Primary electrochemical element of the Li / CFx type

The Li/CFx type primary electrochemical element with a composite block positive electrode and central current collector addresses self-discharge and internal resistance issues, improving lifespan and performance.

FR3147664A1Pending Publication Date: 2024-10-11SAFT GRP SA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
FR2023003433
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing Li/CFx type primary electrochemical elements suffer from high self-discharge rates and internal resistance due to the peripheral arrangement of the current collector, which complicates manufacturing and leads to premature failure.

Method used

A composite block positive electrode made of CFx and polymers, with a central current collector, minimizes self-discharge and internal resistance by optimizing the electrode structure and manufacturing process.

Benefits of technology

The new electrode design significantly reduces self-discharge and internal resistance, enhancing the element's lifespan and performance in connected objects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

An electrochemical element (1) comprising: - a container (2), - a negative electrode (3) comprising a lithium foil or a lithium-based alloy covering at least partially one inner face of the container, - a positive electrode comprising a block (4) made of a mixture comprising one or more compounds of formula CFx with 0
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Primary electrochemical element of the Li / CFx type Technical field of the invention

[0001] The technical field of the present invention is that of primary, i.e., non-rechargeable, electrochemical elements comprising a negative electrode (anode) made of lithium metal or a lithium-based alloy and a positive electrode (cathode) whose active material is based on a CFx-type compound. Background of the invention

[0002] Primary electrochemical elements of the Li / CFx type are known. They comprise a positive electrode containing an active material which is a fluorinated carbon of formula CFx where 0 <x<l,5 et une électrode négative contenant une matière active qui est du lithium métallique ou un alliage de lithium.

[0003] During the discharge of the element, CFx at the positive electrode is transformed into carbon according to the reaction: CFx + xLi -> xLiF + xC At the negative electrode, an oxidation reaction occurs between lithium metal and lithium ions.

[0004] Such electrochemical elements are typically constructed by creating a spiral electrode arrangement. A spiral electrode arrangement is defined as an arrangement obtained by a process comprising the steps of: - provision of a negative electrode made of a lithium sheet or lithium alloy, - provision of a positive electrode comprising a metallic foil coated on at least one of its two faces with an active material composition comprising CFx, one or more polymers acting as a binder, and possibly one or more electronically conductive compounds, - superposition of the positive electrode, a separator and the negative electrode, - winding of the superposition of the positive electrode, the separator and the negative electrode to constitute an electrochemical beam.

[0005] The electrochemical beam is introduced into the container of the electrochemical element. It is then impregnated with an electrolyte. The electrolyte consists of one or more solvents in which one or more lithium salts and one or more additives are dissolved. The organic solvent may be propylene carbonate or dimethoxyethane. The salt used may be chosen from lithium perchlorate (LiCl₂O₄), lithium hexafluoroarsenate (LiAsF₆), lithium hexafluorophosphate (LiPF₆), and the lithium tetrafluoroborate LiBF4.

[0006] US Patent 6,451,483 describes a primary electrochemical element of the Li-CFx type with a spiral electrode arrangement. The positive active material composition consists of a mixture of CFx, a conductive compound, and a binder that has been highly compressed to reduce its volume. Conversely, reducing the volume of the positive electrode allows for an increase in the volume of the negative electrode and maintains a 3% excess of lithium at the negative electrode relative to the amount of positive active material. In this document, the process for preparing the positive electrode does not include a heat treatment step for the active material composition. The absence of heat treatment prevents the long-term mechanical strengthening of the positive electrode and improves the accessibility of the three-dimensional porous network to the discharge products.This results in two consequences: a loss of integrity of the positive active material over time or in case of shocks, and a premature end of life of the element because certain areas of the positive active material cannot be reached by lithium ions.

[0007] US patent 2013 / 0236756 describes a primary electrochemical element comprising a container containing a positive electrode, a negative lithium electrode, a separator interposed between the positive and negative electrodes, and an electrolyte. The positive electrode is surrounded by a current collector consisting of a metallic grid. The positioning of the current collector at the periphery of the positive electrode necessitates the use of a metallic tab to electrically connect the current collector to the current output terminal, which is centrally located on the lid. This peripheral arrangement of the current collector complicates the manufacturing steps of the element.Indeed, the use of the metal strip necessitates two solder points: one between the current collector and one end of the metal strip, and the other between the positive output terminal and the other end of the metal strip. Furthermore, the metal strip is folded back on itself to form a horizontal "U," which lengthens the current path between the current collector and the positive output terminal. This lengthened current path increases the internal resistance of the element and limits the potential for optimizing its performance. Moreover, the placement of the current collector on the periphery of the positive active material leads to areas of inconsistent current flow within the active material. As mentioned above, during the element's discharge, carbon and LiF are formed.LiF is an electrically insulating compound that will gradually clog the porosity, particularly at the periphery of the electrode. The core of the positive active material will not function fully because LiF insulates the surface of the positive electrode, resulting in a loss. of the element's capacity.

