-5%, CeO2-15%).
[0136] The bulkhead penetration is obtained by a glass / metal sealing process at 400°C for 1 hour, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead penetration exhibits a level of airtightness below 10¹¹ mbar.l / s and retains the same airtightness after the same thermal shock test.
[0137] Example 7 - In a seventh example, the components are as follows: - 1 316L stainless steel case with nominal mass composition (Fe-72%, Cr-16%, Ni-10%, Mo-2%) referenced in UNS S31603; - 1 pin with a diameter of 4 mm made of C17200 alloy, having received the pretreatment of Example 1; and - 1 TZTC glass insulation preform with a nominal composition in molar percentages (TeO2-70%, ZnO-15%, TiO2-5%, CeO2-10%).
[0138] The bulkhead penetration is obtained by a glass / metal sealing operation at 420°C for 45 minutes, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead penetration exhibits a level of airtightness below 10¹¹ mbar.l / s and retains the same airtightness after the same thermal shock test.
[0139] Example 8 - In an eighth example, the components are as follows: - 1 case made of 304L stainless steel; - 3 pins with a diameter of 1.6 mm made of alloy that has received the pretreatment of the Example 1; and - 3 TZTC glass insulation preforms with a nominal composition in molar percentages (TeO2-65%, ZnO-27%, TiO2-5%, CeO2-3%).
[0140] The bulkhead fitting, thus including three pins in a single housing, is obtained by a glass / metal sealing operation at 420°C for 45 minutes, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead fitting exhibits a level of airtightness below 1011 mbar.l / s and retains the same airtightness after the same thermal shock test.
[0141] Example 9 - In a ninth example, the components are as follows: - 1 Ni-Cr-Fe alloy case referenced in UNS N06600; - 3 pins with a diameter of 1.6 mm and 2 pins with a diameter of 3 mm, all 5 made of C17200 alloy having received the pretreatment of Example 1; and - 5 TZTC glass insulation preforms with a nominal composition in molar percentages (TeO2-65%, ZnO-27%, TiO2-5%, CeO2-3%).
[0142] The bulkhead penetration, comprising three small-diameter pins and two larger-diameter pins, is obtained by a glass / metal sealing operation at 420°C for 45 minutes, exhibiting mechanical resistance to a pressure of 2000 bar and thermal resistance to a temperature of 300°C. The resulting bulkhead penetration exhibits a level of airtightness below 10¹¹ mbar.l / s and retains the same airtightness after the same thermal shock test.
[0143] Although the present invention has been described with reference to specific embodiments, it is evident that modifications and changes may These examples must be performed without departing from the general scope of the invention as defined by the claims. In particular, individual features of the various embodiments illustrated / mentioned may be combined in additional embodiments. Therefore, the description and drawings should be considered illustrative rather than restrictive.
[0144] It is also evident that all the characteristics described with reference to a process are transposable, alone or in combination, to a device, and conversely, all the characteristics described with reference to a device are transposable, alone or in combination, to a process.
Claims
Claims
1. Bulkhead passage, comprising a metallic housing (10), comprising a front surface (11), a rear surface (12) and a peripheral surface (13), configured to be engaged in a through passage (91) of a partition (90), the peripheral surface (13) of the housing (10) comprising at least one peripheral groove (16) configured to receive a seal (40) intended to be crushed between the housing (10) and the internal surface of the passage (91), at least one metallic pin (20), having a diameter greater than or equal to 1 mm, passing completely through the housing (10) and projecting, on one side, on the front surface (11) of the housing (10) and, on the other side, on the rear surface (12) of the housing (10), and at least one sleeve (30), cylindrical and made of glass, surrounding said at least one pin (20) at least from the front surface (11) to the rear surface (12) of the housing (10) so as to electrically insulate said at least one pin (20) from the housing (10), wherein said at least one pin (20) is made of copper or copper alloy, possibly coated, in which the material of the sleeve (30) is a tellurium oxide-based glass having the composition consisting of, in molar percentage: - from 50 to 80% of TeO2, advantageously from 50 to 70%; - from 8 to 40% of ZnO, advantageously from 15 to 35%; - from 2 to 25% of TiO2, advantageously from 2 to 10% - from 0 to 20% of an oxide axOy, advantageously from 2 to 10%, a being an element chosen from the group consisting of Ba, Ce, Er, Sb, Y, La and B, x being an integer equal to 1 or 2 and y an integer equal to 1, 2 or 3; - possibly ZnF2 in a content of 2 to 10%, advantageously 3 to 8%, - and the inevitable impurities, provided that ZnF2 is present when axOy is BaO, said composition being essentially free of lead oxide, sodium oxide, potassium oxide and vanadium oxide.