[0008] Li / CFx electrochemical elements are typically used in connected devices or in meters, such as gas or electricity meters. They are used, for example, to power a display that provides a user with meter readings. In this type of application, the element does not discharge any current for virtually the entire time it is installed in the meter. It is only when the user needs to know the information recorded by the meter that the element discharges a brief burst of current. Despite this very low utilization rate, it has nevertheless been observed that the element's state of charge decreases due to self-discharge of the anode. The self-discharge current is low, but over a period of 20 years, it can represent an amount of electricity equal to more than half the amount of active material initially present in the negative electrode.We are therefore seeking to provide a Li / CFx type element with a lower self-discharge current. Summary of the invention

[0009] The object of the present invention is an electrochemical element comprising: - a container, - a negative electrode comprising a lithium foil or a lithium-based alloy covering at least partially an inner face of the container, - a positive electrode comprising a block made of a mixture comprising one or more compounds of formula CFX with 0 <x<l,5 et un ou plusieurs polymères, - collecteur de courant l’électrode positive, le étant soit au moins partiellement inséré dans bloc, disposé contact d’une paroi ouverture pratiquée à travers - a separator placed between the positive electrode and the negative electrode, and - an electrolyte.

[0010] The applicant discovered that it was possible to reduce the self-discharge rate of a primary electrochemical element of the Li / CFx type by using a cathode of this element in the form of a composite block made up of a mixture comprising CFx and one or more binding polymers.

[0011] According to one embodiment, the mixture further comprises MnO2.

[0012] According to one embodiment, the container is cylindrical and the lithium foil or of a lithium-based alloy occupies at least 75%, preferably at least 95%, of the circumference of the container.

[0013] According to one embodiment, 0.2 <x<l.

[0014] According to one embodiment, the electrochemical element further comprises a a lid having a wall through which a metal tube is fixed, the the metal tube being electrically insulated from the cover by an electrically insulating insert, the metal tube having a through opening, a first part of the current collector being inserted into the through opening of the metal tube, a second part of the current collector being inserted into the composite block, one end of the current collector being welded to the metal tube thus making the element watertight.

[0015] According to one embodiment, the block is a cylindrical column and the opening made through the block is a through opening in the direction of the length of the cylindrical column.

[0016] According to one embodiment, the electrochemical element further comprises a cover provided with a glass-to-metal through-hole, a first part of the current collector being integral with the glass-to-metal through-hole, a second part of the current collector being disposed in contact with the wall of the through-hole of the block.

[0017] According to one embodiment, the block has a porosity ranging from 30 to 90%.

[0018] According to one embodiment, the separator comprises glass fibers or cellulose fibers or para-aramid fibers.

[0019] According to one embodiment, the electrolyte comprises a solvent selected from cyclic or linear carbonates and lactones.

[0020] According to one embodiment, said one or more polymers are chosen from a homopolymer or copolymer of polyvinylidene fluoride (PVDF) grafted or not, a butadiene-acrylonitrile (NBR) copolymer optionally hydrogenated or carboxylated and a mixture of these.

[0021] According to one embodiment, said one or more polymers are selected from polytetrafluoroethylene (PTFE), carboxymethylcellulose (CMC), a styrene butadiene block copolymer (SBR), a polyvinyl alcohol (PVA) and a mixture thereof.

[0022] According to one embodiment, the positive electrode further contains one or more electronically conductive compounds.

[0023] The invention also relates to a method for manufacturing a positive electrode for an electrochemical element Li / CFx, which method comprises the steps of: a) making available a mixture comprising one or more solvents, one or more compounds of formula CFx with 0 <x<l,5 et un ou plusieurs polymères, b) shaping the mixture by extrusion to form grains, c) evaporation of the solvent(s) by heating the grains, d) heat treatment of the grains at a temperature at least equal to the glass transition temperature of the polymer with the highest glass transition temperature, e) compression of the grains in a mold to form a block made up of the agglomerated grains, f) installation of a current collector on the block, the current collector being either at least partially inserted into the block, or at least partially disposed in contact with a wall of an opening made through the block.

[0024] The invention also relates to a method for manufacturing a positive electrode for an electrochemical element Li / CFx, which method comprises the steps of: a) making available a mixture comprising one or more solvents, one or more compounds of formula CFx with 0 <x<l,5 et un ou plusieurs polymères, b) mise en forme du mélange par extrusion pour former bloc, c) évaporation des solvants chauffage d) heat treatment of the block at a temperature at least equal to the glass transition temperature of the polymer with the highest glass transition temperature, e) shaping the block by cutting the block to the desired dimensions, the process being devoid of a block compression step, f) installation of a current collector on the block, the current collector being either at least partially inserted into the block, or at least partially disposed in contact with a wall of an opening made through the block. Brief description of the figures

[0025] Embodiments of the invention are described below in more detail with reference to the figures below.

[0026] [Fig.1] is a longitudinal section of an electrochemical element according to a first embodiment of the invention.

[0027] [Fig.2] is a longitudinal section of an electrochemical element according to a second embodiment of the invention.

[0028] [Fig.3] represents the discharge curves of three Li / CFx elements comprising a positive electrode which is a composite block.

[0029] Description of embodiments of the invention

[0030] The general structure of the element will now be described in two preferred embodiments. [Fig. 1] schematically shows the structure of an electrochemical element according to a first embodiment in which the composite block consists of grains agglomerated by compression and the current collector is a metal rod comparable to a nail.

[0031] The element (1) comprises a container (2), for example cylindrical, containing: - a sheet (3) of lithium or lithium alloy plated against the inner wall of the container and serving as negative electrode, - a composite block (4) constituting the positive electrode and which is a mixture comprising one or more compounds of formula CFx and one or more polymers, - a separator (5) between the block (4) and the lithium or lithium alloy foil (3), - an electrolyte (6). The opening of the container is sealed by a lid (7). A nail-shaped metal rod (11) serves as the current collector for the positive electrode. The lower part of the nail is inserted into the composite block. The upper part of the rod is inserted into a through-hole in a metal tube (12). The metal tube (12) serves as the positive current output terminal. It also serves as a filling port for introducing electrolyte into the element. The metal tube is sealed by welding the top of the metal rod to the top of the metal tube, forming a weld bead (16) that resembles a nail head. Electrical insulation between the metal rod (11) and the lid is achieved by means of an insulating insert (13), usually made of glass. The bottom (8) of the container and the lid (7) are at the potential of the negative electrode. A first electrical insulating seal (10) isolates the composite block (4) from the bottom of the container.A second electrically insulating seal (9) is located on the upper edge of the composite block. It prevents contact between the upper edge of the composite block and the inner face of the lid, which is electrically connected to the negative electrode. Such contact could occur if the composite block expands excessively or moves upwards. The volume above the composite block absorbs the volume increase due to its swelling during discharge. This swelling creates porosity, hence the need for an excess of electrolyte (6) to gradually fill the resulting porosity.

[0032] Figure 2 schematically shows the structure of an electrochemical element according to a second embodiment in which the composite block is formed directly by extrusion of the composite mixture, without a subsequent step of compressing the block, and the current collector is a metal rod called a "pin." Reference numbers 1 to 11 designate the same components as those used for Figure 1. The positive electrode consists of a single block through which, for example, three holes pass from one end of the block to the other. The number and arrangement of the through holes are not limited to those of Figure 2. The metal rod (11) passes through the central hole. Compared to Figure 1, the metal rod has a larger cross-section relative to its length. Typical dimensions of the cross-section of the pin and the nail are given below in the detailed description of each of the element's components.The upper end of the pin is located outside the element and has an enlarged part (12) serving as an exit terminal of . The lid is equipped with a glass-to-metal (GTM) feedthrough that electrically isolates the pin (11) from the lid (7). The pin is fixed to the glass-to-metal feedthrough (13). Since the junction between the pin and the glass-to-metal feedthrough is sealed, a means of filling the element with electrolyte is necessary. To this end, an opening (14) is provided through the lid (7) for introducing electrolyte into the element. A ball (15) is welded onto the opening (14).

[0033] It is understood that the embodiment described in [Fig. 1] can be modified by using a block preformed directly by extrusion instead of using a block obtained by grain compression. Similarly, the embodiment described in [Fig. 2] can be modified by using a block obtained by grain compression instead of using a block preformed directly by extrusion.

[0034] Generally, in the invention, the current collector of the positive electrode is directly connected to the positive current output terminal. This minimizes the internal resistance of the element and simplifies the manufacturing process, as it eliminates the need for welding between the current collector and the positive current output terminal. Furthermore, the current collector is located in the central region of the composite block, rather than at its periphery. The composite block is generally columnar in shape. Preferably, the current collector is centrally located, meaning its longitudinal axis coincides with the longitudinal axis of the column. Positive electrode

[0035] The positive electrode is a composite block comprising: - one or more active substances, one of which is a fluorinated carbon of formula CFx with 0 <x<l,5, et - one or more polymers acting as a binder. This composite block can be obtained by two processes, which will be described below.