2. Partition bushing according to claim 1, in which the peripheral surface (13) of the housing (10) comprises a shoulder (14) delimiting two housing portions (13a, 13b) having different contours, and wherein the housing (10) comprises a fixing portion (17) configured to cooperate with a fixing portion (95) of the passage (91) of the partition (90), the fixing portion preferably comprising at least one thread (17).
3. A bulkhead fitting according to claim 1 or 2, wherein the alloy or metal of the housing (10) is selected from the group consisting of stainless steel, nickel and nickel-based alloys.
4. A bulkhead bushing according to any one of claims 1 to 3, wherein said at least one pin (20) has a length greater than or equal to 30 mm, preferably greater than or equal to 50 mm, and wherein said at least one pin (20) projects at least 5 mm, preferably at least 10 mm, on each of the front (11) and rear (12) surfaces of the housing (10).
5. Bulkhead fitting according to any one of claims 1 to 4, wherein said at least one pin (120) comprises, at at least one of its ends, a welding barrel (121) or a crimping barrel.
6. A bulkhead feedthrough according to any one of claims 1 to 5, wherein at least one pin (20) is provided with a coating comprising at least one copper-based underlayer of at least 0.1 pm thickness, and one nickel-based layer of at least 1 pm thickness.
7. A bulkhead feedthrough according to any one of claims 1 to 6, comprising a plurality of pins (220), each pin (220) having a diameter greater than or equal to 1 mm, passing right through the housing (210) and projecting, on one side, on the front surface (211) of the housing (210) and, on the other side, on the rear surface (212) of the housing (210), and wherein a separate glass sleeve (230) surrounds each pin (220) at least from the front surface (211) to the rear surface (212) of the housing (210).
8. A bulkhead according to any one of claims 1 to 7, wherein the composition of the tellurium oxide-based glass comprises oxide axOy selected from the group consisting of Y2O3, CeO2, Sb2O3, Er2O3, La2O3jB2O3 and BaO, in particular from the group consisting of CeO2, Sb2O3, La2O3 Y2O3 and B2O3, more particularly it is CeO2.
9. A method of manufacturing a bulkhead fitting according to any one of claims 1 to 8, comprising the successive steps following a) providing a housing (10), metallic, comprising a front surface (11), a rear surface (12) and a peripheral surface (13); b) providing a pin (20), made of copper or copper alloy, optionally coated, having a diameter greater than or equal to 1 mm; c) providing a cylindrical preform of glass based on tellurium oxide having the composition as defined in any one of claims 1 to 8, the cylindrical preform having a longitudinal passage; d) inserting the pin (20) into the longitudinal passage of the cylindrical preform and inserting the assembly formed by the pin (20) and the cylindrical preform into a through passage (19) of the housing (10); e) maintaining contact between the pin (20), the cylindrical preform and the housing (10) using suitable tooling;f) heating the assembly formed by the pin (20), the cylindrical preform and the housing (10) to a temperature and for a time sufficient to obtain the glass-metal seal; and g) recovering the assembly (1) thus sealed.;
10. Method according to claim 9, further comprising, after step b) and before step d), the following step: b') pretreatment of the pin (20) resulting in providing the pin (20) with a coating comprising at least one nickel-based layer at least 1 μm thick, this step b') comprising at least the following steps: bl) copper plating of the pin, then b2) nickel plating of the pin.
11. Method according to claim 10, in which step b') comprises, after step b2), the following step: b3) baking at at least 45°C for at least 3 minutes.
12. Method according to any one of claims 9 to 11, further comprising, after step b) and before step d), the following step: b*) mechanical alteration of all or part of the area which will be covered by the glass sleeve resulting in providing the surface of the pin with a roughness Ra at least equal to 3.2 pm, preferably at least equal to 6.3 pm.
Citation Information
Patent Citations
Hermetic electrical connector
US7442081B2
Electrical connectors and sensors for use in high temperature, high pressure oil and gas wells
US7901247B2
Glass parts for sealed connector
EP3594191A1
Glass composition for micro-d connector sealing
US20190337836A1
Hybrid glass-sealed electrical connectors
US7364451B2