[0036] The index x in the CFx formula preferably ranges from 0.2 to 1. CFx can be combined with one or more other active materials, which may be selected from MnO2FeS2, V2O5, I2, Bi2O3, Bi2Pb2O5, CuCl2, CuF2, CuO, Cu4O(PO4)2, CuS, FeS, MoO3, Ni3S2, AgCl, Ag2 CrO4, V2O5, SVO, MO6S8, or a mixture thereof. Preferably, it is MnO2.

[0037] In one embodiment, the active material composition does not include any active materials other than CFx. Alternatively, two or more CFx materials with different fluorination levels x can be mixed to increase the electronic conductivity of the cathode.

[0038] Since CFx is a poor electronic conductor, it can be associated with one or more electronically conductive compounds, such as graphite, carbon black, acetylene black, soot, graphene, carbon fibers, carbon nanotubes or a mixture thereof.

[0039] Said one or more polymers acting as a binder can be chosen from a homopolymer or copolymer of polyvinylidene fluoride (PVDF) grafted or not, a butadiene-acrylonitrile copolymer optionally hydrogenated or carboxylated, polytetrafluoroethylene (PTFE), carboxymethylcellulose (CMC), a styrene-butadiene block copolymer (SBR), a polyvinyl alcohol (PVA) and a mixture thereof.

[0040] A typical composition of the composite block comprises: - 80 to 98% by mass of CFx, - 0 to 10% by mass of electronic conductive compound(s), - 1 to 10% by mass of polymer(s).

[0041] A typical preferred composition of the composite block comprises: - 85 to 90% by mass of CFx, - 1 to 10% by mass of electronic conductive compound(s), - 1 to 5% by mass of polymer(s).

[0042] Electrical conduction from the composite block to the positive current output terminal is achieved via a current collector in the form of a metal rod, for example, made of nickel, stainless steel, or aluminum. Preferably, this metal rod is straight and is electrically connected directly to the current output terminal, thus minimizing the internal resistance of the element.

[0043] The metal rod may have a cross-section of circular, rectangular or square shape or any other shape.

[0044] The metal rod may have a cross-section with a diameter ranging from 0.50 to 1 mm, preferably from 0.70 to 0.80 mm. The metal rod is comparable to a nail. It is inserted into the opening of the element's filling tube. A weld, for example by laser, creates a seal between the filling tube and the nail. The surface of the rod has preferably been previously chemically or electrochemically etched, which has the effect of creating a micro-roughness and increasing the active surface area with the composite block, thus facilitating the passage of electrons.

[0045] The cross-section of the metal rod may have a larger diameter, for example greater than 1 mm and less than or equal to 5 mm, preferably ranging from 1.5 to 4 mm or from 2 to 3 mm. The metal rod is then referred to as a "pin". The larger diameter of the pin compared to that of the nail increases the active surface area with the composite block without requiring prior preparation of the pin's surface. The pin's surface can therefore be free of micro-roughness.

[0046] The power developed by two elements comprising a nail or a peg is equivalent despite different diameters of positive current collectors.

[0047] The use of a current collector in the form of a metal grid or a solid or perforated metal strip is excluded from the invention.

[0048] The current collector is inserted through the composite block or is placed in contact with an opening made through the block, this opening being either through or non-through. Excluded from the invention is the case of a current collector wound around the composite block.

[0049] The composite block can be in the form of a column with a circular or rectangular cross-section, or petal-shaped, i.e., with bulges around its periphery. The direct extrusion process for forming the composite block, without a subsequent block compression step, can result in a column with a petal-shaped cross-section. To maximize current collection, the length of the metal rod is generally chosen to be close to (i.e., at least 95%) the length of the column after it has swollen due to the impregnation of the block's pores by the electrolyte. However, the rod must not be longer than the column to avoid any risk of an internal short circuit. Fabrication of the positive electrode

[0050] Two embodiments will be described, the first consisting of forming grains from a composite mixture, generally by extrusion, and compressing these grains to form a block of agglomerated grains, the second consisting of forming a block directly by extrusion of the composite mixture without a block compression step. In this second embodiment, the block exiting the extruder is preformed and does not require a compression shaping step.

[0051] First embodiment:

[0052] In a first step a), a composite mixture is prepared by adding to a solvent or a mixture of several solvents, fluorinated carbon CFx, optionally one or more other positively charged active substances, one or more polymers, and optionally one or more electronically conductive compounds. The solvent may be aqueous or organic. The organic solvent is most often N-methyl-2-pyrrolidone (NMP). Said one or more solvents may be a mixture of water and isopropanol.

[0053] In the case of an aqueous solvent, said polymer(s) may be selected from polytetrafluoroethylene (PTFE), carboxymethylcellulose (CMC), a styrene-butadiene block copolymer (SBR), polyvinyl alcohol (PVA), and a mixture thereof. In the case of an organic solvent, said polymer(s) may be selected from a homopolymer or copolymer of polyvinylidene fluoride (PVDF), grafted or not, or a butadiene-acrylonitrile copolymer, optionally hydrogenated or carboxylated. The viscosity of the mixture is adjusted by varying the volume of the solvent(s).

[0054] In a second step b), the composite mixture is extruded. The viscosity of the mixture has been previously adjusted to facilitate its passage through the extruder. The extruder is equipped with a blade that cuts the extruded mixture to the desired length. Grains are obtained. Their length can vary from 0.1 to 1 cm or from 0.1 to 0.5 cm.

[0055] In a third step (c), one or more solvents are evaporated by heating the grains. Those skilled in the art know at what temperature the solvent(s) used begin to evaporate.

[0056] In a fourth step (d), the grains are heat-treated by heating them to a temperature at least equal to the glass transition temperature of the polymer with the highest glass transition temperature. The heat treatment temperature therefore depends on the nature of the polymer(s) used. It can be in the range of 100 to 350°C, 150 to 300°C, or 200 to 250°C. For example, it can be in the range of 100 to 150°C if the binder polymer is PVDF. The duration of the heat treatment can range from 30 minutes to 5 hours or from 45 minutes to 1.5 hours. The heat treatment can consist of heating at a temperature ranging from 100 to 350°C for a period of 45 minutes to 5 hours or heating at a temperature of approximately 300°C for approximately 1 hour.

[0057] Preferably, the heat treatment is carried out without compressing the grains. It causes the polymer(s) to become finer. This allows: - consolidate the three-dimensional porous network of the composite mixture formed by the particles of active material, said one or more polymers, and said one or more optional electronically conductive additives; - homogenize the spatial distribution of this porous network; - open up as many pores as possible to make them accessible as a reactive surface for discharge. Heat treatment is essential for achieving good element performance. It allows for better stability of the element's voltage response during discharge and a longer lifespan at rated voltage.

[0058] In a fifth step (e), grains are compressed in a mold to form a block made up of the agglomerated grains. The polymer-coated grains exhibit a certain elasticity. They contract and densify under pressure. The pressure applied can range from 1 to 200 bar, from 1 to 100 bar, or from 1 to 50 bar. Furthermore, an opening can be made through the block, either through or through.

[0059] The total porosity of the block obtained after compression can range from 30 to 90%, from 40 to 80%, or from 50 to 70%. Porosity is defined as the percentage of the pore volume relative to the geometric volume of the block. The pore volume includes the volume of the void space between the particles of the composite block and the volume of the pores within the particles of the composite block. The pores within the particles of the composite material include both accessible and inaccessible pores.

[0060] The total pore volume can be determined by the mercury porosimetry method. The dimensions of the block, and therefore its geometric volume, are known. The porosity is obtained by calculating the ratio between the total pore volume and the geometric volume of the block.

[0061] Knowledge of the percentage of CFx in the final block as well as the total mass of CFx in the volume of the block are important because, when related to the mass of lithium in the anode, they determine the final capacity of the element.

[0062] In a sixth step f), a current collector is placed on the block, the current collector being either inserted into the block, or disposed in contact with a wall of an opening made through the block.

[0063] Generally, between step e) and step f), the block is introduced into a container of the electrochemical element. Second method of implementation:

[0064] The first step a) is a step of preparing a composite mixture identical to that described in the first embodiment.

[0065] In a second step b), the composite mixture is extruded to form a cord or strand. The die opening may be circular, rectangular, square, oval, or any other shape. The shape and dimensions of the die opening are chosen so that the extruded cord has a circumference or perimeter that allows for its subsequent insertion into the opening of the element's container.

[0066] In a third step (c), said one or more solvents are evaporated by heating the bead. Those skilled in the art know at what temperature the solvent(s) used begin to evaporate.

[0067] In a fourth step (d), the cord is heat-treated by heating it to a temperature at least equal to the glass transition temperature of the polymer with the highest glass transition temperature. The duration and temperature of the heat treatment are identical to those described in the first embodiment.

[0068] In a fifth step (e), the cord is cut at predetermined intervals to obtain a plurality of blocks of a length adapted to the depth of the container and to the height of the lithium or lithium alloy foil attached to the inner face of the container. The choice of block dimensions also takes into account that the block's volume increases by 5 to 15% depending on its composition and initial porosity after impregnation with the electrolyte. A through or non-through opening may be made along the length of the block.

[0069] The porosity values ​​of the block obtained in this second embodiment can be found in the same ranges as those described for the first embodiment.

[0070] In a sixth step f), a current collector is placed on the block. The current collector is either inserted into the block or placed in contact with a wall of the opening made through the block.

[0071] Generally, between step e) and step f), the block is introduced into a container of the electrochemical element. Negative electrode

[0072] The inner face of the container is covered at least partially by a sheet of lithium or a lithium-based alloy.

[0073] According to one embodiment, the lithium or lithium-based alloy foil occupies at least 75%, preferably at least 95%, of the circumference of the container. Preferably, it occupies at least half of the internal height of the container, preferably at least 75%, and preferably again at least 95% of the internal height of the container.

[0074] According to one embodiment, the lithium or lithium-based alloy foil reaches 95% to 105% of the height of the electrochemical beam.

[0075] Generally, the capacitance of the negative electrode is greater than that of the positive electrode. The capacitance of the negative electrode can represent up to 110% of that of the positive electrode.

[0076] According to another embodiment, the lithium or lithium-based alloy foil completely covers the inner face of the container that is in contact with the electrochemical beam.

[0077] The foil may be made of pure lithium or a lithium-based alloy of formula LiM, in which M is selected from the group consisting of Mg, Al, Si, B, Ge, Ga, or a mixture of several of these. Preferably, M is Mg or Al. Those skilled in the art will choose the alloying element according to the environment in which the element is used, in particular its temperature. Preferably, the lithium foil is made of pure lithium.

[0078] The lithium or lithium-based alloy sheet can have a thickness of between 0.1 and 1.2 mm or between 0.2 and 1 mm or between 0.5 and 0.8 mm.

[0079] In one embodiment, the inner face of the container is used as a current collector. Separator

[0080] A separator is disposed between the negative electrode and the composite block. The separator material can be chosen from polyolefins, for example polypropylene, polyethylene, polyesters, polymer-bonded glass fibers, polyimides, polyamides, polyaramid, polyamideimide, para-aramids, and cellulose, or a mixture thereof. The polyester can be chosen from the following: Polyethylene phthalate (PET) and polybutylene terephthalate (PBT). Advantageously, polyester, polypropylene, or polyethylene contains or is coated with a material selected from the group consisting of a metal oxide, a carbide, a nitride, a boride, a silicide, and a sulfide. This material may be SiO2 or Al2O3.

[0081] Preferably, the chosen separator is composed of glass fibers bonded together by a polymer or of a porous polymer film. The polymers that can be used may be chosen from para-aramid, PEEK (polyetheretherketone), PPS (polyphenylene sulfide) or a mixture of one or more of these polymers with cellulose or PAN (polyacrylonitrile). Electrolyte

[0082] The electrolyte is a liquid organic electrolyte comprising: - one or more organic solvents chosen from among cyclic carbonates (propylene carbonate (PC), ethylene carbonate (EC)), linear carbonates (dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), the cyclic or linear carbonates possibly being fluorinated (monofluoroethyl carbonate (FEC)), ethers (dimethoxyethane, furan, tetrahydrofuran) and their fluorinated derivatives, lactones and ionic liquids. The ionic liquid(s) may represent from 20 to 80% of the volume of all solvents; - one or more lithium salts selected from the group consisting of lithium perchlorate LiC104, lithium hexafluorophosphate LiPF6, lithium tetrafluoroborate LiBF4, lithium hexafluoroarsenate LiAsF6, lithium hexafluoroantimonate LiSbF6, lithium trifluoromethanesulfonate LiCF3SO3, lithium bis(fluorosulfonyl)imidide Li(FSO2)2N (LiFSI), lithium bis(trifluoromethanesulfonyl)imidide LiN(CF3SO2)2 (LiTFSI), lithium tris(fluoromethanesulfonyl)methylide LiC(CF3SO2)3 (LiTFSM), lithium bis(pentafluoroethylsulfonyl)imidide LiN(C2F5SO2)2 (LiBETI), lithium 4,5-dicyano-2-(trifluoromethyl)imidazolide (LiTDI), the lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LIDFOB), lithium tris(pentafluoroethyl)trifluorophosphate LiPF3(CF2CF3)3 (LiFAP) and mixtures thereof; - Optionally, additives to improve the stability of the lithium passivation layer, such as vinylene carbonate (VC), LiPO2F2, or to capture water in the element, also known as "water scavengers". These additives are added at a mass percentage representing at most 10%, preferably at most 5%, of the electrolyte mass.

[0083] In one embodiment, the electrolyte solvent consists only of cyclic or linear carbonates. Manufacturing steps for the component

[0084] The manufacturing steps for the element include: - the plating of a lithium sheet or a lithium-based alloy against the inner face of the container, - the introduction of the separator into the container, - the introduction of the composite block consisting of a mixture comprising at least one compound of formula CFx, one or more polymers, and possibly one or more electronically conductive compounds, - in the embodiment illustrated in [Fig. 1], the lid is assembled onto the container before an electrical connection is made between the positive electrode and the positive current output terminal of the element: first, the lid fitted with the filling tube is welded, for example by laser, to the upper edge of the container, then the nail is inserted into the composite block and through the opening of the filling tube, or - in the embodiment illustrated in [Fig.2], an electrical connection is made between the positive electrode and the positive current output terminal of the element before the lid is assembled on the container: the pin is brought into contact with the opening of the composite block, the pin being integral with the glass-to-metal through-hole of the lid, then the lid is welded, for example by laser, to the upper edge of the container, - Filling the element with an electrolyte to saturate the positive and negative electrodes. Filling can be done either through the filling tube (12) visible in [Fig. 1], or through a filling hole (14) located on the lid, visible in [Fig. 2]. Filling can also be done from the bottom of the container. - the closure of the element. According to the embodiment illustrated in [Fig. 1], a weld, for example laser weld, is made between the top of the nail and the filling tube (12). According to the embodiment illustrated in [Fig. 2], the filling hole (14) is hermetically sealed by a stainless steel ball (15) by means of a weld, for example electric weld, of the ball onto the hole. EXAMPLES

[0085] Three primary Li-CFx cells of the invention, in AA format, were manufactured. The composite block of these cells consists of 87% by mass of CFx, 8% by mass of electronic conductive material, and 5% by mass of binder. They were discharged at 20°C at a current of 5 mA to a cutoff voltage of 2.0 V. The cells include a separator of glass fibers embedded in a polymer matrix. The voltage of the cells during discharge was measured and is shown in [Fig. 3]. The discharged capacities range from 1.22 to 1.26 Ah. This test shows that the new design of the positive electrode does not affect the performance of the element in discharge.

[0086] The performance of an element A according to the invention was compared to that of a primary element B of the Li-CFx type comprising a spiral mounting of the electrodes and to that of a primary element C of the Li-SOCl2 type.

[0087] [Tables 1] Technical Advantage Element Type User Safety in Case of Internal Short Circuit Passivation Resistance at Intermediate Temperature of 40-50°C Self-Discharge at Intermediate Temperature of 40-50°C Service Life for Meter Application A. Li-CFx with CFx Block Excellent Excellent Very Low Excellent B*. Li-CFx with Spiral Electrode Mounting Good Good Average Average C*. Li-SOCl2 Average Average Average Good * element outside the invention

[0088] In the event of an internal short circuit, element A, whose positive electrode is a CFx block, is the one that heats up the least. It therefore offers the best safety for a user.

[0089] Element C is a primary electrochemical element with a liquid cathode of the Li-SOC12 type. The positive electrode is a porous carbon mass with a large specific surface area, the pores of which contain SOC12. SOC12 constitutes both the electrolyte solvent and the positive electrode of the element. The negative electrode of this type of element is made of lithium. It is highly passivated at a temperature above ambient temperature. The passivation layer resists the passage of lithium ions during a discharge, resulting in a transient voltage drop at the beginning of the discharge. This problem no longer occurs for element A according to the invention.

[0090] Element A according to the invention is the one which has the lowest self-discharge and the longest service life.

[0091] If we compare the performance of a Li-CFx element according to the invention (A) comprising a CFx-based composite block with that of a Li-CFx element (B) comprising a spiral structure of its electrodes, it is observed that element A according to the invention surpasses element (B) in terms of safety, passivation, and self-discharge. This demonstrates the advantage of the CFx block structure compared to a spiral electrode arrangement.

Claims

Claims

1. Electrochemical element (1) comprising: - a container (2), - a negative electrode comprising a sheet (3) of lithium or a lithium-based alloy at least partially covering an internal face of the container, - a positive electrode comprising a block (4) consisting of a mixture comprising one or more compounds of formula CFX with 0 <x<l,5 et un ou plusieurs polymères, - un collecteur de courant (11) de l’électrode positive, le collecteur de courant étant soit au moins partiellement inséré dans le bloc, soit au moins partiellement disposé au contact d’une paroi d’une ouverture pratiquée à travers le bloc, - un séparateur (5) disposé entre l’électrode positive et l’électrode négative, et - un électrolyte (6).

2. The electrochemical element (1) of claim 1, wherein the mixture further comprises MnO2.

3. An electrochemical element (1) according to claim 1 or 2, wherein the container (2) is cylindrical and the lithium or lithium-based alloy sheet occupies at least 75%, preferably at least 95%, of the circumference of the container.

4. Electrochemical element (1) according to one of the preceding claims, in which 0.2 <x<l.

5. Electrochemical element (1) according to one of claims 1 to 4, further comprising a cover (7) having a wall through which a metal tube (12) is fixed, the metal tube being electrically insulated from the cover by an electrically insulating insert (13), the metal tube having a through opening, a first part of the current collector being inserted into the through opening of the metal tube, a second part of the current collector being inserted into the composite block, one end of the current collector (11) being welded to the metal tube (12) thus making the element watertight.

6. An electrochemical element (1) according to one of claims 1 to 4, wherein the block (4) is a cylindrical column and the opening made through the block is a through opening in the length direction of the cylindrical column.

7. Electrochemical element (1) according to claim 6, further comprising a cover (7) provided with a glass-metal feedthrough (13), a first part of the current collector being integral with the glass-metal feedthrough, a second part of the current collector being arranged in contact with the wall of the through opening of the block.

8. Electrochemical element (1) according to one of the preceding claims, in which the block (4) has a porosity ranging from 30 to 90%.

9. Electrochemical element (1) according to one of the preceding claims, in which the separator (5) comprises glass fibers or cellulose fibers or para-aramid fibers.

10. Electrochemical element (1) according to any one of the preceding claims, in which the electrolyte comprises a solvent chosen from cyclic or linear carbonates and lactones.

11. Electrochemical element (1) according to one of the preceding claims, in which said one or more polymers is chosen from a homopolymer or a copolymer of polyvinylidene fluoride (PVDF) grafted or not, a copolymer of butadiene-acrylonitrile (NBR) optionally hydrogenated or carboxylated and a mixture thereof.

12. Electrochemical element (1) according to one of claims 1 to 10, wherein said one or more polymers is chosen from polytetrafluoroethylene (PTFE), carboxymethylcellulose (CMC), a styrene and butadiene block copolymer (SBR), a polyvinyl alcohol (PVA) and a mixture thereof.

13. Electrochemical element according to one of the preceding claims, in which the positive electrode further contains one or more electronically conductive compounds.

14. A method of manufacturing a positive electrode (4) for a Li / CFx electrochemical cell (1), which method comprises the steps of: a) providing a mixture comprising one or more solvents, one or more compounds of formula CFx with 0 <x<l,5 et un ou plusieurs polymères, b) mise en forme du mélange par extrusion pour former des grains, c) évaporation du ou des solvants par chauffage des grains, d) traitement thermique des grains à une température au moins égale à la température de transition vitreuse du polymère présentant la température de transition vitreuse la plus élevée, e) compression des grains dans un moule pour former un bloc (4) constitué des grains agglomérés, f) placing a current collector (11) on the block, the current collector being either at least partially inserted into the block or at least partially arranged in contact with a wall of an opening made through the block.

15. A method of manufacturing a positive electrode (4) for a Li / CFx electrochemical cell (1), which method comprises the steps of: a) providing a mixture comprising one or more solvents, one or more compounds of formula CFx with 0 <x<l,5 et un ou plusieurs polymères, b) mise en forme du mélange par extrusion pour former un bloc (4), c) évaporation du ou des solvants par chauffage du bloc, d) traitement thermique du bloc à une température au moins égale à la température de transition vitreuse du polymère présentant la température de transition vitreuse la plus élevée, e) mise en forme du bloc par coupure du bloc aux dimensions souhaitées, le procédé étant dépourvu d’une étape de compression du bloc, f) mise en place d’un collecteur de courant (11) sur le bloc, le collecteur de courant étant soit au moins partiellement inséré dans le bloc, soit au moins partiellement disposé au contact d’une paroi d’une ouverture pratiquée à travers le bloc.

Citation Information

Patent Citations

  • Enhanced capacity Li / CFx electrochemical cell

    US6451483B1

  • Lithium bobbin cell with cathode using wrapped metal grid as current collector

    US20130236756A1

  • Battery for use with medical devices

    US20150221898A1